Water-based acrylic polyurethane topcoat for locomotive and rolling stock interior and its preparation method

By introducing fluorosilicone segments into water-based coatings and forming a cross-linked network, the problems of easy cleaning, water resistance, and weather resistance of interior coatings for locomotives and vehicles have been solved, achieving an environmentally friendly coating effect with low VOC emissions.

CN123107529APending Publication Date: 2026-11-17ZHUZHOU JIUHUA NEW MATERIAL COATING IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611438004.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing water-based coatings for the application of interior parts in locomotives and rolling stock have shortcomings in terms of stain resistance, ease of cleaning, weather resistance, and film hardness, making it difficult to meet the requirements for anti-graffiti performance and low VOC emissions.

Method used

A chemical grafting method is used to introduce fluorosilicone segments into the main chain of acrylic resin to form a self-assembled monomolecular fluorosilicone film. This film forms a dense cross-linked network with an isocyanate curing agent. Combined with an associative thickener and an anti-settling agent, a stable coating system is constructed.

Benefits of technology

It achieves coating performance with low surface energy, easy cleaning, water and chemical resistance, and strong adhesion, meeting the stringent requirements of locomotive and rolling stock interiors, while reducing VOC emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107529A_ABST
    Figure CN123107529A_ABST
Patent Text Reader

Abstract

This invention discloses a water-based acrylic polyurethane topcoat for locomotive and vehicle interiors and its preparation method, belonging to the field of coatings. The topcoat consists of a paint and a curing agent in a weight ratio of 3:1. The paint contains components such as a fluorosilicone-modified water-based acrylic dispersion; the curing agent contains isocyanate and an environmentally friendly solvent. The preparation method includes: hydrolyzing a perfluoroalkyltriethoxysilane to obtain a fluorosilicone hydrolysate, then grafting it with the water-based acrylic dispersion to obtain a modified dispersion, then combining it with pigments and fillers to obtain the paint, and finally mixing it with the curing agent. This paint forms a self-assembled fluorosilicone film layer through chemical bonding between silanol and the substrate, giving the coating extremely low surface energy, excellent hydrophobicity and antifouling properties, easy cleaning, weather resistance, water resistance, and strong adhesion, and low VOC emissions, making it suitable for locomotive and vehicle interiors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating technology, specifically to a water-based acrylic polyurethane topcoat for locomotive and vehicle interiors and its preparation method. Background Technology

[0002] With the increasing emphasis on environmental protection by the government, the coatings industry is gradually shifting from solvent-based coatings to water-based coatings. Water-based coatings use water as a diluent during application, using little or no organic solvents, significantly reducing VOC emissions during painting and improving the working environment for painting workers. In recent years, the coating industry in rail transit has also begun to move towards water-based solutions, especially in the painting of interior parts and cabinets. This requires the paint film to have excellent adhesion to various substrates, as well as excellent easy-to-clean and anti-graffiti properties (key performance indicators for exported models), and good water resistance, chemical resistance, and high film hardness.

[0003] Traditional solvent-based coatings have high VOC emissions during application and also release high levels of TVOCs long-term after film formation, negatively impacting the health of vehicle occupants. Furthermore, traditional coatings lack long-term easy-to-clean and anti-graffiti properties, failing to meet the coating process requirements for locomotive and vehicle interior parts. Existing water-based coatings still have certain shortcomings in terms of stain resistance, easy cleaning, weather resistance, and film hardness, particularly exhibiting issues such as increased surface energy and decreased anti-graffiti performance over long-term use.

[0004] Therefore, developing a water-based acrylic polyurethane topcoat with good adhesion to various substrates, low surface energy, anti-graffiti and easy cleaning, good water and chemical resistance, high film hardness, and low VOC emissions during construction is of great practical significance. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to provide a water-based acrylic polyurethane topcoat for locomotive and vehicle interiors and its preparation method. The topcoat should have excellent adhesion, low surface energy, easy cleaning and anti-graffiti performance, good water and chemical resistance and high film hardness, while having low VOC emissions during construction.

[0006] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: A water-based acrylic polyurethane topcoat for locomotive and rolling stock interiors, comprising separately packaged paint and curing agent, wherein the paint and curing agent are mixed in a weight ratio of 3:1 during use; The paint contains the following components by weight: 40-50 parts of fluorosilicone-modified waterborne acrylic dispersion, 0.5-0.8 parts of anti-settling agent, 3.0-4.0 parts of anionic polymer dispersant, 0.5-1.0 parts of nonionic surfactant, 0.2-0.3 parts of defoamer, 0.3-0.5 parts of wetting agent, 0.3-0.4 parts of leveling agent, 25-35 parts of pigments and fillers, 0.3-0.5 parts of associative thickener, 3.0-5.0 parts of cosolvent, and 6-10 parts of deionized water; The curing agent comprises the following components: isocyanate curing agent and environmentally friendly solvent, wherein the mass ratio of isocyanate curing agent to environmentally friendly solvent is (45-55):(45-55); The fluorosilicone-modified aqueous acrylic dispersion is a product of the condensation and grafting reaction of fluorosilicone hydrolysate and aqueous acrylic dispersion, wherein the fluorosilicone hydrolysate is a hydrolysate of perfluoroalkyltriethoxysilane, and the aqueous acrylic dispersion is an aqueous acrylic polyurethane copolymer dispersion.

[0007] Preferably, the paint comprises the following components by weight: 42-48 parts of fluorosilicone-modified waterborne acrylic dispersion, 0.6-0.7 parts of anti-settling agent, 3.2-3.8 parts of anionic polymer dispersant, 0.6-0.9 parts of nonionic surfactant, 0.22-0.28 parts of defoamer, 0.35-0.45 parts of wetting agent, 0.32-0.38 parts of leveling agent, 27-33 parts of pigments and fillers, 0.35-0.45 parts of associative thickener, 3.5-4.5 parts of cosolvent, and 7-9 parts of deionized water.

[0008] Preferably, in the curing agent, the mass ratio of the isocyanate curing agent to the environmentally friendly solvent is (48-52):(48-52); The fluorosilicone-modified aqueous acrylic dispersion is made from the following raw materials in parts by weight: 70-85 parts of aqueous acrylic dispersion, 3-8 parts of aqueous dispersant, and 15-25 parts of fluorosilicone hydrolysate. Preferably, the fluorosilicone-modified aqueous acrylic dispersion is made from the following raw materials in parts by weight: 72-82 parts of aqueous acrylic dispersion, 4-7 parts of aqueous dispersant, and 16-24 parts of fluorosilicone hydrolysate.

[0009] The fluorosilicone hydrolysate is prepared by hydrolyzing the following raw materials in parts by weight: 60-80 parts of perfluoroalkyltriethoxysilane, 10-30 parts of low-carbon alcohol, and 5-15 parts of water. Preferably, the fluorosilicone hydrolysate is prepared by hydrolyzing the following raw materials in parts by weight: 65-75 parts of perfluoroalkyltriethoxysilane, 15-25 parts of low-carbon alcohol, and 8-12 parts of water.

[0010] Preferably, the perfluoroalkyltriethoxysilane is selected from one or more of tridecafluorooctyltriethoxysilane, heptadecafluorodecyltriethoxysilane, and nonafluorohexyltriethoxysilane; more preferably, it is tridecafluorooctyltriethoxysilane and / or heptadecafluorodecyltriethoxysilane.

[0011] Preferably, the lower alcohol is selected from one or more of ethanol, propanol and isopropanol; more preferably, it is ethanol.

[0012] The preparation of the fluorosilicone-modified aqueous acrylic dispersion includes: adding the fluorosilicone hydrolysate dropwise to a mixture of aqueous acrylic dispersion and aqueous dispersant under stirring conditions, and reacting at 50-70°C for 2-4 hours to allow the silanol in the fluorosilicone hydrolysate to undergo a condensation grafting reaction with the polar groups in the aqueous acrylic dispersion. After the reaction is completed, the pH value is adjusted to 7-7.5 to obtain the final product.

[0013] The key feature of this invention is that it first hydrolyzes perfluoroalkyltriethoxysilane under specific pH conditions to form a fluorosilicone hydrolysate containing active silanols (Si-OH). This fluorosilicone hydrolysate is then added dropwise to a mixture of an aqueous acrylic dispersion and an aqueous dispersant under stirring. At 50–70°C, the active silanols in the fluorosilicone hydrolysate undergo a condensation grafting reaction with the polar groups such as hydroxyl and carboxyl groups on the molecular chain of the aqueous acrylic dispersion, forming stable chemical bonds and thus introducing fluorosilicone segments into the acrylic resin backbone. This chemical grafting method fundamentally avoids the phase separation problems that easily occur in physical blending, ensuring long-term storage stability.

[0014] Preferably, the aqueous acrylic dispersion is a hydroxyl-containing aqueous acrylic polyurethane copolymer dispersion with a solid content of 30%–50% and a hydroxyl content of 2.5%–4.0%; more preferably, the solid content is 35%–45% and the hydroxyl content is 3.0%–3.6%. Using the above-mentioned hydroxyl-containing aqueous acrylic polyurethane copolymer dispersion, the hydroxyl groups can crosslink with the -NCO groups in the isocyanate curing agent to form polyurethane bonds, creating a dense crosslinked network, thus improving the hardness, water resistance, chemical resistance, and weather resistance of the paint film. The solid content and hydroxyl content are within the above ranges, ensuring sufficient hydroxyl groups to participate in curing after the grafting reaction with the fluorosilicone hydrolysate, while avoiding excessively high hydroxyl content leading to a shortened pot life and increased film brittleness, or excessively low hydroxyl content leading to insufficient crosslinking density and decreased water and chemical resistance.

[0015] Preferably, the isocyanate curing agent is hexamethylene diisocyanate trimer, isophorone diisocyanate trimer, or a mixture thereof; the environmentally friendly solvent refers to an ester or alcohol ether solvent with low VOC content and free from benzene and ketone controlled solvents, preferably one or more of ethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, and diethylene glycol butyl ether acetate.

[0016] Preferably, the pigments and fillers are selected from one or more of titanium dioxide, barium sulfate, talc, mica powder, and calcium carbonate; the co-solvent is selected from one or more of dipropylene glycol butyl ether, propylene glycol methyl ether, dipropylene glycol methyl ether, and ethylene glycol butyl ether.

[0017] Preferably, the defoamer is a polysiloxane defoamer, the wetting agent is a polyether siloxane wetting agent, and the leveling agent is an acrylate leveling agent.

[0018] Preferably, the associative thickener is a hydrophobic modified polyurethane associative thickener, more preferably a polyethylene glycol-diisocyanate block polyurethane containing hydrophobic end groups, and more preferably a nonionic hydrophobic modified polyurethane block copolymer (HEUR).

[0019] The polyurethane associative thickener is a hydrophobic associative water-soluble polymer with a small number of hydrophobic groups on its hydrophilic macromolecular chains. In the polymer aqueous solution, the hydrophobic groups aggregate due to hydrophobic interactions, causing intramolecular and intermolecular associations in the macromolecular chains. Above the critical association concentration, a supramolecular structure dominated by intermolecular association is formed, increasing the hydrodynamic volume and thus exhibiting good thickening properties. Because the water-soluble chains of the associative thickener, which have relatively low molecular weights, contain two or more lipophilic groups, it exhibits surfactant behavior in water and can form micelles; however, the two lipophilic groups in the molecule are not necessarily in the same micelle, so they connect to form a structure. The lipophilic groups in the associative thickener can adsorb emulsion particles and pigment / filler particles, which further enhances the structure. The particles bridged by the thickener macromolecules form a physical network (crosslinked) structure, which can be gradually destroyed in a shear field, thus controlling the flow properties of the system. Such associations break down at high shear rates, reducing viscosity; after shear removal, they reform, restoring viscosity. However, the formation of association takes time, so the viscosity recovery is not as fast as that of cellulose-based thickeners, thus providing a certain flow time, which is beneficial for film leveling and anti-sagging. In the paint, the concentration of the associative thickener, as determined by the viscosity-concentration curve, is higher than its critical associative concentration, for example, the content is 0.3 to 0.5 parts.

[0020] Preferably, the anti-settling agent is bentonite. Bentonite is a layered silicate that forms a colloidal network upon contact with water, imparting thixotropic properties to the coating: it has a high viscosity when stationary, preventing pigment and filler sedimentation; the viscosity decreases during shearing, facilitating brushing or spraying; and the viscosity recovers after film formation, preventing sagging. The electrostatic repulsion generated by the charged particles and the network structure support the pigments / fillers, preventing delamination and clumping, ensuring color uniformity, and helping to reduce coating gloss and make the gloss more stable.

[0021] More preferably, the bentonite is sodium-modified bentonite. Sodium-modified bentonite is bentonite that has undergone sodium ion exchange treatment, exhibiting more significant thixotropic and thickening abilities, as well as good thermal and chemical stability, maintaining stable performance over a long period. It also possesses partial matting properties, which is beneficial for controlling the product's storage stability and gloss stability.

[0022] Preferably, the paint further comprises functional additives, which are selected from one or more of ultraviolet absorbers, hindered amine light stabilizers, and bactericides, and the amount of the functional additives added is 0.5% to 3.0% of the total weight of the paint.

[0023] The water-based acrylic polyurethane topcoat for locomotive interiors prepared by this invention has the following performance indicators after curing: static water contact angle ≥90°, cross-cut adhesion ≤1 grade, bending performance ≤5mm, cupping test ≥4mm, accelerated aging resistance under artificial climate for 1000h with a comprehensive rating ≤2 grade, water resistance at 40℃×48h without blistering, peeling, or obvious discoloration, and no exposure of the substrate after 25 cycles of methyl ethyl ketone wiping; the above properties are tested according to GB / T 9286, GB / T 1731, GB / T 9753, GB / T 1865, GB / T1733, and GB / T 23989 respectively.

[0024] The key feature of this invention is that it first hydrolyzes perfluoroalkyltriethoxysilane under specific pH conditions to form a fluorosilicone hydrolysate containing active silanols. This fluorosilicone hydrolysate is then added dropwise to a mixture of an aqueous acrylic dispersion and an aqueous dispersant under stirring. At 50–70°C, the active silanols in the fluorosilicone hydrolysate undergo a condensation grafting reaction with the polar groups such as hydroxyl and carboxyl groups on the molecular chain of the aqueous acrylic dispersion, forming stable chemical bonds and thus introducing fluorosilicone segments into the acrylic resin backbone. This chemical grafting method fundamentally avoids the phase separation problems that easily occur in physical blending, ensuring long-term storage stability.

[0025] The reactive silanols produced by the hydrolysis of fluorosilanes can chemically bond with hydroxyl, carboxyl, and oxygen-containing groups in many inorganic and organic substrates, forming self-assembled monomolecular fluorosilicone films on inorganic surfaces. This results in treated substrates with extremely low surface energy and very poor wettability, exhibiting excellent hydrophobic, oleophobic, and antifouling properties.

[0026] Fluorosilicone modified liquid is slowly added dropwise to waterborne acrylic polyurethane dispersion under the presence of an aqueous dispersant, causing a condensation grafting reaction between the silanol and the polar groups of the resin. Due to the low surface energy characteristics of the waterborne acrylic polyurethane dispersion modified by the fluorosilicone modified liquid, a monomolecular fluorosilicone film is formed on the coating surface, making the coating surface smooth to the touch and easy to clean.

[0027] This invention also provides a method for preparing the above-mentioned water-based acrylic polyurethane topcoat for locomotive and rolling stock interiors, comprising the following steps: Step S1: Preparation of fluorosilicone hydrolysate: Mix perfluoroalkyltriethoxysilane, low carbon alcohol and water, adjust the pH value to 4-5 with glacial acetic acid, and stir hydrolyze at 45-55℃ until the conductivity no longer changes. Step S2: Preparation of fluorosilicone modified waterborne acrylic dispersion: The fluorosilicone hydrolysate obtained in step S1 is added dropwise to a mixture of waterborne acrylic dispersion and waterborne dispersant under stirring conditions. The mixture is kept at 50-70℃ for 2-4 hours and the pH value is adjusted to 7-7.5 to obtain the fluorosilicone modified waterborne acrylic dispersion. Step S3: Preparation of paint: Deionized water, anionic polymer dispersant, anti-settling agent, nonionic surfactant, defoamer and pigments are dispersed at high speed and ground to a fineness of ≤20μm. Then, fluorosilicone modified waterborne acrylic dispersion, wetting agent, leveling agent, associative thickener and cosolvent are added, mixed and filtered to obtain the paint. Step S4: Prepare curing agent: Mix isocyanate curing agent with environmentally friendly solvent to obtain curing agent.

[0028] When using, mix the paint and hardener at a weight ratio of 3:1, and add deionized water to adjust the viscosity for application.

[0029] Preferably, in the preparation of the fluorosilicone-modified aqueous acrylic dispersion, the dropwise addition is completed within 0.5 to 1.5 hours, and after the dropwise addition is completed, the mixture is kept at 60°C for 3 to 4 hours, with a stirring speed of 500 to 800 rpm.

[0030] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: (1) Excellent storage stability. The present invention uses chemical grafting to graft fluorosilicone segments onto acrylic resin in a covalent manner, eliminating the risk of phase separation in physical blending; at the same time, sodium bentonite and polyurethane associative thickener synergistically construct a dual thickening system, so that the coating does not settle or clump during long-term storage; (2) Excellent hydrophobic, antifouling, and easy-to-clean properties. After the active silanol produced by the hydrolysis of fluorosilane is grafted onto the resin backbone, during the film-forming and curing process, the fluorosilicone segments migrate directionally to the coating surface and hydrolyze and crosslink with air, forming a self-assembled monomolecular fluorosilicone film layer in situ on the coating surface. This film layer endows the coating with extremely low surface energy and extremely poor wettability, with a static water contact angle ≥90°, giving the coating excellent hydrophobic, oleophobic, and antifouling properties, while also providing excellent smooth feel and easy cleaning. (3) Excellent weather resistance and water resistance. The acrylic resin grafted with fluorosilicone segments contains a large number of hydroxyl groups, which can undergo cross-linking reaction with isocyanate curing agents to form a dense urethane bond cross-linking network; combined with the high stability of the fluorocarbon bonds on the coating surface, the paint film can withstand artificial accelerated aging ≥1000h and water resistance (40℃) ≥48h, and can adapt to outdoor and humid and hot environments for a long time; (4) Strong adhesion and wide substrate adaptability. The active silanols produced by the hydrolysis of fluorosilanes, in addition to being grafted with acrylic resins, the unreacted silanols can chemically bond with the hydroxyl, carboxyl and oxygen-containing groups on the surface of various substrates such as carbon steel, aluminum alloy and fiberglass at the interface between the coating and the substrate, thereby significantly improving the adhesion between the paint film and inorganic / organic substrates, with cross-cut adhesion ≤ Grade 1; (5) Good construction adaptability and comprehensive performance. Thanks to the shear thinning and time-dependent recovery characteristics of the associative polyurethane thickener, the viscosity of the coating is reduced during construction and spraying, making it easy to atomize. After film formation, the viscosity recovers effectively to prevent sagging. The paint film has good flexibility, impact resistance and chemical resistance, which can meet the strict requirements of locomotive and vehicle interior coatings. (6) Green and environmentally friendly. The coating system is a water-based system with extremely low VOC content and good environmental performance. Attached Figure Description

[0031] Figure 1 This is a process flow diagram of the preparation method of the waterborne acrylic polyurethane topcoat of the present invention. The flow diagram includes the following steps: step S1 preparing fluorosilicone hydrolysate, step S2 preparing fluorosilicone modified waterborne acrylic dispersion, step S3 preparing paint, step S4 preparing curing agent, and step S5 mixing paint and curing agent for use. Detailed Implementation

[0032] To enable those skilled in the art to better understand the technical solution of the present invention, the present invention will be described in detail below. The description in this part is only exemplary and explanatory, and should not be used to limit the scope of protection of the present invention in any way.

[0033] refer to Figure 1 As shown, this embodiment provides a method for preparing a water-based acrylic polyurethane topcoat for locomotive interiors, comprising the following steps: Step S1: Preparation of fluorosilicone hydrolysate: Mix perfluoroalkyltriethoxysilane, low carbon alcohol and water, adjust the pH value to 4-5 with glacial acetic acid, and stir hydrolyze at 45-55℃ until the conductivity no longer changes. Step S2: Preparation of fluorosilicone modified waterborne acrylic dispersion: The fluorosilicone hydrolysate obtained in step S1 is added dropwise to a mixture of waterborne acrylic dispersion and waterborne dispersant under stirring conditions. The mixture is kept at 50-70℃ for 2-4 hours and the pH value is adjusted to 7-7.5 to obtain the fluorosilicone modified waterborne acrylic dispersion. Step S3: Preparation of paint: Deionized water, anionic polymer dispersant, anti-settling agent, nonionic surfactant, defoamer and pigments are dispersed at high speed and ground to a fineness of ≤20μm. Then, fluorosilicone modified waterborne acrylic dispersion, wetting agent, leveling agent, associative thickener and cosolvent are added, mixed and filtered to obtain the paint. Step S4: Prepare curing agent: Mix isocyanate curing agent with environmentally friendly solvent to obtain curing agent.

[0034] When using, mix the paint and hardener at a weight ratio of 3:1, and add deionized water to adjust the viscosity for application.

[0035] The water-based acrylic polyurethane topcoat for locomotive interiors prepared by this invention has the following performance indicators after curing: static water contact angle ≥90°, cross-cut adhesion ≤1 grade, bending performance ≤5mm, cupping test ≥4mm, accelerated aging resistance to artificial climate for 1000h with a comprehensive rating ≤2 grade, water resistance at 40℃×48h without blistering, peeling, or obvious discoloration, and no exposure of the substrate after 25 repeated wipings with methyl ethyl ketone.

[0036] Raw materials and mechanism description: In this invention, the anti-settling agent is preferably bentonite, more preferably sodium bentonite. Bentonite, as an anti-settling agent, has significant thixotropic and thickening properties. It forms a colloidal network upon contact with water, exhibiting high viscosity to prevent settling when stationary, decreasing viscosity for easy application during shearing, and recovering viscosity after film formation to prevent sagging. The electrostatic repulsion generated by charged particles and the network structure support pigments / fillers, preventing delamination and clumping, ensuring uniform color, and simultaneously reducing coating gloss for greater gloss stability. Sodium bentonite possesses good thermal and chemical stability, maintaining stable performance over a long period, while also exhibiting partial matting properties, resulting in good storage and gloss stability of the product.

[0037] Polyurethane associative thickeners, due to their unique hydrophobic association mechanism, provide medium-to-low shear viscosity to ensure anti-settling properties. Simultaneously, their viscosity decreases under high shear, recovers after shear removal with a certain time delay, and this recovery provides a perfect balance for coatings, offering easy atomization during application, anti-sagging properties after application, and good leveling. The silanols generated from the hydrolysis of fluorosilanes are grafted onto the acrylic resin chains. During film formation, cross-linking reactions occur between the silanol groups and with the active groups on the substrate surface. Simultaneously, fluorocarbon segments accumulate on the surface, forming a self-assembled arrangement, which is key to achieving low surface energy antifouling in this invention.

[0038] The present invention will be further described in detail below with reference to the embodiments. In the following embodiments, all raw materials used are commercially available products unless otherwise stated, such as: J&Y 3213 tridecafluorooctyltriethoxysilane, Shanghai Jianyi Synthetic Chemical Co., Ltd.; Clayminton LB bentonite, Zhejiang Chang'an Renheng Technology Co., Ltd.; aqueous dispersant lucramul Wns, und Käll, Germany; aqueous dispersant BYK-190, manufactured by BYK AG, Germany; anionic polymer dispersant, manufactured by TEGO, Germany; nonionic surfactant, manufactured by Evonik Specialty Chemicals GmbH, Germany; polysiloxane defoamer, manufactured by BYK, Germany; polyether siloxane wetting agent, manufactured by TEGO, Germany; Vesmody® U905 polyurethane associative thickener, produced by Wanhua Chemical Group Co., Ltd., China; acrylate leveling agent, produced by BYK GmbH, Germany; cosolvent, produced by Shanghai Tikham Industrial Co., Ltd.; titanium dioxide, produced by DuPont, USA; deionized water, self-made; isocyanate curing agent HT-100, produced by Wanhua Chemical Group Co., Ltd., China; propylene glycol methyl ether, produced by Shanghai Tikham Industrial Co., Ltd.

[0039] Preparation Example 1: Fluorosilicone Hydrolysate A1 70 parts by weight of tridecafluorooctyltriethoxysilane, 20 parts by weight of ethanol, and 10 parts by weight of deionized water were mixed, and the pH was adjusted to 4.5 with glacial acetic acid. The mixture was stirred and hydrolyzed at 50°C for 3 hours. The conductivity of the system was found to no longer change, and the fluorosilicone hydrolysate A1 was obtained.

[0040] Preparation Example 2: Fluorosilicone Hydrolysate A2 75 parts by weight of heptadecafluorodecyltriethoxysilane, 15 parts by weight of isopropanol, and 10 parts by weight of deionized water were mixed, and the pH was adjusted to 4.5 with glacial acetic acid. The mixture was stirred and hydrolyzed at 55°C for 2.5 hours to obtain fluorosilicone hydrolysate A2.

[0041] Preparation Example 3: Fluorosilicone Hydrolysate A3 Mix 65 parts by weight of nonafluorohexyltriethoxysilane, 25 parts by weight of propanol, and 10 parts by weight of deionized water, adjust the pH to 5.0 with glacial acetic acid, and stir and hydrolyze at 45°C for 3 hours to obtain fluorosilicone hydrolysate A3.

[0042] Preparation Example 4: Fluorosilicone-modified aqueous acrylic dispersion B1 80 parts by weight of hydroxyl-containing waterborne acrylic polyurethane copolymer dispersion (solid content 45%, hydroxyl content 3.2%) were mixed with 5 parts by weight of waterborne dispersant BYK-190. Under stirring at 600 rpm, 20 parts by weight of fluorosilicone hydrolysate A1 were added dropwise over 1 hour. The mixture was heated to 60°C and kept at that temperature for 3 hours. The pH was adjusted to 7.2 with triethylamine to obtain fluorosilicone-modified waterborne acrylic dispersion B1.

[0043] Infrared spectroscopy analysis was performed on the grafted product B1, with values ​​ranging from 1000 to 1100 cm⁻¹. -1 Characteristic absorption peaks of Si-OC bonds appear at 1100–1250 cm⁻¹. -1 The presence of a characteristic absorption peak for CF bonds indicates that the fluorosilicone segment has been chemically grafted onto the acrylic polyurethane molecular chain. Simultaneously, the hydroxyl content before and after grafting was determined by chemical titration. The hydroxyl content decreased from 3.2% to 2.7% after grafting, further demonstrating that a condensation grafting reaction occurred between the silanol and the hydroxyl group.

[0044] Preparation Example 5: Fluorosilicone-modified aqueous acrylic dispersion B2 Following the method of Preparation Example 4, the fluorosilicone hydrolysate A1 was replaced with A2 to obtain the fluorosilicone-modified aqueous acrylic dispersion B2.

[0045] Preparation Example 6: Fluorosilicone-modified aqueous acrylic dispersion B3 Following the method of Preparation Example 4, the fluorosilicone hydrolysate A1 was replaced with A3 to obtain the fluorosilicone-modified aqueous acrylic dispersion B3.

[0046] Comparative preparation example: Waterborne acrylic dispersion B0 without fluorosilicone modification A hydroxyl-containing waterborne acrylic polyurethane copolymer dispersion (45% solids content, 3.2% hydroxyl content) was used directly as a comparison.

[0047] Example 1 Paint formulation (parts by weight): 45 parts of fluorosilicone modified waterborne acrylic dispersion B1; 0.6 parts of sodium bentonite; 3.5 parts of anionic polymer dispersant; 0.8 parts of nonionic surfactant; 0.25 parts of polysiloxane defoamer; 0.4 parts of polyether siloxane wetting agent; 0.35 parts of acrylate leveling agent; 30 parts of pigments and fillers (15 parts of titanium dioxide, 10 parts of barium sulfate, and 5 parts of talc); 0.4 parts of polyurethane associative thickener; 4 parts of cosolvent (2 parts of dipropylene glycol butyl ether and 2 parts of propylene glycol methyl ether); 8 parts of deionized water; 1 part of functional additives (0.5 parts of ultraviolet absorber and 0.5 parts of hindered amine light stabilizer).

[0048] Paint preparation: Deionized water, anionic polymer dispersant, sodium bentonite, nonionic surfactant, defoamer and pigments are dispersed at high speed and ground to a fineness of ≤20μm. Then, fluorosilicone modified waterborne acrylic dispersion B1, wetting agent, leveling agent, associative thickener and cosolvent are added, mixed evenly and filtered.

[0049] Curing agent formulation (parts by weight): 50 parts hexamethylene diisocyanate trimer, 50 parts propylene glycol methyl ether acetate, mixed evenly.

[0050] When using, mix the paint and hardener at a weight ratio of 3:1, add an appropriate amount of deionized water to adjust to the spraying viscosity, spray it onto the phosphated tinplate, level it at room temperature, and bake it at 80℃ for 30 minutes to obtain the coating film.

[0051] Example 2 The difference from Example 1 is that the fluorosilicone-modified waterborne acrylic dispersion B1 is replaced with B2, otherwise it is the same as Example 1.

[0052] Example 3 The difference from Example 1 is that the fluorosilicone-modified aqueous acrylic dispersion B1 is replaced with B3, and the cosolvent is adjusted to 3 parts dipropylene glycol methyl ether and 1 part ethylene glycol butyl ether, while the rest is the same as in Example 1.

[0053] Comparative Example 1 The difference from Example 1 is that the fluorosilicone-modified waterborne acrylic dispersion B1 is replaced with the unmodified fluorosilicone-modified waterborne acrylic dispersion B0, otherwise the same as in Example 1.

[0054] Comparative Example 2: Physical Blending Comparison The difference from Example 1 is that the fluorosilicone-modified aqueous acrylic dispersion B1 is replaced with a physically blended dispersion B0': 20 parts by weight of fluorosilicone hydrolysate A1, 80 parts by weight of hydroxyl-containing aqueous acrylic polyurethane copolymer dispersion (solid content 45%, hydroxyl content 3.2%), and 5 parts by weight of aqueous dispersant BYK-190 are directly mixed evenly and stirred at 600 rpm for 1 hour without thermal grafting reaction. The pH is adjusted to 7.2 with triethylamine to obtain the physically blended dispersion B0'. The rest is the same as in Example 1.

[0055] Tests: static water contact angle, contact angle retention rate after 7 days of storage at 50℃, water resistance at 40℃ for 48 hours, and 25 cycles of methyl ethyl ketone (MEK) wiping.

[0056] Comparative Example 3: Gradient of Fluorosilicone Hydrolysate Dosage Comparative Example 3-1: The difference from Preparation Example 4 is that the amount of fluorosilicone hydrolysate A1 was changed from 20 parts by weight to 5 parts by weight, and the rest was the same as in Preparation Example 4, to obtain fluorosilicone modified waterborne acrylic dispersion B1-5; paint and film were prepared according to Example 1.

[0057] Comparative Example 3-2: The difference from Preparation Example 4 is that the amount of fluorosilicone hydrolysate A1 was changed from 20 parts by weight to 35 parts by weight, and the rest is the same as Preparation Example 4, to obtain fluorosilicone modified waterborne acrylic dispersion B1-35; paint and film were prepared according to Example 1.

[0058] Tests: Static water contact angle, cross-cut adhesion, flexural properties, cupping test, appearance and viscosity changes after 7 days of storage at 50°C.

[0059] Comparative Example 4: Comparison of Hydrolysis pH Values Comparative Example 4-1: The difference from Preparation Example 1 is that the pH was adjusted to 3 with glacial acetic acid, and the rest was the same as Preparation Example 1 to obtain fluorosilicone hydrolysate A1-pH3; then grafting was performed according to Preparation Example 4 to obtain fluorosilicone modified waterborne acrylic dispersion B1-pH3; paint and film were prepared according to Example 1.

[0060] Comparative Example 4-2: The difference from Preparation Example 1 is that the pH was adjusted to 6 with glacial acetic acid, and the rest was the same as Preparation Example 1 to obtain fluorosilicone hydrolysate A1-pH6; then grafting was performed according to Preparation Example 4 to obtain fluorosilicone modified waterborne acrylic dispersion B1-pH6; paint and film were prepared according to Example 1.

[0061] Tests: hydrolysate conductivity stabilization time, graft product appearance, coating static water contact angle, and water resistance at 40℃ for 48 hours.

[0062] Comparative Example 5: Grafting Temperature Comparison Comparative Example 5-1: The difference from Preparation Example 4 is that the heat preservation temperature was changed from 60℃ to 40℃, and the rest is the same as Preparation Example 4, to obtain fluorosilicone modified waterborne acrylic dispersion B1-40; paint and film were prepared according to Example 1.

[0063] Comparative Example 5-2: The difference from Preparation Example 4 is that the heat preservation temperature was changed from 60℃ to 80℃, and the rest is the same as Preparation Example 4, to obtain fluorosilicone modified waterborne acrylic dispersion B1-80; paint and film were prepared according to Example 1.

[0064] Tests: Hydroxyl content before and after grafting (chemical titration), static water contact angle of coating, water resistance at 40℃ for 48 hours, methyl ethyl ketone (MEK) wiping 25 times, cross-cut adhesion, and bending performance.

[0065] Comparative Example 6: Comparison of Thickening Systems Comparative Example 6-1: The difference from Example 1 is that 0.6 parts by weight of sodium bentonite was replaced with 0.6 parts by weight of ordinary bentonite, and the rest is the same as in Example 1.

[0066] Comparative Example 6-2: The difference from Example 1 is that 0.4 parts by weight of polyurethane associative thickener was replaced with 0.4 parts by weight of hydroxyethyl cellulose, and the rest is the same as in Example 1.

[0067] Tests included: sedimentation at 50℃ for 7 and 30 days, flowability, leveling, static water contact angle, water resistance at 40℃ for 48 hours, and 25 cycles of methyl ethyl ketone (MEK) wiping.

[0068] Performance testing: The coatings prepared in Examples 1-3 and Comparative Example 1 were subjected to performance tests, and the results are shown in Table 1.

[0069] Table 1 Performance Test Results

[0070] The above performance indicators were tested according to the following standards: cross-cut adhesion according to GB / T 9286, flexural properties according to GB / T1731, cupping test according to GB / T 9753, accelerated aging resistance according to artificial weathering according to GB / T 1865, water resistance according to GB / T 1733, and methyl ethyl ketone (MEK) wiping test according to GB / T 23989.

[0071] Table 1 shows that Comparative Example 1, without fluorosilicone chemical modification, had a static water contact angle of only 68°, blistered after 40℃×48h of water resistance, and showed the substrate after wiping with methyl ethyl ketone (MEK). Its overall rating for 1000h of artificial aging was 3, indicating that the surface energy, cross-linking network, and chemical resistance were insufficient without grafted fluorosilicone segments. Examples 1-3, using fluorosilicone hydrolysate and aqueous acrylic dispersion condensation grafting, achieved contact angles of 105°, 108°, and 102° respectively, all ≥90°. Examples 1-2 were rated 0, and Example 3 was rated 1, both ≤1. The bending diameter was 2-4mm, and the cupping diameter was 4.8-5.5mm, indicating good flexibility. The 1000h artificial aging resistance was rated 1-2, with no change / virtually no change in water resistance, and no substrate exposure after 25 repeated wipings with MEK. Among them, Example 2 uses heptadecafluorodecyltriethoxysilane, which has the highest contact angle and the best water resistance; Example 1 has balanced overall performance; Example 3 uses nonafluorohexyltriethoxysilane, and its performance still meets the requirements. It can be seen that this invention, through chemical grafting of fluorosilicone segments, forms a self-assembled monomolecular fluorosilicone film on the coating surface, and then cures it with isocyanate to form a polyurethane crosslinking network. This significantly improves the low surface energy, anti-graffiti and easy-to-clean properties, water and chemical resistance, and aging resistance, while maintaining adhesion and flexibility, meeting the requirements for interior paints in locomotives and vehicles.

[0072] Table 2. Performance test results of Example 1 and Comparative Examples 1-3

[0073] Table 3. Performance test results of Example 1, Comparative Example 1 and Comparative Examples 4-5

[0074] Table 4. Performance test results of Example 1 and Comparative Example 6

[0075] As shown in Tables 2-4, Comparative Example 2, using physical blending, initially achieved a contact angle of 96°, but after 7 days of storage at 50°C, the contact angle dropped to 82°, with a contact angle retention rate of only 85%. Slight bubbling occurred during water resistance at 40°C for 48 hours, and slight exposure of the substrate was observed at the edges after wiping with methyl ethyl ketone (MEK). In contrast, Example 1, after chemical grafting, achieved a contact angle retention rate as high as 98%, with no change in water resistance, and no exposure of the substrate after 25 MEK cycles. This indicates that chemical grafting effectively avoids phase separation in physical blending and maintains low surface energy over a long period. Comparative Example 3-1 used too little fluorosilicone hydrolysate, resulting in a contact angle of only 85° and insufficient antifouling performance. Comparative Example 3-2 used too much, resulting in a higher contact angle but also thickening during storage and difficulty in filtration. Comparative Examples 4-1 and 4-2 exhibited hydrolysis pH deviations from 4-5, prolonged hydrolysis conductivity stabilization time, gel particles or stratification of the grafted product, and a decrease in the contact angle of the coating. Comparative Example 5-1 showed that the grafting temperature was too low, resulting in a decrease of only 0.15 percentage points in hydroxyl groups, insufficient grafting rate, and a contact angle of only 88°. Comparative Example 5-2 showed that the temperature was too high, leading to the appearance of particles and microgels in the dispersion, and slight whitening of the coating film due to water resistance issues. Comparative Example 6-1 showed that after replacing sodium bentonite with ordinary bentonite, significant sedimentation occurred after 7 days of storage, resulting in substandard flow performance. Comparative Example 6-2 showed that after replacing the associative thickener with cellulose thickener, although storage was stable, the leveling was poor and brush marks were present. Therefore, this invention, through chemical grafting of fluorosilicone segments and the use of a dual thickening system of sodium bentonite and polyurethane associative thickener, can achieve a balance of low surface energy, water and methyl ethyl ketone (MEK) resistance, storage stability, and application leveling properties under conditions of 50–70°C, pH 4–5, and 15–25 parts of fluorosilicone hydrolysate, meeting the requirements for interior paints for locomotives and vehicles.

[0076] The above description is merely a preferred embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention specification, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.

Claims

1. A water-based acrylic polyurethane topcoat for locomotive and rolling stock interiors, characterized in that, It includes separately packaged paint and hardener, and the paint and hardener are mixed at a weight ratio of 3:1 when used; The paint contains the following components by weight: 40-50 parts of fluorosilicone-modified waterborne acrylic dispersion, 0.5-0.8 parts of anti-settling agent, 3.0-4.0 parts of anionic polymer dispersant, 0.5-1.0 parts of nonionic surfactant, 0.2-0.3 parts of defoamer, 0.3-0.5 parts of wetting agent, 0.3-0.4 parts of leveling agent, 25-35 parts of pigments and fillers, 0.3-0.5 parts of associative thickener, 3.0-5.0 parts of cosolvent, and 6-10 parts of deionized water; The curing agent comprises the following components: isocyanate curing agent and environmentally friendly solvent, wherein the mass ratio of isocyanate curing agent to environmentally friendly solvent is (45-55):(45-55); The fluorosilicone-modified aqueous acrylic dispersion is a product of the condensation and grafting reaction of fluorosilicone hydrolysate and aqueous acrylic dispersion, wherein the fluorosilicone hydrolysate is a hydrolysate of perfluoroalkyltriethoxysilane, and the aqueous acrylic dispersion is an aqueous acrylic polyurethane copolymer dispersion.

2. The waterborne acrylic polyurethane topcoat according to claim 1, characterized in that, The aqueous acrylic dispersion is a hydroxyl-containing aqueous acrylic polyurethane copolymer dispersion with a solid content of 30% to 50% and a hydroxyl content of 2.5% to 4.0%.

3. The waterborne acrylic polyurethane topcoat according to claim 1, characterized in that, The isocyanate curing agent, environmentally friendly solvent, pigments, fillers, and co-solvents meet at least one of the following conditions: The isocyanate curing agent is hexamethylene diisocyanate trimer, isophorone diisocyanate trimer, or a mixture thereof; The environmentally friendly solvent is one or more of ethylene glycol butyl ether acetate, propylene glycol methyl ether acetate, and diethylene glycol butyl ether acetate; The pigments and fillers are selected from one or more of titanium dioxide, barium sulfate, talc, mica powder, and calcium carbonate; The co-solvent is selected from one or more of dipropylene glycol butyl ether, propylene glycol methyl ether, dipropylene glycol methyl ether, and ethylene glycol butyl ether.

4. The waterborne acrylic polyurethane topcoat according to claim 1, characterized in that, The anti-settling agent is bentonite, the defoamer is a polysiloxane defoamer, the wetting agent is a polyether siloxane wetting agent, the leveling agent is an acrylate leveling agent, and the associative thickener is a hydrophobically modified polyurethane associative thickener.

5. The waterborne acrylic polyurethane topcoat according to claim 4, characterized in that, The anti-settling agent is sodium bentonite, and the associative thickener is polyethylene glycol-diisocyanate block polyurethane or nonionic hydrophobic modified polyurethane block copolymer containing hydrophobic end groups.

6. The waterborne acrylic polyurethane topcoat according to claim 1, characterized in that, In the paint, the concentration of the associative thickener is higher than its critical associative concentration; and / or, the associative thickener is a hydrophobically modified polyurethane associative thickener with two or more oleophilic groups on its molecular chain.

7. The waterborne acrylic polyurethane topcoat according to claim 1, characterized in that, The paint also contains functional additives, which are selected from one or more of ultraviolet absorbers, hindered amine light stabilizers, and bactericides. The amount of the functional additives added is 0.5% to 3.0% of the total weight of the paint.

8. The waterborne acrylic polyurethane topcoat according to claim 1, characterized in that, The cured coating meets the following performance indicators: static water contact angle ≥90°, cross-cut adhesion ≤1 grade, bending performance ≤5mm, cupping test ≥4mm, artificial weathering accelerated aging resistance ≤2 grade after 1000h, water resistance at 40℃×48h without blistering, peeling, or obvious discoloration, and no exposure of the substrate after 25 cycles of methyl ethyl ketone wiping.

9. A method for preparing the waterborne acrylic polyurethane topcoat according to any one of claims 1 to 6, characterized in that, Includes the following steps: Step S1: Preparation of fluorosilicone hydrolysate: Mix perfluoroalkyltriethoxysilane, low carbon alcohol and water, adjust the pH value to 4-5 with glacial acetic acid, and stir hydrolyze at 45-55℃ until the conductivity no longer changes. Step S2: Preparation of fluorosilicone-modified aqueous acrylic dispersion: The fluorosilicone hydrolysate obtained in step S1 is added dropwise to a mixture of aqueous acrylic dispersion and aqueous dispersant under stirring. The mixture is kept at 50-70°C for 2-4 hours to allow the silanol in the fluorosilicone hydrolysate to undergo a condensation grafting reaction with the polar groups in the aqueous acrylic dispersion. After the reaction is completed, the pH value is adjusted to 7-7.5 to obtain the fluorosilicone-modified aqueous acrylic dispersion. Step S3: Preparation of paint: Deionized water, anionic polymer dispersant, anti-settling agent, nonionic surfactant, defoamer and pigments are dispersed at high speed and ground to a fineness of ≤20μm. Then, fluorosilicone modified waterborne acrylic dispersion, wetting agent, leveling agent, associative thickener and cosolvent are added, mixed and filtered to obtain the paint. Step S4: Prepare curing agent: Mix isocyanate curing agent with environmentally friendly solvent to obtain curing agent.

10. The method for preparing the waterborne acrylic polyurethane topcoat according to claim 9, characterized in that, In step S2, the dripping is completed within 0.5 to 1.5 hours. After the dripping is completed, the mixture is kept at 60°C for 3 to 4 hours and the stirring speed is 500 to 800 rpm.