A high-temperature resistant and waterproof coating for enameled copper flat wire and its preparation method
By introducing cross-linked networks and functionalized nanosphere structures into the enameled copper flat wire coating, the problems of interfacial water absorption and decreased adhesion of the coating in humid and hot environments and thermal cycling processes were solved, achieving the stability and waterproofness of the coating at high temperatures.
Patent Information
- Application Number
- CN202611319694.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing enameled copper flat wire coatings are prone to problems such as interface water absorption, decreased adhesion, decreased mechanical strength, and deterioration of insulation performance in humid and hot environments and during thermal cycling.
The material employs carboxyl-terminated polyamide-imide resin, copper-affinity bisbenzoxazine, amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres, and triglycidyl isocyanurate, among other components. Through cross-linking network and nanosphere structure design, a dense cross-linked coating is formed to improve interfacial bonding strength and water resistance.
Under high temperature conditions, the bonding strength between the coating and the copper conductor is improved, inhibiting interface debonding, reducing interface water absorption, maintaining good adhesion and insulation properties, preventing coating cracking, and exhibiting good high-temperature adhesion stability and waterproof performance.
Abstract
Description
Technical Field
[0001] This invention relates to the field of paint technology, and in particular to a high-temperature resistant and waterproof paint for enameled copper flat wire and its preparation method. Background Technology
[0002] Enameled copper flat wire can achieve a high conductor fill rate within a limited slot space, making it suitable for motor windings, transformer windings, and other electrical equipment requiring high power density. Compared to round wire, copper flat wire has regions with different curvatures, such as the plane, rounded corners, and side surfaces. During continuous coating, bending, and thermal cycling, local stress concentration is more likely to occur in the rounded corner areas and the plane-rounded corner transition areas.
[0003] Polyamide-imide possesses good high-temperature resistance, mechanical properties, and electrical insulation properties, and has been used in enameled wire insulation varnishes. However, polyamide-imide molecules contain amide bonds, imide bonds, and other polar structures. Under long-term humid and hot conditions, moisture can gradually enter the coating through free volume, filler interfaces, and microcracks, and may diffuse along the copper-coating interface.
[0004] Traditional methods for improving water resistance typically involve adding silicone resins, fluorinated additives, or ordinary hydrophobic particles to the paint. Low-molecular-weight hydrophobic additives are prone to migration, volatilization, or the formation of weak boundary layers at the interface during high-temperature baking and long-term use. Solid inorganic particles and polymers have a significant modulus difference, and excessive addition can easily cause coating embrittlement, particle agglomeration, and cracking of the coating in rounded corner areas.
[0005] Therefore, there is a need to develop a high-temperature resistant waterproof paint that can simultaneously control moisture penetration at the copper-coating interface and thermal stress cracking of the coating itself. Summary of the Invention
[0006] The purpose of this invention is to provide a high-temperature resistant and waterproof coating for enameled copper flat wire and its preparation method, so as to solve the problems that existing high-temperature resistant enameled wire coatings are prone to interfacial water absorption, decreased adhesion, decreased mechanical strength and decreased insulation performance in humid and hot environments and thermal cycling processes.
[0007] A high-temperature resistant and waterproof coating for enameled copper flat wire comprises, by weight, the following components: 100-120 parts of carboxyl-terminated polyamide-imide resin, 4-8 parts of copper-affinity bisbenzoxazine, 1.5-2.2 parts of amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres, 2-3.5 parts of triglycidyl isocyanate, 0.05-0.15 parts of curing catalyst, 0.05-0.15 parts of leveling agent, 0.02-0.08 parts of defoamer, and 250-280 parts of organic solvent; The copper-affinity bisbenzoxazine is prepared by a condensation reaction of 4,4′-dihydroxydiphenyl ether, 5-aminobenzotriazole and paraformaldehyde in a molar ratio of 1:(1.95~2.1):(3.9~4.3); The ammonium acid-grafted phenylsiloxane-coated hollow silica nanospheres include an internal hollow silica nanosphere, a phenylsiloxane sealing layer disposed outside the hollow silica nanosphere, and trimellitic acid ammonium acid groups grafted onto the surface of the phenylsiloxane sealing layer.
[0008] Furthermore, the curing catalyst is triphenylphosphine.
[0009] Furthermore, the leveling agent is a polyether-modified polysiloxane leveling agent; the defoamer is an organosilicone defoamer.
[0010] Furthermore, the organic solvent is composed of N-methylpyrrolidone and γ-butyrolactone in a mass ratio of 1:(0.4 to 1.0).
[0011] A method for preparing a high-temperature resistant and waterproof coating for enameled copper flat wire includes the following steps: S1: Preparation of copper-affinity bisbenzoxazine; S2: Preparation of hollow silica nanospheres coated with ammonium acid grafted with phenylsiloxane; S3: Blending of paints.
[0012] Furthermore, the preparation of copper-affinity bisbenzoxazine in step S1 specifically includes the following steps: S1.1: Add 4,4′-dihydroxydiphenyl ether and paraformaldehyde to a container. The molar ratio of formaldehyde structural units in 4,4′-dihydroxydiphenyl ether and paraformaldehyde is 1:(3.9-4.3). Add a mixed solvent of 4 to 7 times the total mass of the reactants and stir until homogeneous. The mixed solvent is composed of 1,4-dioxane and toluene in a volume ratio of 1:(0.8-1.2) to obtain a pre-reaction solution. S1.2: Dissolve 5-aminobenzotriazole in N,N-dimethylformamide at a mass ratio of 1:(3-4) to obtain a 5-aminobenzotriazole solution. Under nitrogen protection, slowly add the 5-aminobenzotriazole solution to the pre-reaction solution, and then add triethylenediamine to make the molar ratio of 4,4′-dihydroxydiphenyl ether, 5-aminobenzotriazole and triethylenediamine 1:(1.95-2.1):(0.03-0.04). Then stir at 55-65℃ and 200-300 rpm for 1-2 hours, then raise the temperature to 88-96℃ and keep the reaction at this temperature for 8-12 hours. Remove the water generated in the reaction through a water separator to obtain the reaction solution. S1.3: The reaction solution is concentrated under reduced pressure at 60-65℃ to 1 / 12-1 / 10 of its original volume to obtain a concentrate. The concentrate is then added to an ethanol-water solution at a mass ratio of 1:(6-10). The ethanol-water solution is a mixture of anhydrous ethanol and deionized water at a volume ratio of (2-4):1. After stirring evenly, the mixture is allowed to stand for 1-2 hours. The precipitate is collected by filtration and washed three times with ethanol and deionized water. Then, it is vacuum dried at 65-75℃ for 10-14 hours to obtain a copper-affinity bisbenzoxazine.
[0013] Furthermore, the preparation of the hollow silica nanospheres coated with ammonium acid-grafted phenylsiloxane in step S2 specifically includes the following steps: S2.1: Disperse 10 parts by weight of hollow silica nanospheres with an average particle size of 200-300 nm in 80-100 parts by weight of 90% ethanol solution to obtain a hollow silica nanosphere dispersion. Add 1.2-1.8 parts by weight of phenyltriethoxysilane and 0.2-0.35 parts by weight of 3-aminopropyltriethoxysilane to 12-15 parts by weight of 90% ethanol solution. Adjust the pH to 4-4.5 using acetic acid and pre-hydrolyze for 30-45 minutes to obtain a silane pre-hydrolyzed solution. S2.2: The silane pre-hydrolyzed solution obtained in step S2.1 is slowly added dropwise to the hollow silica nanosphere dispersion, and the addition time is controlled to be 2-2.5h. The pH is adjusted to 8-9 using ammonia water, and the reaction is carried out at 55-65℃ for 4-6 hours. After centrifugation, the precipitate is collected and washed 3 times with anhydrous ethanol. Then it is placed in a vacuum drying oven at 60℃ and dried for 6-8 hours to obtain amino-phenylsiloxane-coated hollow silica nanospheres. S2.3: 10-12 parts by weight of aminated phenylsiloxane-coated hollow silica nanospheres were dispersed in 80-100 parts by weight of anhydrous N-methylpyrrolidone, and 0.3-0.6 parts by weight of trimellitic anhydride were added. The mixture was reacted at 60-70°C for 3-5 hours under nitrogen protection. The precipitate was then collected by centrifugation and washed three times with anhydrous N-methylpyrrolidone and deionized water. The precipitate was dried to constant weight in a vacuum drying oven at 65°C to obtain aminated acid-grafted phenylsiloxane-coated hollow silica nanospheres.
[0014] Furthermore, the compounding of the paint in step S3 specifically includes the following steps: S3.1: Dissolve carboxyl-terminated polyamide-imide resin in an organic solvent and transfer it to a dry container. Slowly add amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres under stirring at 500-800 rpm. Continue stirring for 20-30 minutes, and then ultrasonically disperse at a frequency of 25-35 kHz for 10-15 minutes to obtain a mixture. S3.2: At 40-50℃, copper-affinity bisbenzoxazine and triglycidyl isocyanate are added to the mixture obtained in step S3.1 and stirred evenly. Then, the temperature is lowered to 20-25℃ and a curing catalyst, leveling agent, and defoamer are added. The mixture is stirred at 500-700 rpm for 40-60 minutes. Then, it is added to a filter and filtered with a filtration accuracy of 3-10 μm. Finally, it is degassed under a vacuum of -0.08 to -0.095 MPa for 20-30 minutes, sealed, and packaged to obtain a high-temperature resistant and waterproof coating for enameled copper flat wire. Beneficial effects
[0015] 1. This invention prepares a copper-affinity bisbenzoxazine containing benzotriazole groups by condensing 4,4′-dihydroxydiphenyl ether, 5-aminobenzotriazole, and paraformaldehyde. After coating the copper-affinity bisbenzoxazine-containing paint onto the surface of a copper flat wire, the benzotriazole groups in the copper-affinity bisbenzoxazine can adsorb and coordinate with the copper surface through multiple nitrogen-containing sites, causing the copper-affinity bisbenzoxazine to preferentially accumulate in the interface region between the copper conductor and the insulating coating. During the subsequent heat curing process, the benzoxazine ring undergoes ring-opening polymerization to form a crosslinked network containing aromatic rings, ether bridges, and nitrogen-containing heterocyclic structures, fixing the benzotriazole groups in the cured resin, thereby forming an interface locking layer on the copper surface that is not easily migrated or precipitated. This interface locking layer enhances the bonding strength between the coating and the copper conductor, suppressing interfacial debonding caused by the difference in thermal expansion coefficients between the copper conductor and the organic coating under high-temperature conditions. Furthermore, it seals the channels for rapid moisture diffusion along the copper-coating interface, reducing the probability of water absorption, blistering, and decreased adhesion under humid and hot conditions. Simultaneously, the highly aromatic cross-linked structure formed after the curing of bisbenzoxazine exhibits high thermal stability, restricting the movement of polymer chains at high temperatures and reducing softening, creep, and structural relaxation of the coating during continuous heating. This results in a coating that possesses both excellent high-temperature adhesion stability and interfacial waterproofing performance.
[0016] 2. This invention prepares phenylsiloxane-coated hollow silica nanospheres (hereinafter referred to as functionalized hollow nanospheres) by sequentially constructing a phenylsiloxane sealing layer and a trimellitic amide acid grafted layer on the surface of hollow silica nanospheres. The hollow structure is used directly as a stress-buffering inorganic filler added to the paint. The hollow silica shell has good heat resistance and stability. During high-temperature baking and long-term thermal aging, it can play an inorganic skeleton support role for the polyamide-imide resin network, limiting the thermal shrinkage and local deformation of the coating. Compared with solid inorganic particles of the same size, the hollow structure can mitigate the modulus difference between inorganic fillers and organic resins, so that it can produce limited elastic deformation and micro-buckling during the rounded corner bending of copper flat wire, curing shrinkage and thermal cycling. This disperses the concentrated stress inside the coating and hinders the propagation of microcracks, thereby preventing moisture from entering the interior of the insulating coating through thermally induced microcracks. The phenylsiloxane sealing layer on the surface of the nanospheres covers the hydrophilic silanol groups on the silica surface and seals the shell pores, reducing the water absorption tendency of the hollow particles. The phenyl groups distributed on the outer surface of the particles also improve the compatibility between the particles and the aromatic polyamide-imide resin, ensuring uniform dispersion of the particles in the coating. Therefore, the hollow nanospheres not only improve the thermal shock stability and crack resistance of the coating but also reduce water penetration caused by filler interfaces and inorganic pores, thus improving the waterproofness of the coating itself.
[0017] 3. This invention utilizes triglycidyl isocyanurate as a multifunctional crosslinking component, allowing its epoxy groups to crosslink with the carboxyl groups in carboxyl-terminated polyamide-imide, the ammonium carboxyl groups on the surface of hollow nanospheres, and some phenolic hydroxyl groups formed after ring-opening of copper-affinity bisbenzoxazine, thereby combining the polyamide-imide resin, copper-affinity bisbenzoxazine, and functionalized hollow nanospheres into a continuous three-dimensional crosslinked network. The isocyanuric acid ring in triglycidyl isocyanurate has high rigidity and thermal stability, which can improve the crosslinking density and high-temperature dimensional stability of the coating, and reduce the instantaneous free volume formed by molecular chain segment movement under high-temperature conditions. At the same time, multi-point crosslinking can reduce the interfacial gap between the functionalized hollow nanospheres and the resin, preventing moisture diffusion along the filler-resin interface. The resulting dense crosslinked structure can reduce the dissolution and diffusion rate of water molecules in the coating and inhibit the swelling of the resin network after water absorption, enabling the insulating coating to maintain good mechanical strength, adhesion, and electrical insulation properties even under high temperature, high humidity, and alternating high and low temperature environments. Detailed Implementation
[0018] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0019] Carboxyl-terminated polyamide-imide resin is prepared by the following method: (1) Trimeric trihydric anhydride and 4,4′-diphenylmethane diisocyanate were dissolved in anhydrous N-methylpyrrolidone to prepare a 35% trimellitic anhydride solution and a 55% 4,4′-diphenylmethane diisocyanate solution. Under nitrogen protection at 60°C, the 4,4′-diphenylmethane diisocyanate solution was slowly added to the trimellitic anhydride solution at a molar ratio of 1:0.94. The addition time was controlled to be 2 hours. The mixture was stirred continuously at a stirring speed of 150 rpm during the addition process to obtain a mixed solution. (2) Heat the mixture to 85°C and react for 1.5 hours, then heat it to 130°C and react for 5 hours until the mass fraction of free isocyanate groups in the reaction system is less than 0.3%. Cool it to 75°C and remove the solvent by vacuum distillation to obtain a dry solid, which is the carboxyl-terminated polyamide-imide resin. Example 1
[0020] A high-temperature resistant and waterproof coating for enameled copper flat wire comprises, by weight, the following components: 100 parts of carboxyl-terminated polyamide-imide resin, 4 parts of copper-affinity bisbenzoxazine, 1.5 parts of amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres, 2 parts of triglycidyl isocyanate, 0.05 parts of triphenylphosphine, 0.05 parts of BYK-333 leveling agent, 0.02 parts of BYK-072 silicone defoamer, and 250 parts of an organic solvent composed of N-methylpyrrolidone and γ-butyrolactone in a mass ratio of 1:0.4.
[0021] A method for preparing a high-temperature resistant and waterproof coating for enameled copper flat wire includes the following steps: S1: Preparation of copper-affinity bisbenzoxazine S1.1: Add 4,4′-dihydroxydiphenyl ether and paraformaldehyde to a container. The molar ratio of formaldehyde structural units in 4,4′-dihydroxydiphenyl ether and paraformaldehyde is 1:3.9. Add a mixed solvent of 4 times the total mass of the reactants and stir until homogeneous. The mixed solvent is composed of 1,4-dioxane and toluene in a volume ratio of 1:0.8 to obtain a pre-reaction solution. S1.2: 5-Aminobenzotriazole was dissolved in N,N-dimethylformamide at a mass ratio of 1:3 to obtain a 5-aminobenzotriazole solution. Under nitrogen protection, the 5-aminobenzotriazole solution was slowly added to the pre-reaction solution, followed by the addition of triethylenediamine, so that the molar ratio of 4,4′-dihydroxydiphenyl ether, 5-aminobenzotriazole and triethylenediamine was 1:1.95:0.03. The mixture was then stirred at 55°C and 200 rpm for 1 hour, then heated to 88°C and kept at that temperature for 8 hours. The water generated in the reaction was removed by a water separator to obtain the reaction solution. S1.3: The reaction solution was concentrated under reduced pressure at 60°C to 1 / 12 of its original volume to obtain a concentrate. The concentrate was then added to an ethanol-water solution at a mass ratio of 1:6. The ethanol-water solution was prepared by mixing anhydrous ethanol and deionized water at a volume ratio of 2:1. After stirring evenly, the mixture was allowed to stand for 1 hour. The precipitate was collected by filtration and washed three times with ethanol and deionized water. Then, it was vacuum dried at 65°C for 10 hours to obtain copper-affinity bisbenzoxazine.
[0022] S2: Preparation of hollow silica nanospheres coated with ammonium acid-grafted phenylsiloxane S2.1: 10 parts by weight of hollow silica nanospheres with an average particle size of 200 nm were dispersed in 80 parts by weight of 90% ethanol solution to obtain a hollow silica nanosphere dispersion. 1.2 parts by weight of phenyltriethoxysilane and 0.2 parts by weight of 3-aminopropyltriethoxysilane were added to 12 parts by weight of 90% ethanol solution. The pH was adjusted to 4 using acetic acid, and the solution was pre-hydrolyzed for 30 minutes to obtain a silane pre-hydrolyzed solution. S2.2: The silane pre-hydrolyzed solution obtained in step S2.1 was slowly added dropwise to the hollow silica nanosphere dispersion, and the addition time was controlled to be 2h. The pH was adjusted to 8 using ammonia water, and the reaction was carried out at 55℃ for 4 hours. The precipitate was separated by centrifugation, washed 3 times with anhydrous ethanol, and then dried in a vacuum drying oven at 60℃ for 6 hours to obtain amino-phenylsiloxane-coated hollow silica nanospheres. S2.3: 10 parts by weight of amino-modified phenylsiloxane-coated hollow silica nanospheres were dispersed in 80 parts by weight of anhydrous N-methylpyrrolidone, and 0.3 parts by weight of trimellitic anhydride were added. The mixture was reacted at 60°C for 3 hours under nitrogen protection. The precipitate was then collected by centrifugation and washed three times with anhydrous N-methylpyrrolidone and deionized water. The precipitate was dried to constant weight in a vacuum drying oven at 65°C to obtain ammonium acid-grafted phenylsiloxane-coated hollow silica nanospheres.
[0023] S3: Paint compounding S3.1: Dissolve carboxyl-terminated polyamide-imide resin in an organic solvent and transfer it to a dry container. Slowly add amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres under stirring at 500 rpm. Continue stirring for 20 minutes, and then ultrasonically disperse at a frequency of 25 kHz for 10 minutes to obtain a mixture. S3.2: At 40℃, copper-affinity bisbenzoxazine and triglycidyl isocyanurate are added to the mixture obtained in step S3.1 and stirred evenly. Then, the mixture is cooled to 20℃ and a curing catalyst, leveling agent and defoamer are added. The mixture is stirred at 500 rpm for 40 minutes. Then, it is added to a filter and filtered with a filtration accuracy of 3 μm. Finally, it is degassed under a vacuum of -0.095 MPa for 20 minutes and sealed and packaged to obtain a high-temperature resistant and waterproof coating for enameled copper flat wire. Example 2
[0024] A high-temperature resistant and waterproof coating for enameled copper flat wire comprises, by weight, the following components: 110 parts of carboxyl-terminated polyamide-imide resin, 6 parts of copper-affinity bisbenzoxazine, 1.8 parts of amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres, 2.8 parts of triglycidyl isocyanate, 0.1 parts of triphenylphosphine, 0.1 parts of BYK-333 leveling agent, 0.05 parts of BYK-072 silicone defoamer, and 265 parts of an organic solvent composed of N-methylpyrrolidone and γ-butyrolactone in a mass ratio of 1:0.7.
[0025] A method for preparing a high-temperature resistant and waterproof coating for enameled copper flat wire includes the following steps: S1: Preparation of copper-affinity bisbenzoxazine S1.1: Add 4,4′-dihydroxydiphenyl ether and paraformaldehyde to a container. The molar ratio of formaldehyde structural units in 4,4′-dihydroxydiphenyl ether and paraformaldehyde is 1:4.1. Add a mixed solvent of 5 times the total mass of the reactants and stir until homogeneous. The mixed solvent is composed of 1,4-dioxane and toluene in a volume ratio of 1:1 to obtain a pre-reaction solution. S1.2: Dissolve 5-aminobenzotriazole in N,N-dimethylformamide at a mass ratio of 1:3.5 to obtain a 5-aminobenzotriazole solution. Under nitrogen protection, slowly add the 5-aminobenzotriazole solution to the pre-reaction solution, and then add triethylenediamine to make the molar ratio of 4,4′-dihydroxydiphenyl ether, 5-aminobenzotriazole and triethylenediamine 1:2:0.06. Then stir at 65℃ and 200 rpm for 1.5 hours, then raise the temperature to 88℃ and keep the reaction at this temperature for 12 hours. Remove the water generated in the reaction through a water separator to obtain the reaction solution. S1.3: The reaction solution was concentrated under reduced pressure at 60°C to 1 / 12 of its original volume to obtain a concentrate. The concentrate was then added to an ethanol-water solution at a mass ratio of 1:8. The ethanol-water solution was prepared by mixing anhydrous ethanol and deionized water at a volume ratio of 3:1. After stirring evenly, the solution was allowed to stand for 1.5 hours. The precipitate was collected by filtration and washed three times with ethanol and deionized water. Then, it was dried under vacuum at 75°C for 10 hours to obtain copper-affinity bisbenzoxazine.
[0026] S2: Preparation of hollow silica nanospheres coated with ammonium acid-grafted phenylsiloxane S2.1: 10 parts by weight of hollow silica nanospheres with an average particle size of 250 nm were dispersed in 90 parts by weight of 90% ethanol solution to obtain a hollow silica nanosphere dispersion. 1.5 parts by weight of phenyltriethoxysilane and 0.28 parts by weight of 3-aminopropyltriethoxysilane were added to 13 parts by weight of 90% ethanol solution. The pH was adjusted to 4 using acetic acid, and the solution was pre-hydrolyzed for 45 minutes to obtain a silane pre-hydrolyzed solution. S2.2: The silane pre-hydrolyzed solution obtained in step S2.1 was slowly added dropwise to the hollow silica nanosphere dispersion, and the addition time was controlled to be 2h. The pH was adjusted to 8 using ammonia water, and the reaction was carried out at 65℃ for 4 hours. The precipitate was separated by centrifugation, washed 3 times with anhydrous ethanol, and then dried in a vacuum drying oven at 60℃ for 7 hours to obtain amino-phenylsiloxane-coated hollow silica nanospheres. S2.3: 11 parts by weight of amino-modified phenylsiloxane-coated hollow silica nanospheres were dispersed in 90 parts by weight of anhydrous N-methylpyrrolidone, and 0.5 parts by weight of trimellitic anhydride were added. The mixture was reacted at 65°C for 4 hours under nitrogen protection. The precipitate was then collected by centrifugation and washed three times with anhydrous N-methylpyrrolidone and deionized water. The precipitate was dried to constant weight in a vacuum drying oven at 65°C to obtain ammonium acid-grafted phenylsiloxane-coated hollow silica nanospheres.
[0027] S3: Paint compounding S3.1: Dissolve carboxyl-terminated polyamide-imide resin in an organic solvent and transfer it to a dry container. Slowly add amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres under stirring at 800 rpm. Continue stirring for 20 minutes, and then ultrasonically disperse at a frequency of 35 kHz for 10 minutes to obtain a mixture. S3.2: At 45℃, copper-affinity bisbenzoxazine and triglycidyl isocyanurate are added to the mixture obtained in step S3.1 and stirred evenly. Then, the mixture is cooled to 25℃ and a curing catalyst, leveling agent and defoamer are added. The mixture is stirred at 500 rpm for 60 minutes. Then, it is added to a filter and filtered with a filtration accuracy of 6 μm. Finally, it is degassed under a vacuum of -0.08 MPa for 30 minutes and sealed and packaged to obtain a high-temperature resistant and waterproof coating for enameled copper flat wire. Example 3
[0028] A high-temperature resistant and waterproof coating for enameled copper flat wire comprises, by weight, the following components: 120 parts of carboxyl-terminated polyamide-imide resin, 8 parts of copper-affinity bisbenzoxazine, 2.2 parts of amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres, 3.5 parts of triglycidyl isocyanate, 0.15 parts of triphenylphosphine, 0.15 parts of BYK-333 leveling agent, 0.08 parts of BYK-072 silicone defoamer, and 280 parts of an organic solvent composed of N-methylpyrrolidone and γ-butyrolactone in a mass ratio of 1:1.0.
[0029] A method for preparing a high-temperature resistant and waterproof coating for enameled copper flat wire includes the following steps: S1: Preparation of copper-affinity bisbenzoxazine S1.1: Add 4,4′-dihydroxydiphenyl ether and paraformaldehyde to a container. The molar ratio of formaldehyde structural units in 4,4′-dihydroxydiphenyl ether and paraformaldehyde is 1:4.3. Add a mixed solvent of 7 times the total mass of the reactants and stir until homogeneous. The mixed solvent is composed of 1,4-dioxane and toluene in a volume ratio of 1:1.2 to obtain a pre-reaction solution. S1.2: 5-Aminobenzotriazole was dissolved in N,N-dimethylformamide at a mass ratio of 1:4 to obtain a 5-aminobenzotriazole solution. Under nitrogen protection, the 5-aminobenzotriazole solution was slowly added to the pre-reaction solution, followed by the addition of triethylenediamine, so that the molar ratio of 4,4′-dihydroxydiphenyl ether, 5-aminobenzotriazole and triethylenediamine was 1:2.1:0.07. The mixture was then stirred at 65°C and 300 rpm for 2 hours, then heated to 96°C and kept at that temperature for 12 hours. The water generated in the reaction was removed by a water separator to obtain the reaction solution. S1.3: The reaction solution was concentrated under reduced pressure at 65°C to 1 / 10 of its original volume to obtain a concentrate. The concentrate was then added to an ethanol-water solution at a mass ratio of 1:10. The ethanol-water solution was prepared by mixing anhydrous ethanol and deionized water at a volume ratio of 4:1. After stirring evenly, the mixture was allowed to stand for 2 hours. The precipitate was collected by filtration and washed three times with ethanol and deionized water. Then, it was vacuum dried at 75°C for 14 hours to obtain copper-affinity bisbenzoxazine.
[0030] S2: Preparation of hollow silica nanospheres coated with ammonium acid-grafted phenylsiloxane S2.1: Disperse 10 parts by weight of hollow silica nanospheres with an average particle size of 300 nm in 100 parts by weight of 90% ethanol solution to obtain a hollow silica nanosphere dispersion. Add 1.8 parts by weight of phenyltriethoxysilane and 0.35 parts by weight of 3-aminopropyltriethoxysilane to 15 parts by weight of 90% ethanol solution, adjust the pH to 4.5 with acetic acid, and pre-hydrolyze for 45 minutes to obtain a silane pre-hydrolyzed solution. S2.2: The silane pre-hydrolyzed solution obtained in step S2.1 was slowly added dropwise to the hollow silica nanosphere dispersion, and the addition time was controlled to be 2.5h. The pH was adjusted to 9 using ammonia water, and the reaction was carried out at 65℃ for 6 hours. The precipitate was separated by centrifugation, washed 3 times with anhydrous ethanol, and then dried in a vacuum drying oven at 60℃ for 8 hours to obtain amino-phenylsiloxane-coated hollow silica nanospheres. S2.3: 12 parts by weight of aminated phenylsiloxane-coated hollow silica nanospheres were dispersed in 100 parts by weight of anhydrous N-methylpyrrolidone, and 0.6 parts by weight of trimellitic anhydride were added. The mixture was reacted at 70°C for 5 hours under nitrogen protection. The precipitate was then collected by centrifugation and washed three times with anhydrous N-methylpyrrolidone and deionized water. The precipitate was dried to constant weight in a vacuum drying oven at 65°C to obtain aminated acid-grafted phenylsiloxane-coated hollow silica nanospheres.
[0031] S3: Paint compounding S3.1: Dissolve carboxyl-terminated polyamide-imide resin in an organic solvent and transfer it to a dry container. Slowly add amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres under stirring at 800 rpm. Continue stirring for 30 minutes, and then ultrasonically disperse at a frequency of 35 kHz for 15 minutes to obtain a mixture. S3.2: At 50°C, copper-affinity bisbenzoxazine and triglycidyl isocyanate are added to the mixture obtained in step S3.1 and stirred evenly. Then, the mixture is cooled to 25°C and a curing catalyst, leveling agent, and defoamer are added. The mixture is stirred at 700 rpm for 60 minutes. Then, it is added to a filter and filtered with a filtration accuracy of 10 μm. Finally, it is degassed under a vacuum of -0.08 MPa for 30 minutes and sealed in a package to obtain a high-temperature resistant and waterproof coating for enameled copper flat wire.
[0032] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 did not add ammonium acid-grafted phenylsiloxane-coated hollow silica nanospheres in step S3.1, while the remaining steps were the same as in Example 1.
[0033] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres in step S3.1 are replaced with hollow silica nanospheres of equal mass, while the remaining steps are the same as in Example 1.
[0034] Comparative Example 3 The difference from Example 1 is that Comparative Example 3 did not add copper-affinity bisbenzoxazine in step S3.2, and the remaining steps were the same as in Example 1.
[0035] Comparative Example 4 The difference from Example 1 is that Comparative Example 4 did not add triglycidyl isocyanurate in step S3.2, and the remaining steps were the same as in Example 1.
[0036] Sample preparation: Copper flat wires from the same batch, with a width of 15.00 mm, a thickness of 4.00 mm, and a corner radius of 0.5 mm, were selected and coated using the enamels prepared in Examples 1-3 and Comparative Examples 1-4. The coating process was standardized as follows: the copper flat wires were degreased, cleaned, and dried; coating was performed using an enameled dip coating process; the final dry film thickness was controlled at 35 ± 2 μm; the actual peak temperature of the copper flat wires was controlled at 300 ± 5℃; three coats were applied, with an effective baking time of 30 ± 3 seconds for each coat, resulting in enameled copper flat wire samples.
[0037] High temperature resistance test: Heat resistance test: Take three weight portions of enameled copper flat wire samples for each group, use a voltage breakdown tester to test the breakdown voltage of the coating before heat aging, then age at 300℃ for 500h, and then use a voltage breakdown tester to test the breakdown voltage of the coating after heat aging. Calculate the breakdown voltage retention rate = breakdown voltage after heat aging / breakdown voltage before heat aging × 100%. According to the standard GB / T1735-2009 "Determination of heat resistance of paints and varnishes", observe whether the coating has chalking or peeling. If neither is present, it is qualified; otherwise, it is unqualified. Peel strength test: Three weight samples of enameled copper flat wire were taken from each group and aged at 300℃ for 500h. The peel strength of the coating after aging was tested according to GB / T4074.3-2024 "Test methods for winding wires - Part 3: Mechanical properties". The average value of each group was taken.
[0038] Thermal cycling: Take three weight samples of enameled copper flat wire from each group, heat to 300℃, and then quench them with high-pressure water at 25℃ according to ISO16925:2021 standard. Repeat 50 times and observe the coating condition.
[0039] The results of the high temperature resistance test are shown in Table 1.
[0040] Table 1 Waterproof performance test: Water absorption weight gain rate: Take three parts by weight of enameled copper flat wire samples from each group, dry them at 120℃ to constant weight, weigh the initial mass m0, soak them in deionized water at 23℃ for 72 hours, wipe off the surface moisture and weigh m1. Water absorption weight gain rate = (m1-m0) / m0×100%.
[0041] Damp heat aging: Three weight samples of enameled copper flat wire were taken from each group. The breakdown voltage of the coating before damp heat was tested using a voltage breakdown tester. After being placed in an environment of 85℃ and 85%RH for 500 hours, the cracking of the coating was observed. Then, the breakdown voltage of the coating after damp heat was tested using a voltage breakdown tester, and the breakdown voltage retention rate was calculated as follows: breakdown voltage after damp heat / breakdown voltage before damp heat × 100%. The average value was taken.
[0042] The results of the waterproof performance test are shown in Table 2.
[0043] Table 2 As shown in Tables 1 and 2, none of the Examples 1-3 exhibited powdering or peeling after aging at 300℃ for 500 hours. Their peel strength and breakdown voltage retention rate after high-temperature aging were significantly higher than those of the comparative example. After 50 cycles of thermal cycling, the coatings remained crack-free. Furthermore, Examples 1-3 showed low water absorption and weight gain rates, and none exhibited cracking after aging at 85℃ and 85%RH for 500 hours, maintaining a high breakdown voltage retention rate. This indicates that the coatings prepared by this invention possess excellent high-temperature resistance, thermal shock resistance, water resistance, and insulation stability.
[0044] Comparative Example 1, without the addition of ammonium acid-grafted phenylsiloxane-coated hollow silica nanospheres, failed the heat resistance test, exhibiting slight cracking after thermal cycling, and showing a significant increase in water absorption and weight gain. This indicates that the functionalized hollow nanospheres can utilize their cavity structure to disperse internal stress in the coating and reduce moisture penetration through the phenylsiloxane sealing layer, thereby improving the coating's high-temperature crack resistance and waterproof performance.
[0045] Comparative Example 2 used unmodified hollow silica nanospheres, whose heat resistance, water resistance, and peel strength were significantly reduced. Cracking occurred after thermal cycling, and the reduction was greater than that of Comparative Example 1. Not only did it fail to enhance the paint, but it also led to the deterioration of the paint's performance. This indicates that the hydrophilic silanol groups on the surface of bare hollow silica and its poor resin compatibility easily form water absorption and stress concentration interfaces. In contrast, phenylsiloxane sealing and ammonium acid grafting can improve the hydrophobicity of the particles and the interfacial bonding ability.
[0046] Comparative Example 3, without the addition of copper-affinity bisbenzoxazine, exhibited a relatively low water absorption weight gain, but its peel strength after high-temperature aging decreased significantly, and its breakdown voltage retention rate after both high-temperature and humid-heat aging was also significantly reduced. This indicates that copper-affinity bisbenzoxazine can form a stable interfacial locking layer on the copper surface through the adsorption and coordination of benzotriazole groups, reducing interfacial debonding and moisture penetration under high-temperature and humid-heat conditions.
[0047] Comparative Example 4, without the addition of triglycidyl isocyanurate, showed a significant decrease in peel strength and breakdown voltage retention after high-temperature aging, and slight cracking after thermal cycling. After damp-heat aging, the sample exhibited cracks, and the breakdown voltage retention also decreased significantly. This indicates that triglycidyl isocyanurate can connect polyamide-imide resin, copper-affinity bisbenzoxazine, and functionalized hollow nanospheres to form a dense three-dimensional cross-linked network, reducing the free volume and interfacial gaps within the coating, thereby ensuring the coating's mechanical strength, adhesion, and electrical insulation properties.
[0048] In summary, copper-affinity bisbenzoxazine primarily enhances the heat resistance, adhesion, and water resistance of the copper-coating interface; functionalized hollow nanospheres mainly improve the crack resistance and water resistance of the coating itself; and triglycidyl isocyanate strengthens the overall cross-linking structure. The combined effect of these three components gives the coating excellent high-temperature resistance, water resistance, and electrical insulation stability.
[0049] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A high temperature resistant water proof paint for enameled copper rectangular wire, characterized in that, By weight, it includes the following ingredients: The composition includes 100-120 parts of carboxyl-terminated polyamide-imide resin, 4-8 parts of copper-affinity bisbenzoxazine, 1.5-2.2 parts of amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres, 2-3.5 parts of triglycidyl isocyanate, 0.05-0.15 parts of curing catalyst, 0.05-0.15 parts of leveling agent, 0.02-0.08 parts of defoamer, and 250-280 parts of organic solvent; The copper-affinity bisbenzoxazine is prepared by a condensation reaction of 4,4′-dihydroxydiphenyl ether, 5-aminobenzotriazole and paraformaldehyde in a molar ratio of 1:(1.95~2.1):(3.9~4.3); The ammonium acid-grafted phenylsiloxane-coated hollow silica nanospheres include an internal hollow silica nanosphere, a phenylsiloxane sealing layer disposed outside the hollow silica nanosphere, and trimellitic acid ammonium acid groups grafted onto the surface of the phenylsiloxane sealing layer.
2. A high temperature resistant water proof paint for enameled copper rectangular wire according to claim 1, characterized in that, The curing catalyst is triphenylphosphine.
3. The high-temperature resistant and waterproof coating for enameled copper flat wire as described in claim 1, characterized in that, The leveling agent is a polyether-modified polysiloxane leveling agent, and the defoamer is an organosilicone defoamer.
4. A high temperature resistant water proof paint for enameled copper rectangular wire according to claim 1, wherein The organic solvent is composed of N-methylpyrrolidone and γ-butyrolactone in a mass ratio of 1:(0.4 to 1.0).
5. A process for the preparation of a high temperature resistant, water repellent paint for enamelled copper flat wire according to any one of claims 1 to 4, characterized in that, Includes the following steps: S1: Preparation of copper-affinity bisbenzoxazine; S2: Preparation of hollow silica nanospheres coated with ammonium acid grafted with phenylsiloxane; S3: Coating of paint: Dissolve carboxyl-terminated polyamide-imide resin in an organic solvent, add amyl acid-grafted phenylsiloxane to coat hollow silica nanospheres, stir and ultrasonically disperse evenly, add copper-affinity bisbenzoxazine and triglycidyl isocyanate at 40-45℃ and stir evenly, then cool to 20-25℃, add curing catalyst, leveling agent and defoamer, stir and filter and vacuum degas to obtain a high-temperature resistant and waterproof paint for enameled copper flat wire.
6. A process for the preparation of a high temperature resistant water proof paint for enameled copper rectangular wire as claimed in claim 5 wherein, Step S1, the preparation of copper-affinity bisbenzoxazine, specifically includes the following steps: S1.1: Add 4,4′-dihydroxydiphenyl ether and paraformaldehyde to a container. The molar ratio of formaldehyde structural units in 4,4′-dihydroxydiphenyl ether and paraformaldehyde is 1:(3.9-4.3). Add a mixed solvent of 4 to 7 times the total mass of the reactants and stir until homogeneous. The mixed solvent is composed of 1,4-dioxane and toluene in a volume ratio of 1:(0.8-1.2) to obtain a pre-reaction solution. S1.2: Dissolve 5-aminobenzotriazole in N,N-dimethylformamide at a mass ratio of 1:(3-4) to obtain a 5-aminobenzotriazole solution. Under nitrogen protection, slowly add the 5-aminobenzotriazole solution to the pre-reaction solution, and then add triethylenediamine to make the molar ratio of 4,4′-dihydroxydiphenyl ether, 5-aminobenzotriazole and triethylenediamine 1:(1.95-2.1):(0.03-0.04). Then stir at 55-65℃ and 200-300 rpm for 1-2 hours, then raise the temperature to 88-96℃ and keep the reaction at this temperature for 8-12 hours. Remove the water generated in the reaction through a water separator to obtain the reaction solution. S1.3: The reaction solution is concentrated under reduced pressure at 60-65℃ to 1 / 12-1 / 10 of its original volume to obtain a concentrate. The concentrate is then added to an ethanol-water solution at a mass ratio of 1:(6-10). The ethanol-water solution is a mixture of anhydrous ethanol and deionized water at a volume ratio of (2-4):
1. After stirring evenly, the mixture is allowed to stand for 1-2 hours. The precipitate is collected by filtration and washed successively with ethanol and deionized water. Then, it is vacuum dried at 65-75℃ for 10-14 hours to obtain a copper-affinity bisbenzoxazine.
7. A process for the preparation of a high temperature resistant water proof paint for enameled copper rectangular wire as claimed in claim 5 wherein, Step S2, the preparation of amyl acid-grafted phenylsiloxane-coated hollow silica nanospheres, specifically includes the following steps: S2.1: Disperse 10 parts by weight of hollow silica nanospheres with an average particle size of 200-300 nm in 80-100 parts by weight of 90% ethanol solution to obtain a hollow silica nanosphere dispersion. Add 1.2-1.8 parts by weight of phenyltriethoxysilane and 0.2-0.35 parts by weight of 3-aminopropyltriethoxysilane to 12-15 parts by weight of 90% ethanol solution. Adjust the pH to 4-4.5 using acetic acid and pre-hydrolyze for 30-45 minutes to obtain a silane pre-hydrolyzed solution. S2.2: The silane pre-hydrolyzed solution obtained in step S2.1 is slowly added dropwise to the hollow silica nanosphere dispersion, and the addition time is controlled to be 2-2.5h. The pH is adjusted to 8-9 using ammonia water, and the reaction is carried out at 55-65℃ for 4-6 hours. After centrifugation, the precipitate is collected and washed 3 times with anhydrous ethanol. Then it is placed in a vacuum drying oven at 60℃ and dried for 6-8 hours to obtain amino-phenylsiloxane-coated hollow silica nanospheres. S2.3: 10-12 parts by weight of aminated phenylsiloxane-coated hollow silica nanospheres were dispersed in 80-100 parts by weight of anhydrous N-methylpyrrolidone, and 0.3-0.6 parts by weight of trimellitic anhydride were added. The mixture was reacted at 60-70°C for 3-5 hours under nitrogen protection. The precipitate was then collected by centrifugation and washed successively with anhydrous N-methylpyrrolidone and deionized water. The precipitate was dried to constant weight in a vacuum drying oven at 65°C to obtain aminated acid-grafted phenylsiloxane-coated hollow silica nanospheres.