High-efficiency low-damage silicon wafer fine polishing liquid and preparation method thereof

By combining small- and large-particle-size colloidal silica and imidazole-catalyzed silicon surface hydrolysis in a silicon wafer polishing slurry, and combining it with a siloxane copolymer modifier, the problem of achieving both high removal rate and low roughness in existing silicon wafer polishing slurries is solved, thus achieving a highly efficient and low-damage silicon wafer polishing effect.

CN123107550APending Publication Date: 2026-11-17SHENZHEN XINLIYAN TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611456632.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing chemical mechanical polishing slurries for silicon wafers have problems such as difficulty in achieving both high removal rate and low roughness, the tendency of single organic bases or strong bases to cause over-etching and surface deterioration, excessive adhesion and agglomeration of polymers and surfactants and their residues, and insufficient storage and cycling stability of dual-particle-size systems.

Method used

Colloidal silica with a small particle size of 30 to 60 nanometers and a large particle size of 80 to 120 nanometers are compounded in a certain mass ratio. Combined with imidazole nitrogen-containing catalyst for silicon surface hydrolysis, AMPD polyhydroxyamine buffering alkalinity, and siloxane copolymer modifier, abrasive mechanics, organic base reaction kinetics and interfacial stress are synergistically formed within a set pH range. Through the distribution of small particle size colloidal silica in the gap between large particle size abrasive particles, the transport of interfacial hydration layer and weak base hydrolysis products is enhanced, and micro-scratches caused by local hard contact are reduced.

Benefits of technology

It achieves efficient and low-damage silicon wafer polishing, simultaneously improving material removal rate and surface roughness, enhancing removal efficiency in chemical mechanical polishing, improving surface quality, strengthening the stability of polishing fluid circulation and storage, and reducing micro-scratches and localized corrosion defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107550A_ABST
    Figure CN123107550A_ABST
Patent Text Reader

Abstract

This invention discloses a high-efficiency, low-damage silicon wafer polishing slurry and its preparation method, belonging to the field of chemical polishing technology. The polishing slurry is composed of the following raw materials in parts by weight: 1 to 5 parts of small-particle-size colloidal silica, 4 to 10 parts of large-particle-size colloidal silica, 0.1 to 0.3 parts of imidazole, 0.2 to 0.8 parts of 2-amino-2-methyl-1,3-propanediol, 0.01 to 0.03 parts of siloxane copolymer modifier, 0.01 to 0.05 parts of nonionic wetting agent, 0.1 to 0.2 parts of low-molecular-weight polyol, 0.01 to 0.05 parts of dispersion stabilizer, 0.1 to 0.5 parts of ammonia, and 80 to 120 parts of deionized water. This invention solves the problem that existing polishing slurries cannot simultaneously achieve high removal rate and low surface damage by combining dual-particle-size abrasives and composite organic base, along with an interface modifier, thus achieving a comprehensive improvement in polishing rate, surface quality, and storage stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chemical polishing technology, specifically referring to a high-efficiency, low-damage silicon wafer polishing slurry and its preparation method. Background Technology

[0002] Silicon wafer polishing slurries typically employ nano-sized silicon oxide, aluminum oxide, or cerium oxide abrasives, combined with oxidants, pH adjusters, dispersants, surfactants, and complexing agents to form a synergistic system. A suitable alkaline environment promotes the formation of an easily removable softening layer on the silicon wafer surface, allowing for the controlled removal of microscopic protrusions by uniformly abrasive particles. The high dispersion and narrow particle size distribution of the abrasives ensure stable suspension, surfactants improve wetting and cleaning, and complexing agents inhibit metal ion residue. Overall, the slurry achieves high removal efficiency, global planarization, and low damage, resulting in a highly smooth, low-roughness, and atomically flat silicon wafer surface.

[0003] However, existing chemical mechanical polishing (CMP) for silicon wafers uses colloidal silica as an abrasive. While fine particles can reduce damage, they have weak removal power, while coarse particles can improve efficiency but increase local stress and induce micro-scratches. When nitrogen-containing organic bases or strong bases promote the reaction, if the alkalinity is mismatched with the accelerator, chemical dissolution will be stronger than mechanical removal, leading to over-etching, increased roughness, and corrosion. In order to improve wetting and dispersion, polymers or surfactants are added, but excessive amounts will increase viscosity, hinder filtration, cause abrasive agglomeration, and produce organic residues. The combination of these defects makes it difficult to achieve a balance between removal rate, surface quality, micro-scratch suppression, and storage stability, thus limiting the application of fine polishing solutions. Summary of the Invention

[0004] To address the above issues and overcome the shortcomings of existing technologies, this invention provides a high-efficiency, low-damage silicon wafer polishing slurry and its preparation method. The slurry is prepared by mixing small-particle-size (30-60 nm) and large-particle-size (80-120 nm) colloidal silica in a specific mass ratio. The large particles provide mechanical removal, while the small particles homogenize the contact. Imidazole nitrogen catalyzes the hydrolysis of the silicon surface, and AMPD polyhydroxyamine buffers alkalinity and improves interfacial hydration. Furthermore, a siloxane copolymer is used to weakly coat the large-particle surface, disperse the small particles, and regulate amide hydrogen bonding. This allows abrasive mechanics, organic base reaction kinetics, and interfacial stress to synergize within a set pH range, achieving a balance between removal rate, low damage, and stability. This effectively solves the problems currently found in commercially available silicon polishing slurries: difficulty in achieving both high removal rate and low roughness; the tendency of single organic bases or strong bases to cause over-etching and surface deterioration; excessive adhesion and agglomeration of polymers and surfactants leading to residues; and insufficient storage and cycling stability of dual-particle-size systems.

[0005] The technical solution adopted in this invention is as follows: This invention proposes a high-efficiency, low-damage silicon wafer polishing slurry and its preparation method, comprising the following raw materials in parts by weight: 1-5 parts of small-particle-size colloidal silica, 4-10 parts of large-particle-size colloidal silica, 0.1-0.3 parts of imidazole; 0.2-0.8 parts of 2-amino-2-methyl-1,3-propanediol; 0.01-0.03 parts of siloxane copolymer modifier; 0.01-0.05 parts of nonionic wetting agent, 0.1-0.2 parts of low-molecular-weight polyol, 0.01-0.05 parts of dispersion stabilizer, 0.1-0.5 parts of ammonia, and 80-120 parts of deionized water; The primary particle size of the small-particle-size colloidal silica is 30-60 nm, and the primary particle size of the large-particle-size colloidal silica is 80-120 nm. The nonionic wetting agent is selected from one or more of polyethers and acetylenic diols; The low molecular weight polyol is selected from one or more of glycerol, sorbitol, xylitol, and erythritol; The dispersing stabilizer is selected from one or more low molecular weight polycarboxylate salts or their ammonium salts; The ammonia solution is a 25% ammonia solution by mass.

[0006] Furthermore, the preparation method of the siloxamide copolymer modifier includes the following steps: S1. Under nitrogen protection, α,ω-hydrogen-containing polydimethylsiloxane and monoallyl polyoxyethylene are subjected to hydrosilylation reaction with the addition of chloroplatinic acid, so that the Si-H groups of the hydrogen-containing polysiloxane and the carbon-carbon double bonds of monoallyl polyoxyethylene form Si-C bonds, generating an oligomeric siloxane-polyether backbone intermediate. S2. The oligomeric siloxane-polyether main chain intermediate obtained in step S1 is subjected to an addition reaction with an epoxy-functionalized monomer to introduce terminal and side epoxy groups, and then subjected to a ring-opening reaction with an amide-containing amine small molecule to convert the epoxy groups into polar segments containing hydroxyl and amide groups, thereby obtaining a siloxane-amide copolymer reaction solution that simultaneously has siloxane oligomeric segments, polyether hydrophilic segments and amide polar segments; S3. The reaction solution of the siloxamide copolymer obtained in step S2 is subjected to catalyst removal, ion exchange to remove metal ions, desalting, concentration and filtration in sequence. The pH is adjusted to 10 with 25% ammonia water to obtain a siloxamide copolymer modifier with a solid content of 0.5%-2%.

[0007] Further, in step S1, the molar ratio of α,ω-hydrogen-containing polydimethylsiloxane to monoallyl polyoxyethylene is 1:(0.9-1.1); the hydrosilylation reaction temperature is 80-90℃, and the reaction time is 3-6 hours; chloroplatinic acid accounts for 1-10 mg / kg of the mass of α,ω-hydrogen-containing polydimethylsiloxane.

[0008] Furthermore, the degree of polymerization of the α,ω-hydrogen-containing polydimethylsiloxane is 3-8, and the Si-H content based on the total mass of the α,ω-hydrogen-containing polydimethylsiloxane is 0.3%-1.2%; the number of polyoxyethylene units is 2-8, and the number average molecular weight is 200-600.

[0009] Further, in step S1, the α,ω-hydrogen-containing polydimethylsiloxane is first subjected to dehydration at 100-110℃ and 1-5kPa absolute pressure for 2-3 hours, and then subjected to 0.2μm filtration and H+ cation exchange to remove sodium, potassium, iron, copper, and zinc, so that the sodium, potassium, iron, copper, and zinc in the obtained α,ω-hydrogen-containing polydimethylsiloxane do not exceed 0.01mg / kg each; the monoallyl polyoxyethylene is first treated with 0.01%-0.02% activated carbon at 50-70℃ for 20-40 minutes, and then subjected to 0.45μm filtration and 3A molecular sieve dehydration until the water content does not exceed 300mg / kg before being added to the hydrosilylation reaction.

[0010] Further, in step S2, the epoxy-functionalized monomer is one of allyl glycidyl ether, epoxy-terminated polyether, and epoxy-terminated oligosiloxane; the amide-containing amine small molecule is one of β-alanine amide, N-(2-aminoethyl)acetamide, and glycine amide.

[0011] Furthermore, the obtained siloxane copolymer has a mass percentage of 5%-25% for the siloxane segment, 60%-90% for the polyether segment, and 1%-8% for the amide segment, with a number average molecular weight of 800-5000.

[0012] Further, in step S2, the molar ratio of the epoxy-functionalized monomer to the amide-amine small molecule is 1:(1-1.2); in the ring-opening reaction, the reaction temperature is 60-70℃ and the reaction time is 2-4 hours.

[0013] Further, in step S3, the catalyst removal step uses activated carbon adsorption to remove chloroplatinic acid; in the ion exchange to remove metal ions step, the metal is first complexed with 0.1-0.5% ethylenediaminetetraacetic acid tetrasodium salt, and then the metal ions are removed sequentially by passing through a strong acid cation exchange resin and a strong base anion exchange resin; the desalination step uses dialysis to remove salt until the conductivity is ≤5μS / cm.

[0014] Furthermore, a method for preparing a high-efficiency, low-damage silicon wafer polishing slurry includes the following steps: (1) Take 70% of the deionized water and add it to the mixing tank. Then add small-particle-size colloidal silica and large-particle-size colloidal silica in sequence and stir to disperse the dual-particle-size abrasive evenly. (2) Imidazole and siloxane copolymer modifier are diluted to prepare diluted imidazole solution and siloxane copolymer modifier solution respectively for later use. Then, the imidazole solution is added to the kettle and stirred. 2-amino-2-methyl-1,3-propanediol is added and stirred. Then, the siloxane copolymer modifier solution is added to the kettle and stirred. The modifier forms a weak coating hydration layer on the surface of large-particle abrasive under the action of the oligomeric siloxane segment and improves the dispersion and homogenization on the surface of small-particle abrasive. (3) Add the nonionic wetting agent, low molecular weight polyol and dispersant stabilizer in sequence and stir each time; (4) Adjust the pH to 9.8-11.2 with ammonia water, add the remaining deionized water and continue stirring for 10-20 minutes to obtain a fine polishing solution for chemical mechanical polishing and CMP polishing of single crystal silicon wafers.

[0015] Further, in step (1), the stirring speed is 300-500 r / min and the stirring time is 10-15 minutes; in step (2), the stirring speed of the imidazole dilution added to the reactor is 300-500 r / min and the stirring time is 5-10 minutes; the stirring speed after adding 2-amino-2-methyl-1,3-propanediol is 300-500 r / min and the stirring time is 5-10 minutes; the stirring speed after adding the siloxane copolymer modifier dilution is 300-500 r / min and the stirring time is 5-10 minutes.

[0016] Further, in step (2), the imidazole diluent is diluted with 5 times the amount of deionized water during the preparation of the imidazole solution; the concentration of the siloxane copolymer modifier diluent is diluted to 0.4%-1%.

[0017] Furthermore, the total amount of the nonionic wetting agent, low molecular weight polyol, and dispersant stabilizer added does not exceed 0.30 parts, and after the dispersant stabilizer is added, it forms a segmented adsorption with the modifier. The dispersant stabilizer does not replace the weak coating effect of the modifier on the large-particle abrasive.

[0018] The beneficial effects achieved by the present invention using the above scheme are as follows: This scheme proposes a high-efficiency, low-damage silicon wafer polishing slurry and its preparation method. By using small-particle-size and large-particle-size colloidal silica in a set mass ratio, the large-particle-size abrasive undertakes the main indentation and cutting action during the polishing process, stably removing material. At the same time, the small-particle-size abrasive is distributed in the gaps between the large-particle-size abrasive and in the area where the polishing pad contacts the silicon wafer, increasing the effective contact points and reducing the maximum stress of a single abrasive grain. The small-particle-size component can increase the overall specific surface area of ​​the abrasive, enhance the transport of the interfacial hydration layer and weak alkaline hydrolysis products, and make the softened layer on the silicon surface more uniformly removed under mechanical action. The large-particle-size component maintains strength and avoids insufficient removal efficiency due to the use of all fine abrasive. The dual-particle-size system complements each other in rheology and contact distribution, reducing micro-scratches and surface undulations caused by local hard contact, thereby improving both material removal rate and surface roughness in chemical mechanical polishing.

[0019] By constructing a composite organic base system using imidazole and 2-amino-2-methyl-1,3-propanediol, the nitrogen heterocycles contained in imidazole are selectively adsorbed on the silicon wafer surface, resulting in a non-uniform distribution of silicon bonds and silicon-oxygen bonds in silicon. This reduces the activation requirements for hydrolysis reactions and accelerates the transformation of silicon surfaces into soluble silanol species, thereby improving the efficiency of chemical removal during polishing. Simultaneously, the polyhydroxyamine structure of 2-amino-2-methyl-1,3-propanediol provides mild alkalinity, buffer capacity, and interfacial hydration, inhibiting local over-alkaliness, excessive hydrolysis, and non-uniform corrosion caused by excessive amounts of a single strong base or a single nitrogen-containing promoter. Imidazole is responsible for directionally accelerating the surface reaction, while 2-amino-2-methyl-1,3-propanediol is responsible for stabilizing the pH environment and regulating the electrostatic and adsorption states between the abrasive and the silicon wafer. Through a special ratio, the two are combined to maintain a dynamic balance between chemical and physical effects, reducing high surface roughness and localized corrosion defects.

[0020] By introducing α,ω-hydrogen-containing polydimethylsiloxane with oligomeric siloxane segments, monoallylic polyoxyethylene with short polyether segments, and siloxamide copolymers with terminal amide groups, the oligomeric siloxane segments form a thin coating through weak physical adsorption on the surface of large-particle colloidal silica, reducing the local impact stress when large-particle abrasives contact the silicon wafer. The short polyether segments construct a continuous hydration layer in an alkaline environment, improving the spreadability of the polishing slurry on the silicon wafer and polishing pad surfaces and enhancing the dispersion uniformity of small-particle abrasives. The terminal amide groups interact with the silanol groups, 2-amino-2-methyl-1,3-propanediol hydroxyl groups, and imidazole adsorption layer on the silicon wafer surface through hydrogen bonds, promoting the desorption of hydrolysis products from the silicon wafer surface and their entry into the liquid phase. The siloxamide copolymer modifier redistributes the contact state of the dual-particle abrasives and the reaction interface of the composite organic base, thereby reducing the micro-scratch density, improving surface uniformity, and enhancing the circulation and storage stability of the polishing slurry. Attached Figure Description

[0021] Figure 1 This is a process flow diagram of a high-efficiency, low-damage silicon wafer polishing slurry proposed in this invention; The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used together with the embodiments of the invention to explain the invention and do not constitute a limitation thereof. Detailed Implementation

[0022] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.

[0023] It should be noted that, unless otherwise specified, all chemical reagents involved in this invention were purchased through commercial channels.

[0024] Example 1: A high-efficiency, low-damage silicon wafer polishing slurry and its preparation method This embodiment prepares a high-efficiency, low-damage silicon wafer polishing slurry, and prepares a siloxane copolymer modifier in advance before the main material is prepared.

[0025] The preparation of the siloxane copolymer modifier begins with the purification of α,ω-hydrogen-containing polydimethylsiloxane. The raw material is dehydrated under reduced pressure at 100℃ and 1kPa for 2 hours. Then, it is filtered through 0.2μm and H+ cation exchange is used to remove sodium, potassium, iron, copper and zinc, so that each metal does not exceed 0.01mg / kg, thus establishing a low-metal basis for subsequent hydrosilylation.

[0026] In addition, monoallyl polyoxyethylene was treated with 0.01% activated carbon at 50°C for 20 minutes, then filtered through 0.45μm and dehydrated with 3A molecular sieve until the water content did not exceed 300mg / kg, so that both it and the aforementioned hydrogen-containing polysiloxane reached a low-water and low-metal state before feeding.

[0027] Based on this, the above-mentioned hydrogen-containing polysiloxane with a degree of polymerization of 3 and a Si-H content of 0.3% by its total mass was mixed with monoallyl polyoxyethylene with 2 polyoxyethylene units and a number average molecular weight of 200 at a molar ratio of 1:0.9 under nitrogen protection. Chloroplatinic acid at a mass of 1 mg / kg of the hydrogen-containing polysiloxane was added, and the reaction was continued at 80°C for 3 hours to complete the hydrosilylation, so that the Si-H groups formed Si-C bonds with the carbon-carbon double bonds and generated an oligomeric siloxane-polyether backbone intermediate. Then, allyl glycidyl ether is added to introduce terminal and side epoxy groups. Subsequently, ring-opening is carried out at a molar ratio of 1:1 between epoxy functional groups and β-alanine amide. The reaction is carried out at 60°C for 2 hours to convert the epoxy into polar segments containing hydroxyl and amide groups, thereby obtaining a siloxane-amide copolymer reaction solution that combines siloxane oligomer segments, polyether hydrophilic segments, and amide polar segments. The siloxane segment accounts for 25% by mass, the polyether segment accounts for 60%, the amide segment accounts for 1%, and the number average molecular weight is 800.

[0028] To convert the reaction solution into a usable stable modifier, chloroplatinic acid was then removed by adsorption with activated carbon, and the metal was complexed with 0.1% tetrasodium ethylenediaminetetraacetate. The metal ions were then removed by passing the solution through a strong acid cation exchange resin and a strong base anion exchange resin in sequence. After that, the solution was dialyzed to remove salt until the conductivity did not exceed 5 μS / cm, and then concentrated and filtered. Finally, the pH was adjusted to 10 with 25% ammonia water and the solid content was fixed at 0.5%, thus completing the preparation of the siloxane copolymer modifier for later use.

[0029] After preparing the siloxane copolymer modifier, we began to prepare the high-efficiency, low-damage silicon wafer polishing slurry. First, we measured 80 parts of deionized water and transferred 70% of it into a stirring tank. Then, we added 1 part of small-particle-size colloidal silica with a primary particle size of 30 nm and 4 parts of large-particle-size colloidal silica with a primary particle size of 80 nm in sequence. We stirred at 300 r / min for 10 minutes to uniformly disperse the dual-particle-size abrasive and leave an interface for subsequent modification.

[0030] Separately, 0.1 parts of imidazole were diluted with 5 times its weight of deionized water to prepare a liquid for later use. At the same time, 0.01 parts of the above-mentioned prepared modifier were diluted to a concentration of 0.4% for later use. First, the imidazole dilution was added to the reactor and stirred at 300 r / min for 5 minutes. Then, 0.2 parts of 2-amino-2-methyl-1,3-propanediol were added and stirred at 300 r / min for 5 minutes. Subsequently, the modifier dilution was introduced and stirred at 300 r / min for 5 minutes, so that the oligomeric siloxane segments formed a weak coating hydration layer on the surface of large-particle abrasives and improved the dispersion and homogenization on the surface of small-particle abrasives.

[0031] Then add 0.01 parts of polyether nonionic wetting agent, 0.1 parts of glycerol low molecular weight polyol, and 0.01 parts of low molecular weight polycarboxylate dispersant and stabilizer in sequence and stir each time. The total amount of the three should be controlled within 0.30 parts. After the dispersant and stabilizer is added, it forms segmented adsorption with the modifier without replacing its weak coating of large-particle abrasive.

[0032] Next, the pH of the system was adjusted to 9.8 with 0.1 parts of 25% ammonia water, the remaining deionized water was added, and the mixture was stirred for another 10 minutes to obtain the fine polishing solution for CMP of single crystal silicon wafers.

[0033] Example 2: A high-efficiency, low-damage silicon wafer polishing slurry and its preparation method This embodiment prepares a high-efficiency, low-damage silicon wafer polishing slurry, and prepares a siloxane copolymer modifier in advance before the main material is prepared.

[0034] The preparation of the siloxane copolymer modifier begins with the purification of α,ω-hydrogen-containing polydimethylsiloxane. The raw material is dehydrated under reduced pressure at 105℃ and 3kPa for 3 hours. Then, it is filtered through 0.2μm and H+ cation exchange is used to remove sodium, potassium, iron, copper and zinc, so that each metal does not exceed 0.01mg / kg, thus establishing a low-metal basis for subsequent hydrosilylation.

[0035] In addition, monoallyl polyoxyethylene was treated with 0.015% activated carbon at 60°C for 30 minutes, then filtered through 0.45μm and dehydrated with 3A molecular sieve until the water content did not exceed 300mg / kg, so that both it and the aforementioned hydrogen-containing polysiloxane reached a low-water and low-metal state before feeding.

[0036] Based on this, the above-mentioned hydrogen-containing polysiloxane with a degree of polymerization of 6 and a Si-H content of 0.8% by its total mass was mixed with monoallyl polyoxyethylene with 5 polyoxyethylene units and a number average molecular weight of 400 at a molar ratio of 1:1.0 under nitrogen protection. Chloroplatinic acid at a mass of 6 mg / kg of the hydrogen-containing polysiloxane was added, and the reaction was continued at 85°C for 5 hours to complete the hydrosilylation, causing the Si-H groups to form Si-C bonds with the carbon-carbon double bonds and generating an oligomeric siloxane-polyether backbone intermediate. Then... The process involves adding epoxy-terminated polyether to introduce terminal and side epoxy groups, followed by ring-opening at a molar ratio of 1:1.1 between epoxy functional groups and N-(2-aminoethyl)acetamide. The reaction is carried out at 65°C for 3 hours to convert the epoxy into polar segments containing hydroxyl and amide groups, thereby obtaining a siloxane-amide copolymer reaction solution that combines siloxane oligomer segments, polyether hydrophilic segments, and amide polar segments. The siloxane segment accounts for 25% by mass, the polyether segment 75%, the amide segment 5%, and the number average molecular weight is 2900.

[0037] To convert the reaction solution into a usable stable modifier, chloroplatinic acid was then removed by adsorption with activated carbon, and the metal was complexed with 0.3% ethylenediaminetetraacetic acid tetrasodium salt. The metal ions were then removed by passing the solution through a strong acid cation exchange resin and a strong base anion exchange resin in sequence. After that, the solution was dialyzed to remove salt until the conductivity did not exceed 5 μS / cm. The solution was then concentrated and filtered. Finally, the pH was adjusted to 10 with 25% ammonia water and the solid content was fixed at 1%, thus completing the preparation of the siloxane copolymer modifier for later use.

[0038] After preparing the siloxane copolymer modifier, we began to prepare the high-efficiency, low-damage silicon wafer polishing slurry. First, we measured 100 parts of deionized water and transferred 70% of it into a stirring tank. Then, we added 3 parts of small-particle-size colloidal silica with a primary particle size of 45 nm and 7 parts of large-particle-size colloidal silica with a primary particle size of 100 nm in sequence. We stirred at 400 r / min for 13 minutes to uniformly disperse the dual-particle-size abrasive and leave an interface for subsequent modification.

[0039] Separately, 0.2 parts of imidazole were diluted with 5 times its weight of deionized water to prepare a liquid for later use. At the same time, 0.02 parts of the above-mentioned prepared modifier were diluted to a concentration of 0.7% for later use. First, the imidazole dilution was added to the reactor and stirred at 400 r / min for 8 minutes. Then, 0.5 parts of 2-amino-2-methyl-1,3-propanediol were added and stirred at 400 r / min for 8 minutes. Subsequently, the modifier dilution was introduced and stirred at 400 r / min for 8 minutes, so that the oligomeric siloxane segments formed a weak coating hydration layer on the surface of large-particle abrasives and improved the dispersion and homogenization on the surface of small-particle abrasives.

[0040] Then, add 0.03 parts of acetylation diol nonionic wetting agent, 0.15 parts of sorbitol low molecular weight polyol, and 0.03 parts of low molecular weight polycarboxylate ammonium salt dispersant and stabilizer in sequence and stir each time. The total amount of the three should be controlled within 0.30 parts. After the dispersant and stabilizer is added, it forms segmented adsorption with the modifier without replacing its weak coating on large-particle abrasive.

[0041] Next, the pH of the system was adjusted to 10.5 with 0.3 parts of 25% ammonia water, the remaining deionized water was added, and the mixture was stirred for another 15 minutes to obtain the fine polishing solution for CMP of single crystal silicon wafers.

[0042] Example 3: A high-efficiency, low-damage silicon wafer polishing slurry and its preparation method This embodiment prepares a high-efficiency, low-damage silicon wafer polishing slurry, and prepares a siloxane copolymer modifier in advance before the main material is prepared.

[0043] The preparation of the siloxane copolymer modifier begins with the purification of α,ω-hydrogen-containing polydimethylsiloxane. The raw material is dehydrated under reduced pressure at 110℃ and 5kPa for 3 hours. Then, it is filtered through 0.2μm and H+ cation exchange is used to remove sodium, potassium, iron, copper and zinc, so that each metal does not exceed 0.01mg / kg, thus establishing a low-metal basis for subsequent hydrosilylation.

[0044] In addition, monoallyl polyoxyethylene was treated with 0.02% activated carbon at 70°C for 40 minutes, then filtered through 0.45μm and dehydrated with 3A molecular sieve until the water content did not exceed 300mg / kg, so that both it and the aforementioned hydrogen-containing polysiloxane reached a low-water and low-metal state before feeding.

[0045] Based on this, the above-mentioned hydrogen-containing polysiloxane with a degree of polymerization of 8 and a Si-H content of 1.2% by its total mass was mixed with monoallyl polyoxyethylene with 8 polyoxyethylene units and a number average molecular weight of 600 at a molar ratio of 1:1.1 under nitrogen protection. Chloroplatinic acid at a mass of 10 mg / kg of the hydrogen-containing polysiloxane was added, and the reaction was continued at 90°C for 6 hours to complete the hydrosilylation, so that the Si-H groups formed Si-C bonds with the carbon-carbon double bonds and generated an oligomeric siloxane-polyether backbone intermediate. Then, epoxy-terminated oligomeric siloxanes are added to introduce terminal and side epoxy groups. Subsequently, ring-opening is performed at a molar ratio of 1:1.2 between epoxy functional groups and glycine amides. The reaction is carried out at 70°C for 4 hours to convert the epoxy into polar segments containing hydroxyl and amide groups, thereby obtaining a siloxane-amide copolymer reaction solution that combines oligomeric siloxane segments, hydrophilic polyether segments, and polar amide segments. The siloxane segment accounts for 25% by mass, the polyether segment for 90%, the amide segment for 8%, and the number average molecular weight is 5000.

[0046] To convert the reaction solution into a usable stable modifier, chloroplatinic acid was then removed by adsorption with activated carbon, and the metal was complexed with 0.5% ethylenediaminetetraacetic acid tetrasodium salt. The metal ions were then removed by passing the solution through a strong acid cation exchange resin and a strong base anion exchange resin in sequence. After that, the solution was dialyzed to remove salt until the conductivity did not exceed 5 μS / cm. The solution was then concentrated and filtered. Finally, the pH was adjusted to 10 with 25% ammonia water and the solid content was fixed at 2%, thus completing the preparation of the siloxane copolymer modifier for later use.

[0047] After preparing the siloxane copolymer modifier, we began to prepare the high-efficiency, low-damage silicon wafer polishing slurry. First, we measured 120 parts of deionized water and transferred 70% of it into a stirring tank. Then, we added 5 parts of small-particle-size colloidal silica with a primary particle size of 60 nm and 10 parts of large-particle-size colloidal silica with a primary particle size of 120 nm in sequence. We stirred at 500 r / min for 15 minutes to uniformly disperse the dual-particle-size abrasive and leave an interface for subsequent modification.

[0048] Separately, 0.3 parts of imidazole were diluted with 5 times its weight of deionized water to prepare a liquid for later use. At the same time, 0.03 parts of the above-mentioned prepared modifier were diluted to a concentration of 1% for later use. First, the imidazole dilution was added to the reactor and stirred at 500 r / min for 10 minutes. Then, 0.8 parts of 2-amino-2-methyl-1,3-propanediol were added and stirred at 500 r / min for 10 minutes. Subsequently, the modifier dilution was introduced and stirred at 500 r / min for 10 minutes, so that the oligomeric siloxane segments formed a weak coating hydration layer on the surface of large-particle abrasives and improved the dispersion and homogenization on the surface of small-particle abrasives.

[0049] Then, add 0.05 parts of a nonionic wetting agent composed of polyether and acetylacetonate diol, 0.2 parts of xylitol low molecular weight polyol, and 0.05 parts of low molecular weight polycarboxylate dispersant and stabilizer in sequence, and stir each time. The total amount of the three should be controlled within 0.30 parts. After the dispersant and stabilizer is added, it forms segmented adsorption with the modifier without replacing its weak coating on large-particle abrasive.

[0050] Next, the pH of the system was adjusted to 11.2 with 0.5 parts of 25% ammonia water, the remaining deionized water was added, and the mixture was stirred for another 20 minutes to obtain a fine polishing solution for CMP of single crystal silicon wafers.

[0051] Comparative Example 1: The specific implementation method is the same as in Example 1, except that no silicone amide copolymer modifier is added, and all other raw material types, dosages, and operating conditions are consistent with those in Example 1.

[0052] This comparative example aims to verify the necessity of siloxamide copolymer modifiers by comparing their actual effects on reducing damage and improving dispersion, which can be quantitatively evaluated.

[0053] Comparative Example 2: The specific implementation method is the same as in Example 1, except that the siloxane copolymer modifier is replaced with an equal part by weight of polyvinylpyrrolidone (PVP K30, number average molecular weight of about 40,000), and all other raw materials, dosages and operating conditions are consistent with those in Example 1.

[0054] Polyvinylpyrrolidone is a commonly used nonionic polymeric dispersant, often used in polishing fluids to disperse abrasives and reduce surface tension. This comparative example aims to compare the advantages and disadvantages of the silicone amide copolymer modifier of this invention with similar functional substances already available on the market, and to verify whether the silicone amide copolymer modifier is irreplaceable.

[0055] Comparative Example 3: The specific implementation method is the same as in Example 1, except that: when preparing the polishing liquid, small-particle-size colloidal silica, large-particle-size colloidal silica, imidazole, and 2-amino-2-methyl-1,3-propanediol are not added.

[0056] This comparative example aims to verify whether there is a synergistic effect between the dual-particle-size abrasive system in Example 1 and the imidazole, AMPD, and siloxamide copolymer modifier.

[0057] Experimental Example 1: Test samples: Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3. The process flow of the examples is as follows: Figure 1 As shown.

[0058] Experimental Procedure: Prepare the solutions for each of the above samples. Dry 6-inch monocrystalline silicon wafers using the same cleaning process. Use a 910 polishing device with a damping cloth polishing pad at a pressure of 200 g / cm². Keep the head / disk speed constant according to the same batch process. Keep the polishing solution flow rate constant. Polish 3 wafers for each sample consecutively and take the average. Measure the thickness of the silicon wafer using a triangulation tester. Take 5 5μm×5μm areas from the same wafer and measure Ra using an atomic force microscope. Take the average value. Scan the entire wafer at 1000x magnification using an optical microscope to count the number of micro-scratches. Calculate the scratch rate by dividing the number of scratched wafers by the total number of polished wafers. Perform a static corrosion test. Use polishing solution of the same composition in a 50°C water bath. Soak the pretreated silicon wafer for 30 minutes. After ultrasonic cleaning and drying, weigh the difference in quality to calculate the static corrosion rate, which is used to determine localized chemical over-corrosion.

[0059] Table 1. Test results data for each sample The experimental results are shown in Table 1. The system using a combination of colloidal silica with large and small particle sizes, combined with imidazole and 2-amino-2-methyl-1,3-propanediol composite organic base, showed better material removal performance than the control system lacking the modifier, dual-particle-size abrasive, or composite base. Simultaneously, it exhibited lower surface roughness, fewer micro-scratches, and better controlled static corrosion. In Comparative Example 1, without the addition of the siloxamide modifier, the abrasive dispersion stability decreased, and the scratches related to the large-particle-size abrasive increased significantly. Comparative Example 2, which used a conventional polymeric dispersant, had some dispersing effect, but it was still inferior to the modifier of this invention in reducing micro-scratches and improving surface uniformity. Without the addition of dual-particle-size silica and composite organic base, there was almost no effective removal, only weak chemical corrosion, demonstrating that the mechanical action of the abrasive and the chemical promotion of the composite base jointly determine the polishing efficiency and surface quality.

[0060] The above comparison illustrates that the dual-particle-size abrasive, composite organic base, and siloxane modifier in this embodiment can work together to achieve a comprehensive effect of high removal, low roughness, low micro-scratches, and good storage dispersion, thus achieving a balance between efficiency and low damage in the fine polishing of silicon wafers.

[0061] Experimental Example 2: Test samples: Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, Comparative Example 3.

[0062] Experimental Procedure: Fresh liquid samples were divided into two portions. For the first portion, the surface tension was measured using the platinum plate method or platinum ring method. The liquid was then dropped onto the surface of a single-crystal silicon wafer using a contact angle meter, and the equilibrium contact angle was recorded to assess spreading and wetting. For the second portion, the apparent viscosity was measured using a rotational viscometer at 30°C. The initial particle size distribution and polydispersity index were then measured using a laser particle size analyzer / dynamic light scattering, and the absolute value of the abrasive surface potential was measured using a zeta potential meter. Subsequently, each sample was sealed and stored at 25°C. The median particle size, zeta potential, and surface tension were remeasured at 0, 7, and 14 days.

[0063] Table 2 Test results data for each sample The experimental results are shown in Table 2. Compared with the control examples without modifier, the series of examples showed lower surface tension and silicon wafer contact angle, indicating that nonionic wetting agents can effectively improve the spreading performance of polishing slurry on silicon wafer surfaces. Meanwhile, the apparent viscosity of each example did not increase significantly, while the median particle size shift, polydispersity index expansion, and potential decay during storage were all less than the control sample, and the supernatant turbidity was also lower. This indicates that low molecular weight polyols can improve interfacial hydration, and dispersant stabilizers can inhibit colloidal silica agglomeration. The synergistic effect of these two agents with the wetting agent maintained the uniform dispersion of the dual-particle-size abrasive without significantly increasing the system viscosity. Although the initial dispersion of control example 2, which used a high molecular weight dispersant instead of the modifier, was acceptable, the viscosity increased and the long-term particle size stability was inferior to the examples. Control example 1, without modifier, showed decreased spreading ability and more pronounced storage agglomeration. Overall, the results indicate that a small amount of nonionic wetting agent, low molecular weight polyol, and dispersant stabilizer together achieved a balanced improvement in wetting, hydration, and dispersion stability. Experimental Example 3: Test samples: Example 1, Example 2, Example 3, and control examples 1, 2, and 3.

[0064] Experimental Procedure: Products were prepared according to the processes described in each embodiment. Total solids content, pH, and the mass ratio of DLS particles were measured for verification. For each batch, 6-inch silicon wafers were polished using a 910 equipment, damping cloth, and the same process at 200 g / cm². The removal rate, Ra, and micro-scratching rate were recorded. Each batch of polishing solution was circulated three times in a closed-loop supply system at a fixed flow rate, with an equal amount of fresh solution added each time. After storage / circulation, the solids content, pH, median DLS particle size, removal rate, and Ra were re-measured.

[0065] Table 3 Test results data for each sample The experimental results are shown in Table 3. Examples 1 to 3 showed good intra-batch consistency in multiple repeated preparations. The fluctuation range of total solids content, pH value and polishing performance was small. The decrease in removal rate and the recovery of surface roughness after three cycles of polishing and static storage were both at a low level. No obvious agglomeration growth of abrasive particle size was observed. Overall, it showed stable repeatability and excellent cyclic storage stability.

[0066] In contrast, Comparative Example 1, lacking a siloxane copolymer modifier, showed a significant increase in removal rate decay after cycling, aggravated abrasive particle size shift, and a marked increase in surface roughness. Comparative Example 2, after replacing the modifier with polyvinylpyrrolidone, experienced a significant extension in filtration time and more pronounced performance degradation during cycling. Comparative Example 3, lacking dual-particle-size abrasives and a composite organic alkali system, had almost no effective polishing ability and could not meet the requirements for fine polishing.

[0067] The above comparison clearly demonstrates that the formulation and preparation process proposed in this invention not only use readily available raw materials and are easy to operate, but also maintain stable polishing performance during repeated use and long-term storage, showing good prospects for industrial scale-up. It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such process, method, article, or apparatus.

[0068] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

[0069] The present invention and its embodiments have been described above. This description is not restrictive, and the accompanying drawings are only one embodiment of the present invention; the actual structure is not limited thereto. In conclusion, if those skilled in the art are inspired by this description and design similar structures and embodiments without departing from the spirit of the invention, such designs should fall within the protection scope of the present invention.

Claims

1. A high-efficiency, low-damage silicon wafer polishing slurry, characterized in that: The raw materials include the following parts by weight: 1-5 parts of small-particle-size colloidal silica, 4-10 parts of large-particle-size colloidal silica, 0.1-0.3 parts of imidazole; 0.2-0.8 parts of 2-amino-2-methyl-1,3-propanediol; 0.01-0.03 parts of siloxane copolymer modifier; 0.01-0.05 parts of nonionic wetting agent; 0.1-0.2 parts of low-molecular-weight polyol; 0.01-0.05 parts of dispersion stabilizer; 0.1-0.5 parts of ammonia; and 80-120 parts of deionized water. The primary particle size of the small-particle-size colloidal silica is 30-60 nm, and the primary particle size of the large-particle-size colloidal silica is 80-120 nm. The nonionic wetting agent is selected from one or more of polyethers and acetylenic diols; The low molecular weight polyol is selected from one or more of glycerol, sorbitol, xylitol, and erythritol; The dispersing stabilizer is selected from one or more low molecular weight polycarboxylate salts or their ammonium salts; The ammonia solution is a 25% ammonia solution by mass.

2. The high-efficiency, low-damage silicon wafer polishing slurry according to claim 1, characterized in that: The preparation method of the siloxamide copolymer modifier includes the following steps: S1. Under nitrogen protection, α,ω-hydrogen-containing polydimethylsiloxane and monoallyl polyoxyethylene are reacted with chloroplatinic acid and hydrosilylation reaction to generate an oligomeric siloxane-polyether backbone intermediate. S2. The oligomeric siloxane-polyether backbone intermediate obtained in step S1 is subjected to an addition reaction with an epoxy-functionalized monomer, and then subjected to a ring-opening reaction with an amide-containing amine small molecule to convert the epoxy group into a polar chain segment containing hydroxyl and amide groups, resulting in a siloxane-amide copolymer reaction solution. S3. The reaction solution of the siloxamide copolymer obtained in step S2 is subjected to catalyst removal, ion exchange to remove metal ions, desalting, concentration and filtration in sequence. The pH is adjusted to 10 with 25% ammonia water to obtain a siloxamide copolymer modifier with a solid content of 0.5%-2%.

3. The high-efficiency, low-damage silicon wafer polishing slurry according to claim 2, characterized in that: In step S1, the molar ratio of α,ω-hydrogen-containing polydimethylsiloxane to monoallyl polyoxyethylene is 1:(0.9-1.1); the hydrosilylation reaction temperature is 80-90℃, and the reaction time is 3-6 hours; chloroplatinic acid accounts for 1-10 mg / kg of the mass of α,ω-hydrogen-containing polydimethylsiloxane.

4. The high-efficiency, low-damage silicon wafer polishing slurry according to claim 2, characterized in that: In step S1, the α,ω-hydrogen-containing polydimethylsiloxane is first dehydrated at 100-110℃ and 1-5kPa absolute pressure for 2-3 hours, and then filtered through 0.2μm; the monoallyl polyoxyethylene is first treated with 0.01%-0.02% activated carbon at 50-70℃ for 20-40 minutes, and then filtered through 0.45μm and dehydrated with 3A molecular sieve until the water content does not exceed 300mg / kg before being added to the hydrosilylation reaction.

5. The high-efficiency, low-damage silicon wafer polishing slurry according to claim 2, characterized in that: In step S2, the epoxy-functionalized monomer is one of allyl glycidyl ether, epoxy-terminated polyether, and epoxy-terminated oligosiloxane; the amide-containing amine small molecule is one of β-alanine amide, N-(2-aminoethyl)acetamide, and glycine amide.

6. The high-efficiency, low-damage silicon wafer polishing slurry according to claim 2, characterized in that: In step S2, the molar ratio of the epoxy-functionalized monomer to the amide-amine small molecule is 1:(1-1.2); in the ring-opening reaction, the reaction temperature is 60-70℃ and the reaction time is 2-4 hours.

7. The high-efficiency, low-damage silicon wafer polishing slurry according to claim 2, characterized in that: In step S3, the catalyst removal step uses activated carbon adsorption to remove chloroplatinic acid; in the ion exchange step to remove metal ions, the metal is first complexed with 0.1-0.5% ethylenediaminetetraacetic acid tetrasodium salt, and then the metal ions are removed sequentially by passing through a strong acid cation exchange resin and a strong base anion exchange resin; the desalination step uses dialysis to remove salt until the conductivity is ≤5μS / cm.

8. A method for preparing a high-efficiency, low-damage silicon wafer polishing slurry, the method being used to prepare the high-efficiency, low-damage silicon wafer polishing slurry according to any one of claims 1-7, characterized in that: Includes the following steps: (1) Take 70% of the deionized water and add it to the mixing tank. Then add small-particle-size colloidal silica and large-particle-size colloidal silica in sequence and stir to disperse the dual-particle-size abrasive evenly. (2) Prepare diluted imidazole and siloxamide copolymer modifier solutions by diluting them respectively. Then add the diluted imidazole solution to the reactor and stir. Add 2-amino-2-methyl-1,3-propanediol and stir. Then add the diluted siloxamide copolymer modifier solution to the reactor and stir. (3) Add the nonionic wetting agent, low molecular weight polyol and dispersant stabilizer in sequence and stir each time; (4) Adjust the pH to 9.8-11.2 with ammonia water, add the remaining deionized water and continue stirring for 10-20 minutes to obtain a fine polishing solution for chemical polishing and CMP polishing of single crystal silicon wafers.

9. The method for preparing a high-efficiency, low-damage silicon wafer polishing slurry according to claim 8, characterized in that: In step (1), the stirring speed is 300-500 r / min and the stirring time is 10-15 minutes; in step (2), the stirring speed of the imidazole dilution added to the reactor is 300-500 r / min and the stirring time is 5-10 minutes; the stirring speed after adding 2-amino-2-methyl-1,3-propanediol is 300-500 r / min and the stirring time is 5-10 minutes; the stirring speed after adding the siloxane copolymer modifier dilution is 300-500 r / min and the stirring time is 5-10 minutes.

10. The method for preparing a high-efficiency, low-damage silicon wafer polishing slurry according to claim 8, characterized in that: In step (2), the imidazole diluent is diluted with 5 times the amount of deionized water during the preparation of the imidazole solution; the concentration of the siloxane copolymer modifier diluent is diluted to 0.4%-1%.