Low-permeability butyl hot melt adhesive for bonding diving suit fabrics and its preparation method
By optimizing the material formulation and post-vulcanization crosslinking process, a chemical-physical dual crosslinking network structure is formed, which solves the shortcomings of existing butyl hot melt adhesives in terms of bonding strength, elongation at break and water vapor permeability, and achieves a balance between high strength and high airtightness, meeting the high water pressure environment requirements of diving suits.
Patent Information
- Application Number
- CN202611163736.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing butyl hot melt adhesives cannot simultaneously meet the high water pressure requirements of diving suits in terms of bonding strength, elongation at break, and water vapor permeability, and it is also difficult to balance bonding strength and airtightness.
An optimized material formulation and post-curing crosslinking process are used to form a chemical-physical dual crosslinking network structure, including butyl rubber, plasticizer, filler, vulcanizing agent and vulcanization accelerator, which are formed by high-temperature vulcanization.
It improves bonding strength and elongation at break, reduces water vapor permeability, and achieves a balance between high strength and high airtightness, meeting the performance requirements of diving suits in high water pressure environments.
Smart Images

Figure CN123107576A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of wastewater treatment technology, specifically to a low-permeability butyl hot melt adhesive for bonding diving suit fabrics and its preparation method. Background Technology
[0002] Currently, butyl hot melt adhesives commonly used for bonding wetsuit fabrics have the following drawbacks: The bonding strength is insufficient. The tensile strength of existing butyl hot melt adhesives is generally ≥0.15MPa, and the shear strength of some butyl hot melt adhesives is ≥0.5MPa, but it is difficult to meet the strength requirements of diving suits in high water pressure environments. Limited elongation at break; existing products typically have an elongation at break of over 400%, but this parameter is still insufficient for wetsuit applications. The water vapor transmission rate is relatively high, with existing products typically having a rate of ≤0.8 g / (m²·24h). Some high-performance products, such as butyl hot melt sealant, have a water vapor transmission rate as low as 0.17 g / (m²·24h), but this still cannot meet the stringent water tightness requirements of dry diving suits. It is difficult to achieve both bonding strength and air tightness. Traditional butyl hot melt adhesives often sacrifice air tightness and water tightness while improving bonding strength, and conversely, it is difficult to guarantee sufficient bonding strength while improving air tightness and water tightness.
[0003] Therefore, designing a butyl hot melt adhesive that improves bonding strength, increases elongation at break, and reduces water vapor permeability is the core problem that the inventors need to solve. Summary of the Invention
[0004] To address the shortcomings of existing technologies, the purpose of this invention is to provide a low-permeability butyl hot melt adhesive for bonding wetsuit fabrics and its preparation method, which can improve bonding strength, increase elongation at break, and reduce water vapor permeability.
[0005] The technical solution adopted by this invention to solve its technical problem is: a low-permeability butyl hot melt adhesive for bonding diving suit fabrics, wherein the components of the butyl hot melt adhesive include butyl rubber, plasticizer, filler, vulcanizing agent, and vulcanization accelerator, and the butyl rubber, plasticizer, filler, vulcanizing agent, and vulcanization accelerator are calculated by weight percentage as follows: butyl rubber 29.2%~34.4%, plasticizer 16.3%~19.1%, filler 40.3%~47.3%, vulcanizing agent 1.0%~1.2%, and vulcanization accelerator 5.2%~6.0%.
[0006] Optional. It also includes ethylene propylene diene monomer (EPDM) rubber, wherein the butyl rubber, plasticizer, filler, vulcanizing agent, vulcanization accelerator, and EPDM rubber, calculated by weight percentage, are 23.2%~28.4% butyl rubber, 16.3%~19.1% plasticizer, 40.3%~47.3% filler, 1.0%~1.2% vulcanizing agent, 5.2%~6.0% vulcanization accelerator, and 5.0%~8.0% EPDM rubber.
[0007] Furthermore, the butyl rubber includes at least one of brominated butyl rubber and cis-butadiene rubber.
[0008] Furthermore, the filler includes at least one of nano-calcium carbonate and carbon black.
[0009] Furthermore, the vulcanization accelerator includes at least one of zinc oxide and stearic acid.
[0010] A method for preparing a low-water-permeable butyl hot melt adhesive for bonding wetsuit fabrics, comprising the following steps: 1) Prepare and mix the ingredients according to the recipe; 2) Add butyl rubber and filler to a kneader and mix for 30 minutes at a temperature of 130℃ and a speed of 40Hz. 3) Add plasticizer, thickener and filler to the material obtained in the previous step, and mix for 45 minutes at a temperature of 120℃ and a speed of 40Hz. 4) Add vulcanizing agent and vulcanization accelerator to the material obtained in the previous step, and stir for 5 minutes; 5) Dispense the adhesive to obtain butyl hot melt adhesive.
[0011] Furthermore, the butyl hot melt adhesive is coated onto a layer of wetsuit fabric using a coating machine, and another layer of wetsuit fabric is laminated on the other side to produce a coated fabric semi-finished product. The coated fabric semi-finished product is then placed in a high-temperature environment of 180°C for 30 minutes for colloid vulcanization.
[0012] Furthermore, the vulcanized fabric is cooled at room temperature for 24 hours before being packaged.
[0013] The beneficial effects of this invention are: 1. This invention optimizes the material formulation and adopts a post-vulcanization crosslinking process to form a chemical-physical double crosslinking network structure, which solves the contradiction between bonding strength and air tightness in traditional butyl hot melt adhesives, and achieves the functions of improving bonding strength, increasing elongation at break, and reducing water vapor permeability. Attached Figure Description
[0014] Figure 1 This is a flowchart of the preparation, coating, and post-treatment methods of the present invention.
[0015] Explanation of reference numerals in the attached figures: 1-Sintering furnace; 2-Jacket; 3-Furnace chamber; 4-Cold water inlet; 5-Hot water outlet; 6-Vacuum tube; 7-Vacuum pump; 8-Exhaust pipe; 9-Exhaust fan; 10-Protective gas inlet pipe; 11-Cold water pipe; 12-Water collection tank; 13-Return water pipe; 14-Hot water pipe; 15-Proportional valve; 16-Hot water transfer pump; 17-PID controller; 18-Drying room. Detailed Implementation
[0016] To provide a more detailed understanding of the features and technical content of the embodiments of this disclosure, the implementation of the embodiments of this disclosure will be described in detail below with reference to the accompanying drawings. The accompanying drawings are for illustrative purposes only and are not intended to limit the embodiments of this disclosure. In the following technical description, for ease of explanation, several details are used to provide a full understanding of the disclosed embodiments. However, one or more embodiments may still be implemented without these details. In other cases, well-known structures and devices may be simplified in their depiction to simplify the drawings.
[0017] The terms "first," "second," etc., used in the specification, claims, and accompanying drawings of this disclosure are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate for the embodiments of this disclosure described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion.
[0018] In this disclosure, the terms "upper," "lower," "inner," "middle," "outer," "front," and "rear," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. These terms are primarily for better description of the embodiments of this disclosure and their implementations, and are not intended to limit the indicated devices, elements, or components to having a specific orientation, or to require them to be constructed and operated in a specific orientation. Furthermore, some of the aforementioned terms may be used to indicate other meanings besides orientation or positional relationship; for example, the term "upper" may in some cases indicate a dependency or connection relationship. Those skilled in the art can understand the specific meaning of these terms in the embodiments of this disclosure according to the specific circumstances.
[0019] Furthermore, the terms "set up," "connect," and "fix" should be interpreted broadly. For example, "connection" can be a fixed connection, a detachable connection, or an integral structure; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, or it can be an internal connection between two devices, components, or parts. Those skilled in the art can understand the specific meaning of the above terms in the embodiments of this disclosure according to the specific circumstances.
[0020] Unless otherwise stated, the term "multiple" means two or more.
[0021] It should be noted that, unless otherwise specified, the embodiments and features described in the present disclosure can be combined with each other.
[0022] A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The butyl hot melt adhesive comprises butyl rubber, plasticizer, filler, vulcanizing agent, and vulcanization accelerator. The weight percentages of butyl rubber, plasticizer, filler, vulcanizing agent, and vulcanization accelerator are as follows: butyl rubber 29.2%~34.4%, plasticizer 16.3%~19.1%, filler 40.3%~47.3%, vulcanizing agent 1.0%~1.2%, and vulcanization accelerator 5.2%~6.0%.
[0023] Optional. Also includes EPDM rubber, butyl rubber, plasticizer, filler, vulcanizing agent, vulcanization accelerator, and EPDM rubber by weight percentage as follows: butyl rubber 23.2%~28.4%, plasticizer 16.3%~19.1%, filler 40.3%~47.3%, vulcanizing agent 1.0%~1.2%, vulcanization accelerator 5.2%~6.0%, and EPDM rubber 5.0%~8.0%.
[0024] Furthermore, butyl rubber includes at least one of brominated butyl rubber and cis-butadiene rubber.
[0025] Furthermore, the filler includes at least one of nano-calcium carbonate and carbon black.
[0026] Furthermore, the vulcanization accelerator includes at least one of zinc oxide and stearic acid.
[0027] Example 1: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The components of the butyl hot melt adhesive include brominated butyl rubber, plasticizer, nano-calcium carbonate, vulcanizing agent, and zinc oxide. The weight percentages of brominated butyl rubber, plasticizer, nano-calcium carbonate, vulcanizing agent, and zinc oxide are as follows: brominated butyl rubber 34.4%, plasticizer 17.0%, nano-calcium carbonate 41.4%, vulcanizing agent 1.2%, and zinc oxide 6.0%.
[0028] Example 2: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The components of the butyl hot melt adhesive include butadiene rubber, plasticizer, carbon black, vulcanizing agent, and stearic acid. The weight percentages of butadiene rubber, plasticizer, carbon black, vulcanizing agent, and stearic acid are as follows: butadiene rubber 29.2%, plasticizer 18.5%, carbon black 46.1%, vulcanizing agent 1.0%, and stearic acid 5.2%.
[0029] Example 3: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The components of the butyl hot melt adhesive include brominated butyl rubber, butadiene rubber, plasticizer, nano-calcium carbonate, carbon black, vulcanizing agent, zinc oxide, and stearic acid. The weight percentages of brominated butyl rubber, butadiene rubber, plasticizer, nano-calcium carbonate, carbon black, vulcanizing agent, zinc oxide, and stearic acid are as follows: brominated butyl rubber 15.0%, butadiene rubber 14.2%, plasticizer 19.1%, nano-calcium carbonate 23.0%, carbon black 20.3%, vulcanizing agent 1.1%, zinc oxide 2.7%, and stearic acid 2.6%.
[0030] Example 4: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The components of the butyl hot melt adhesive include brominated butyl rubber, plasticizer, nano-calcium carbonate, carbon black, vulcanizing agent, and stearic acid. The weight percentages of brominated butyl rubber, plasticizer, nano-calcium carbonate, carbon black, vulcanizing agent, and stearic acid are as follows: brominated butyl rubber 31.8%, plasticizer 16.3%, nano-calcium carbonate 24.0%, carbon black 20.0%, vulcanizing agent 1.1%, and stearic acid 6.0%.
[0031] Example 5: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The components of the butyl hot melt adhesive include butadiene rubber, plasticizer, nano-calcium carbonate, vulcanizing agent, zinc oxide, and stearic acid. The weight percentages of butadiene rubber, plasticizer, nano-calcium carbonate, vulcanizing agent, zinc oxide, and stearic acid are as follows: butadiene rubber 33.0%, plasticizer 17.6%, nano-calcium carbonate 42.1%, vulcanizing agent 1.1%, zinc oxide 2.8%, and stearic acid 3.4%.
[0032] Example 6: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The butyl hot melt adhesive comprises brominated butyl rubber, plasticizer, nano-calcium carbonate, vulcanizing agent, zinc oxide, and EPDM rubber. The weight percentages of brominated butyl rubber, plasticizer, nano-calcium carbonate, vulcanizing agent, zinc oxide, and EPDM rubber are as follows: brominated butyl rubber 23.2%, plasticizer 17.2%, nano-calcium carbonate 44.4%, vulcanizing agent 1.0%, zinc oxide 6.0%, and EPDM rubber 8.0%.
[0033] Example 7: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The components of the butyl hot melt adhesive include butadiene rubber, plasticizer, carbon black, vulcanizing agent, stearic acid, and EPDM rubber. The weight percentages of butadiene rubber, plasticizer, carbon black, vulcanizing agent, stearic acid, and EPDM rubber are as follows: butadiene rubber 28.4%, plasticizer 18.0%, carbon black 41.4%, vulcanizing agent 1.2%, stearic acid 5.2%, and EPDM rubber 5.0%.
[0034] Example 8: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The components of the butyl hot melt adhesive include brominated butyl rubber, butadiene rubber, plasticizer, nano-calcium carbonate, carbon black, vulcanizing agent, zinc oxide, stearic acid, and EPDM rubber. The weight percentages of brominated butyl rubber, butadiene rubber, plasticizer, nano-calcium carbonate, carbon black, vulcanizing agent, zinc oxide, stearic acid, and EPDM rubber are as follows: brominated butyl rubber 13.0%, butadiene rubber 13.4%, plasticizer 19.1%, nano-calcium carbonate 21.0%, carbon black 20.3%, vulcanizing agent 1.1%, zinc oxide 2.6%, stearic acid 2.6%, and EPDM rubber 6.0%.
[0035] Example 9: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The butyl hot melt adhesive comprises brominated butyl rubber, plasticizer, nano-calcium carbonate, carbon black, vulcanizing agent, zinc oxide, and EPDM rubber. The weight percentages of brominated butyl rubber, plasticizer, nano-calcium carbonate, carbon black, vulcanizing agent, zinc oxide, and EPDM rubber are as follows: brominated butyl rubber 25.0%, plasticizer 16.3%, nano-calcium carbonate 22.0%, carbon black 21.3%, vulcanizing agent 1.1%, zinc oxide 5.6%, and EPDM rubber 8.0%.
[0036] Example 10: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The components of the butyl hot melt adhesive include butadiene rubber, plasticizer, nano-calcium carbonate, carbon black, vulcanizing agent, stearic acid, and EPDM rubber. The weight percentages of butadiene rubber, plasticizer, nano-calcium carbonate, carbon black, vulcanizing agent, stearic acid, and EPDM rubber are as follows: butadiene rubber 26.2%, plasticizer 17.8%, nano-calcium carbonate 23.5%, carbon black 20.0%, vulcanizing agent 1.1%, stearic acid 5.8%, and EPDM rubber 5.6%.
[0037] Example 11: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The butyl hot melt adhesive comprises brominated butyl rubber, plasticizer, carbon black, vulcanizing agent, zinc oxide, stearic acid, and EPDM rubber. The weight percentages of brominated butyl rubber, plasticizer, carbon black, vulcanizing agent, zinc oxide, stearic acid, and EPDM rubber are as follows: brominated butyl rubber 24.5%, plasticizer 18.2%, carbon black 43.5%, vulcanizing agent 1.1%, zinc oxide 2.8%, stearic acid 2.7%, and EPDM rubber 7.2%.
[0038] Example 12: A low-permeability butyl hot melt adhesive for bonding diving suit fabrics. The components of the butyl hot melt adhesive include brominated butyl rubber, butadiene rubber, plasticizer, nano-calcium carbonate, vulcanizing agent, zinc oxide, stearic acid, and EPDM rubber. The weight percentages of brominated butyl rubber, butadiene rubber, plasticizer, nano-calcium carbonate, vulcanizing agent, zinc oxide, stearic acid, and EPDM rubber are as follows: brominated butyl rubber 12.0%, butadiene rubber 13.8%, plasticizer 17.0%, nano-calcium carbonate 47.3%, vulcanizing agent 1.1%, zinc oxide 2.5%, stearic acid 2.3%, and EPDM rubber 5.0%.
[0039] See Figure 1 This is a flowchart of the preparation, coating, and post-treatment method of the present invention. A method for preparing a low-permeability butyl hot melt adhesive for bonding diving suit fabric includes the following steps: 1) Prepare and mix the ingredients according to the recipe; 2) Add butyl rubber and filler to a kneader and mix for 30 minutes at a temperature of 130℃ and a speed of 40Hz. 3) Add plasticizer, thickener and filler to the material obtained in the previous step, and mix for 45 minutes at a temperature of 120℃ and a speed of 40Hz. 4) Add vulcanizing agent and vulcanization accelerator to the material obtained in the previous step, and stir for 5 minutes; 5) Dispense the adhesive to obtain butyl hot melt adhesive.
[0040] Furthermore, butyl hot melt adhesive is coated onto a layer of wetsuit fabric using a coating machine, and another layer of wetsuit fabric is laminated on the other side to produce a coated fabric semi-finished product. The coated fabric semi-finished product is then placed in a high-temperature environment of 180°C for 30 minutes for adhesive vulcanization.
[0041] Furthermore, after the vulcanized fabric is cooled at room temperature for 24 hours, it is packaged to obtain the product.
[0042] This invention optimizes the material formulation and adopts a post-vulcanization crosslinking process to form a chemical-physical double crosslinking network structure, which solves the contradiction between bonding strength and air tightness in traditional butyl hot melt adhesives, and achieves the functions of improving bonding strength, increasing elongation at break, and reducing water vapor permeability.
[0043] The post-curing butyl hot melt adhesive of the present invention has a tensile strength of 2.4 MPa after curing and an elongation at break of over 800%, which is far superior to similar products in the prior art. This excellent mechanical property can ensure the structural integrity of the diving suit fabric under high water pressure.
[0044] The post-cured butyl hot melt adhesive of this invention has a water vapor transmission rate of less than 0.1 g / (m²·24h), which is far superior to the industry average. This low water vapor transmission rate can effectively prevent moisture penetration and maintain the dryness and heat preservation performance of the inside of the diving suit.
[0045] This invention forms a chemical-physical double cross-linked network structure through a post-curing process, which not only ensures high-temperature stability but also endows the material with self-healing ability. It solves the problem that traditional butyl hot melt adhesives cannot achieve both high strength and high airtightness at the same time, achieving a perfect combination of bonding strength and airtightness.
[0046] The butyl hot melt adhesive of the present invention has a moderate melt viscosity and good fluidity and wettability at 110°C, which facilitates coating and construction. At this temperature, no cross-linking reaction will occur. After coating, the material is transferred to a high temperature environment of 180°C for 30 minutes to completely vulcanize the butyl hot melt adhesive, which can firmly bond the double-layer diving suit together and has good processing performance.
[0047] The post-vulcanized butyl hot melt adhesive of the present invention is particularly suitable for bonding diving suit fabrics, and can meet the stringent requirements of underwater environment for material performance, and has broad application prospects.
[0048] The reaction mechanism of this invention is as follows: The ionic crosslinking reaction between the bromine sites of brominated butyl rubber (BIIR) and ZnO occurs at 180°C. The allyl bromide (—CH2—Br) active sites on the BIIR molecular chain undergo a dehalogenation reaction with zinc oxide (ZnO) in the formulation, generating a C—O—Zn bond structure and forming ionic crosslinks. Essentially, this reaction involves the substitution of Zn²⁺ atoms in ZnO with bromine atoms on the BIIR molecular chain, bridging the two polymer chains. Existing literature reports that the reaction rate between the bromine sites of BIIR and ZnO is significantly accelerated at high temperatures. Furthermore, ZnO not only acts as a vulcanizing agent in the BIIR vulcanization system but also synergistically forms a zinc stearate intermediate with stearic acid, further activating the vulcanization reaction. Under vulcanization conditions of 180°C for 30 min, the density of ionic crosslinks is much higher than under room temperature conditions.
[0049] The covalent cross-linking reaction of 2402 p-tert-butylphenolic resin with BIIR: 2402 p-tert-butylphenolic resin, a special resin with both tackifying and vulcanizing functions, can undergo a covalent cross-linking reaction with the active sites on the BIIR molecular chain during high-temperature vulcanization at 180℃. The reaction mechanism is as follows: the phenolic hydroxyl groups (—OH) and active hydroxymethyl groups (—CH2OH) contained in the 2402 resin molecule undergo a condensation reaction with the allyl bromide or unsaturated double bonds on the BIIR molecular chain under high temperature and the catalysis of the ZnO / stearic acid system, generating stable C—O—C ether bonds or C—C covalent cross-linking bonds. The bond energy of these covalent cross-linking bonds is much higher than that of physical entanglement and hydrogen bonds, which can significantly improve the cohesive strength and durability of the adhesive layer. Literature clearly demonstrates the dual role of 2402 resin in butyl rubber systems: "tackifying + vulcanization". Especially in the resin vulcanization system, phenolic resin reacts with rubber molecular chains through active functional groups to form a cross-linking network, and it is also a good tackifier and reinforcing agent.
[0050] Butadiene rubber (BR) double bonds participate in sulfur crosslinking reactions. In the BIIR / BR blend system, the BR molecular chain contains a large number of unsaturated carbon-carbon double bonds (—C=C—), which can participate in the vulcanization reaction at a high temperature of 180℃. The vulcanization system in the formulation (which may contain sulfur, accelerators, etc.) is activated at high temperature, causing the double bonds of the BR molecular chain to undergo open-chain crosslinking reactions, generating C—S—C sulfur crosslinking bonds. The sulfur crosslinking of BR complements the ionic and covalent crosslinking of BIIR, forming a three-dimensional interpenetrating double crosslinking network structure. The sulfur crosslinking network of the BR phase endows the rubber layer with good elasticity and dynamic fatigue properties, while the ionic / covalent crosslinking network of the BIIR phase provides excellent airtightness and aging resistance.
[0051] This cross-linked network has the following unique advantages: The ionic cross-linked network of the BIIR phase provides excellent air tightness and chemical stability, giving the material low water vapor permeability and good aging resistance; the covalent cross-linked network of the BR phase provides high elastic recovery rate and dynamic fatigue performance, improving the material's flexibility and processing performance; the partial interpenetration and physical entanglement of the two-phase interface enhance the interphase bonding force, effectively suppressing macroscopic phase separation, and achieving a synergistic balance between air tightness and mechanical properties.
[0052] The dual-function mechanism of 2402 p-tert-Butylphenol Formaldehyde Resin: In this formulation, 2402 p-tert-Butylphenol Formaldehyde Resin simultaneously functions as a tackifier and a vulcanizing agent, making it one of the key components that distinguishes this formulation from conventional butyl hot melt adhesives.
[0053] Tackifying Mechanism: The 2402 resin molecule contains a large number of phenolic hydroxyl groups (-OH) and polar groups such as p-tert-butyl groups. These groups can form strong intermolecular interactions with the butyl rubber molecular chain through hydrogen bonds and van der Waals forces. The aromatic ring structure of the resin molecule endows it with good compatibility. Its low molecular weight components can migrate to the surface during the cooling process of the rubber compound, providing excellent initial tack; while the high molecular weight components are embedded in the rubber matrix, giving the rubber compound long-lasting adhesion and retention.
[0054] Vulcanization Mechanism: In the presence of ZnO and stearic acid, the phenolic hydroxyl groups of 2402 resin can be activated by forming a phenolic resin-zinc oxide complex. The activated phenolic resin can undergo a nucleophilic substitution reaction with the allyl bromide on the BIIR molecular chain to generate phenolic ether crosslinks (Ar—O—C), thereby participating in the construction of the crosslink network. This resin vulcanization mechanism is an effective supplement to the direct vulcanization of BIIR by ZnO, increasing the crosslink density and enriching the types of crosslinks.
[0055] The synergistic reinforcement mechanism of nano-calcium carbonate + carbon black composite filler: This formulation uses a composite filler system composed of nano-calcium carbonate (nano-CaCO3) and carbon black (Carbon Black), which form a synergistic and complementary effect in terms of particle size, surface chemistry and reinforcement mechanism.
[0056] The reinforcing effect of nano-calcium carbonate: Nano-calcium carbonate particles have a diameter of 40~100 nm, a large specific surface area, and are rich in carbonate groups on the surface. After surface modification (such as stearic acid coating), nano-calcium carbonate particles can be well dispersed in the BIIR matrix. Through physical adsorption and mechanical anchoring effects, they combine with rubber molecular chains and play the following roles: as a rigid dispersed phase to bear and transfer stress, increasing tensile strength to 2.4 MPa; and as physical crosslinking points to restrict molecular chain slippage, keeping the elongation at break above 800%.
[0057] The reinforcing effect of carbon black: Carbon black has a primary particle size of 20-50 nm, with high structural density and abundant surface functional groups (carboxyl groups, phenolic hydroxyl groups, quinone groups, etc.). Carbon black particles form strong physical adsorption and chemical bonds with BIIR / BR molecular chains, constituting a "bonded rubber" layer that significantly improves modulus and tear strength. Furthermore, the high structural density of carbon black allows it to form an aggregate network within the matrix, effectively dispersing external forces.
[0058] Synergistic effect: Nano-calcium carbonate and carbon black form a gradient distribution in particle size—carbon black provides nanoscale (20~50 nm) reinforcement, while nano-calcium carbonate provides submicron (40~100 nm) filling, together constructing a multi-level reinforcing network from the molecular scale to the micron scale. At the same time, the lamellar carbon black aggregates can form tortuous gas diffusion paths in the matrix, significantly reducing water vapor permeability.
[0059] The synergistic activation mechanism of ZnO / stearic acid in vulcanization: The synergistic activation system composed of ZnO (zinc oxide) and stearic acid is the most classic and indispensable component combination in the vulcanization formulation of brominated butyl rubber. Its mechanism of action can be divided into the following levels: Zinc stearate formation: stearic acid (C 17 H 35 COOH) first reacts with ZnO to form zinc stearate Zn(C) 17 H 35 COO)2. This reaction begins during the mixing process, and the resulting zinc stearate has good solubility and dispersibility in the rubber matrix.
[0060] Direct sulfidation of BIIR: ZnO can directly react with allyl bromide (—CH2Br) on the BIIR molecular chain, removing ZnBr2 and forming C—O—Zn—O—C type ionic crosslinking bonds. This is the core reaction of BIIR sulfidation. The presence of zinc stearate can activate the ZnO surface and promote this reaction.
[0061] Auxiliary functions: ZnO also acts as an acid acceptor, neutralizing acidic byproducts such as HBr that may be generated during vulcanization, preventing their degradation and damage to the rubber molecular chains. Stearic acid, on the other hand, has an internal lubricating effect, improving filler dispersion and processing fluidity.
[0062] White oil plasticizing and antioxidant protection mechanism: White oil is a highly refined mixture of saturated alkanes and cycloalkanes, used as a plasticizer / processing oil in this formulation. Its mechanism of action includes: white oil molecules embedding between rubber molecular chains, increasing intermolecular distance, weakening intermolecular van der Waals forces, lowering the glass transition temperature (Tg), and improving the mobility of molecular chain segments, thereby improving the flowability and processing performance of the rubber compound; the saturated hydrocarbon structure of white oil makes it highly compatible with the nonpolar backbone of BIIR, making it less prone to migration and precipitation; an appropriate amount of white oil can adjust the hardness and flexibility of the rubber compound, ensuring that the final hot melt adhesive maintains sufficient softness and adhesion at room temperature.
[0063] Antioxidant protection mechanism: Antioxidants (such as hindered phenols and phosphites) protect rubber compounds from oxidative degradation through the following mechanisms: Hindered phenolic antioxidants (such as BHT, Irganox 1010, etc.) serve as primary antioxidants. Their phenolic hydroxyl groups can provide hydrogen atoms to capture and terminate peroxide radicals (ROO·) and alkoxy radicals (RO·) generated during oxidation, thus interrupting the free radical chain oxidation reaction. Phosphite antioxidants serve as secondary antioxidants, which can reduce hydroperoxides (ROOH) to non-radical alcohol products, forming a synergistic effect with the primary antioxidants. The presence of antioxidants plays a crucial role in ensuring the stability of the rubber compound's properties and its long-term weather resistance during post-curing.
[0064] During the melt mixing stage, the molecular chains of brominated butyl rubber (BIIR), butadiene rubber (BR), and ethylene propylene diene monomer (EPDM) become intertwined. During vulcanization, the crosslinking points of the three rubbers interpenetrate, forming an interpenetrating polymer network (IPN). The ionic crosslinking network of BIIR provides airtightness, the sulfur crosslinking of BR enhances tensile toughness, and the covalent crosslinking of EPDM provides weather resistance and low-temperature elasticity. These three crosslinking phases do not interfere with each other and have strong interfacial bonding. The airtightness of BIIR, the toughening effect of BR, and the weather resistance and elasticity of EPDM are achieved through co-vulcanization. The saturated main chain of EPDM is ozone-resistant and exhibits high low-temperature elasticity, thus balancing the low-temperature brittleness and poor weather resistance of butyl rubber.
[0065] The technical basis of this invention is shown in the following table: Table 1
[0066] The simultaneous achievement of tensile strength of 2.4 MPa and elongation at break ≥ 800% is due to the following three mechanisms: The BR phase provides flexible segments: BR molecular chains have a high cis structure and good flexibility, with a Tg of approximately −100°C. At room temperature, they exhibit a highly elastic state, providing the material with excellent molecular chain extension and resilience, ensuring the foundation for high elongation. Nano-calcium carbonate disperses stress: Modified nano-CaCO3 particles are uniformly dispersed in the BIIR matrix, forming numerous physical cross-linking points and stress concentration points. When the material is subjected to stress, the matrix surrounding the nanoparticles undergoes local yielding and cavitation, absorbing a large amount of energy and uniformly dispersing the stress to a larger volume of material, thereby improving strength while maintaining high elongation. Controllable slippage of the double crosslinked network: The ionic crosslinks of BIIR can undergo dynamic exchange of "break-reorganization" under stress, while the covalent crosslinks of BR provide permanent elastic recovery. The synergy of the two crosslinks enables the network to withstand large deformations without destructive breakage.
[0067] This formulation achieves a tensile strength of 2.4 MPa and an elongation at break of ≥ 800%. In a butyl hot melt adhesive system, these combined data (maintaining a certain strength despite high elongation) indicate that the formulation achieves a good balance between stiffness and flexibility. The strength of 2.4 MPa is within a reasonable range for a hot melt adhesive system with a relatively high plasticizer content, while the elongation of ≥ 800% demonstrates the significant effects of BR toughening and optimized dispersion of nanofillers.
[0068] The achievement of water vapor transmission rate (WVTR) < 0.1 g / (m²·24h) is based on the superposition effect of a triple barrier mechanism: BIIR's intrinsic low permeability: The BIIR molecular backbone is a saturated carbon chain with tightly packed segments and an extremely low free volume fraction (≈0.025). The solubility and diffusion coefficient of gas molecules within it are far lower than those of other general-purpose rubbers. This is the fundamental guarantee for achieving ultra-low WVTR. Carbon black lamellar tortuous path effect: Carbon black aggregates form a lamellar arrangement of impermeable phases in the matrix. Gas molecules are forced to bypass these obstacles during diffusion, which significantly increases the actual diffusion path length (torsional factor effect) and effectively reduces macroscopic permeability. Cross-linking densification: During the cross-linking process, the vulcanization active sites undergo cross-linking reactions, increasing the cross-linking density, restricting the mobility of molecular chain segments, and reducing the free volume, thereby achieving an additional improvement on the basic airtightness.
[0069] Data shows that WVTR < 0.1 g / (m²·24h), which has reached the advanced level of high-quality butyl waterproof sealant in the industry.
[0070] Achieving a peel strength > 1.5 N / mm involves two dimensions: interfacial adhesion and cohesive strength. Interfacial Adhesion: The low molecular weight components of 2402 resin can rapidly migrate to the adhesive / fabric interface during hot melt adhesive application. Through polar groups (phenolic hydroxyl groups), they form hydrogen bonds and van der Waals forces with amide and ether groups on the surface of the wetsuit fabric (typically nylon, spandex, or neoprene sponge, etc.), providing excellent initial tack and interfacial bonding. The moderate plasticizing effect of the white oil gives the adhesive good fluidity at the application temperature, allowing it to fully wet the microscopic irregularities of the fabric surface and increase the actual contact area. Cohesive strength: The BIIR / BR dual crosslinking network provides high cohesive strength to the adhesive layer bulk, causing peel failure to occur preferentially at the interface rather than within the adhesive layer. Further increases in crosslinking density during the crosslinking process continuously enhance cohesive strength, leading to a corresponding increase in peel strength.
[0071] The data shows a peel strength > 1.5 N / mm. This is above average for fabric / hot melt adhesive systems and is sufficient for waterproof sealing applications (non-structural bonding) in diving suits.
[0072] The 180℃×30min high-temperature post-curing process employed in this solution utilizes external forced heating to ensure the adhesive layer achieves full curing in a short time, resulting in a high degree of cross-linking. The process sequence can be summarized as: coating → bonding → high-temperature curing (180℃ / 30min). This process is characterized by high curing temperature, short curing time, and deep cross-linking, enabling the butyl rubber to form a strong chemical bond and physical anchor between the butyl rubber and the wetsuit fabric. This is the core process for achieving excellent overall performance in the final product.
[0073] Under high-temperature vulcanization conditions of 180℃, the three crosslinking reaction pathways in the BIIR / BR blend system are simultaneously activated and their rates are significantly accelerated. The bromine sites of BIIR react with ZnO to form ionic crosslinks, the phenolic hydroxyl groups of 2402 resin undergo covalent crosslinking with BIIR, and the double bonds of BR participate in sulfur crosslinking—these three crosslinking reactions are efficiently advanced at high temperatures, resulting in a significant increase in crosslinking density compared to curing at room temperature. Furthermore, the increased polymer chain segment mobility at high temperatures facilitates the uniform spatial distribution of crosslinking points and avoids crosslinking defects.
[0074] After high-temperature vulcanization at 180℃ for 30 minutes, the crosslinking density of the rubber layer reaches a high level, exhibiting complete rubber elastomer characteristics.
[0075] Weather resistance and dimensional stability are ensured by the following mechanisms: Chemical inertness of BIIR: The BIIR molecule has a saturated carbon backbone with only a small amount of active bromine in the side groups, resulting in excellent overall chemical stability. Compared to unsaturated rubbers (such as natural rubber and SBR), BIIR exhibits significantly stronger resistance to ozone, ultraviolet radiation, and thermo-oxidative aging. Free radical scavenging by antioxidants: The hindered phenolic primary antioxidant and phosphite auxiliary antioxidant added to the formulation form a synergistic protection system, which effectively inhibits free radical chain degradation during thermo-oxidative aging. Dimensional stability with high crosslinking density: The three-channel crosslinking system gives the adhesive layer a high crosslinking density. The full crosslinking between molecular chains restricts the irreversible slippage and creep of molecular chains under stress or temperature changes, thus ensuring dimensional stability. Carbon black's light-shielding effect: As an excellent light-shielding agent and ultraviolet absorber, carbon black can effectively shield the interior of the adhesive layer from ultraviolet rays, extending its outdoor service life.
[0076] This hot melt adhesive is used in bonding diving suit fabrics and must withstand harsh environments such as seawater immersion, temperature fluctuations, and sunlight exposure. Customer feedback after testing is positive. The multiple protective mechanisms of the BIIR matrix, antioxidants, and carbon black in the formula ensure long-term weather resistance.
[0077] The foregoing description and accompanying drawings fully illustrate embodiments of this disclosure to enable those skilled in the art to practice them. Other embodiments may include structural, logical, electrical, procedural, and other changes. The embodiments represent only possible variations. Individual components and functions are optional unless explicitly required, and the order of operation may vary. Parts and features of some embodiments may be included in or replace parts and features of other embodiments. Moreover, the terminology used in this application is for descriptive purposes only and is not intended to limit the claims. As used in the description of the embodiments and claims, the singular forms “a,” “an,” and “the” are intended to equally include the plural forms unless the context clearly indicates otherwise. Similarly, the term “and / or,” as used herein, means including one or more of the associated listed items and all possible combinations thereof. Additionally, when used in this application, the term "comprise" and its variations "comprises" and / or "comprising" refer to the presence of stated features, integrals, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integrals, steps, operations, elements, components, and / or groups thereof. Without further limitations, an element defined by the phrase "comprises a..." does not exclude the presence of other identical elements in the process, method, or apparatus that includes the element. In this document, each embodiment may focus on the differences from other embodiments, and similar or identical parts between embodiments can be referred to mutually. For methods, products, etc., disclosed in the embodiments, if they correspond to the method section disclosed in the embodiments, the relevant parts can be referred to the description of the method section.
[0078] The flowcharts and block diagrams in the accompanying drawings illustrate the architecture, functionality, and operation of possible implementations of systems, methods, and computer program products according to embodiments of the present disclosure. In this regard, each block in a flowchart or block diagram may represent a module, segment, or portion of code, which contains one or more executable instructions for implementing a specified logical function. In some alternative implementations, the functions marked in the blocks may occur in a different order than that shown in the drawings. For example, two consecutive blocks may actually be executed substantially in parallel, and they may sometimes be executed in reverse order, depending on the functions involved. In the descriptions corresponding to the flowcharts and block diagrams in the accompanying drawings, the operations or steps corresponding to different blocks may also occur in a different order than disclosed in the description, and sometimes there is no specific order between different operations or steps. For example, two consecutive operations or steps may actually be executed substantially in parallel, and they may sometimes be executed in reverse order, depending on the functions involved. Each block in a block diagram and / or flowchart, and combinations of blocks in a block diagram and / or flowchart, can be implemented using a dedicated hardware-based system that performs the specified function or action, or using a combination of dedicated hardware and computer instructions.
Claims
1. A low-water-permeability butyl hot melt adhesive for bonding diving suit fabrics, characterized in that: The butyl hot melt adhesive comprises butyl rubber, plasticizer, filler, vulcanizing agent, and vulcanization accelerator. The butyl rubber, plasticizer, filler, vulcanizing agent, and vulcanization accelerator are calculated by weight percentage as follows: butyl rubber 29.2%~34.4%, plasticizer 16.3%~19.1%, filler 40.3%~47.3%, vulcanizing agent 1.0%~1.2%, and vulcanization accelerator 5.2%~6.0%.
2. The low-permeability butyl hot melt adhesive for bonding diving suit fabric according to claim 1, characterized in that: It also includes ethylene propylene diene monomer (EPDM) rubber, wherein the butyl rubber, plasticizer, filler, vulcanizing agent, vulcanization accelerator, and EPDM rubber are calculated by weight percentage as follows: butyl rubber 23.2%~28.4%, plasticizer 16.3%~19.1%, filler 40.3%~47.3%, vulcanizing agent 1.0%~1.2%, vulcanization accelerator 5.2%~6.0%, and EPDM rubber 5.0%~8.0%.
3. The low-permeability butyl hot melt adhesive for bonding diving suit fabric according to claim 1 or 2, characterized in that: The butyl rubber includes at least one of brominated butyl rubber and cis-butadiene rubber.
4. A low-permeability butyl hot melt adhesive for bonding diving suit fabrics according to claim 1 or 2, characterized in that: The filler includes at least one of nano-calcium carbonate and carbon black.
5. A low-permeability butyl hot melt adhesive for bonding diving suit fabrics according to claim 1 or 2, characterized in that: The vulcanization accelerator includes at least one of zinc oxide and stearic acid.
6. A method for preparing butyl hot melt adhesive according to any one of claims 1-5, comprising the following steps: 1) Prepare and mix the ingredients according to the recipe; 2) Add butyl rubber and filler to a kneader and mix for 30 minutes at a temperature of 130℃ and a speed of 40Hz. 3) Add plasticizer, thickener and filler to the material obtained in the previous step, and mix for 45 minutes at a temperature of 120℃ and a speed of 40Hz. 4) Add vulcanizing agent and vulcanization accelerator to the material obtained in the previous step, and stir for 5 minutes; 5) Dispense the adhesive to obtain butyl hot melt adhesive.
7. The method for preparing a low-permeability butyl hot melt adhesive for bonding diving suit fabric according to claim 6, characterized in that: The butyl hot melt adhesive is coated onto a layer of wetsuit fabric using a coating machine, and another layer of wetsuit fabric is laminated on the other side to produce a coated fabric semi-finished product. The coated fabric semi-finished product is then placed in a high-temperature environment of 180°C for 30 minutes for adhesive vulcanization.
8. The method for preparing a low-permeability butyl hot melt adhesive for bonding diving suit fabric according to claim 7, characterized in that: The vulcanized fabric is cooled at room temperature for 24 hours before being packaged.