A high-bonding-strength, moisture-resistant white latex and its preparation method
By introducing vinyl acetate and highly branched saturated monocarboxylic acid vinyl ester comonomers into white glue, and by adding poly(N-vinylcaprolactam) grafted polyvinyl alcohol in stages, the problem of the attenuation of the bonding strength of white glue under humid and hot conditions is solved, and a balance between high bonding strength and stability is achieved.
Patent Information
- Application Number
- CN202611507452.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing polyvinyl acetate white latex adhesives exhibit bond strength degradation under long-term high temperature and high humidity conditions, making it difficult to simultaneously maintain emulsion polymerization stability, substrate wetting properties, and bond retention performance under humid and hot environments.
Vinyl acetate and highly branched saturated monocarboxylic acid vinyl ester containing 9 carbon atoms were used as comonomers. Poly(N-vinylcaprolactam) grafted polyvinyl alcohol was introduced as a functionalized protective colloid. By controlling the staged addition sequence during the emulsion polymerization process, it was ensured that part of the grafted protective colloid participated in the early emulsion stabilization, and the remainder acted on the particle interface after the latex particles were formed.
While maintaining the stability of emulsion polymerization and the wettability of the substrate, it reduces the hydration of the protective colloid interface under humid heat conditions, improves the humid heat resistance and bond strength retention of the adhesive layer, and enhances the bond strength and thermal stability of white latex after humid heat aging.
Smart Images

Figure CN123107578A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of water-based adhesives, and more particularly to a high-bonding-strength, moisture-resistant white latex and its preparation method. Background Technology
[0002] White glue is a type of water-based adhesive produced by emulsion polymerization of vinyl acetate as the main monomer. It features convenient application, good film-forming properties, fast bonding speed, and low volatile organic compound content, making it widely used in wood processing, furniture manufacturing, paper products, and decorative material bonding. Polyvinyl alcohol, due to its protective colloid and interfacial wetting properties, is often used in vinyl acetate emulsion polymerization to improve emulsion stability and enhance wetting and bonding performance on cellulose substrates such as white wood and plywood. To improve the water and heat resistance of traditional polyvinyl acetate white glue, current research typically employs the introduction of hydrophobic comonomers such as branched vinyl carboxylate and acrylate, or uses modified polyvinyl alcohol, reactive emulsifiers, self-crosslinking monomers, and external crosslinking agents to improve the hydrophobicity, crosslinking degree, or cohesive strength of the adhesive film at high temperatures. The above measures can improve the overall performance of white latex to a certain extent, but different modified components have different effects on emulsion polymerization stability, film formation process and substrate interface wetting performance. Simply increasing the degree of hydrophobicity or crosslinking density often makes it difficult to balance the normal bonding performance and the bonding retention performance under humid and hot conditions.
[0003] Especially under prolonged high temperature and humidity conditions, the numerous hydroxyl groups in polyvinyl alcohol (PVA) protective colloids still exhibit strong hydration properties. Water easily penetrates and accumulates between latex particles and at the interface between the adhesive layer and the substrate, causing water absorption and plasticization in this area. This leads to a decrease in the interparticle bonding force and a reduction in the cohesive strength of the adhesive layer. Existing technologies that improve hygrothermal resistance by reducing the hydrophilicity of PVA or adding hydrophobic or crosslinking components often result in decreased emulsion polymerization stability, insufficient substrate wetting, film embrittlement, or reduced normal bonding strength. Furthermore, current emulsion polymerization processes typically focus on adjusting the total amount of protective colloid and the monomer ratio, paying insufficient attention to the addition method of functionalized protective colloids at different stages of latex particle formation and their interfacial distribution. Therefore, how to maintain good polymerization stability and substrate wetting and bonding ability of white adhesives while reducing the continuous hydration of the protective colloid interface under hygrothermal conditions, and ensuring that functionalized protective colloids effectively act on the latex particle interface to improve the adhesion strength retention after hygrothermal aging, remains a key technical problem that existing polyvinyl acetate (PVC) white adhesives need to solve. Summary of the Invention
[0004] To address the aforementioned problems, this invention proposes a high-adhesion-strength, moisture-resistant white latex and its preparation method. This invention uses vinyl acetate and highly branched saturated monocarboxylic acid vinyl ester containing nine carbon atoms as comonomers, and introduces poly(N-vinylcaprolactam)-grafted polyvinyl alcohol as a functionalized protective colloid. By controlling the ratio of grafted colloid to ordinary polyvinyl alcohol and the staged addition sequence during emulsion polymerization, part of the grafted protective colloid participates in the early emulsion stabilization, while the remainder is added after latex particle formation and acts on the particle interface. Thus, while maintaining emulsion polymerization stability and substrate wetting and adhesion properties, it reduces the continuous hydration of the protective colloid interface under moisture-heat conditions, improving the moisture-heat resistance and adhesion strength retention of the adhesive layer.
[0005] This invention can be achieved through the following technical solutions:
[0006] A high-adhesion, moisture-resistant white latex, by weight, with a total monomer content of 100 parts, comprises the following raw materials: 86-90 parts vinyl acetate, 10-14 parts highly branched saturated monocarboxylic acid vinyl ester containing 9 carbon atoms, 3.2-4.8 parts poly(N-vinylcaprolactam)-grafted polyvinyl alcohol, 0.6-1.2 parts polyvinyl alcohol, 0.2-0.4 parts reactive emulsifier, 0.3-0.5 parts free radical initiator, 0.08-0.15 parts buffer, and 90-115 parts water; the mass ratio of poly(N-vinylcaprolactam)-grafted polyvinyl alcohol to polyvinyl alcohol is (3.0-6.0):1; the monomers comprise vinyl acetate and highly branched saturated monocarboxylic acid vinyl ester containing 9 carbon atoms; the poly(N-vinylcaprolactam)-grafted polyvinyl alcohol is prepared by the following method: 100 parts of a polymer with a degree of alcoholysis of 88-92... Polyvinyl alcohol (PVA) with an average degree of polymerization of 1200–1800 mol% was dissolved in water to form a PVA aqueous solution with a mass concentration of 8–12%. The pH of the system was adjusted to 1.5–2.5 using nitric acid under an inert atmosphere. 0.25–0.625 parts of cerium ammonium nitrate were added at 35–40°C, and Ce(IV) was pre-contaminated with PVA for 10–20 min. Then, 20–35 parts of N-vinylcaprolactam were added, and graft polymerization was carried out at 40–45°C for 2–3 h. After the reaction was completed, sodium bisulfite was added to terminate the reaction, and the pH of the system was adjusted to 5.0–6.5 to obtain poly(N-vinylcaprolactam)-grafted PVA. The amounts of poly(N-vinylcaprolactam)-grafted PVA and PVA are based on solid mass, and the water includes water carried over from the aqueous solutions of the raw materials.
[0007] Preferably, the highly branched saturated monocarboxylic acid vinyl ester containing 9 carbon atoms is a branched saturated monocarboxylic acid vinyl ester with 9 carbon atoms in the acid group and a quaternary carbon atom at the α-position adjacent to the carboxyl group; the reactive emulsifier is an anionic reactive emulsifier that contains both polymerizable carbon-carbon double bonds and sulfonate groups in its molecule.
[0008] Preferably, the white latex does not contain N-hydroxymethylacrylamide, diacetone acrylamide-adipic acid dihydrazide crosslinking system, or phthalate plasticizers.
[0009] A method for preparing a high-adhesion-strength, moisture-heat-resistant white latex includes the following steps:
[0010] S1. Polyvinyl alcohol, a first part of poly(N-vinylcaprolactam)-grafted polyvinyl alcohol accounting for 30-45% of the total mass of poly(N-vinylcaprolactam)-grafted polyvinyl alcohol, a reactive emulsifier, and a buffer are added to water to form a polymerization aqueous phase. After heating, a mixed monomer accounting for 8-12% of the total mass of the polymerization monomers and a portion of the free radical initiator are added to carry out seed polymerization to obtain a seed emulsion. The mixed monomer is composed of vinyl acetate and highly branched saturated monocarboxylic acid vinyl ester containing 9 carbon atoms.
[0011] S2. Continuously add the remaining mixed monomers and the remaining free radical initiator to the seed emulsion. When the cumulative amount of mixed monomers added reaches 60-70% of the total mass of the polymerizable monomers, start adding the remaining 55-70% of the second part of poly(N-vinylcaprolactam) grafted polyvinyl alcohol. When the cumulative amount of mixed monomers added reaches 85-95% of the total mass of the polymerizable monomers, the addition of the second part of poly(N-vinylcaprolactam) grafted polyvinyl alcohol is completed. Then continue to add the remaining mixed monomers to complete the emulsion polymerization.
[0012] S3. After the mixed monomers are added, the mixture is kept at a constant temperature and then polymerized to reduce the residual monomer content. After cooling and pH adjustment, the mixture is filtered to obtain a high-bonding-strength, moisture-resistant white latex.
[0013] Preferably, in S1, the mixed monomers and free radical initiator are added after the polymer aqueous phase is heated to 75-80°C, and the seed polymerization time is 15-30 min; in S2, the emulsion polymerization temperature is 76-82°C, and the remaining mixed monomers are added at a time of 2-4 h.
[0014] Preferably, in step S2, the second part of poly(N-vinylcaprolactam) grafted polyvinyl alcohol is prepared as an aqueous solution with a mass concentration of 6-10% before being added, and the addition time is 30-60 min; after the second part of poly(N-vinylcaprolactam) grafted polyvinyl alcohol is added, the mixed monomers are continued to be added for 15-30 min, so that the second part of poly(N-vinylcaprolactam) grafted polyvinyl alcohol forms an interface with the latex particles during the continued polymerization of the remaining monomers.
[0015] Preferably, in step S3, after the mixed monomers are added, the mixture is kept at 76-82°C for 30-60 min, and then a post-treatment initiation system composed of peroxide oxidant and bisulfite reducing agent is added to reduce the residual monomer content. Subsequently, the mixture is cooled to below 40°C, the pH of the system is adjusted to 4.5-6.0, and the solid content of the resulting white latex is adjusted to 48-53%.
[0016] The beneficial effects of this invention are:
[0017] This invention constructs a functionalized protective colloid that combines emulsion stability, substrate wetting, and hygrothermal response by grafting poly(N-vinylcaprolactam) segments onto the polyvinyl alcohol backbone. Compared to ordinary polyvinyl alcohol or a physical mixture of polyvinyl alcohol and poly(N-vinylcaprolactam), the grafting structure allows the poly(N-vinylcaprolactam) segments to act together with the polyvinyl alcohol protective colloid at the latex particle interface, reducing the migration or redistribution of independent polymers during film formation and hygrothermal processes. During room temperature coating and film formation, the polyvinyl alcohol backbone maintains its wetting and stabilizing effect on the white latex system and cellulose substrate. Upon entering a high-temperature and high-humidity environment, the grafted poly(N-vinylcaprolactam) segments undergo a hydration change, reducing the protective colloid interface's ability to continuously bind water. This inhibits water accumulation at latex particle boundaries and the colloid interface, mitigating plasticization and interfacial weakening caused by water absorption.
[0018] Building upon this foundation, the present invention further employs a segmented addition method of poly(N-vinylcaprolactam) grafted polyvinyl alcohol. Only a portion of the grafted protective colloid is used for seed polymerization and early emulsion stabilization, while the majority is added during the stage where latex particles have already formed and continue to grow. The remaining monomer polymerization continues after the grafted protective colloid is added. Thus, the functionalized protective colloid does not simply exist as an external polymer in the aqueous phase, but can more effectively act on the interface of the latex particles formed later, allowing the temperature-sensitive segments to concentrate their interfacial regulation role. Simultaneously, the copolymer latex matrix formed by vinyl acetate and highly branched saturated monocarboxylic acid vinyl ester containing nine carbon atoms provides excellent film-forming properties and cohesive stability under humid and hot conditions, allowing the structural advantages resulting from reduced interfacial hydration to be further transformed into overall strength retention of the adhesive layer. Therefore, this invention establishes a direct link between the molecular structure design of the grafted protective colloid and the timing of its addition during the emulsion polymerization stage, forming a continuous action mechanism of "graft structure stabilizing interface function - subsequent addition strengthening interface effect - reducing interface hydration under humid and hot conditions - mitigating plasticization of the adhesive layer - maintaining cohesion and bonding strength of the adhesive layer". While maintaining high normal bonding performance, it improves the ability of white latex to retain bonding strength and thermal stability after humid and hot aging. Attached Figure Description
[0019] The accompanying drawings are provided to further illustrate the invention and form part of the specification. They are used in conjunction with embodiments of the invention to explain the invention and do not constitute a limitation thereof. In the drawings:
[0020] Figure 1 The images show the microstructure of the white latex film; the left image shows the microstructure of the white latex film obtained in Comparative Example 1, and the right image shows the microstructure of the white latex film obtained in Example 1.
[0021] Figure 2 The microstructure changes of the white latex film before and after hydrothermal treatment are shown; among them, Figure 2 (a) shows the microstructure of the adhesive film before the wet heat treatment in Comparative Example 1. Figure 2 (b) shows the microstructure of the film of Comparative Example 1 after treatment at 60°C and 95% relative humidity for 72 h. Figure 2 (c) shows the microstructure of the film before the wet heat treatment in Example 1. Figure 2 (d) shows the microstructure of the film after being treated at 60°C and 95% relative humidity for 72 h in Example 1. Detailed Implementation
[0022] The following provides a detailed description of the embodiments of the present invention: These embodiments are implemented based on the technical solution of the present invention, and provide detailed implementation methods and processes. However, the scope of protection of the present invention is not limited to the following embodiments. Experimental methods in the following embodiments that do not specify specific conditions are generally performed under conventional conditions.
[0023] Example 1: A method for preparing a high-bonding-strength, moisture-resistant white latex, comprising the following steps:
[0024] S1. By mass, 100 parts of polyvinyl alcohol with a degree of hydrolysis of 88 mol% and an average degree of polymerization of 1200 were added to water and dissolved at 90°C to prepare an 8% polyvinyl alcohol aqueous solution. After cooling, nitrogen gas was introduced for 30 min, and the pH of the system was adjusted to 1.5 using nitric acid. 0.25 parts of cerium ammonium nitrate were added at 35°C and maintained for 10 min. Then, 20 parts of N-vinylcaprolactam were added within 30 min, and the temperature was raised to 40°C and reacted for 2 h. After the reaction was completed, 0.5 parts of sodium bisulfite were added to terminate the reaction, and the pH of the system was adjusted to 5.5 to obtain a poly(N-vinylcaprolactam) grafted polyvinyl alcohol aqueous solution. The following calculations are based on the mass of the grafted product solids.
[0025] S2. Based on a total monomer mass of 100 parts, the raw materials for white latex include 86 parts vinyl acetate, 14 parts C9 highly branched saturated monocarboxylic acid vinyl ester, 3.6 parts poly(N-vinylcaprolactam) grafted polyvinyl alcohol, 1.2 parts polyvinyl alcohol, 0.2 parts sodium allyl hydroxypropyl sulfonate, 0.3 parts ammonium persulfate, 0.08 parts sodium bicarbonate, and 90 parts water; the mass ratio of poly(N-vinylcaprolactam) grafted polyvinyl alcohol to polyvinyl alcohol is 3:1.
[0026] S3. Polyvinyl alcohol, 1.08 parts of poly(N-vinylcaprolactam) grafted polyvinyl alcohol, sodium allyl hydroxypropyl sulfonate and sodium bicarbonate were added to a portion of water and mixed. The mixture was heated to 75°C. Vinyl acetate / C9 highly branched saturated monocarboxylic acid vinyl ester mixed monomers accounting for 8% of the total mass of the monomers were added and 0.06 parts of ammonium persulfate were added. Seed polymerization was carried out for 15 min.
[0027] S4. Subsequently, the remaining mixed monomers were continuously added at 76℃, and the remaining 0.24 parts of ammonium persulfate were added simultaneously. The total addition time of the remaining mixed monomers was 2 h. When the cumulative amount of mixed monomers added reached 60% of the total mass of the polymerized monomers, the remaining 2.52 parts of poly(N-vinylcaprolactam) grafted polyvinyl alcohol were added. It was prepared in advance as a 6% aqueous solution and added within 30 min. When the addition was completed, the cumulative amount of mixed monomers added reached 85%. Then, the remaining mixed monomers were added for another 15 min.
[0028] S5. After the mixed monomers are added, the mixture is kept at 76℃ for 30 min. Then, 0.1 parts of tert-butyl hydrogen peroxide and 0.08 parts of sodium bisulfite are added for post-treatment. The mixture is then cooled to 35℃, and the pH of the system is adjusted to 4.5. The total amount of water added is adjusted and controlled to 90 parts with reserved water. The solid content of the resulting white latex is 53%.
[0029] Example 2: A method for preparing a high-bonding-strength, moisture-resistant white latex, comprising the following steps:
[0030] S1. 100 parts of polyvinyl alcohol with a degree of alcoholysis of 92 mol% and an average degree of polymerization of 1800 were added to water and dissolved at 90℃ to prepare a 12% (w / w) polyvinyl alcohol aqueous solution. After cooling, nitrogen gas was introduced for 30 min, and the pH of the system was adjusted to 2.5 with nitric acid. 0.625 parts of cerium ammonium nitrate were added at 40℃ and maintained for 20 min. Then, 35 parts of N-vinylcaprolactam were added within 30 min, and the reaction was carried out at 45℃ for 3 h. After the reaction was completed, 0.5 parts of sodium bisulfite were added to terminate the reaction, and the pH of the system was adjusted to 5.5 to obtain poly(N-vinylcaprolactam) grafted polyvinyl alcohol.
[0031] S2. Based on a total mass of 100 parts of polymerizable monomers, the raw materials for white latex include 90 parts of vinyl acetate, 10 parts of C9 highly branched saturated monocarboxylic acid vinyl ester, 3.2 parts of poly(N-vinylcaprolactam) grafted polyvinyl alcohol, 0.6 parts of polyvinyl alcohol, 0.4 parts of sodium allyl hydroxypropyl sulfonate, 0.5 parts of ammonium persulfate, 0.15 parts of sodium bicarbonate, and 115 parts of water; the mass ratio of poly(N-vinylcaprolactam) grafted polyvinyl alcohol to polyvinyl alcohol is 5.33:1;
[0032] S3. Add polyvinyl alcohol, 1.44 parts of poly(N-vinylcaprolactam) grafted polyvinyl alcohol, sodium allyl hydroxypropyl sulfonate and sodium bicarbonate to a portion of water, heat to 80°C, add mixed monomers accounting for 12% of the total mass of the monomers and 0.1 parts of ammonium persulfate, and carry out seed polymerization for 30 min.
[0033] S4. Subsequently, the remaining mixed monomers were continuously added at 82℃, and the remaining 0.4 parts of ammonium persulfate were added simultaneously. The total addition time of the remaining mixed monomers was 4 hours. When the cumulative amount of mixed monomers added reached 70% of the total mass of the polymerized monomers, the remaining 1.76 parts of poly(N-vinylcaprolactam) grafted polyvinyl alcohol were added. It was prepared into a 10% aqueous solution and added within 60 minutes. The feed rate of the mixed monomers was adjusted so that the cumulative amount of mixed monomers added reached 95% when the grafted polyvinyl alcohol was added. Then, the remaining mixed monomers were added for another 30 minutes to complete the total feeding.
[0034] S5. After the mixed monomers are added, the mixture is kept at 82℃ for 60 min. Then, 0.1 parts of tert-butyl hydroperoxide and 0.08 parts of sodium bisulfite are added for post-treatment. The mixture is then cooled to 35℃, and the pH of the system is adjusted to 6.0. The total amount of water added is adjusted and controlled to 115 parts with reserved water. The solid content of the resulting white latex is 48%.
[0035] Example 3: A method for preparing a high-bonding-strength, moisture-resistant white latex, comprising the following steps:
[0036] S1. 100 parts of polyvinyl alcohol with a degree of alcoholysis of 90 mol% and an average degree of polymerization of 1500 were added to water and dissolved at 90℃ to prepare a 10% (w / w) polyvinyl alcohol aqueous solution. After cooling, nitrogen gas was purged for 30 min, and the pH of the system was adjusted to 2.0 using nitric acid. 0.4375 parts of cerium ammonium nitrate were added at 37.5℃ and maintained for 15 min. Then, 27.5 parts of N-vinylcaprolactam were added within 30 min, and the reaction was carried out at 42.5℃ for 2.5 h. After the reaction was completed, 0.5 parts of sodium bisulfite were added to terminate the reaction, and the pH of the system was adjusted to 5.5 to obtain poly(N-vinylcaprolactam) grafted polyvinyl alcohol.
[0037] S2. Based on a total monomer mass of 100 parts, the raw materials for white latex include 88 parts of vinyl acetate, 12 parts of C9 highly branched saturated monocarboxylic acid vinyl ester, 4.8 parts of poly(N-vinylcaprolactam) grafted polyvinyl alcohol, 0.8 parts of polyvinyl alcohol, 0.3 parts of sodium allyloxyhydroxypropyl sulfonate, 0.4 parts of ammonium persulfate, 0.115 parts of sodium bicarbonate, and 102.5 parts of water; the mass ratio of poly(N-vinylcaprolactam) grafted polyvinyl alcohol to polyvinyl alcohol is 6:1.
[0038] S3. Polyvinyl alcohol, 1.8 parts of poly(N-vinylcaprolactam) grafted polyvinyl alcohol, sodium allyl hydroxypropyl sulfonate and sodium bicarbonate were added to a portion of water, the temperature was raised to 77.5℃, and mixed monomers accounting for 10% of the total mass of the monomers and 0.08 parts of ammonium persulfate were added to carry out seed polymerization for 22.5 min.
[0039] S4. Subsequently, the remaining mixed monomers were continuously added at 79℃, and the remaining 0.32 parts of ammonium persulfate were added simultaneously. The total addition time of the remaining mixed monomers was 3 h. When the cumulative amount of mixed monomers added reached 65% of the total mass of the polymerized monomers, the remaining 3 parts of poly(N-vinylcaprolactam) grafted polyvinyl alcohol were added. It was prepared into an 8% aqueous solution and added within 45 min, so that the cumulative amount of mixed monomers added reached 90% when the addition was completed. Then, the remaining mixed monomers were added for another 22.5 min.
[0040] S5. After the mixed monomers are added, the mixture is kept at 79°C for 45 min. Then, 0.1 parts of tert-butyl hydroperoxide and 0.08 parts of sodium bisulfite are added for post-treatment. The mixture is then cooled to 35°C, and the pH of the system is adjusted to 5.25. The total amount of water added is adjusted and controlled to 102.5 parts with reserved water. The solid content of the resulting white latex is 50.5%.
[0041] Comparative Example 1: The difference between this comparative example and Example 1 is that poly(N-vinylcaprolactam) grafted polyvinyl alcohol is not used; instead, ordinary polyvinyl alcohol of equal mass is used to replace poly(N-vinylcaprolactam) grafted polyvinyl alcohol.
[0042] The specific preparation method is as follows:
[0043] S1. Based on a total mass of 100 parts of polymerized monomers, the raw materials for white latex include 86 parts of vinyl acetate, 14 parts of C9 highly branched saturated monocarboxylic acid vinyl ester, 4.8 parts of polyvinyl alcohol, 0.2 parts of sodium allyl hydroxypropyl sulfonate, 0.3 parts of ammonium persulfate, 0.08 parts of sodium bicarbonate, and 90 parts of water.
[0044] S2. Polyvinyl alcohol, sodium allyl hydroxypropyl sulfonate and sodium bicarbonate are added to a portion of water and mixed. The mixture is heated to 75°C. Vinyl acetate / C9 highly branched saturated monocarboxylic acid vinyl ester mixed monomers, accounting for 8% of the total mass of the monomers, and 0.06 parts of ammonium persulfate are added. Seed polymerization is carried out for 15 min.
[0045] S3. Subsequently, the remaining mixed monomers were continuously added at 76℃, and the remaining 0.24 parts of ammonium persulfate were added simultaneously. The total addition time of the remaining mixed monomers was 2 h. After the mixed monomers were added, the mixture was kept at 76℃ for 30 min. 0.1 parts of tert-butyl hydroperoxide and 0.08 parts of sodium bisulfite were added for post-treatment. The mixture was then cooled to 35℃, and the pH of the system was adjusted to 4.5. The total amount of water added was adjusted and controlled to 90 parts with reserved water to obtain white latex solid.
[0046] Comparative Example 2: The difference between this comparative example and Example 1 is that a physical mixture of ordinary polyvinyl alcohol and poly(N-vinylcaprolactam) is used instead of poly(N-vinylcaprolactam) grafted polyvinyl alcohol.
[0047] The specific preparation method is as follows:
[0048] S1. Following the 100:20 ratio of polyvinyl alcohol to N-vinylcaprolactam in the preparation of poly(N-vinylcaprolactam)-grafted polyvinyl alcohol according to Example 1, the 3.6 parts of poly(N-vinylcaprolactam)-grafted polyvinyl alcohol in Example 1 were replaced with 3.0 parts of polyvinyl alcohol and 0.6 parts of poly(N-vinylcaprolactam), while retaining 1.2 parts of polyvinyl alcohol from the formulation of Example 1. Therefore, based on a total monomer mass of 100 parts, this comparative example uses 86 parts of vinyl acetate, 14 parts of C9 highly branched saturated monocarboxylic acid vinyl ester, 4.2 parts of polyvinyl alcohol, 0.6 parts of poly(N-vinylcaprolactam), 0.2 parts of sodium allyl hydroxypropyl sulfonate, 0.3 parts of ammonium persulfate, 0.08 parts of sodium bicarbonate, and 90 parts of water.
[0049] S2. Dissolve 0.9 parts of polyvinyl alcohol and 0.18 parts of poly(N-vinylcaprolactam) in a portion of water and mix them to obtain the first part of the physically mixed protective colloid; dissolve 2.1 parts of polyvinyl alcohol and 0.42 parts of poly(N-vinylcaprolactam) in a portion of water and mix them to prepare the second part of the physically mixed protective colloid; the first part and the second part of the physically mixed protective colloid correspond to 30% and 70% of the total amount of poly(N-vinylcaprolactam) grafted polyvinyl alcohol in Example 1, respectively;
[0050] S3. Add the remaining 1.2 parts of polyvinyl alcohol, the first part of the physical mixing protective colloid, sodium allyl hydroxypropyl sulfonate and sodium bicarbonate to a portion of water and mix. Heat to 75°C, add 8% of the total mass of the polymerizable monomers, vinyl acetate / C9 highly branched saturated monocarboxylic acid vinyl ester mixed monomers and 0.06 parts of ammonium persulfate, and carry out seed polymerization for 15 min.
[0051] S4. Subsequently, the remaining mixed monomers were continuously added at 76℃, and the remaining 0.24 parts of ammonium persulfate were added simultaneously. The total addition time of the remaining mixed monomers was 2 hours. When the cumulative amount of mixed monomers added reached 60% of the total mass of the polymerizable monomers, the second part of the physical mixed protective colloid was added and the addition was completed within 30 minutes, so that the cumulative amount of mixed monomers added reached 85% of the total mass of the polymerizable monomers when the addition was completed. Then, the remaining mixed monomers were added for another 15 minutes to complete the emulsion polymerization.
[0052] S5. After the mixed monomers are added, keep warm at 76℃ for 30 min, add 0.1 parts of tert-butyl hydroperoxide and 0.08 parts of sodium bisulfite for post-treatment, then cool to 35℃, adjust the pH of the system to 4.5, adjust with reserved water and control the total water addition to 90 parts to obtain white latex.
[0053] Comparative Example 3: The difference between this comparative example and Example 1 is that all poly(N-vinylcaprolactam) grafted polyvinyl alcohol was added to the initial aqueous polymerization phase along with polyvinyl alcohol, reactive emulsifier and buffer, and no more poly(N-vinylcaprolactam) grafted polyvinyl alcohol was added in the subsequent polymerization process.
[0054] The specific preparation method is as follows:
[0055] S1. By mass, 100 parts of polyvinyl alcohol with a degree of hydrolysis of 88 mol% and an average degree of polymerization of 1200 were added to water and dissolved at 90°C to prepare an 8% polyvinyl alcohol aqueous solution. After cooling, nitrogen gas was introduced for 30 min, and the pH of the system was adjusted to 1.5 using nitric acid. 0.25 parts of cerium ammonium nitrate were added at 35°C and maintained for 10 min. Then, 20 parts of N-vinylcaprolactam were added within 30 min, and the temperature was raised to 40°C and reacted for 2 h. After the reaction was completed, 0.5 parts of sodium bisulfite were added to terminate the reaction, and the pH of the system was adjusted to 5.5 to obtain a poly(N-vinylcaprolactam) grafted polyvinyl alcohol aqueous solution. The following calculations are based on the mass of the grafted product solids.
[0056] S2. Based on a total monomer mass of 100 parts, the raw materials for white latex include 86 parts vinyl acetate, 14 parts C9 highly branched saturated monocarboxylic acid vinyl ester, 3.6 parts poly(N-vinylcaprolactam) grafted polyvinyl alcohol, 1.2 parts polyvinyl alcohol, 0.2 parts sodium allyl hydroxypropyl sulfonate, 0.3 parts ammonium persulfate, 0.08 parts sodium bicarbonate, and 90 parts water; the mass ratio of poly(N-vinylcaprolactam) grafted polyvinyl alcohol to polyvinyl alcohol is 3:1.
[0057] S3. Polyvinyl alcohol, 3.6 parts of poly(N-vinylcaprolactam) grafted polyvinyl alcohol, sodium allyl hydroxypropyl sulfonate and sodium bicarbonate were added to a portion of water and mixed. The mixture was heated to 75°C. Vinyl acetate / C9 highly branched saturated monocarboxylic acid vinyl ester mixed monomers accounting for 8% of the total mass of the monomers were added and 0.06 parts of ammonium persulfate were added. Seed polymerization was carried out for 15 min.
[0058] S4. Subsequently, the remaining mixed monomers were continuously added at 76℃, and the remaining 0.24 parts of ammonium persulfate were added simultaneously. The total addition time of the remaining mixed monomers was 2 h, and then the remaining mixed monomers were added for another 15 min.
[0059] S5. After the mixed monomers are added, keep warm at 76℃ for 30 min, add 0.1 parts of tert-butyl hydroperoxide and 0.08 parts of sodium bisulfite for post-treatment, then cool to 35℃, adjust the pH of the system to 4.5, adjust with reserved water and control the total water addition to 90 parts to obtain white latex.
[0060] Comparative Example 4: The difference between this comparative example and Example 1 is that N-vinylpyrrolidone is used instead of N-vinylcaprolactam.
[0061] The specific preparation method is as follows:
[0062] S1. By mass, 100 parts of polyvinyl alcohol with a degree of alcoholysis of 88 mol% and an average degree of polymerization of 1200 were added to water and dissolved at 90℃ to prepare an 8% polyvinyl alcohol aqueous solution. After cooling, nitrogen gas was introduced for 30 min, and the pH of the system was adjusted to 1.5 using nitric acid. 0.25 parts of cerium ammonium nitrate were added at 35℃ and maintained for 10 min. Then, 20 parts of N-vinylpyrrolidone were added within 30 min, and the temperature was raised to 40℃ for 2 h. After the reaction was completed, 0.5 parts of sodium bisulfite were added to terminate the reaction, and the pH of the system was adjusted to 5.5 to obtain a poly(N-vinylpyrrolidone) grafted polyvinyl alcohol aqueous solution. The following calculations are based on the mass of the grafted product solids.
[0063] S2. Based on a total monomer mass of 100 parts, the raw materials for white latex include 86 parts vinyl acetate, 14 parts C9 highly branched saturated monocarboxylic acid vinyl ester, 3.6 parts poly(N-vinylpyrrolidone) grafted polyvinyl alcohol, 1.2 parts polyvinyl alcohol, 0.2 parts sodium allyl hydroxypropyl sulfonate, 0.3 parts ammonium persulfate, 0.08 parts sodium bicarbonate, and 90 parts water; the mass ratio of poly(N-vinylpyrrolidone) grafted polyvinyl alcohol to polyvinyl alcohol is 3:1.
[0064] S3. Polyvinyl alcohol, 1.08 parts of poly(N-vinylpyrrolidone) grafted polyvinyl alcohol, sodium allyl hydroxypropyl sulfonate and sodium bicarbonate were added to a portion of water and mixed. The mixture was heated to 75°C. Vinyl acetate / C9 highly branched saturated monocarboxylic acid vinyl ester mixed monomers, accounting for 8% of the total mass of the monomers, and 0.06 parts of ammonium persulfate were added. Seed polymerization was carried out for 15 min.
[0065] S4. Subsequently, the remaining mixed monomers were continuously added at 76℃, and the remaining 0.24 parts of ammonium persulfate were added simultaneously. The total addition time of the remaining mixed monomers was 2 h. When the cumulative amount of mixed monomers added reached 60% of the total mass of the polymerized monomers, the remaining 2.52 parts of poly(N-vinylpyrrolidone) grafted polyvinyl alcohol were added. It was prepared in advance as a 6% aqueous solution and added within 30 min. When the addition was completed, the cumulative amount of mixed monomers added reached 85%. Then, the remaining mixed monomers were added for another 15 min.
[0066] S5. After the mixed monomers are added, keep warm at 76℃ for 30 min, add 0.1 parts of tert-butyl hydroperoxide and 0.08 parts of sodium bisulfite for post-treatment, then cool to 35℃, adjust the pH of the system to 4.5, adjust with reserved water and control the total water addition to 90 parts to obtain white latex.
[0067] Performance testing
[0068] 1. Normal tensile shear strength
[0069] The test was conducted according to GB / T 33333-2016 standard. White beech wood was processed into test pieces measuring 100 mm × 25 mm × 5 mm, with the bonding surface aligned with the grain of the wood. Two test pieces were taken, and the white glue to be tested was evenly applied to the bonding surface of one of the test pieces at a rate of (180±10) g / m². 2 After applying the adhesive and allowing it to stand for 3 minutes, two specimens were overlapped with an overlap area of 25 mm × 25 mm and pressed together under a pressure of 0.8 MPa for 60 minutes. After depressurization, the specimens were cured for 7 days at a temperature of (23±2)℃ and a relative humidity of (50±5)%. Tensile shear tests were performed using a universal testing machine with a loading rate of 10 mm / min, and the maximum load F at specimen failure was recorded.
[0070] Tensile shear strength is calculated using the following formula:
[0071] Tensile shear strength σ = F / A;
[0072] In the formula, σ is the tensile shear strength, MPa; F is the maximum failure load, N; and A is the actual overlap area, mm. 2 .
[0073] Ten parallel specimens were tested in each group, and the arithmetic mean was taken as the normal tensile shear strength.
[0074] 2. Tensile shear strength and strength retention rate after damp heat aging
[0075] The specimens were prepared according to the above-described method for preparing tensile shear specimens under normal conditions and cured for 7 days at a temperature of (23±2)℃ and a relative humidity of (50±5)%. The cured specimens were then placed in a constant temperature and humidity chamber and treated for 72 hours at a temperature of (60±2)℃ and a relative humidity of (95±3)%. Immediately after the damp heat treatment, the specimens were removed and placed in a sealed polyethylene bag to cool to room temperature for 20 minutes. The tensile shear test was completed within 30 minutes of removing the specimens from the chamber. The test method and loading rate were the same as for the normal tensile shear strength test. Ten parallel specimens were tested in each group, and the average tensile shear strength after damp heat aging was calculated.
[0076] The strength retention rate after damp heat aging is calculated using the following formula:
[0077] Strength retention rate R = σ1 / σ0 × 100%;
[0078] In the formula, R is the strength retention rate after damp heat aging, %; σ1 is the tensile shear strength after damp heat aging, MPa; and σ0 is the normal tensile shear strength of the same group of samples, MPa.
[0079] 3. Moisture absorption and weight gain rate of the film under wet heat
[0080] Each group of white latex was uniformly coated onto the surface of a polytetrafluoroethylene (PTFE) plate and allowed to form a film naturally for 72 h at a temperature of (23±2)℃ and a relative humidity of (50±5)%. After peeling off the film, it was dried in a vacuum drying oven at 50℃ until constant weight. The resulting film was cut into 50 mm × 50 mm samples, with the dry film thickness controlled at (0.50±0.05) mm. The samples were then vacuum dried again at 50℃ until the mass change between two consecutive weighings did not exceed 0.2%. After cooling to room temperature, the initial mass m0 was measured. Subsequently, the film was placed in a constant temperature and humidity chamber at a temperature of (60±2)℃ and a relative humidity of (95±3)% for 72 h. Immediately after removal, it was placed in a sealed weighing bottle for cooling for 20 min, and weighed within 30 min after removal from the constant temperature and humidity chamber. The mass m1 after the damp heat treatment was recorded.
[0081] The rate of weight gain due to moisture absorption and heat, W, is calculated using the following formula:
[0082] W = (m1 - m0) / m0 × 100%;
[0083] In the formula, W is the moisture absorption and weight gain rate of the adhesive film under humid heat, %; m0 is the mass of the adhesive film before humid heat treatment, g; and m1 is the mass of the adhesive film after humid heat treatment, g.
[0084] Five parallel samples were tested in each group, and the average value was taken.
[0085] 4. Thermal shear creep displacement
[0086] White beech wood lapped specimens were prepared according to the normal tensile shear strength test method, with an overlap area of 25 mm × 25 mm, and cured for 7 days at a temperature of (23±2)℃ and a relative humidity of (50±5)%. The specimens were preheated in a constant temperature environment of 60℃ for 30 min to bring the entire bonded specimen to the test temperature. Subsequently, a constant shear stress of 0.10 MPa was applied along the shear direction of the lap surface, and the loading was continued at 60℃ for 120 min. The relative displacement of the two bonded specimens was recorded using a displacement measuring device at the start of loading and after 120 min of loading; the difference between the two displacements was taken as the hot shear creep displacement. If the bonded interface completely failed during the test, it was recorded as a failure.
[0087] Five parallel specimens were tested in each group. The average creep displacement of the specimens that did not completely fail was taken, and the number of specimen failures was recorded.
[0088] Table 1 Performance test results of white latex
[0089] sample Normal tensile shear strength / MPa Tensile shear strength after damp heat aging / MPa Strength retention rate after damp heat aging / % Film moisture absorption and weight gain rate (%) Hot shear creep displacement / mm Example 1 10.6 7.8 73.6 7.4 0.42 Example 2 11.0 8.5 77.3 6.6 0.35 Example 3 10.8 8.2 75.9 6.9 0.38 Comparative Example 1 10.0 5.1 51.0 12.8 0.78 Comparative Example 2 10.2 6.0 58.8 10.7 0.67 Comparative Example 3 10.5 6.8 64.8 8.8 0.56 Comparative Example 4 10.3 6.3 61.2 9.6 0.62
[0090] Table 1 shows that the white latex obtained in Examples 1-3 has a normal tensile shear strength of 10.6–11.0 MPa, which remains at 7.8–8.5 MPa after hygrothermal aging, with a strength retention rate of 73.6%–77.3%. Meanwhile, the moisture absorption weight gain of the film under hygrothermal conditions is only 6.6%–7.4%, and the hot shear creep displacement is 0.35–0.42 mm. These results indicate that the present invention does not simply improve performance by increasing the initial cohesive strength of the adhesive layer, but rather significantly reduces the moisture absorption and adhesion performance degradation of the film under hygrothermal conditions while maintaining a high normal bonding strength. This is because poly(N-vinylcaprolactam)-grafted polyvinyl alcohol combines the emulsion stability and substrate wetting effect of the polyvinyl alcohol backbone with the temperature-sensitive hydration characteristics of the poly(N-vinylcaprolactam) segments, reducing the continuous hydration of the protective colloid interface under hygrothermal conditions. Simultaneously, the highly branched saturated monocarboxylic acid vinyl ester containing nine carbon atoms improves the hydrophobicity and cohesive stability of the latex matrix under elevated temperatures. Furthermore, by adding most of the grafted protective colloid during the polymerization stage after the latex particles are formed, it can act more effectively on the latex particle interface, thereby forming a continuous relationship from interfacial moisture absorption inhibition to the maintenance of humid heat cohesion of the colloid layer. This shows that the various technical features are not simply superimposed, but work together to address the problem of easy hydration and instability of the protective colloid interface under humid heat conditions.
[0091] Compared to Example 1, Comparative Example 1, which completely replaced poly(N-vinylcaprolactam) grafted polyvinyl alcohol with ordinary polyvinyl alcohol, still achieved a normal tensile shear strength of 10.0 MPa, but its strength decreased to 5.1 MPa after hygrothermal aging, with a retention rate of only 51.0%, and the hygrothermal weight gain increased to 12.8%. This indicates that although ordinary polyvinyl alcohol can meet the requirements of emulsion stability and normal adhesion, it is prone to strong hydration and hygroscopic plasticization of the adhesive layer under hygrothermal conditions. This shows that introducing the poly(N-vinylcaprolactam) graft structure is an important factor in improving the hygrothermal adhesion retention. Comparative Example 2 physically mixed polyvinyl alcohol and poly(N-vinylcaprolactam). After hygrothermal aging, the strength and retention rate decreased to 6.0 MPa and 58.8%, respectively, while the hygroscopic weight gain increased to 10.7%. This indicates that simply adding both polymers to the system simultaneously cannot achieve the same effect as covalently grafted protective colloids. Covalent grafting is beneficial for stabilizing the temperature-sensitive segments at the latex particle interface along with the polyvinyl alcohol protective colloid. Comparative Example 3 added all of the poly(N-vinylcaprolactam)-grafted polyvinyl alcohol at the initial stage of polymerization. After hygrothermal aging, the strength retention rate decreased to 64.8%, and the hot shear creep displacement increased to 0.56 mm. This indicates that the timing of adding the grafted protective colloid affects its effective role in the latex system. This invention, by adding part of it pre-addition and adding most of the grafted protective colloid after the latex particles are formed, can further improve the adhesion strength retention under hygrothermal conditions. Comparative Example 4 used N-vinylpyrrolidone instead of N-vinylcaprolactam. After hygrothermal aging, the strength was only 6.3 MPa, the strength retention rate was 61.2%, the film's hygrothermal moisture absorption weight gain was 9.6%, and the hot shear creep displacement increased to 0.62 mm, all significantly worse than Example 1.
[0092] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A high-adhesion-strength, moisture-heat-resistant white latex, characterized in that, Based on mass parts, with a total monomer content of 100 parts, the raw materials for preparing white latex include 86-90 parts of vinyl acetate, 10-14 parts of highly branched saturated monocarboxylic acid vinyl ester containing 9 carbon atoms, 3.2-4.8 parts of poly(N-vinylcaprolactam)-grafted polyvinyl alcohol, 0.6-1.2 parts of polyvinyl alcohol, 0.2-0.4 parts of reactive emulsifier, 0.3-0.5 parts of free radical initiator, 0.08-0.15 parts of buffer, and 90-115 parts of water; the mass ratio of poly(N-vinylcaprolactam)-grafted polyvinyl alcohol to polyvinyl alcohol is (3.0-6.0):1; the monomers include vinyl acetate and highly branched saturated monocarboxylic acid vinyl ester containing 9 carbon atoms; the poly(N-vinylcaprolactam)-grafted polyvinyl alcohol is prepared by the following method: 100 parts of alcoholysis with a degree of 88-92 Polyvinyl alcohol (PVA) with an average degree of polymerization of 1200–1800 mol% was dissolved in water to form a PVA aqueous solution with a mass concentration of 8–12%. The pH of the system was adjusted to 1.5–2.5 using nitric acid under an inert atmosphere. 0.25–0.625 parts of cerium ammonium nitrate were added at 35–40°C, and Ce(IV) was pre-contaminated with PVA for 10–20 min. Then, 20–35 parts of N-vinylcaprolactam were added, and graft polymerization was carried out at 40–45°C for 2–3 h. After the reaction was completed, sodium bisulfite was added to terminate the reaction, and the pH of the system was adjusted to 5.0–6.5 to obtain poly(N-vinylcaprolactam)-grafted PVA. The amounts of poly(N-vinylcaprolactam)-grafted PVA and PVA are based on solid mass, and the water includes water carried over from the aqueous solutions of the raw materials.
2. The high-adhesion-strength, moisture-resistant white latex according to claim 1, characterized in that, The highly branched saturated monocarboxylic acid vinyl ester containing 9 carbon atoms is a branched saturated monocarboxylic acid vinyl ester with 9 carbon atoms in the acid group and a quaternary carbon atom at the α position adjacent to the carboxyl group; the reactive emulsifier is an anionic reactive emulsifier that contains both polymerizable carbon-carbon double bonds and sulfonate groups in its molecule.
3. The high-bonding-strength, moisture-resistant white latex according to claim 1, characterized in that, The white latex does not contain N-hydroxymethylacrylamide, diacetone acrylamide-adipic acid dihydrazide crosslinking system, or phthalate plasticizers.
4. A method for preparing the high-adhesion-strength, moisture-resistant white latex according to claim 1, characterized in that, Includes the following steps: S1. Polyvinyl alcohol, a first part of poly(N-vinylcaprolactam)-grafted polyvinyl alcohol accounting for 30-45% of the total mass of poly(N-vinylcaprolactam)-grafted polyvinyl alcohol, a reactive emulsifier, and a buffer are added to water to form a polymerization aqueous phase. After heating, a mixed monomer accounting for 8-12% of the total mass of the polymerization monomers and a portion of the free radical initiator are added to carry out seed polymerization to obtain a seed emulsion. The mixed monomer is composed of vinyl acetate and highly branched saturated monocarboxylic acid vinyl ester containing 9 carbon atoms. S2. Continuously add the remaining mixed monomers and the remaining free radical initiator to the seed emulsion. When the cumulative amount of mixed monomers added reaches 60-70% of the total mass of the polymerizable monomers, start adding the remaining 55-70% of the second part of poly(N-vinylcaprolactam) grafted polyvinyl alcohol. When the cumulative amount of mixed monomers added reaches 85-95% of the total mass of the polymerizable monomers, the addition of the second part of poly(N-vinylcaprolactam) grafted polyvinyl alcohol is completed. Then continue to add the remaining mixed monomers to complete the emulsion polymerization. S3. After the mixed monomers are added, the mixture is kept at a constant temperature and then polymerized to reduce the residual monomer content. After cooling and pH adjustment, the mixture is filtered to obtain a high-bonding-strength, moisture-resistant white latex.
5. The method for preparing high-adhesion-strength, moisture-resistant white latex according to claim 4, characterized in that, In S1, the mixed monomers and free radical initiator are added after the aqueous phase of polymerization is heated to 75-80°C, and the seed polymerization time is 15-30 min; in S2, the emulsion polymerization temperature is 76-82°C, and the remaining mixed monomers are added at a time of 2-4 h.
6. The method for preparing high-adhesion-strength, moisture-resistant white latex according to claim 4, characterized in that, In step S2, the second part of poly(N-vinylcaprolactam) grafted polyvinyl alcohol is prepared as an aqueous solution with a mass concentration of 6-10% before being added, and the addition time is 30-60 min. After the second part of poly(N-vinylcaprolactam) grafted polyvinyl alcohol is added, the mixed monomers are continued to be added for 15-30 min, so that the second part of poly(N-vinylcaprolactam) grafted polyvinyl alcohol forms an interface with the latex particles during the continued polymerization of the remaining monomers.
7. The method for preparing high-adhesion-strength, moisture-resistant white latex according to claim 4, characterized in that, In step S3, after the mixed monomers are added, the mixture is kept at 76–82°C for 30–60 min. Then, a post-treatment initiation system consisting of peroxide oxidant and bisulfite reducing agent is added to reduce the residual monomer content. The mixture is then cooled to below 40°C, the pH of the system is adjusted to 4.5–6.0, and the solid content of the resulting white latex is adjusted to 48–53%.