Adhesives, slurries, electrodes, and secondary batteries for secondary battery electrodes

By using binders with specific structures of (meth)acrylate-based and ethylene-based monomer units, the balance between electrolyte solubility and adhesion of binders in lithium secondary batteries was solved, improving the initial efficiency and cycle life of the battery and achieving high energy density battery performance.

CN123107580APending Publication Date: 2026-11-17HANSOL CHEM
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610656496.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-14
Filing Date
2026-05-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing lithium secondary battery adhesives struggle to balance slurry processability and electrolyte solubility, resulting in insufficient adhesion, which affects electrode dispersion and flexibility, and consequently impacts battery initial efficiency and cycle life.

Method used

Adhesives containing (meth)acrylate and ethylene monomer units with specific structures are used. By introducing sterically hindered side-chain functional groups and polar functional groups, their content is adjusted to suppress electrolyte solubility while maintaining good adhesion and flexibility.

Benefits of technology

Without reducing adhesion, the initial efficiency and cycle life of lithium secondary batteries were improved, and the amount of adhesive used was reduced, achieving high energy density battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to an adhesive, a slurry comprising the same, an electrode, and a secondary battery. The adhesive comprises a first monomer unit and a second monomer unit. The first monomer unit comprises: a (meth)acrylate monomer unit having a straight-chain hydrocarbon side chain having 1 to 12 carbon atoms, an ethylene monomer unit having an acyl group, or a combination thereof. The second monomer unit comprises: a (meth)acrylate monomer unit having a branched hydrocarbon side chain having 3 or more carbon atoms, a cyclic hydrocarbon side chain having 3 or more carbon atoms, or a combination thereof; an ethylene monomer unit having one or more aromatic ring side chains; or a combination thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an adhesive for a secondary battery electrode, a slurry comprising the adhesive, an electrode to which the adhesive is applied, and a secondary battery comprising the electrode, the adhesive comprising a copolymer containing (meth)acrylate monomer units. Background Technology

[0002] Lithium-ion batteries have high energy density and are widely used in portable devices in the electrical, electronic, communication, and computer fields. Their application is also expanding in high-capacity batteries for hybrid and electric vehicles. To achieve such high-capacity, long-life batteries, it is preferable to maximize the content of active materials and conductive agents in the electrodes while minimizing the content of binders. However, if the binder ratio is too low, the dispersibility of the active material / conductive agent, electrode adhesion, and electrode layer flexibility will decrease, leading to the shedding of active material from the current collector during charge and discharge, ultimately causing degradation of cycle characteristics. Therefore, a highly functional binder is needed that can simultaneously ensure dispersion stability, electrode adhesion, and electrode flexibility even in small quantities.

[0003] Polyvinylidene fluoride (PVDF), a representative fluorinated adhesive, exhibits minimal swelling in the electrolyte and readily maintains the electrode structure. However, it suffers from insufficient dispersibility of the conductive agent and inadequate adhesion to the electrode plates. Furthermore, due to the inherent stable structure of perfluorinated polymers, it cannot decompose naturally and accumulates in the natural environment, leading to various problems, including physiological issues. On the other hand, non-fluorinated adhesives such as hydrogenated acrylonitrile-butadiene (H-NBR), while offering improved flexibility, still suffer from insufficient adhesion.

[0004] Therefore, there is a need for an adhesive made from (meth)acrylate and vinyl monomers that can overcome the limitations of existing technologies, ensuring the dispersibility, plate adhesion, and flexibility of the electrode active material / conductive agent even with small amounts added, while avoiding the inherent problems of fluorinated adhesives. However, ordinary adhesives made from (meth)acrylate and vinyl monomers should be good in both slurry solvents and electrolytes, but in reality, as the solubility in slurry solvents increases, the solubility in electrolytes also increases, making it difficult to ensure the required physical properties.

[0005] Therefore, the adhesive of this invention introduces sterically hindered side-chain functional groups while maintaining solvent affinity for the slurry, thereby effectively suppressing electrolyte solubility. Furthermore, by precisely adjusting the content of sterically hindered functional groups and polar functional groups, the swelling degree and adhesion of the electrolyte are balanced, thereby improving the initial efficiency and cycle life of the lithium secondary battery.

[0006] Existing technical documents

[0007] Patent documents

[0008] Patent Document 1: Korean Patent Publication No. 10-2016-0040125 Summary of the Invention

[0009] Technical problems to be solved

[0010] Therefore, the purpose of this invention is to provide a fluorine-free adhesive that, while maintaining the processability of the slurry, inhibits excessive dissolution and swelling in the electrolyte, thereby improving the initial efficiency and cycle life of lithium secondary batteries without reducing the bonding strength.

[0011] Meanwhile, the present invention aims to provide a slurry composition that uses the above-mentioned binder to improve the characteristics of secondary batteries.

[0012] Meanwhile, the present invention aims to provide an electrode with excellent performance using the above-mentioned slurry composition and a low-cost, high-performance secondary battery containing the electrode.

[0013] However, the problems to be solved by the present invention are not limited to those mentioned above, and those skilled in the art will clearly understand from the following description other problems not mentioned.

[0014] Technical solution

[0015] The present invention provides an adhesive comprising a first monomer unit and a second monomer unit, wherein the first monomer unit comprises: a (meth)acrylate monomer unit having a straight-chain hydrocarbon side chain having 1 to 12 carbon atoms, an ethylene monomer unit having an acyl group, or a combination thereof; and the second monomer unit comprises: a (meth)acrylate monomer unit having a branched hydrocarbon side chain having 3 or more carbon atoms, a cyclic hydrocarbon side chain having 3 or more carbon atoms, or a combination thereof; an ethylene monomer unit having one or more aromatic cyclic side chains; or a combination thereof.

[0016] The adhesive provided in another aspect of this application further comprises: a third monomer unit comprising a (meth)acrylate monomer unit having a polar functional group substituted with a heteroatom, an ethylene monomer unit having a polar functional group substituted with a heteroatom, or a combination thereof.

[0017] Another aspect of this application provides a slurry comprising: the aforementioned binder; and an active substance.

[0018] Another aspect of this application provides an electrode comprising: a current collector; and an active material layer comprising the aforementioned adhesive formed on the current collector.

[0019] Another aspect of this application provides a secondary battery comprising the aforementioned electrodes.

[0020] The effects of the invention

[0021] The adhesive of the present invention maintains the processability of the slurry while inhibiting excessive dissolution and swelling in the electrolyte, thereby improving the initial efficiency and cycle life of lithium secondary batteries without reducing the bonding strength.

[0022] At the same time, the improved adhesion of the adhesive of the present invention can increase the amount of active material and conductive agent while reducing the amount of adhesive used, thereby enabling the provision of high energy density lithium secondary batteries at low cost. Detailed Implementation

[0023] The effects and functions of the present invention will be described in more detail below through specific embodiments. However, such embodiments are presented merely as examples of the invention and do not define the scope of the invention.

[0024] Prior to this, the terms or words used in this specification and claims should not be interpreted in their usual or dictionary meanings, but should be interpreted in accordance with the meanings and concepts consistent with the technical ideas of the invention, based on the principle that the inventors may appropriately define the concepts of the terms in order to best describe their invention.

[0025] Therefore, the embodiments described in this specification are only one of the most preferred embodiments of the present invention and do not represent all the technical ideas of the present invention. It should be understood that at the time of this application, there may be many equivalents and modifications that can replace them.

[0026] In this specification, unless the context clearly defines otherwise, singular expressions include plural expressions. Terms such as “comprising,” “having,” or “possessing” are intended to specify the presence of a implemented feature, number, step, constituent element, or combination thereof, and should be understood not to preclude the possibility of the presence or addition of one or more other features or numbers, steps, constituent elements, or combinations thereof.

[0027] In this specification, the terms “a to b” and “a ~ b” that indicate numerical ranges are defined as ≥ a and ≤ b.

[0028] An adhesive according to one aspect of this application may comprise a first monomer unit and a second monomer unit, wherein the first monomer unit comprises: a (meth)acrylate monomer unit having a straight-chain hydrocarbon side chain having 1 to 12 carbon atoms, an ethylene monomer unit having an acyl group, or a combination thereof; and the second monomer unit comprises: a (meth)acrylate monomer unit having a branched hydrocarbon side chain having 3 or more carbon atoms, a cyclic hydrocarbon side chain having 3 or more carbon atoms, or a combination thereof; an ethylene monomer unit having one or more aromatic cyclic side chains; or a combination thereof.

[0029] In one embodiment of this application, the adhesive of this application may be a block copolymer or a random copolymer.

[0030] The (meth)acrylate monomers refer to those with an α,β-unsaturated ester structure CH2=CR 1 C(=O)OR 2 (where R) 1 For H or CH3, R 2 Monomers whose basic skeleton is a hydrocarbon group or a substituted hydrocarbon group.

[0031] The vinyl monomers refer to monomers that directly contain terminal vinyl CH2=CHX (X is a bonded atom that is connected to substituents by C, O, N, etc.) in the main chain and do not have a (meth)acrylate structure.

[0032] For example, the acyl group can be a straight-chain aliphatic acyl group with 1 to 12 carbon atoms.

[0033] On the other hand, the aforementioned vinyl monomer units having linear aliphatic acyl groups having 1 to 12 carbon atoms can be formed by the polymerization of vinyl acetate.

[0034] In one embodiment of this application, the number of carbon atoms in the branched hydrocarbon side chain with 3 or more carbon atoms or the cyclic hydrocarbon side chain with 3 or more carbon atoms can be 3 or more and 22 or less.

[0035] For example, the number of carbon atoms in the branched hydrocarbon side chain with 3 or more carbon atoms or the cyclic hydrocarbon side chain with 3 or more carbon atoms can be 3 or more and 20 or less, 3 or more and 18 or less, 3 or more and 15 or less, or 3 or more and 12 or less.

[0036] In one embodiment of this application, the cyclic side chain with 3 or more carbon atoms may contain heteroatoms such as oxygen and nitrogen within the ring.

[0037] In one embodiment of this application, the (meth)acrylate monomer unit having a cyclic hydrocarbon side chain with 3 or more carbon atoms may include: a (meth)acrylate monomer unit having an aliphatic cyclic hydrocarbon side chain with 3 or more carbon atoms, a (meth)acrylate monomer unit having one or more aromatic cyclic side chains, or a combination thereof.

[0038] In one embodiment of this application, the adhesive may further comprise: a third monomer unit comprising a (meth)acrylate monomer unit having a heteroatom-substituted polar functional group, an ethylene monomer unit having the heteroatom-substituted polar functional group, an α,β-unsaturated polycarboxylic acid monomer unit, or a combination thereof.

[0039] In one embodiment of this application, the polar functional group may be a carboxylic acid group (-COOH), a sulfonic acid group (-SO3H), a phosphonic acid group (-PO3H2), a cyano group (-CN), a pyrrolidone group (-C4H6NO), an amide group (-CONH2), a hydroxyl group (-OH), an epoxy group (-C3H5O), or a caprolactam group (-C6H2O). 10 NO), oxazolidinone (-C3H4NO2), or combinations thereof.

[0040] The α,β-unsaturated polycarboxylic acid monomers refer to monomers having an unsaturated polycarboxylic acid structure with a double bond between the α and β carbons and containing two or more carboxylic acid groups (COOH), and may include their anhydride, salt, or ester forms.

[0041] For example, the polar functional group can be a carboxylic acid group (-COOH), a sulfonic acid group (-SO3H), a phosphonic acid group (-PO3H2), a cyano group (-CN), or a combination thereof.

[0042] In one embodiment of this application, the first monomer unit may be formed by polymerization of methyl(meth)acrylate, ethyl(meth)acrylate, n-propyl(meth)acrylate, n-butyl(meth)acrylate, n-pentyl(meth)acrylate, n-hexyl(meth)acrylate, n-heptyl(meth)acrylate, n-octyl(meth)acrylate, n-nonyl(meth)acrylate, n-decyl(meth)acrylate, n-undecyl(meth)acrylate, n-lauryl(meth)acrylate, vinyl acetate, or combinations thereof.

[0043] For example, the first monomer unit may be formed by polymerization of n-butyl (meth)acrylate, ethyl (meth)acrylate, n-lauryl (meth)acrylate, vinyl acetate, methyl (meth)acrylate, n-propyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, or combinations thereof.

[0044] On the other hand, the first monomer unit may be formed by polymerization of n-butyl (meth)acrylate, ethyl (meth)acrylate, n-lauryl (meth)acrylate, vinyl acetate, or a combination thereof.

[0045] In one embodiment of this application, the branched hydrocarbon side chain with 3 or more carbon atoms or the aliphatic cyclic hydrocarbon side chain with 3 or more carbon atoms can be isopropyl, isobutyl, isopentyl, tert-butyl, neoopentyl, 2-ethylhexyl, isooctyl, cyclohexyl, isobornyl, tert-pentyl, tert-hexyl, 3-methylbutyl, 2-propylheptyl, cycloheptyl, norbornyl, or combinations thereof.

[0046] In one embodiment of this application, the (meth)acrylate monomer unit having a branched hydrocarbon side chain having 3 or more carbon atoms, an aliphatic cyclic hydrocarbon side chain having 3 or more carbon atoms, or a combination thereof, can be composed of isopropyl (meth)acrylate, isobutyl (meth)acrylate, isopentyl (meth)acrylate, tert-butyl (meth)acrylate, neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, isolauryl (meth)acrylate, or cyclopentyl (meth)acrylate. It is formed by the polymerization of (meth)acrylate, cyclohexyl(meth)acrylate, isobornyl(meth)acrylate, dicyclopentadienyl(meth)acrylate, tetrahydrofurfuryl(meth)acrylate, or combinations thereof.

[0047] For example, the (meth)acrylate monomer unit having a branched hydrocarbon side chain with 3 or more carbon atoms, an aliphatic cyclic hydrocarbon side chain with 3 or more carbon atoms, or a combination thereof, can be formed by polymerization of tert-butyl(meth)acrylate, 2-ethylhexyl(meth)acrylate, isobornyl(meth)acrylate, isooctyl(meth)acrylate, isononyl(meth)acrylate, isodecyl(meth)acrylate, cyclohexyl(meth)acrylate, dicyclopentadienyl(meth)acrylate, tetrahydrofurfuryl(meth)acrylate, or a combination thereof.

[0048] On the other hand, the (meth)acrylate monomer unit having a branched hydrocarbon side chain with 3 or more carbon atoms, an aliphatic cyclic hydrocarbon side chain with 3 or more carbon atoms, or a combination thereof, can be formed by polymerization of tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate, or a combination thereof.

[0049] In one embodiment of this application, the (meth)acrylate monomer unit having one or more aromatic ring side chains can be formed by polymerization of benzyl (meth)acrylate, phenyl (meth)acrylate, 3-phenoxybenzyl (meth)acrylate, o-phenylphenoxyethyl (meth)acrylate, 1-naphthyl (meth)acrylate, or combinations thereof.

[0050] For example, the (meth)acrylate monomer unit having one or more aromatic ring side chains can be formed by polymerization of benzyl (meth)acrylate, phenyl (meth)acrylate, 3-phenoxybenzyl (meth)acrylate, or combinations thereof.

[0051] In one embodiment of this application, the ethylene monomer unit having one or more aromatic ring side chains can be formed by polymerization of styrene, α-methylstyrene, or combinations thereof.

[0052] For example, the ethylene monomer unit having one or more aromatic ring side chains can be formed by the polymerization of styrene.

[0053] In one embodiment of this application, the third monomer unit may be composed of methacrylic acid, acrylic acid, N-vinylpyrrolidone, acrylonitrile, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, acrylamide, N,N-dimethylacrylamide, glycidyl methacrylate, N-vinylcaprolactam, 2-oxazolidin-5-ylmethacrylate, 2-cyanoethyl methacrylate, 2-acrylamido-2-methylpropane sulfonic acid, carboxyethyl acrylate, or maleic acid. It is formed by the polymerization of aconitic acid, itaconic acid, fumaric acid, aconitic acid, vinylbenzoic acid, vinylsulfonic acid, 4-styrenesulfonic acid, vinylphosphonic acid, N-methylacrylamide, or combinations thereof.

[0054] For example, the third monomer unit may be formed by polymerization of methacrylic acid, N-vinylpyrrolidone, acrylic acid, acrylonitrile, 2-hydroxyethyl methacrylate, glycidylmethacrylate, or combinations thereof.

[0055] On the other hand, the third monomer unit may be formed by polymerization of methacrylic acid, N-vinylpyrrolidone, or a combination thereof.

[0056] In one embodiment of this application, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of the first monomer unit can be 20 mol% or more and 80 mol% or less, the content of the second monomer unit can be 20 mol% or more and 80 mol% or less, and the content of the third monomer unit can be 0 mol% or more and 15 mol% or less.

[0057] For example, in the adhesive, based on the total molar percentage of the first monomer unit, the second monomer unit, and the third monomer unit of 100 mol%, the content of the first monomer unit can be 20 mol% or more and 70 mol% or less, 25 mol% or more and 80 mol% or less, 25 mol% or more and 70 mol% or less, 20 mol% or more and 30 mol% or less, 30 mol% or more and 50 mol% or less, 50 mol% or more and 70 mol% or less, 20 mol% or more and 25 mol% or less, 25 mol% or more and 45 mol% or less, or 45 mol% or more and 65 mol% or less.

[0058] When the content of the first single cell is greater than the range of this application, the battery will excessively absorb electrolyte, resulting in a decrease in adhesion and possible detachment from the current collector. Furthermore, the slurry viscosity will increase sharply, and the coating thickness will be uneven, which may lead to a decrease in electrode dimensional stability.

[0059] Conversely, when the content of the first monomer unit is lower than the range of this application, the adhesion between the binder-current collector and the binder-active material is insufficient, which makes the electrode layer easy to peel off and may generate microcracks. As a result, there is a concern that the internal resistance may increase and the output characteristics may decrease.

[0060] For example, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of the second monomer unit can be 20 mol% or more and 75 mol% or less, 25 mol% or more and 80 mol% or less, 25 mol% or more and 75 mol% or less, 20 mol% or more and 35 mol% or less, 35 mol% or more and 55 mol% or less, 55 mol% or more and 68 mol% or less, 68 mol% or more and 73 mol% or less, 73 mol% or more and 80 mol% or less, 20 mol% or more and 30 mol% or less, 30 mol% or more and 50 mol% or less, 50 mol% or more and 65 mol% or less, 65 mol% or more and 70 mol% or less, or 70 mol% or more and 75 mol% or less.

[0061] When the content of the second monomer unit exceeds the range of this application, the flexibility of the electrode film decreases, and cracks may occur during drying and charge / discharge processes. Conversely, when the content of the second monomer unit is below the range of this application, the increased swelling caused by the electrolyte leads to electrode volume instability, and the adhesion force within the battery decreases, thus raising concerns that active material may detach from the current collector and that surface cracks may occur.

[0062] For example, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of the third monomer unit can be 2 mol% or more and 15 mol% or less, 0 mol% or more and 13 mol% or less, 2 mol% or more and 13 mol% or less, 0 mol% or more and 5 mol% or less, 5 mol% or more and 10 mol% or less, 10 mol% or more and 15 mol% or less, 0 mol% or more and 7 mol% or less, 7 mol% or more and 12 mol% or less, or 12 mol% or more and 15 mol% or less.

[0063] When the content of the third monomer unit exceeds the range of this application, the adhesive will gel, the viscosity of the slurry will increase sharply, resulting in decreased coatability, and may also lead to an increase in electrolyte swelling. Therefore, it is preferable to add a small amount to achieve the effect of increased adhesion while minimizing the increase in slurry viscosity and swelling.

[0064] In one embodiment of this application, the adhesive does not contain fluorine atoms, so that hydrogen fluoride may not be generated during the charging and discharging process of the battery using the adhesive.

[0065] In contrast, currently commercially available PVDF-based adhesives contain fluorine atoms, which raises the issue of hydrogen fluoride generation during battery charging and discharging.

[0066] In one embodiment of this application, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of n-butyl methacrylate can be 62 mol% or more and 68 mol% or less, the content of 2-ethylhexyl methacrylate can be 17 mol% or more and 23 mol% or less, the content of isobornyl methacrylate can be 7 mol% or more and 13 mol% or less, and the content of methacrylic acid can be 2 mol% or more and 8 mol% or less.

[0067] In one embodiment of this application, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of n-butyl methacrylate can be 42 mol% or more and 48 mol% or less, the content of 2-ethylhexyl methacrylate can be 17 mol% or more and 23 mol% or less, the content of isobornyl methacrylate can be 27 mol% or more and 33 mol% or less, and the content of methacrylic acid can be 2 mol% or more and 8 mol% or less.

[0068] In one embodiment of this application, the adhesive contains, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, butyl methacrylate (BMA) ester ...

[0069] In one embodiment of this application, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of ethyl (meth)acrylate can be 22 mol% or more and 28 mol% or less, the content of 2-ethylhexyl (meth)acrylate can be 17 mol% or more and 23 mol% or less, the content of isobornyl (meth)acrylate can be 47 mol% or more and 53 mol% or less, and the content of methacrylic acid can be 2 mol% or more and 8 mol% or less.

[0070] In one embodiment of this application, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of lauryl methacrylate can be 22 mol% or more and 28 mol% or less, the content of 2-ethylhexyl methacrylate can be 17 mol% or more and 23 mol% or less, the content of isobornyl methacrylate can be 47 mol% or more and 53 mol% or less, and the content of methacrylic acid can be 2 mol% or more and 8 mol% or less.

[0071] In one embodiment of this application, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of vinyl acetate may be 22 mol% or more and 28 mol% or less, the content of 2-ethylhexyl (meth)acrylate may be 17 mol% or more and 23 mol% or less, the content of isobornyl (meth)acrylate may be 47 mol% or more and 53 mol% or less, and the content of methacrylic acid may be 2 mol% or more and 8 mol% or less.

[0072] In one embodiment of this application, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of n-butyl (meth)acrylate can be 22 mol% or more and 28 mol% or less, the content of 2-ethylhexyl (meth)acrylate can be 17 mol% or more and 23 mol% or less, the content of styrene can be 47 mol% or more and 53 mol% or less, and the content of methacrylic acid can be 2 mol% or more and 8 mol% or less.

[0073] In one embodiment of this application, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of n-butyl methacrylate can be 23 mol% or more and 27 mol% or less, the content of 2-ethylhexyl methacrylate can be 17 mol% or more and 23 mol% or less, and the content of isobornyl methacrylate can be 52 mol% or more and 58 mol% or less.

[0074] In one embodiment of this application, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of n-butyl methacrylate can be 22 mol% or more and 28 mol% or less, the content of 2-ethylhexyl methacrylate can be 17 mol% or more and 23 mol% or less, the content of isobornyl methacrylate can be 42 mol% or more and 48 mol% or less, and the content of methacrylic acid can be 7 mol% or more and 13 mol% or less.

[0075] In one embodiment of this application, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of n-butyl methacrylate can be 22 mol% or more and 28 mol% or less, the content of 2-ethylhexyl methacrylate can be 17 mol% or more and 23 mol% or less, the content of isobornyl methacrylate can be 47 mol% or more and 53 mol% or less, and the content of N-vinylpyrrolidone can be 2 mol% or more and 8 mol% or less.

[0076] In one embodiment of this application, in the adhesive, based on a total molar percentage of 100 mol% for the first monomer unit, the second monomer unit, and the third monomer unit, the content of n-butyl methacrylate can be 22 mol% or more and 28 mol% or less, the content of 2-ethylhexyl methacrylate can be 17 mol% or more and 23 mol% or less, the content of tert-butyl methacrylate can be 47 mol% or more and 53 mol% or less, and the content of methacrylic acid can be 2 mol% or more and 8 mol% or less.

[0077] In one embodiment of this application, when the adhesive is immersed in an electrolyte at 40°C to 80°C for 2 to 6 hours, the degree of swelling can be 20% to 95%.

[0078] For example, when the adhesive is immersed in an electrolyte at 40°C to 80°C for 2 to 6 hours, the degree of swelling can be 32% to 93%, 33% to 92%, 20% to 33%, 33% to 35%, 35% to 38%, 38% to 40%, 40% to 42%, 42% to 45%, 45% to 47%, 47% to 55%, 55% to 62%, 62% to 89%, 89% to 95%, 32% to 34%, 34% to 36%, 37% to 39%, 39% to 41%, 41% to 43%, 44% to 46%, 46% to 48%, 54% to 56%, 61% to 63%, or 88% to 90%.

[0079] The swelling degree described above can be determined as follows: First, an adhesive is uniformly coated onto a 1t thick stainless steel separator, resulting in a polymer mass of 0.03g before drying. The coated sample is then dried in a vacuum oven at 130℃ for 4 hours to completely remove residual solvent, followed by cooling to room temperature, and the weight W0 is measured. Next, the sample is completely immersed in an electrolyte solution and maintained in a 60℃ oven for 4 hours to allow the adhesive to absorb the electrolyte. After immersion, the sample is removed, the surface electrolyte is gently wiped off, and the weight W1 is measured immediately. At this point, the swelling degree is calculated according to the following mathematical formula 1.

[0080] [Mathematical Expression 1]

[0081] Swelling degree (%) = (W1 - W0) / W0 × 100

[0082] In one embodiment of this application, the adhesive may be a positive electrode adhesive, a negative electrode adhesive, or a separator adhesive.

[0083] For example, the adhesive described in this application may be an adhesive for positive electrodes.

[0084] Another aspect of the slurry in this application may include the binder and active material.

[0085] In one embodiment of this application, the slurry may be a positive electrode slurry containing the positive electrode binder and the positive electrode active material.

[0086] In one embodiment of this application, the slurry may be a negative electrode slurry containing the negative electrode binder and the negative electrode active material.

[0087] In one embodiment of this application, the viscosity of the slurry can be from 2000 mPa·s to 56000 mPa·s.

[0088] For example, the viscosity of the slurry can be from 2050 mPa·s to 55500 mPa·s, 2075 mPa·s to 55000 mPa·s, 2000 mPa·s to 2087 mPa·s, 2087 mPa·s to 3709 mPa·s, 3709 mPa·s to 4233 mPa·s, 4233 mPa·s to 4467 mPa·s, 4467 mPa·s to 5527 mPa·s, 5527 mPa·s to 7829 mPa·s, 7829 mPa·s to 8185 mPa·s, 8185 mPa·s to 9826 mPa·s, 9826 mPa·s to 10175 mPa·s, 10175 mPa·s to 10340 mPa·s, 10340 mPa·s to 10520 mPa·s. mPa·s, 10520 mPa·s to 10823 mPa·s, 10823 mPa·s to 11954 mPa·s, 11954 mPa·s to 12044 mPa·s, 12044 mPa·s to 12549 mPa·s, 12549 mPa·s to 13371 mPa·s, 13371 mPa·s to 18242 mPa·s, 18242 mPa·s to 18701 mPa·s, 18701 mPa·s to 34172 mPa·s, 34172 mPa·s to 54724 mPa·s, 2001 mPa·s to 2186 mPa·s, 3600 mPa·s to 3800 mPa·s, 4100 mPa·s to 4350 mPa·s, 4360 mPa·s to 4560 mPa·s, 5400 mPa·s to 5650 mPa·s, 7700 mPa·s to 7950 mPa·s, 8050 mPa·s to 8300 mPa·s, 9700 mPa·s to 9950 mPa·s, 10050 mPa·s to 10300 mPa·s, 10200 mPa·s to 10500 mPa·s, 10400 mPa·s to 10700 mPa·s, 10700 mPa·s to 10950 mPa·s, 11800 mPa·s to 12100 mPa·s, 11900 mPa·s to 12200 mPa·s, 12400 mPa·s to 12700 mPa·s, 13200 mPa·s to 13500 mPa·s mPa·s, 18100 mPa·s to 18400 mPa·s, 18600 mPa·s to 18900 mPa·s, 34000 mPa·s to 34400 mPa·s, or 54500 mPa·s to 55800 mPa·s.

[0089] The viscosity of the slurry can be determined by the following methods.

[0090] The slurry was maintained at 25°C, and its viscosity was measured using an Anton Paar rheometer (MCR 302e). The measurement was performed using a parallel flat plate clamp (25 mm diameter) with a 1 mm gap, and the measurement time was 0.01 s. -1 up to 200 s -1 Data was collected while the shear rate was varied in stages within a certain range. In the measured viscosity-shear rate curves, the shear rate was set at 1 s⁻¹. -1 The viscosity at that point is used as a representative value.

[0091] The positive electrode active material used in this application for electrode formation can be any positive electrode active material available in the art. Specific examples of such positive electrode active materials include: lithium metal; lithium cobalt oxides such as LiCoO2; and Li... 1+ xMn 2-x Lithium manganese oxides such as O4 (where x is 0 to 0.33), LiMnO3, LiMn2O3, and LiMnO2; lithium copper oxides such as Li2CuO2; vanadium oxides such as LiV3O8, V2O5, and Cu2V2O7; and LiNi 1-x Lithium-nickel oxides represented by MxO2 (where M = Co, Mn, Al, Cu, Fe, Mg, B or Ga, x = 0.01 to 0.3); LiMn 2-x M x Lithium manganese composite oxides represented by O2 (where M = Co, Ni, Fe, Cr, Zn or Ta, x = 0.01 to 0.1) or Li2Mn3MO8 (where M = Fe, Co, Ni, Cu or Zn); Li(Ni a Co b Mn c Lithium-nickel-manganese-cobalt oxides represented by O2 (where 0 < a < 1, 0 < b < 1, 0 < c < 1, a + b + c = 1); sulfur or disulfide compounds; phosphates such as LiFePO4, LiMnPO4, LiCoPO4, and LiNiPO4; Fe2(MoO4)3, etc., but not limited to these.

[0092] In one embodiment of this application, the positive electrode active material may be the lithium-nickel-manganese-cobalt oxide, the lithium-nickel oxide, the lithium-cobalt oxide, the phosphate, or a combination thereof.

[0093] In one embodiment of this application, the positive electrode active material may be lithium-nickel-cobalt-manganese oxide (NCM), lithium-nickel-cobalt-aluminum oxide (NCA), lithium-cobalt oxide (LCO), lithium iron phosphate (LFP), or a combination thereof.

[0094] In one embodiment of this application, the lithium-nickel-cobalt-manganese oxide (NCM) may be NCM 811(Li(Ni 0.8 Co 0.1 Mn 0.1 O2).

[0095] At this point, in addition to the positive electrode active material, the positive electrode active material layer may further include dispersants, conductive agents, fillers, and other additives.

[0096] Based on the solid content, the content of the positive electrode active material can be 95-99% by weight. If the content of the active material is low, the battery cannot achieve high capacity; if the content of the active material is too high, the content of binders, conductive agents, etc. will be relatively reduced, and thus the electrode adhesion, conductivity, etc. may decrease.

[0097] There are no particular limitations on the conductive agent used, and it can be selected appropriately according to the type of battery and storage device. For example, in the case of lithium-ion secondary batteries, carbon such as graphite and activated carbon can be used; in the case of nickel-metal hydride secondary batteries, cobalt oxide can be used, and nickel powder, cobalt oxide, titanium oxide, carbon, etc. can be used in the negative electrode.

[0098] Examples of carbon species mentioned above include acetylene black, furnace black, graphite, carbon fiber, fullerenes, and carbon nanotubes.

[0099] Based on 100 parts by weight of electrode active material, the amount of the above-mentioned conductive agent used is usually 0.5 to 20 parts by weight, preferably 0.5 to 2 parts by weight.

[0100] The energy density of a secondary battery can be increased by reducing the amount of conductive agent and increasing the amount of positive electrode active material. Therefore, it is important to maximize the amount of active material to increase energy density while ensuring conductivity with minimal use of conductive agent.

[0101] The finer and more uniformly the conductive agent is dispersed in the electrode slurry for secondary batteries, the higher the conductivity, thereby reducing the internal resistance of the battery and exhibiting improved output characteristics, as well as extending battery life. If the dispersion is large and uneven, even using the same amount, the binding properties and conductivity will decrease, thus adversely affecting the battery's life and output characteristics. Furthermore, a lower dispersion viscosity allows for a higher solids content in the slurry, thereby increasing the electrode production speed.

[0102] As a binder for the positive electrode of a secondary battery, in addition to the binder for the positive electrode described in this application, any one or more of the following can be used together: poly(meth)acrylic acid, poly(meth)acrylamide, carboxymethyl cellulose, polyvinylidene fluoride, copolymers of polyhexafluoropropylene and polyvinylidene fluoride (P(VdF / HFP)), poly(vinyl acetate), polyvinyl alcohol, polyethylene oxide, polyvinylpyrrolidone, alkylated polyethylene oxide, polyvinyl ether, poly(methyl methacrylate), poly(ethyl acrylate), polytetrafluoroethylene, polyvinyl chloride, polyacrylonitrile, polyvinylpyridine, styrene-butadiene rubber, acrylonitrile-butadiene rubber, and copolymers thereof.

[0103] Based on solid content conversion, the content of the binder in the positive electrode slurry composition is preferably 0.3 wt% or more and 10 wt% or less, more preferably 0.7 wt% or more and 3 wt% or less. When the content is less than 0.3 wt%, it is difficult to expect sufficient bonding force in the current collector and electrode composition; when the content is greater than 10 wt%, the proportion of binder in the electrode slurry composition increases, reducing the battery capacity and potentially increasing the battery resistance.

[0104] The electrode of another aspect of this application may include: a current collector; and an active material layer containing the binder of this application formed on the current collector.

[0105] In one embodiment of this application, the electrode may be a positive electrode, which may include: a current collector; and a layer of positive electrode active material containing the positive electrode adhesive of this application formed on the current collector.

[0106] In one embodiment of this application, the electrode may be a negative electrode, which may include: a current collector; and a layer of negative electrode active material containing the negative electrode adhesive of this application formed on the current collector.

[0107] In one embodiment of this application, the bonding force of the positive electrode can be from 50 gf / 25 mm to 650 gf / 25 mm.

[0108] For example, the bonding strength of the positive electrode can be from 110 gf / 25 mm to 640 gf / 25 mm, 115 gf / 25 mm to 630 gf / 25 mm, 100 gf / 25 mm to 117.16 gf / 25 mm, 117.16 gf / 25 mm to 125.92 gf / 25 mm, 125.92 gf / 25 mm to 142.60 gf / 25 mm, 142.60 gf / 25 mm to 153.14 gf / 25 mm, 153.14 gf / 25 mm to 166.83 gf / 25 mm, 166.83 gf / 25 mm to 211.35 gf / 25 mm, and 211.35 gf / 25 mm to 249.04 gf / 25 mm. mm, 249.04 GF / 25 mm to 287.52 GF / 25 mm, 287.52 GF / 25 mm to 320.98 GF / 25 mm, 320.98 GF / 25 mm to 447.39 GF / 25 mm, 447.39 GF / 25 mm to 459.04 GF / 25 mm, 459.04 GF / 25 mm to 472.78 GF / 25 mm, 472.78 GF / 25 mm to 499.59 GF / 25 mm, 499.59 GF / 25 mm to 501.07 GF / 25 mm, 501.07 GF / 25 mm to 520.22 GF / 25 mm, 520.22 gf / 25 mm to 523.91 GF / 25mm, 523.91 GF / 25mm to 527.03 GF / 25mm, 527.03 GF / 25mm to 540.75 GF / 25mm, 540.75 GF / 25mm to 557.24 GF / 25mm, 557.24 GF / 25mm to 621.50 GF / 25 mm, or 621.50 gf / 25 mm to 650 gf / 25 mm.

[0109] For example, the bonding strength of the positive electrode can be 110 gf / 25 mm to 120 gf / 25 mm, 120 gf / 25 mm to 130 gf / 25 mm, 135 gf / 25 mm to 150 gf / 25 mm, 145 gf / 25 mm to 160 gf / 25 mm, 160 gf / 25 mm to 175 gf / 25 mm, 205 gf / 25 mm to 220 gf / 25 mm, 240 gf / 25 mm to 260 gf / 25 mm, 280 gf / 25 mm to 295 gf / 25 mm, 310 gf / 25 mm to 330 gf / 25 mm, 440 gf / 25 mm to 455 gf / 25 mm, 450 gf / 25 mm to 470 gf / 25 mm. 25 mm, 465 gf / 25 mm to 480 gf / 25 mm, 490 gf / 25 mm to 510 gf / 25 mm, 495 gf / 25 mm to 505 gf / 25 mm, 510 gf / 25 mm to 530 gf / 25 mm, 515 gf / 25 mm to 535 gf / 25 mm, 520 gf / 25 mm to 540 gf / 25 mm, 550 gf / 25 mm to 565 gf / 25 mm, 610 gf / 25 mm to 630 gf / 25 mm, or 640 gf / 25 mm to 650 gf / 25 mm.

[0110] The bonding force of the positive electrode can be determined in the following ways.

[0111] The positive electrode was cut into 15 cm × 2.5 cm pieces. The coated side of the cut positive electrode was then firmly adhered to an acrylic plate with double-sided tape attached, and pressed four times with a rubber roller to prepare a sample for the adhesion test. After mounting the prepared sample on a UTM device capable of measuring adhesion force, a 2.5 cm length was peeled off from the end of the positive electrode along a 180° direction to measure the peel force. At least five samples were tested for each positive electrode, and the average peel stress was calculated.

[0112] The positive electrode can be manufactured by the following steps: (a) manufacturing a positive electrode active material layer forming composition comprising a positive electrode active material and the binder of this application; and (b) applying the positive electrode active material layer forming composition onto a positive electrode current collector and then drying it.

[0113] The composition for forming the positive electrode active material layer can be mixed using a conventional mixer, such as a high-speed shear mixer or a homogenizer, by conventional methods.

[0114] Step (b) above involves coating the positive electrode active material layer forming composition manufactured in step (a) onto the positive electrode current collector and then drying it to manufacture a positive electrode for a lithium secondary battery.

[0115] At this time, there are no limitations on the method of forming the positive active material layer of the slurry, and it can be manufactured by methods such as doctor blade coating, dip coating, gravure coating, slit die coating, spin coating, comma coating, bar coating, reverse roll coating, screen coating, and cap coating.

[0116] After coating and drying, a positive electrode for secondary batteries (especially lithium secondary batteries) with a positive electrode active material layer can be finally manufactured.

[0117] The current collector only needs to be conductive and not chemically react with the electrode forming slurry to be used. Representative examples include aluminum foil and copper foil. Current collectors with a thickness between 3 and 50 micrometers can be selected.

[0118] Another aspect of the secondary battery of this application may include the aforementioned electrodes.

[0119] In one embodiment of this application, the secondary battery may include the aforementioned positive electrode.

[0120] In one embodiment of this application, the secondary battery may include the aforementioned negative electrode.

[0121] On the other hand, a secondary battery composed of a positive electrode, a negative electrode, a separator, and an electrolyte made of the positive electrode adhesive of this application can be manufactured.

[0122] In one embodiment of this application, the initial efficiency of the secondary battery can be 88% to 91%.

[0123] For example, the initial efficiency of the secondary battery can be 88.4% to 91%, 88.8% to 91%, 88% to 88.83%, 88.83% to 88.98%, 88.98% to 89.05%, 89.05% to 89.27%, 89.27% ​​to 89.64%, 89.64% to 89.82%, 89.82% to 90.12%, or 90.12% to 90%. 0.14%, 90.14% to 90.27%, 90.27% to 90.31%, 90.31% to 90.33%, 90.33% to 90.42%, 90.42% to 90.47%, 90.47% to 90.53%, 90.53% to 90.59%, 90.59% to 90.66%, 90.66% to 90.74%, 90.74% to 90. 98%, 88.80% to 88.86%, 88.95% to 89.01%, 89.00% to 89.08%, 89.02% to 89.07%, 89.22% to 89.32%, 89.60% to 89.68%, 89.78% to 89.86%, 90.08% to 90.16%, 90.10% to 90.18%, 90.23% to 90.3%. 1%, 90.27% to 90.35%, 90.29% to 90.37%, 90.38% to 90.46%, 90.43% to 90.51%, 90.49% to 90.57%, 90.55% to 90.63%, 90.62% to 90.70%, 90.70% to 90.78%, 90.71% to 90.77%, or 90.94% to 91%.

[0124] The initial efficiency of the secondary battery can be determined in the following ways.

[0125] The secondary charge was charged and discharged at 25°C in CC / CV mode. The voltage ranges for the active materials were set as follows: NCM 2.8 V to 4.2 V, NCA 2.8 V to 4.25 V, LCO 2.75 V to 4.5 V, and LFP 2.5 V to 3.65 V. Within each range, the charge was 0.1 C, followed by discharge at 0.1 C to the lower limit voltage of the corresponding range. Then, the formation was completed by sequentially charging and discharging at 0.2 C and 0.5 C within the same voltage range. The capacity obtained by charging again at 0.1 C was measured as the "initial charge capacity," and the capacity obtained by discharging at 0.1 C within the same voltage range was measured as the "initial discharge capacity." The initial efficiency was then calculated according to the following mathematical formula 2.

[0126] [Mathematical Expression 2]

[0127] Initial efficiency [%] = [Initial discharge capacity / Initial charge capacity] × 100

[0128] In one embodiment of this application, the capacity retention rate (100 cycles) of the secondary battery can be 86% to 95%.

[0129] For example, the capacity retention rate of the secondary battery can be 86.3% to 94.5%, 86.4% to 94.4%, 86% to 86.44%, 86.44% to 86.58%, 86.58% to 86.84%, 86.84% to 89.06%, 89.06% to 90.31%, 90.31% to 90.44%, 90.44% to 90.69%, 90.69% to 90.91%, 90.91% to 90.94%, 90.94% to 91.30%, 91.30% to 91.46%, 91.46% to 91.49%, 91.49% to 92.04%, 92.04% to 93.58%, 93.58% to 93.72%, 93.72% to 93.87%, 93.87% to 94.03%, 94.03% to 94.27%, 94.27% to 94.39%, or 94.39% to 95%.

[0130] For example, the capacity retention rate of the secondary battery can be 86.40% to 86.50%, 86.54% to 86.62%, 86.80% to 86.90%, 88.90% to 89.20%, 90.20% to 90.40%, 90.40% to 90.50%, 90.60% to 90.75%, 90.85% to 90.97%, 90.96% to 91.02%, or 91.25%. % to 91.35%, 91.40% to 91.52%, 91.47% to 91.52%, 92.00% to 92.08%, 93.50% to 93.65%, 93.65% to 93.78%, 93.80% to 93.93%, 93.95% to 94.10%, 94.20% to 94.35%, 94.35% to 94.50%, or 94.90% to 95.00%.

[0131] The capacity retention rate can be determined in the following ways.

[0132] First, the battery was placed in a 25°C test chamber and charged and discharged in CC / CV mode. Within voltage ranges set as follows: NCM electrode 2.8 V to 4.2 V, NCA electrode 2.8 V to 4.25 V, LCO electrode 2.75 V to 4.5 V, and LFP electrode 2.5 V to 3.65 V, the battery was charged sequentially once at current conditions of 0.1 C, 0.2 C, and 0.5 C, respectively, and then discharged to the lower limit voltage of the corresponding range to complete initialization. Next, the current was set to 1 C, and the battery was charged to the upper limit voltage within the same voltage range (at this point, the cutoff current for the CV stage is 0.005 C), and then discharged to the lower limit voltage. This process constitutes one cycle, which was repeated 100 times. The capacity retention rate was then calculated using the following mathematical formula 3 as the ratio of the discharge capacity of the 100th cycle to the discharge capacity of the 1st cycle.

[0133] [Mathematical Expression 3]

[0134] Capacity retention rate [%] = [Discharge capacity at 100th cycle / Discharge capacity at 1st cycle] × 100

[0135] The separator should be an insulator to separate the negative and positive electrodes and should provide channels for lithium ions to move only. For this purpose, it needs good wettability to the electrolyte and should use porous polymer membranes such as PE / PP or porous nonwoven fabrics. To prevent battery short circuits, a coated separator, such as one coated with ceramics to enhance heat resistance and mechanical strength, can be used, and can be coated in single or multiple layers.

[0136] The aforementioned diaphragm can be made of a porous substrate. Any porous substrate commonly used in electrochemical devices can be used as the porous substrate, such as polyolefin porous membranes or nonwoven fabrics, but it is not particularly limited to these.

[0137] The aforementioned diaphragm can be a porous substrate composed of any one or a mixture of two or more of the following: polyethylene, polypropylene, polybutene, polypentene, polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenylene ether, polyphenylene sulfide, and polyethylene naphthalate.

[0138] The electrolyte of the aforementioned lithium secondary battery is a non-aqueous electrolyte containing lithium salt, consisting of lithium salt and solvent. The solvent can be a non-aqueous organic solvent, an organic solid electrolyte, or an inorganic solid electrolyte.

[0139] The lithium salt is a substance that is readily soluble in the non-aqueous electrolyte, such as LiCl, LiBr, LiI, LiClO4, LiBF4, or LiB2. 10 Cl10 LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiC4BO8, LiCF3CO2, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiN(SO2F)2, LiN(SO2C2F5)2, LiC4F9SO3, LiC(CF3SO2)3, (CF3SO2)·2NLi, lithium chloroborane, lower aliphatic carboxylic acids, lithium 4-phenylborate imide, etc.

[0140] As the aforementioned non-aqueous organic solvents, for example, non-protic organic solvents such as N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butyl carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, 1,2-diethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, 4-methyl-1,3-dioxane, diethyl ether, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triphosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate can be used.

[0141] As the organic solid electrolyte, for example, polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, agitation lysine, polyester sulfides, polyvinyl alcohol, polyvinylidene fluoride, polymers containing secondary dissociation groups, etc., can be used.

[0142] As the inorganic solid electrolyte, for example, nitrides, halides, sulfates of Li such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2 can be used.

[0143] In addition, the non-aqueous electrolyte may also contain other additives to improve charge-discharge characteristics, flame retardancy, etc. Examples of such additives include pyridine, triethyl phosphite, triethanolamine, cyclic ethers, ethylenediamine, n-glyme, hexamethylphosphoramide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidinyl ethers, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, fluoroethylene carbonate (FEC), propylene sulpholone (PRS), and vinylene carbonate (VC).

[0144] In addition to the conventional winding process, the lithium secondary battery of the present invention can also undergo lamination stacking and folding processes for the separator and electrodes. Furthermore, the battery casing can be cylindrical, square, pouch-shaped, or coin-shaped, etc.

[0145] In one embodiment of this application, the secondary battery can be used not only as a battery cell for powering small devices, but also preferably as a cell battery in a medium-to-large battery module that includes multiple battery cells for powering medium-to-large devices.

[0146] Preferred examples of the aforementioned medium to large-sized equipment include: power tools that operate by receiving power from a battery motor; electric vehicles, including electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); electric two-wheelers, including electric bicycles (E-bikes) and electric scooters (E-scooters); electric golf carts, etc., but not limited to these.

[0147] The present invention will now be described in more detail through embodiments. However, the following embodiments are used to illustrate the present invention more specifically, and the scope of the present invention is not limited to the following embodiments.

[0148] Examples and Comparative Examples: Manufacturing of Copolymer Particles

[0149] [Example 1]

[0150] 295 g of deionized water, 0.9 g of DOWFAX, and 0.15 g of EDTA were added to a five-necked flask that had been fully purged with nitrogen. The mixture was heated to 70°C and maintained at 70°C for 15 minutes to stabilize the temperature. Nitrogen gas was then introduced for at least one hour to completely replace the internal gas with nitrogen. Next, 100 g of a monomer mixture consisting of 65 mol% n-butyl acrylate, 20 mol% 2-ethylhexyl acrylate, 10 mol% isobornyl acrylate, and 5 mol% methacrylic acid was added dropwise over 30 minutes along with an initiator solution of 0.05 g potassium persulfate (KPS) dissolved in 5 g of water. After the addition was complete, the reaction was continued at the same 70°C for 6 hours to form a copolymer latex. After the reaction was complete, the resulting latex was vacuum dried at 90°C to completely remove moisture. The dried polymer was then dissolved in N-methyl-2-pyrrolidone at 60°C to be used as an adhesive solution.

[0151] [Example 2]

[0152] The composition of 100g of the above monomer mixture was adjusted to 45 mol% n-butyl acrylate, 20 mol% 2-ethylhexyl acrylate, 30 mol% isobornyl acrylate, and 5 mol% methacrylic acid. The remaining process conditions were the same as in Example 1, thereby producing a copolymer.

[0153] [Example 3]

[0154] The composition of 100g of the above monomer mixture was adjusted to 25 mol% n-butyl acrylate, 20 mol% 2-ethylhexyl acrylate, 50 mol% isobornyl acrylate, and 5 mol% methacrylic acid. The remaining process conditions were the same as in Example 1, thereby producing a copolymer.

[0155] [Example 4]

[0156] The composition of 100g of the above monomer mixture was adjusted to 25 mol% ethyl acrylate, 20 mol% 2-ethylhexyl acrylate, 50 mol% isobornyl acrylate, and 5 mol% methacrylic acid. The remaining process conditions were the same as in Example 1, thereby producing a copolymer.

[0157] [Example 5]

[0158] The composition of 100g of the above monomer mixture was adjusted to 25 mol% lauryl acrylate, 20 mol% 2-ethylhexyl acrylate, 50 mol% isobornyl acrylate, and 5 mol% methacrylic acid. The remaining process conditions were the same as in Example 1, thereby producing a copolymer.

[0159] [Example 6]

[0160] The composition of 100g of the above monomer mixture was adjusted to 25 mol% vinyl acetate, 20 mol% 2-ethylhexyl acrylate, 50 mol% isobornyl acrylate, and 5 mol% methacrylic acid. The remaining process conditions were the same as in Example 1, thereby producing a copolymer.

[0161] [Example 7]

[0162] The composition of 100g of the above monomer mixture was adjusted to 25 mol% n-butyl acrylate, 20 mol% 2-ethylhexyl acrylate, 50 mol% styrene, and 5 mol% methacrylic acid, with the remaining process conditions being the same as in Example 1, thereby producing a copolymer.

[0163] [Example 8]

[0164] The composition of 100g of the above monomer mixture was adjusted to 25 mol% n-butyl acrylate, 20 mol% 2-ethylhexyl acrylate, and 55 mol% isobornyl acrylate. The remaining process conditions were the same as in Example 1, thereby producing a copolymer.

[0165] [Example 9]

[0166] The composition of 100g of the above monomer mixture was adjusted to 25 mol% n-butyl acrylate, 20 mol% 2-ethylhexyl acrylate, 45 mol% isobornyl acrylate, and 10 mol% methacrylic acid. The remaining process conditions were the same as in Example 1, thereby producing a copolymer.

[0167] [Example 10]

[0168] The composition of 100g of the above monomer mixture was adjusted to 25 mol% n-butyl acrylate, 20 mol% 2-ethylhexyl acrylate, 50 mol% isobornyl acrylate, and 5 mol% N-vinylpyrrolidone. The remaining process conditions were the same as in Example 1, thereby producing a copolymer.

[0169] [Example 11]

[0170] The composition of 100g of the above monomer mixture was adjusted to 25 mol% n-butyl acrylate, 20 mol% 2-ethylhexyl acrylate, 50 mol% tert-butyl acrylate, and 5 mol% methacrylic acid, with the remaining process conditions being the same as in Example 1, thereby producing a copolymer.

[0171] [Comparative Example 1]

[0172] The composition of 100g of the above monomer mixture was adjusted to 5 mol% n-butyl acrylate, 20 mol% 2-ethylhexyl acrylate, 70 mol% isobornyl acrylate, and 5 mol% methacrylic acid. The remaining process conditions were the same as in Example 1, thereby producing a copolymer.

[0173] [Comparative Example 2]

[0174] The composition of 100g of the monomer mixture was adjusted to 90 mol% n-butyl acrylate, 5 mol% 2-ethylhexyl acrylate, and 5 mol% methacrylic acid, with the remaining process conditions being the same as in Example 1, thereby producing a copolymer.

[0175] [Comparative Example 3]

[0176] The composition of 100g of the above monomer mixture was adjusted to 25 mol% n-butyl acrylate, 20 mol% 2-ethylhexyl acrylate, 35 mol% isobornyl acrylate, and 20 mol% methacrylic acid, with the remaining process conditions being the same as in Example 1, thereby producing a copolymer.

[0177] [Comparative Example 4]

[0178] The composition of 100g of the above monomer mixture was adjusted to 25 mol% n-butyl acrylate, 20 mol% 2-ethylhexyl acrylate, 35 mol% isobornyl acrylate, and 20 mol% N-vinylpyrrolidone, with the remaining process conditions being the same as in Example 1, thereby producing a copolymer.

[0179] [Comparative Example 5]

[0180] Comparative Example 5 uses Solvay's fluoropolymer PVDF adhesive (Solef 5130) instead of the self-polymer.

[0181] Table 1 below shows the composition of the monomer mixtures used in the manufacture of copolymers in Examples 1 to 11 and Comparative Examples 1 to 5.

[0182] [Table 1]

[0183]

[0184] In Table 1 above, “EA” represents ethyl acrylate, “BA” represents n-butyl acrylate, “LA” represents n-lauryl acrylate, “VAc” represents vinyl acetate, “2-EHA” represents 2-ethylhexyl acrylate, “IBOA” represents isobornyl acrylate, “tert-BA” represents tert-butyl acrylate, “SM” represents styrene, “MAA” represents methacrylic acid, and “VP” represents N-vinylpyrrolidone.

[0185] Slurry manufacturing

[0186] [Manufacturing Example 1]

[0187] First, based on the solids content, 97.72 parts by weight of NCM811 active material, 0.78 parts by weight of MWCNT (multi-walled carbon nanotube) dispersion, and 1.5 parts by weight of the copolymer binder synthesized in Example 1 were weighed, totaling 100 parts by weight. Next, N-methyl-2-pyrrolidone was added and diluted until the solids content of the overall slurry was 65% by weight. Then, the mixture was put into a homogenizer and stirred at 3000 rpm for 30 minutes to ensure uniform dispersion of the components, thereby preparing the NCM cathode slurry.

[0188] [Manufacturing Examples 2 to 11, and Comparative Manufacturing Examples 1 to 5]

[0189] Manufacturing Examples 2 to 11 used the copolymer adhesives synthesized in Examples 2 to 11, respectively. Comparative Manufacturing Examples 1 to 5 used the copolymers or PVDF adhesives of Comparative Examples 1 to 5, respectively. Apart from this, the other process conditions were the same as those in Manufacturing Example 1, thereby manufacturing the slurry.

[0190] [Manufacturing Example 12]

[0191] First, based on the solids content, 96 parts by weight of LFP active material, 1.2 parts by weight of MWCNT dispersion, and 2.8 parts by weight of the copolymer binder synthesized in Example 3, totaling 100 parts by weight, were weighed. Next, N-methyl-2-pyrrolidone was added and diluted until the solids content of the overall slurry was 55% by weight. Then, the mixture was added to a homogenizer and stirred at 3000 rpm for 30 minutes to ensure uniform dispersion of the components, thereby producing the LFP cathode slurry.

[0192] [Manufacturing Examples 13, 14 and Comparative Manufacturing Example 6]

[0193] Manufacturing Examples 13 and 14 used the copolymer adhesives synthesized in Examples 8 and 9, respectively, while Comparative Manufacturing Example 6 used the PVDF adhesive from Comparative Example 5. Apart from this, the remaining process conditions were the same as in Manufacturing Example 12, thereby producing the slurry.

[0194] [Manufacturing Example 15]

[0195] First, based on the solids content, 97.8 parts by weight of NCA active material, 1.2 parts by weight of MWCNT dispersion, and 1.0 part by weight of the copolymer binder synthesized in Example 3 were weighed, totaling 100 parts by weight. Next, N-methyl-2-pyrrolidone was added and diluted until the solids content of the overall slurry was 75% by weight. Then, the mixture was put into a homogenizer and stirred at 3000 rpm for 30 minutes to ensure uniform dispersion of the components, thereby producing the NCA cathode slurry.

[0196] [Manufacturing Examples 16, 17 and Comparative Manufacturing Example 7]

[0197] Manufacturing Examples 16 and 17 used the copolymer adhesives synthesized in Examples 8 and 9, respectively, while Comparative Manufacturing Example 7 used the PVDF adhesive from Comparative Example 5. Apart from this, the remaining process conditions were the same as in Manufacturing Example 15, thereby producing the slurry.

[0198] [Manufacturing Example 18]

[0199] First, based on the solids content, 98 parts by weight of LCO active material, 1.2 parts by weight of MWCNT dispersion, and 0.8 parts by weight of the copolymer binder synthesized in Example 3 were weighed, totaling 100 parts by weight. Next, N-methyl-2-pyrrolidone was added and diluted until the solids content of the overall slurry was 75% by weight. Then, the mixture was put into a homogenizer and stirred at 3000 rpm for 30 minutes to ensure uniform dispersion of the components, thereby producing the LCO cathode slurry.

[0200] [Manufacturing Examples 19, 20 and Comparative Manufacturing Example 8]

[0201] Manufacturing Examples 19 and 20 used the copolymer adhesives synthesized in Examples 8 and 9, respectively. Comparative Manufacturing Example 8 used the PVDF adhesive of Comparative Example 5. Apart from this, the other process conditions were the same as those in Manufacturing Example 18, thereby producing the slurry.

[0202] Table 2 below shows the types of active substances and binders used in the slurries of Manufacturing Examples 1 to 20 and Comparative Manufacturing Examples 1 to 8, respectively.

[0203] In Table 2 below, NCM (lithium-nickel-cobalt-manganese oxide) refers to NCM 811 (Li(Ni 0. 8Co 0.1 Mn 0.1 LFP stands for lithium iron phosphate, NCA stands for lithium-nickel-cobalt-aluminum oxide, and LCO stands for lithium-cobalt oxide.

[0204] [Table 2]

[0205]

[0206] Manufacturing of the positive electrode

[0207] The slurry compositions of Manufacturing Examples 1 to 20 and Comparative Manufacturing Examples 1 to 8 were uniformly coated onto an aluminum foil (positive electrode current collector) with a thickness of 20 μm using a doctor blade. Next, the electrodes were dried in an oven at 130°C for 1 hour to completely remove the solvent, and then the dried electrodes were rolled using a roll press to manufacture the positive electrode.

[0208] Battery (secondary battery) manufacturing

[0209] Based on 100 parts by weight of a solvent containing ethylene carbonate (EC) and ethyl methyl carbonate (EMC) in a volume ratio of 25:75, 1 part by weight each of fluoroethylene carbonate (FEC), PS, and LiPOF2 were added, and lithium hexafluorophosphate (LiPF6) was dissolved at a concentration of 1 mol / L to obtain a non-aqueous electrolyte, which was used as the electrolyte. After interposition of a polyolefin separator between the previously manufactured positive electrode and a commercial graphite negative electrode, the electrode stack was packaged into a 2032 coin cell or a pouch cell and sealed, thus completing the lithium secondary battery.

[0210] [Evaluation Example 1] Electrolyte Swelling Degree Determination

[0211] First, the adhesives of the examples and comparative examples were coated onto a 1t thick stainless steel spacer, so that the polymer mass before drying was 0.03g. The prepared sample was dried in a vacuum oven at 130°C for 4 hours to completely remove residual solvent, and the initial weight W0 was recorded after cooling to room temperature.

[0212] Next, the sample was completely immersed in the electrolyte and kept in a 60°C oven for 4 hours to allow the adhesive to fully absorb the electrolyte. The electrolyte was prepared by adding 1 part by weight each of fluoroethylene carbonate (FEC), PS, and LiPOF2 to a solvent of 100 parts by weight of a 25:75 volume ratio of ethylene carbonate (EC) and methyl ethyl carbonate (EMC), followed by dissolving lithium hexafluorophosphate (LiPF6) at a concentration of 1 mol / L. After the immersion period, the sample was removed, the electrolyte on the surface was gently wiped off, and the weight W1 was immediately measured.

[0213] At this point, the degree of swelling is calculated according to the following mathematical formula 1.

[0214] [Mathematical Expression 1]

[0215] Swelling degree (%) = (W1 - W0) / W0 × 100

[0216] The electrolyte swelling degree of the examples and comparative examples is shown in Table 3 below.

[0217] [Table 3]

[0218]

[0219] According to Table 3 above, the swelling degree of the electrolytes in Examples 1 to 11 is uniformly distributed in the range of 33% to 89%. This is considered to be the result of the first monomer unit and the second monomer unit being evenly proportioned in the range of 20 mol% to 80 mol%, and the introduction of a large side chain in the second monomer unit, thereby appropriately adjusting the electrolyte absorption.

[0220] In contrast, Comparative Example 2, with insufficient second monomer unit content, showed excessive swelling of 208%, indicating a high risk of electrode expansion, active material detachment, and microcracks. Comparative Example 1, with low first monomer unit content, and Comparative Example 5, which used fluorine-based PVDF (Solef 5130), showed insufficient swelling of 21% to 24%, confirming the possibility of insufficient electrolyte penetration leading to increased internal resistance or relatively restricted lithium-ion conduction. Furthermore, comparing Example 3 with Examples 1, 2, 3, and 4, it was clearly observed that the electrolyte swelling increased with increasing first or third monomer unit content, and tended to decrease with increasing second monomer unit content.

[0221] Therefore, it has been confirmed that when the contents of the first monomer unit, the second monomer unit, and the third monomer unit meet the scope of this application, an appropriate degree of swelling can be ensured.

[0222] [Evaluation Example 2] Slurry Viscosity Measurement

[0223] The slurries from Manufacturing Examples 1 to 20 and Comparative Manufacturing Examples 1 to 8 were maintained at 25°C, and their viscosity was measured using an Anton Paar rheometer. A parallel flat plate clamp (25 mm in diameter) with a 1 mm gap was used for the measurement, and the time interval was 0.01 s. -1 up to 200 s -1 Data was collected while the shear rate was varied in stages within a certain range. In the measured viscosity-shear rate curve, the shear rate was set at 1 s⁻¹. -1 The viscosity at that point was used as a representative value. The measurement results are shown in Table 4 below.

[0224] [Evaluation Example 3] Measurement of Positive Electrode Adhesion Force

[0225] The positive electrodes of Manufacturing Examples 1 to 20 and Comparative Manufacturing Examples 1 to 8 were cut into 15 cm × 2.5 cm pieces. The coated surface of the cut positive electrode was tightly adhered to an acrylic sheet with double-sided tape attached, and then pressed four times with a rubber roller to prepare a sample for the adhesion test. After mounting the prepared sample on a UTM device capable of measuring adhesion force, a 2.5 cm length was peeled off from the end of the positive electrode in a 180° direction to measure the peel force. More than five samples were tested for each manufacturing example and comparative manufacturing example, and the average peel stress was calculated. The results are shown in Table 4.

[0226] [Evaluation Example 4] Initial Efficiency Measurement

[0227] Batteries from Manufacturing Examples 1 to 20 and Comparative Manufacturing Examples 1 to 8 were charged and discharged at 25°C in CC / CV mode. The voltage ranges for the active materials were set as follows: NCM 2.8 V to 4.2 V, NCA 2.8 V to 4.25 V, LCO 2.75 V to 4.5 V, and LFP 2.5 V to 3.65 V. Within each range, the batteries were charged at 0.1 C and then discharged at 0.1 C to the lower limit voltage of the corresponding range. Next, after completing formation, the batteries were charged and discharged sequentially at 0.2 C and 0.5 C within the same voltage range. The capacity obtained by charging again at 0.1 C was measured as the "initial charge capacity," and the capacity obtained by discharging at 0.1 C within the same voltage range was measured as the "initial discharge capacity." The initial efficiency was calculated according to the following mathematical formula 2.

[0228] [Mathematical Expression 2]

[0229] Initial efficiency [%] = [Initial discharge capacity / Initial charge capacity] × 100

[0230] The measured initial efficiency values ​​are shown in Table 4 below.

[0231] [Evaluation Example 5] Determination of volume retention (100 cycles)

[0232] Batteries from Manufacturing Examples 1 to 20 and Comparative Manufacturing Examples 1 to 8 were placed in a 25°C test chamber and charged / discharged in CC / CV mode. Each battery was charged once at a current of 0.1 C, 0.2 C, and 0.5 C within a voltage range set for the NCM electrode (2.8 V to 4.2 V), NCA electrode (2.8 V to 4.25 V), LCO electrode (2.75 V to 4.5 V), and LFP electrode (2.5 V to 3.65 V), and then discharged to the lower limit voltage of the same range to complete initialization. Next, the current was set to 1 C, and the batteries were charged to the upper limit voltage within the same voltage range (at which point the cutoff current in the CV stage was 0.005 C), and then discharged to the lower limit voltage. This process constituted one cycle and was repeated 100 times. The capacity retention rate was calculated using the following mathematical formula 3 as the ratio of the discharge capacity of the 100th cycle to the discharge capacity of the 1st cycle.

[0233] [Mathematical Expression 3]

[0234] Capacity retention rate [%] = [Discharge capacity at 100th cycle / Discharge capacity at 1st cycle] × 100

[0235] The results of the capacity retention determination are shown in Table 4 below.

[0236] [Table 4]

[0237]

[0238] According to Table 4 above, the slurry viscosity of Manufacturing Examples 1 to 20 was maintained in the range of 4467 mPa·s to 54724 mPa·s.

[0239] In particular, in the case of NCM slurry, in manufacturing examples 1 to 3, the viscosity increased in stages as the proportion of the first monomer unit was increased; in comparative manufacturing example 2, which was outside the range, only the viscosity increased further, while the adhesion decreased, thus confirming the importance of the optimal range.

[0240] In Manufacturing Examples 4 to 6, despite the various adjustments made to the first monomer unit within the scope of this application, both viscosity and adhesion remained good; in examples such as Manufacturing Examples 7 and 11, where the second monomer unit was selected within an appropriate range, both swelling inhibition effect and appropriate viscosity were ensured.

[0241] On the other hand, compared with Manufacturing Example 3 which changed the third monomer unit, in Manufacturing Examples 8 to 10, the viscosity increased with the increase of the third monomer unit. However, in Comparative Manufacturing Examples 3 and 4, which were outside the range, the viscosity was too high, and it was determined that there was a concern that the slurry could not be uniformly coated on the electrode surface and the adhesion would decrease.

[0242] In manufacturing examples 12 to 20 using LFP, NCA, and LCO active materials, the same tendency for viscosity to increase with the increase of the third monomer unit was also observed. Furthermore, compared to comparative manufacturing examples 5 to 8 (PVDF), the manufacturing examples using the adhesive of this application showed equivalent or higher levels in terms of slurry viscosity and adhesion, demonstrating the substitutability of fluorinated adhesives.

[0243] Therefore, it has been confirmed that the adhesive composition of this application can ensure a balance between slurry viscosity and processability by maintaining the contents of the first monomer unit, the second monomer unit and the third monomer unit within the optimal range.

[0244] Furthermore, according to Table 4 above, it can be confirmed that the bonding strength of the positive electrodes of Manufacturing Examples 1 to 20 is 447 gf / 25 mm to 622 gf / 25 mm, which is equivalent to or higher than that of Comparative Manufacturing Examples 5 to 8, which use commercial fluorine-based adhesives (PVDF).

[0245] In the case of NCM slurry, as manufacturing examples 1 through 3 were carried out, the adhesion increased with the increase of the first monomer unit content. However, in comparative manufacturing example 2, where the first monomer unit content was outside the range, the viscosity was too high, resulting in uneven coating and a decrease in adhesion.

[0246] Furthermore, in Manufacturing Examples 7 and 11, where the content of the second monomer unit was within an appropriate range, both electrolyte swelling suppression and high adhesion were achieved. The adhesion was improved in Manufacturing Examples 8 to 10, which added the third monomer unit; however, in Comparative Manufacturing Examples 3 and 4, where the content of the third monomer unit exceeded the range of this application, the adhesion tended to decrease due to excessively high slurry viscosity.

[0247] In manufacturing examples 12 to 20 using LFP, NCA, and LCO active materials, the same tendency to increase viscosity and adhesion was also observed with the increase of the third monomer unit.

[0248] Therefore, it is confirmed that the adhesive of this application can ensure stable bonding strength by maintaining the contents of the first monomer unit, the second monomer unit and the third monomer unit within the optimal range.

[0249] Furthermore, according to Table 4 above, the initial efficiencies of the batteries in Manufacturing Examples 1 to 20 are in the range of 88.98% to 90.98%, which are equivalent to or higher than those in Comparative Manufacturing Examples 5 to 8, which used commercial fluorine-based adhesives (PVDF). This is attributed to the fact that the adhesive of this application minimizes the loss of active material during initial charge and discharge by simultaneously ensuring appropriate electrolyte swelling and high adhesion.

[0250] For NCM electrodes, Manufacturing Examples 1 to 11 outperformed or maintained the same level as PVDF in terms of initial efficiency and capacity retention. In contrast, Comparative Manufacturing Example 1, despite having similar initial efficiency, deteriorated in subsequent cycles due to insufficient adhesion; Comparative Manufacturing Examples 2 to 4 outperformed excessive swelling and decreased adhesion, with initial efficiency dropping to 85%.

[0251] Manufacturing Examples 12 to 20, which used LFP, NCA, and LCO electrodes, also maintained an initial efficiency of over 90%, thus confirming that the binder composition of this application can stably ensure the initial charge-discharge efficiency regardless of the type of active material.

[0252] Therefore, it has been confirmed that an adhesive with the contents of the first monomer unit, the second monomer unit, and the third monomer unit adjusted to the range of this application can maintain electrolyte permeability and interfacial adhesion evenly during the initial charge and discharge process, thereby achieving high initial efficiency.

[0253] Furthermore, according to Table 4 above, it can be confirmed that the capacity retention rate of the batteries of Manufacturing Examples 1 to 20 after 100 cycles is in the range of 86.44% to 94.39%, which is generally equivalent to or better than the capacity retention rate of the comparative manufacturing examples 5 to 8 using commercial fluorinated adhesives (PVDF).

[0254] For the NCM electrode, it was confirmed that the initial efficiency and capacity retention of Manufacturing Examples 1 to 11 were at or above the same level as those of Comparative Manufacturing Example 5, which used PVDF. This was attributed to the acrylic binder improving lithium-ion conductivity by maintaining appropriate electrolyte swelling and stably fixing the active material during charge and discharge with high adhesion. In contrast, Comparative Manufacturing Example 1, despite having similar initial efficiency, showed cyclic degradation due to insufficient adhesion; Comparative Manufacturing Examples 2 to 4, due to excessive swelling and decreased adhesion, experienced an initial efficiency of approximately 85% and also exhibited inferior capacity retention.

[0255] For LFP, NCA, and LCO electrodes (Manufacturing Examples 12 to 20), the initial efficiency was maintained at over 90% and the capacity retention at over 86%, which is equivalent to or better than the performance of Comparative Manufacturing Examples 6 to 8, which used PVDF. This result is attributed to the fact that the adhesive of this application, regardless of the type of active material, can simultaneously ensure appropriate swelling and excellent bonding properties, thereby maintaining the stability of the electrode structure.

[0256] Therefore, it has been confirmed that adhesives with the contents of the first monomer unit, the second monomer unit, and the third monomer unit adjusted to the range of this application can maintain electrolyte permeability, interfacial adhesion, and dimensional stability evenly after initial charge and discharge, thereby achieving high capacity retention.

[0257] The scope of this invention is defined by the following claims, rather than by the foregoing detailed description, and all modifications or variations derived from the meaning, scope and equivalents of the claims shall be interpreted as falling within the scope of this invention.

Claims

1. An adhesive comprising a first monomer unit and a second monomer unit, The first monomer unit comprises: a (meth)acrylate monomer unit having a straight-chain hydrocarbon side chain having 1 to 12 carbon atoms, an ethylene monomer unit having an acyl group, or a combination thereof. The second monomer unit comprises: a (meth)acrylate monomer unit having a branched hydrocarbon side chain having 3 or more carbon atoms, a cyclic hydrocarbon side chain having 3 or more carbon atoms, or a combination thereof; an ethylene monomer unit having one or more aromatic cyclic side chains; or a combination thereof.

2. The adhesive according to claim 1, wherein, The (meth)acrylate monomer unit having cyclic hydrocarbon side chains with 3 or more carbon atoms comprises: (meth)acrylate monomer units having aliphatic cyclic hydrocarbon side chains with 3 or more carbon atoms, (meth)acrylate monomer units having one or more aromatic cyclic side chains, or combinations thereof.

3. The adhesive according to claim 1, further comprising a third monomer unit, The third monomer unit comprises: a (meth)acrylate monomer unit having a polar functional group substituted with a heteroatom, an ethylene monomer unit having a polar functional group substituted with a heteroatom, an α,β-unsaturated polycarboxylic acid monomer unit, or a combination thereof. The polar functional group is a carboxylic acid group (-COOH), a sulfonic acid group (-SO3H), a phosphonic acid group (-PO3H2), a cyano group (-CN), a pyrrolidinone group (-C4H6NO), an amide group (-CONH2), a hydroxyl group (-OH), an epoxy group (-C3H5O), a caprolactam group (-C6H 10 NO), an oxazolidinone group (-C3H4NO2), or a combination thereof.

4. The adhesive according to claim 1, wherein, The first monomer unit is formed by polymerization of methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, n-pentyl methacrylate, n-hexyl methacrylate, n-heptyl methacrylate, n-octyl methacrylate, n-nonyl methacrylate, n-decyl methacrylate, n-undecyl methacrylate, n-lauryl methacrylate, vinyl acetate, or combinations thereof.

5. The adhesive according to claim 2, wherein, The (meth)acrylate monomer units, or combinations thereof, having branched hydrocarbon side chains with 3 or more carbon atoms, aliphatic cyclic hydrocarbon side chains with 3 or more carbon atoms, are formed by polymerization of isopropyl (meth)acrylate, isobutyl (meth)acrylate, isoamyl (meth)acrylate, tert-butyl (meth)acrylate, neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecanyl (meth)acrylate, isolaryl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentadienyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, or combinations thereof. The (meth)acrylate monomer unit having one or more aromatic ring side chains is formed by polymerization of benzyl (meth)acrylate, phenyl (meth)acrylate, 3-phenoxybenzyl (meth)acrylate, o-phenylphenoxyethyl (meth)acrylate, 1-naphthyl (meth)acrylate, or combinations thereof. The ethylene monomer unit having one or more aromatic ring side chains is formed by polymerization of styrene, α-methylstyrene, or combinations thereof.

6. The adhesive according to claim 3, wherein, The third monomer unit is formed by polymerization of methacrylic acid, acrylic acid, N-vinylpyrrolidone, acrylonitrile, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, acrylamide, N,N-dimethylacrylamide, glycidyl methacrylate, N-vinylcaprolactam, 2-oxazolidinone-5-ylmethacrylate, 2-cyanoethyl methacrylate, 2-acrylamido-2-methylpropanesulfonic acid, carboxyethyl acrylate, maleic acid, itaconic acid, fumaric acid, aconitic acid, vinylbenzoic acid, vinylsulfonic acid, 4-styrenesulfonic acid, vinylphosphonic acid, N-methacrylamide, or combinations thereof.

7. The adhesive according to claim 3, wherein, Based on the total molar number of the first monomer unit, the second monomer unit, and the third monomer unit, which is 100 mol%, The content of the first monomer unit is 20 mol% or more and 80 mol% or less. The content of the second monomer unit is 20 mol% or more and 80 mol% or less. The content of the third monomer unit is 0 mol% or more and 15 mol% or less.

8. The adhesive according to claim 1, wherein, When the adhesive is immersed in an electrolyte at 40°C to 80°C for 2 to 6 hours, the swelling degree is 20% to 95%.

9. A slurry comprising: The adhesive according to any one of claims 1 to 8; and Active substances.

10. An electrode comprising: Current collector; and An active material layer comprising the adhesive according to any one of claims 1 to 8 is formed on the current collector.

11. A secondary battery comprising the electrode of claim 10.

Citation Information

Patent Citations

  • Cathod active material slurry comprising rubber based binder and cathode electrode produced by the same

    KR1020160040125A