A weather-resistant pressure-sensitive adhesive for vehicle license plate reflective film and its preparation method

By combining soft monomers, hard monomers, and nanofillers, a high cross-linking density adhesive is formed, which solves the problems of weather resistance, anti-warping, and unwinding force of automotive license plate film adhesives. It achieves an adhesive with good weather resistance, good anti-warping, low unwinding force, and good moisture resistance, which is suitable for automotive license plate reflective films.

CN123107582APending Publication Date: 2026-11-17常州市晶德锐反光材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611271371.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing automotive license plate films have adhesives that have problems such as insufficient weather resistance, poor anti-blowout properties, excessive unwinding force, and poor environmental performance. In particular, they are prone to yellowing, powdering, peeling, and cracking under long-term outdoor ultraviolet radiation and high temperature environments.

Method used

A composition comprising soft monomers, hard monomers, functional monomers, nanofillers, initiators, solvents, curing agents, and polymerization inhibitors is used. By controlling the crosslinking structure and the use of nanofillers, an adhesive with high crosslinking density and good flexibility is formed. Combined with the strong interfacial bonding between nanofillers and monomers, ultraviolet rays are blocked, internal stress is reduced, and the weather resistance and anti-warping properties of the adhesive layer are improved.

Benefits of technology

It achieves a coating layer that is not prone to yellowing or powdering during long-term outdoor use, is resistant to warping and has low unwinding force, has good moisture resistance and is environmentally friendly, is suitable for high-speed die-cutting processing, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application relates to the field of polymer adhesive technology, specifically disclosing a weather-resistant pressure-sensitive adhesive for automotive license plate reflective film and its preparation method. The weather-resistant pressure-sensitive adhesive for automotive license plate reflective film comprises the following raw materials in parts by weight: 40-55 parts soft monomer, 8-15 parts hard monomer, 6-10 parts functional monomer, 0.27-0.4 parts initiator, 32-48 parts solvent, 0.08-0.13 parts nanofiller, 0.75-1.3 parts curing agent, and 0.005-0.008 parts polymerization inhibitor. The functional monomer comprises cyclohexyl methacrylate and 2-hydroxyethyl acrylate in a mass ratio of 8-12:1. It has advantages such as good weather resistance, good anti-warping properties, low unwinding force, and good moisture resistance, making it less prone to cracking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of polymer adhesive technology, and more specifically, it relates to a weather-resistant pressure-sensitive adhesive for use in reflective film for vehicle license plates and a method for preparing the same. Background Technology

[0002] Most existing car license plate films are engineering-grade reflective films, and the adhesives used have the following problems: First, insufficient weather resistance. Under long-term outdoor ultraviolet radiation and heat radiation from the engine hood, the adhesive layer is prone to yellowing and powdering, resulting in blurred license plate lettering or film peeling. Second, poor anti-lifting performance. License plates have a concave-convex structure during stamping, and ordinary pressure-sensitive adhesives are prone to stress relaxation at the edges of the grooves, leading to rebound and lifting. Third, excessive unwinding force. During the die-cutting process of reflective film rolls, excessive peeling force can easily cause the brittle reflective layer to break. Fourth, poor environmental performance. Traditional processes have high VOC emissions.

[0003] Therefore, how to prepare a special adhesive for car license plate film that has good weather resistance, good anti-warping properties, low unwinding force, good moisture resistance and is not prone to cracking is an urgent problem to be solved. Summary of the Invention

[0004] In order to prepare a special adhesive for automobile license plate film that has good weather resistance, good anti-warping properties, low unwinding force, good moisture resistance and is not prone to cracking, this application provides a weather-resistant pressure-sensitive adhesive for automobile license plate reflective film and its preparation method.

[0005] In a first aspect, this application provides a weather-resistant pressure-sensitive adhesive for automotive license plate reflective film, employing the following technical solution: A weather-resistant pressure-sensitive adhesive for use in reflective film for vehicle license plates, the adhesive comprising the following raw materials in parts by weight: 40-55 parts soft monomer, 8-15 parts hard monomer, 6-10 parts functional monomer, 0.27-0.4 parts initiator, 32-48 parts solvent, 0.08-0.13 parts nanofiller, 0.75-1.3 parts curing agent, and 0.005-0.008 parts polymerization inhibitor; the functional monomer comprises cyclohexyl methacrylate and 2-hydroxyethyl acrylate in a mass ratio of 8-12:1.

[0006] By employing the above technical solutions, soft monomers impart flexibility to the adhesive, preventing the adhesive layer from becoming brittle under extreme temperatures. Hard monomers enhance the cohesiveness and structural stability of the adhesive, reducing the rate of damage to the molecular chains caused by environmental factors, making the adhesive layer less prone to performance degradation under light and temperature changes. The alicyclic structure of cyclohexyl methacrylate in the functional monomer significantly improves the UV resistance and aging resistance of the adhesive layer. The refractive index of the adhesive matches the resin at the bottom of the reflective film, eliminating "fogging" caused by interfacial light scattering. The hydroxyl groups in 2-hydroxyethyl acrylate further enhance the density of the cross-linked structure, reducing the erosion of the molecular chains by UV rays and heat-oxidation, ensuring the weather resistance of the finished adhesive. The large specific surface area of ​​the nanofillers allows them to form strong interfacial bonds with the monomers, effectively blocking UV penetration, slowing down the aging process, and improving the weather resistance of the adhesive.

[0007] Nanofillers can combine with monomers to disperse concentrated internal stress during the curing process, preventing warping caused by localized stress accumulation. Furthermore, the addition of nanofillers directly reduces the volume shrinkage during the curing stage, weakening the warping driving force caused by shrinkage differences. The high cross-linking density of nanofillers and functional monomers enhances the toughness of the adhesive layer, counteracting the warping tendency caused by differences in the formation between different substrates. It can also constrain uneven deformation at the interface, further suppressing warping and improving the wettability of the adhesive layer to the embossed metal lettering of the license plate. Under stress, it generates micropores to dissipate energy, solving the warping problem of stamped license plates. Thus, the adhesive layer formed by the adhesive has the advantage of good anti-warping properties.

[0008] The soft monomer imparts suitable low cohesive strength to the adhesive layer, preventing it from being too hard and causing excessive adhesion during unwinding. The cyclic side chains of cyclohexyl methacrylate in the functional monomer reduce the intermolecular forces between the adhesive layer and the back of the substrate, reducing the peeling resistance during unwinding. Combined with the "seed-shell" structure formed by nanofillers, soft monomers, hard monomers and functional monomers, the adhesive layer can still achieve smooth and quiet unwinding under high peeling force, making it suitable for high-speed die-cutting machine processing.

[0009] The hydrophobic ring structure of cyclohexyl methacrylate in the functional monomer significantly reduces the water absorption rate of the adhesive film and blocks water vapor penetration. Combined with the hydroxyl groups of 2-hydroxyethyl acrylate, it crosslinks with the curing agent to form a dense network, reducing the entry of water molecules into the adhesive layer. In addition, the nanofiller fills the micropores of the adhesive layer, blocking the water vapor diffusion channels and improving the adhesion stability of the adhesive layer in high humidity environments. Combined with the crosslinking and curing effect of the curing agent, it improves the structural density and prevents water from entering the adhesive layer, ensuring the bonding effect and reducing the risk of adhesive layer cracking.

[0010] Preferably, the soft monomer is one or more of butyl acrylate and isooctyl acrylate.

[0011] By adopting the above technical solutions, the carbon-carbon backbone structure of the two soft monomers is stable and not easily oxidized and degraded by ultraviolet light. Combined with the low yellowing functional monomer system in the formula, it is not easy to cause aging and yellowing problems during long-term outdoor use. The long side chain of isooctyl acrylate can reduce the curing shrinkage rate of the adhesive layer. Combined with a small amount of nanofiller, it disperses internal stress, offsets the difference in deformation between the substrate and the adhesive layer, and avoids warping caused by stress concentration.

[0012] Preferably, the hard monomer is one or more of methyl methacrylate and vinyl acetate.

[0013] By adopting the above technical solutions, methyl methacrylate can improve the cohesiveness, hardness, and structural strength of the adhesive layer. Furthermore, methyl methacrylate and vinyl acetate can improve the water resistance and aging resistance of the adhesive layer, prevent water molecules from penetrating the interior of the adhesive layer, and improve moisture resistance and crack resistance. At the same time, vinyl acetate has a lower polymerization volume shrinkage rate, and when combined with methyl methacrylate, it can reduce the overall curing shrinkage of the system, reduce the residual internal stress generated during the curing process, and avoid stress accumulation-induced warping, thus giving the adhesive layer the advantage of good anti-warping properties.

[0014] Preferably, the initiator is azobisisobutyronitrile.

[0015] By adopting the above technical solution, azobisisobutyronitrile can initiate cross-linking polymerization of monomers, improve the structural density and strength and toughness of the adhesive layer, and ensure the weather resistance, moisture resistance and crack resistance of the adhesive layer.

[0016] Preferably, the solvent is composed of ethyl acetate and isopropanol in a mass ratio of 1:1-3.

[0017] By adopting the above technical solution, ethyl acetate and isopropanol can efficiently dissolve monomeric substances, ensuring the polymerization reaction proceeds and forming a stable and uniform film layer. This film layer is suitable for wetting the raised and recessed metal lettering on license plates, ensuring anti-warping and adhesion stability, and preventing problems such as adhesive layer peeling and cracking.

[0018] Preferably, the curing agent is composed of an isocyanate crosslinking agent and an epoxy crosslinking agent in a mass ratio of 1:1-2.

[0019] By adopting the above technical solution, the isocyanate groups in the isocyanate crosslinking agent can quickly react with the active groups such as hydroxyl groups in the acrylic adhesive to build a preliminary three-dimensional crosslinking network in a short time, rapidly improving the cohesiveness and holding power of the adhesive layer. It can also react with the active groups on the surface of the substrate, significantly improving the adhesion of the adhesive layer to substrates such as metals and plastics, and preventing interface delamination and lifting. At the same time, the urethane bonds formed after crosslinking can significantly improve the solvent resistance, weather resistance and creep resistance of the adhesive layer, making it suitable for high temperature and high humidity application scenarios.

[0020] The epoxy groups of epoxy crosslinking agents can slowly react with carboxyl and hydroxyl groups under medium and low temperature conditions to complete deep crosslinking, improve the crosslinking network structure, avoid the uneven crosslinking problem that occurs when isocyanate is used alone, and the ether bond structure formed after crosslinking has extremely strong chemical stability, which greatly reduces the water absorption rate of the film and significantly improves the moisture resistance of the adhesive layer, avoiding adhesion failure in high humidity environments. At the same time, the volume shrinkage rate of the epoxy crosslinking reaction is extremely low, which can effectively alleviate the local internal stress caused by single isocyanate crosslinking and help improve the anti-warping and anti-cracking performance of the adhesive layer.

[0021] Isocyanate first completes the initial cross-linking and shaping quickly, while epoxy completes the deep cross-linking later, forming a dense three-dimensional network with a gradient distribution, which takes into account both the initial tack and long-term tack performance of the adhesive layer. By forming cross-linking points with different bond energies, the residual internal stress generated during the curing process can be evenly dispersed, avoiding adhesive layer cracking and lifting problems caused by local stress concentration. Furthermore, isocyanate makes up for the shortcomings of epoxy in slow cross-linking reaction and insufficient initial tack, while epoxy makes up for the shortcomings of isocyanate in poor water and moisture resistance and sensitivity to moisture, ultimately resulting in a high-performance acrylic adhesive that combines low unwinding force, anti-lifting, moisture resistance and crack resistance.

[0022] Preferably, the nanofiller is nano-silica.

[0023] By adopting the above technical solutions, nano-silica possesses excellent UV shielding capabilities, reducing the degradation and damage of acrylic acid molecular chains by UV light. Simultaneously, its high thermal stability enhances the aging resistance of the adhesive layer, extending its outdoor service life. Furthermore, the uniform dispersion of nano-silica in the adhesive layer allows it to utilize its surface hydroxyl active groups to combine with acrylic substances, increasing the cross-linking density and stability, reducing the curing shrinkage rate of the adhesive layer, and thus resisting warping. HIA can disperse residual internal stress generated during curing, preventing warping caused by localized stress concentration. At the same time, nano-silica can balance the adhesive layer's viscosity and cohesion, resulting in lower peel resistance during tape unwinding and achieving a low unwinding force effect.

[0024] Preferably, the nano-silica is modified nano-silica, which is prepared by loading perfluorooctyl ethyl trichlorosilane onto nano-silica particles and then binding them with pentaerythritol maleic rosin.

[0025] By employing the above technical solution, hydrophobic fluorinated segments are grafted onto the surface of nano-silica using perfluorooctyl ethyl trichlorosilane, significantly reducing the surface energy of nanoparticles, preventing agglomeration, uniformly dispersing curing internal stress, and reducing warping caused by local stress concentration. Combined with the rigid cyclic structure of maleic rosin pentaerythritol ester filling the gaps between resin molecular chains, reducing volume shrinkage during polymerization, this fundamentally reduces residual curing stress and inhibits warping caused by poor deformation between the adhesive layer and the substrate. Furthermore, the modified nano-silica optimizes the uniformity of interfacial adhesion between the adhesive layer and the substrate, facilitating the wetting of the pores in the uneven metal lettering, ensuring sufficient wetting, guaranteeing bonding effect, and preventing edge warping caused by insufficient local adhesion. In addition, the chemical bonding with the hydroxyl groups of 2-hydroxyethyl acrylate strengthens the interfacial adhesion between the adhesive layer and the metal substrate, constrains adhesive layer deformation, and further improves anti-warping performance.

[0026] The perfluorofluorinated segments in the perfluorooctyl ethyl trichlorosilane on the surface of nano-silica particles endow nano-silica with superhydrophobic properties, constructing a hydrophobic barrier inside the adhesive layer, significantly reducing the water molecule penetration rate and improving the moisture resistance of the adhesive layer. Maleic rosin pentaerythritol ester is soluble in ethyl acetate, which facilitates cross-linking with acrylic substances with the assistance of curing agents, initiators and other substances. Using nano-silica particles as stress concentration points, it induces crazing to absorb energy, and works synergistically with the cross-linking of maleic rosin pentaerythritol ester and acrylic acid to further prevent the propagation of microcracks, avoid cracking of the adhesive layer under external force or temperature changes, and ensure the moisture resistance and crack resistance of the finished adhesive.

[0027] Preferably, the raw materials also include POSS composite material, which is prepared by treating POSS with terminal amino hyperbranched polysiloxane and then loading it with polycaprolactone-polyethylene glycol-maleimide.

[0028] By employing the above technical solution, the cage-like nanostructure of POSS can support hyperbranched polysiloxane and polycaprolactone-polyethylene glycol-maleimide. Utilizing the three-dimensional cage-like Si-O-Si rigid inorganic framework of POSS, it is uniformly dispersed at the nanoscale in the acrylic resin matrix, filling the free volume between polymer chains and restricting the random and tight packing of acrylic molecular chains during curing. This effectively reduces the volume shrinkage rate during drying and crosslinking stages, minimizing the generation of residual internal stress from the source. The hyperbranched polysiloxane possesses a flexible Si-O-Si backbone, encapsulating the rigid POSS cage core, forming a structure between the rigid POSS particles and the acrylic resin. A flexible buffer transition layer is constructed to avoid modulus cliffs between rigid fillers and the polymer matrix, eliminating stress singularities at the two-phase interface. Furthermore, the terminal amino groups can react with the maleimide groups of the subsequent loading component, polycaprolactone-polyethylene glycol-maleimide, to stabilize the covalently bonded block polymer. On the other hand, the amino groups can connect with the hydroxyl groups in the acrylic groups and the hydroxyl groups on the surface of the nanofillers, enhancing the interfacial bonding stability. Meanwhile, the polysiloxane chain segments have high flexibility and excellent chain movement capabilities, providing channels for local stress relaxation. The siloxane is resistant to high and low temperatures, which can reduce the thermal expansion coefficient of the filler region and suppress warping induced by thermal stress under thermal cycling conditions.

[0029] The maleimide groups in the polycaprolactone-polyethylene glycol-maleimide on the POSS surface can improve the bonding effect between the POSS composite and the acrylic matrix, increase the density and stability of the cross-linked structure, resist stress, and prevent warping. Furthermore, the flexible segments of polycaprolactone have good stress resistance, and by controlling the movement of these flexible segments, curing stress can be slowly released, alleviating the problem of fixed cross-linking points and restricted chain movement in the pure acrylic cross-linked network, which makes it difficult to release internal stress and ensures anti-warping properties. Combined with the cross-linking of hydroxyl groups in polyethylene glycol with carboxyl groups in the acrylic matrix and hydroxyl groups in functional monomers, compatibility and wettability are further improved. The flexible segments also have a stress-buffering effect, thus improving the wettability of the adhesive on the embossed metal lettering of the license plate and enhancing anti-warping properties. The high cross-linked structure density, combined with polycaprolactone, further improves moisture resistance and crack resistance.

[0030] Secondly, this application provides a method for preparing a weather-resistant pressure-sensitive adhesive for automotive license plate reflective film, employing the following technical solution: A method for preparing a weather-resistant pressure-sensitive adhesive for vehicle license plate reflective film includes the following steps: S1. Disperse the nanofiller in a portion of the soft monomers, and then treat it with ultrasound to obtain a premix. S2. Mix part of the premix with part of the solvent and heat to 78-80℃. Then add dropwise a mixture A consisting of hard monomer, the remaining soft elastomer and part of the initiator. After the dropwise addition is completed, keep the temperature for 14-18 minutes. Then cool down to 72-74℃ and add dropwise a mixture B consisting of functional monomer, the remaining initiator and the remaining solvent. After the dropwise addition is completed, mix well to obtain the reaction solution. S3. The composite liquid is heated to 82-84℃ for maturation, and after cooling, a polymerization inhibitor is added to terminate the process, resulting in the composite liquid. S4. Dilute the composite liquid to a solid content of 35-40%, add curing agent, mix well, and then coat, cure and mature to obtain the finished product.

[0031] By employing the above technical solution, nanofillers are uniformly dispersed at the nanoscale within soft monomers, preventing agglomeration and ensuring that nanoparticles uniformly exert stress dispersion and hydrophobic reinforcement effects within the adhesive layer. This fundamentally guarantees the adhesive layer's resistance to warping and cracking. Hard / soft monomers are first added dropwise at 78-80℃ to complete preliminary polymerization, initiating seed polymerization and forming a high-molecular-weight core. Functional monomers are then added dropwise at 72-74℃, introducing them at a low temperature. This effectively protects the highly reactive groups located at the ends of the molecular chains, improving post-crosslinking efficiency and resulting in a copolymer with a uniform molecular weight distribution and regular structure. This avoids internal stress concentration caused by uneven local crosslinking and simultaneously enhances the activity of the functional monomers. The uniform distribution of functional groups enhances interfacial adhesion and moisture resistance; curing at 82-84℃ allows residual monomers to fully react, perfecting the cross-linking network structure and preventing adhesive layer deformation and warping caused by the subsequent slow reaction of residual monomers; the polymerization inhibitor precisely terminates the reaction, stabilizing the viscosity of the adhesive and preventing performance fluctuations during storage; a solid content of 35-40% allows for precise control of adhesive layer thickness and cross-linking density, preventing abnormal unwinding force caused by excessively thick or thin adhesive layers; subsequent coating, curing, and aging processes allow the curing agent to fully complete deep cross-linking, further reducing residual internal stress, ultimately resulting in a high-performance finished adhesive that combines anti-warping, moisture resistance, crack resistance, and low unwinding force.

[0032] Preferably, the specific curing steps are as follows: drying at 65-70℃ for 30-60s, drying at 85-90℃ for 45-90s, and drying at 100-110℃ for 60-120s.

[0033] Preferably, the curing temperature is 40-50℃.

[0034] By adopting the above technical solution, most of the solvent is evaporated at 65-70℃ to prevent surface skinning, the solvent is completely evaporated at 85-90℃, the adhesive layer is initially cured, and the thermal cross-linking reaction is activated at 100-110℃ to form a preliminary network structure; the deep cross-linking equilibrium is completed after curing.

[0035] In summary, this application has the following beneficial effects: 1. Soft monomers impart flexibility to adhesives, preventing the adhesive layer from becoming brittle under extreme temperatures. Hard monomers enhance the cohesiveness and structural stability of adhesives, reducing the rate of damage to molecular chains caused by environmental factors, making the adhesive layer less prone to performance degradation under light and temperature changes. The alicyclic structure of cyclohexyl methacrylate in the functional monomer significantly improves the UV resistance and aging resistance of the adhesive layer. The adhesive's refractive index matches the resin at the bottom of the reflective film, eliminating "fogging" caused by interfacial light scattering. The hydroxyl groups in 2-hydroxyethyl acrylate further enhance the density of the cross-linked structure, reducing the erosion of molecular chains by UV rays and heat-oxidation, ensuring the weather resistance of the finished adhesive. The large specific surface area of ​​the nanofillers allows them to form strong interfacial bonds with the monomers, effectively blocking UV penetration, slowing down the aging process, and improving the weather resistance of the adhesive.

[0036] 2. Nanofillers can combine with monomers to disperse concentrated internal stress during the curing process, avoiding localized stress accumulation and warping. The addition of nanofillers directly reduces the volume shrinkage during the curing stage, weakening the warping driving force caused by shrinkage difference. The high cross-linking density of nanofillers and functional monomers enhances the toughness of the adhesive layer, counteracts the warping tendency caused by the difference in formation between different substrates, and can also constrain uneven deformation at the interface, further suppressing warping and improving the wettability of the adhesive layer to the embossed metal lettering of the license plate. Under stress, micropores dissipate energy, solving the warping problem of stamped license plates, thus giving the adhesive layer formed by the adhesive good anti-warping properties.

[0037] 3. The rigid cage-like hybrid structure of POSS fills the free volume of the resin, reducing the volume shrinkage caused by the curing / solvent evaporation of acrylic adhesive and reducing the generation of residual stress. Combined with the rigid POSS cage core → flexible hyperbranched siloxane → PCL / PEG flexible block → acrylic resin, a continuous gradient modulus is formed, avoiding the common interface cracking defects between inorganic fillers and organic resins. Furthermore, the polysiloxane segments and the dual flexible phases of polycaprolactone and polyethylene glycol form a large number of micro-regions inside the adhesive film. Relying on the creep of polymer segments, the residual shrinkage stress of curing and the thermal stress of cold and hot cycles are continuously released, improving the resistance to warping and the interfacial bonding force.

[0038] 4. Isocyanate crosslinking agents are used to react with the main chain hydroxyl groups to form a network structure, providing creep resistance at high temperatures; epoxy crosslinking agents are inert at room temperature, but when license plates are used outdoors for a long time, moisture slowly penetrates and activates deep crosslinking, repairing micro-cracks caused by mechanical stress and extending service life. Detailed Implementation

[0039] The present application will be further described in detail below with reference to the embodiments.

[0040] Preparation example of modified nano silica Preparation Example 1: Modified nano-silica was prepared using the following method: Nano-silica particles were ultrasonically dispersed in a perfluorooctyl ethyl trichlorosilane solution at a mass ratio of 1:10 for 60 min, resulting in an average particle size of 40 nm. The perfluorooctyl ethyl trichlorosilane solution had a mass fraction of 5% and toluene was used as the solvent. The nano-silica particles were then separated by centrifugation, washed three times with anhydrous ethanol, dried at 80°C for 24 h, dispersed, and crushed to obtain carrier silica with an average particle size of less than 80 nm. 1 kg of carrier silica was mixed with 0.12 kg of maleic rosin pentaerythritol ester and stirred until homogeneous. The mixture was then heated to 120°C to soften and melt the maleic rosin pentaerythritol ester. The mixture was stirred at 1000 r / min until homogeneous, cooled, dispersed, and crushed to obtain the finished modified nano-silica with an average particle size of less than 100 nm.

[0041] Example of POSS composite material preparation Preparation Example 2: POSS composite material was prepared using the following method: POSS was ultrasonically dispersed in a terminal amino hyperbranched polysiloxane solution at a mass ratio of 1:10 for 60 min. The terminal amino hyperbranched polysiloxane solution had a mass fraction of 5% and was dissolved in anhydrous ethanol. The mixture was allowed to stand for 2 h, then washed three times with anhydrous ethanol and vacuum dried at 80 °C for 12 h to obtain loaded POSS. 1 kg of loaded POSS was dispersed in 10 kg of water, and then 1.5 kg of polycaprolactone-polyethylene glycol-maleimide was added and stirred until homogeneous. The mixture was stirred at 50 °C and 1000 r / min for 6 h, then freeze-dried and crushed to obtain the finished POSS composite material with a particle size of less than 80 nm. Example

[0042] Example 1: A weather-resistant pressure-sensitive adhesive for reflective film on vehicle license plates: The composition includes 48 kg of soft monomer, 12 kg of hard monomer, 8 kg of functional monomer, 0.32 kg of initiator, 40 kg of solvent, 0.1 kg of nanofiller, 1 kg of curing agent, and 0.006 kg of polymerization inhibitor. The soft monomer is butyl acrylate, the hard monomer is methyl methacrylate, the functional monomer is composed of cyclohexyl methacrylate and 2-hydroxyethyl acrylate in a 10:1 mass ratio, the initiator is azobisisobutyronitrile, the solvent is composed of ethyl acetate and isopropanol in a 1:2 mass ratio, the nanofiller is fumed silica with an average particle size of 40 nm, the curing agent is composed of isocyanate crosslinking agent and epoxy crosslinking agent in a 1:1.5 mass ratio, and the polymerization inhibitor is p-hydroxyanisole. The preparation method is as follows: S1. Disperse the nanofiller in 8 kg of soft monomer and ultrasonically disperse for 30 min. After the process is completed, a premix is ​​obtained. S2. Mix 15% of the total premix with ethyl acetate in the solvent and heat to 78°C. Then, add dropwise a mixture A consisting of hard monomer, 40 kg of soft elastomer, and 0.16 kg of initiator to initiate seed polymerization and form a high molecular weight core. After the dropwise addition is complete, keep the temperature for 15 min, then cool to 72°C and add dropwise a mixture B consisting of functional monomer, 0.16 kg of initiator, and isopropanol in the solvent. After the dropwise addition is complete, mix well to obtain the reaction solution. S3. The composite liquid is heated to 82°C for curing, and after cooling, an inhibitor is added to terminate the polymerization and reduce the residual monomer content to less than 0.1% to obtain the composite liquid. S4. Dilute the composite liquid to a solid content of 38%, add curing agent, mix well to obtain a mixture; apply the mixture to the release paper with a doctor blade, dry at 68℃ for 40s, then dry at 86℃ for 60s, and then dry at 105℃ for 90s to complete curing, then roll it up and put it into the curing chamber, and cure at 45℃ for 48h to obtain the finished product.

[0043] Example 2: The difference between this example and Example 1 is that: The composition includes 40 kg of soft monomer, 8 kg of hard monomer, 6 kg of functional monomer, 0.27 kg of initiator, 32 kg of solvent, 0.08 kg of nanofiller, 0.75 kg of curing agent, and 0.005 kg of polymerization inhibitor. The soft monomer is isooctyl acrylate, the hard monomer is vinyl acetate, the functional monomer is composed of cyclohexyl methacrylate and 2-hydroxyethyl acrylate in a mass ratio of 8:1, the solvent is composed of ethyl acetate and isopropanol in a mass ratio of 1:1, the nanofiller is fumed silica with an average particle size of 40 nm, and the curing agent is composed of isocyanate crosslinking agent and epoxy crosslinking agent in a mass ratio of 1:1. The preparation method is as follows: S1. Disperse the nanofiller in 5 kg of soft monomer and ultrasonically disperse for 30 min. After the process is completed, a premix is ​​obtained. S2. Mix 15% of the total premix with ethyl acetate in the solvent and heat to 78°C. Then, add dropwise a mixture A consisting of hard monomer, 35 kg of soft elastomer, and 0.15 kg of initiator to initiate seed polymerization and form a high molecular weight core. After the dropwise addition is complete, keep the temperature for 14 min, then cool to 72°C and add dropwise a mixture B consisting of functional monomer, 0.12 kg of initiator, and isopropanol in the solvent. After the dropwise addition is complete, mix well to obtain the reaction solution. S3. The composite liquid is heated to 82°C for curing, and after cooling, an inhibitor is added to terminate the polymerization and reduce the residual monomer content to less than 0.1% to obtain the composite liquid. S4. Dilute the composite liquid to a solid content of 35%, add curing agent, mix well to obtain a mixture; apply the mixture to the release paper with a doctor blade, dry at 65℃ for 60s, then dry at 85℃ for 90s, and then dry at 100℃ for 120s to complete curing, roll it up and put it into the curing chamber, and cure at 40℃ for 48h to obtain the finished product.

[0044] Example 3: The difference between this example and Example 1 is that: The composition includes 55 kg of soft monomer, 15 kg of hard monomer, 10 kg of functional monomer, 0.4 kg of initiator, 48 kg of solvent, 0.13 kg of nanofiller, 1.3 kg of curing agent, and 0.008 kg of polymerization inhibitor. The soft monomer is butyl acrylate, the hard monomer is methyl methacrylate, the functional monomer is composed of cyclohexyl methacrylate and 2-hydroxyethyl acrylate in a mass ratio of 12:1, the solvent is composed of ethyl acetate and isopropanol in a mass ratio of 1:3, the nanofiller is fumed silica with an average particle size of 40 nm, and the curing agent is composed of isocyanate crosslinking agent and epoxy crosslinking agent in a mass ratio of 1:2. The preparation method is as follows: S1. Disperse the nanofiller in 10 kg of soft monomer and ultrasonically disperse for 30 min. After the process is completed, a premix is ​​obtained. S2. Mix 15% of the total premix with ethyl acetate in the solvent and heat to 80°C. Then, add dropwise a mixture A consisting of hard monomer, 45 kg of soft elastomer, and 0.2 kg of initiator to initiate seed polymerization and form a high molecular weight core. After the dropwise addition is complete, keep the temperature for 18 min, then cool to 74°C and add dropwise a mixture B consisting of functional monomer, 0.2 kg of initiator, and isopropanol in the solvent. After the dropwise addition is complete, mix well to obtain the reaction solution. S3. The composite liquid is heated to 84°C for curing, and after cooling, an inhibitor is added to terminate the polymerization and reduce the residual monomer content to less than 0.1% to obtain the composite liquid. S4. Dilute the composite liquid to a solid content of 40%, add curing agent, mix well to obtain a mixture; apply the mixture to the release paper with a doctor blade, dry at 70℃ for 30s, then dry at 90℃ for 45s, and then dry at 110℃ for 60s to complete curing, roll it up and put it into the curing chamber, and cure at 50℃ for 48h to obtain the finished product.

[0045] Example 4: The difference between this example and Example 1 is that: The nano-silica in the raw materials is the modified nano-silica prepared in Preparation Example 1.

[0046] Example 5: The difference between this example and Example 4 is that: The raw materials also include the POSS composite material prepared in Preparation Example 2.

[0047] Example 6: The difference between this example and Example 4 is that: No maleic rosin pentaerythritol ester was added during the preparation of the modified nano-silica.

[0048] Example 7: The difference between this example and Example 5 is that: During the preparation of POSS composite material, no polycaprolactone-polyethylene glycol-maleimide was added.

[0049] Comparative Example Comparative Example 1: The difference between this comparative example and Example 1 is that: The functional monomer did not contain cyclohexyl methacrylate.

[0050] Performance testing 1. Weather resistance test Adhesives were prepared using the methods of Examples 1-7 and Comparative Example 1, respectively, and aged under QUV for 3000 hours, with yellowing observed.

[0051] 2. Anti-warping test Adhesives were prepared using the methods of Examples 1-7 and Comparative Example 1, respectively. The release paper used for coating during the preparation of adhesives was replaced with a number plate with embossed lettering. The adhesives were placed in a test chamber at 40°C and 85% humidity for 72 hours in accordance with GB / T 34712-2017, and the edge lifting height was tested and the data were recorded.

[0052] 3. Low unwinding force test Adhesives were prepared using the methods of Examples 1-7 and Comparative Example 1, respectively. The unwinding force was tested according to GB / T 4850-2002. The test conditions were: temperature 25℃, relative humidity 55%, and unwinding speed 300mm / min. Data were recorded.

[0053] 4. Moisture resistance and crack resistance test Adhesives were prepared using the methods of Examples 1-7 and Comparative Example 1, respectively. Peel strength was tested according to GB / T 2792-2014. Peel strength was tested again under conditions of 30°C and 95% relative humidity. The peel strength retention rate was calculated and the data recorded. A high peel strength retention rate indicates that moisture is less likely to penetrate the film layer under humid and hot conditions, thus preventing crack formation.

[0054] Table 1 Performance Test Table

[0055] As can be seen from Examples 1-3 and Table 1, the adhesive prepared in this application has good weather resistance, anti-warping and low unwinding force, as well as good moisture resistance and crack resistance.

[0056] Combining Examples 1 and 4 with Table 1, it can be seen that after treatment, nano-silica can further improve the adhesive's resistance to warping and peel strength retention. As can be seen from Examples 4 and 5 and Table 1, the addition of POSS composite material can improve the adhesive's resistance to warping and its resistance to moisture cracking.

[0057] Combining Examples 4 and 6 with Table 1, it can be seen that in Example 6, no maleic rosin pentaerythritol ester was added during the preparation of the modified nano-silica. Compared with Example 4, the curling height was greater than that of Example 4, the unwinding force was lower than that of Example 4, and the peel strength retention rate was lower than that of Example 4. This indicates that the rigid cyclic structure of maleic rosin pentaerythritol ester fills the gaps between the resin molecular chains, reducing the volume shrinkage of the polymerization reaction, reducing the residual stress of curing from the source, and inhibiting curling caused by the difference in deformation between the adhesive layer and the substrate. The crosslinking of maleic rosin pentaerythritol ester and acrylic acid further prevents the propagation of microcracks, avoids cracking of the adhesive layer under external force or temperature change, and ensures the moisture resistance and crack resistance of the finished adhesive. At the same time, it reduces the unwinding force.

[0058] Combining Examples 5 and 7 with Table 1, it can be seen that in the preparation process of the POSS composite material in Example 7, without the addition of polycaprolactone-polyethylene glycol-maleimide, the curling height was greater than that in Example 5, the unwinding force was lower, and the peel strength retention rate was lower than that in Example 5. This indicates that the addition of polycaprolactone-polyethylene glycol-maleimide can improve the interfacial bonding stability. The polysiloxane chain segments have high flexibility and excellent chain segment movement ability, providing a channel for local stress relaxation. Siloxane is resistant to high and low temperatures, which can reduce the thermal expansion coefficient of the filler area and suppress curling induced by thermal stress under thermal cycling conditions. It can also improve the density and stability of the cross-linked structure, making it less susceptible to moisture intrusion and cracking. Combined with the flexible chain segments of polycaprolactone and polyethylene glycol, it further improves the anti-curling property and reduces the unwinding force.

[0059] Combining Example 1 and Comparative Example 1 with Table 1, it can be seen that Comparative Example 1, which did not add cyclohexyl methacrylate to its functional monomer, exhibited yellowing, a greater lifting height, and a lower peel strength retention rate compared to Example 1. This indicates that cyclohexyl methacrylate, with its adhesive refractive index matching the underlying resin of the reflective film, eliminates "fogging" caused by interfacial light scattering. Combined with an aliphatic curing agent, it showed no significant yellowing after 3000 hours of QUV aging.

[0060] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.

Claims

1. A weather-resistant pressure-sensitive adhesive for use in reflective film for vehicle license plates, characterized in that, The adhesive is made from the following raw materials in parts by weight: 40-55 parts of soft monomer, 8-15 parts of hard monomer, 6-10 parts of functional monomer, 0.27-0.4 parts of initiator, 32-48 parts of solvent, 0.08-0.13 parts of nanofiller, 0.75-1.3 parts of curing agent, and 0.005-0.008 parts of polymerization inhibitor; the functional monomer comprises cyclohexyl methacrylate and 2-hydroxyethyl acrylate in a mass ratio of 8-12:

1.

2. The weather-resistant pressure-sensitive adhesive for vehicle license plate reflective film according to claim 1, characterized in that: The soft monomer is one or more of butyl acrylate and isooctyl acrylate.

3. The weather-resistant pressure-sensitive adhesive for vehicle license plate reflective film according to claim 1, characterized in that, The hard monomer is one or more of methyl methacrylate and vinyl acetate.

4. The weather-resistant pressure-sensitive adhesive for vehicle license plate reflective film according to claim 1, characterized in that, The initiator is azobisisobutyronitrile.

5. The weather-resistant pressure-sensitive adhesive for vehicle license plate reflective film according to claim 1, characterized in that, The solvent is composed of ethyl acetate and isopropanol in a mass ratio of 1:1-3.

6. The weather-resistant pressure-sensitive adhesive for vehicle license plate reflective film according to claim 1, characterized in that, The curing agent is composed of isocyanate crosslinking agent and epoxy crosslinking agent in a mass ratio of 1:1-2.

7. The weather-resistant pressure-sensitive adhesive for vehicle license plate reflective film according to claim 1, characterized in that, The nanofiller is nano-silica.

8. The weather-resistant pressure-sensitive adhesive for vehicle license plate reflective film according to claim 7, characterized in that, The nano-silica is modified nano-silica, which is prepared by loading perfluorooctyl ethyl trichlorosilane onto nano-silica particles and then binding them with pentaerythritol maleate.

9. The weather-resistant pressure-sensitive adhesive for vehicle license plate reflective film according to claim 1, characterized in that, The raw materials also include POSS composite material, which is prepared by treating POSS with terminal amino hyperbranched polysiloxane and then loading it with polycaprolactone-polyethylene glycol-maleimide.

10. A method for preparing a weather-resistant pressure-sensitive adhesive for vehicle license plate reflective film according to any one of claims 1-9, characterized in that, Includes the following steps: S1. Disperse the nanofiller in a portion of the soft monomers, and after ultrasonic treatment, obtain a premix; S2. Mix part of the premix with part of the solvent and heat to 78-80℃. Then add dropwise a mixture A consisting of hard monomer, the remaining soft elastomer and part of the initiator. After the dropwise addition is completed, keep the temperature for 14-18 minutes. Then cool down to 72-74℃ and add dropwise a mixture B consisting of functional monomer, the remaining initiator and the remaining solvent. After the dropwise addition is completed, mix well to obtain the reaction solution. S3. The composite liquid is heated to 82-84℃ for maturation, and after cooling, a polymerization inhibitor is added to terminate the process, resulting in the composite liquid. S4. Dilute the composite liquid to a solid content of 35-40%, add curing agent, mix well, and then coat, cure and mature to obtain the finished product.