Solvent-free optical adhesive with tunable dual-stage damping, solvent-free optical adhesive film with tunable dual-stage damping, its preparation method and application
By using a solvent-free optical adhesive with adjustable damping in two stages and employing a design of prepolymer components and post-polymer components, the problems of cumbersome production process, high cost, low efficiency and poor terminal quality of UV-OCA have been solved, achieving efficient and stable film preparation and meeting the needs of large-scale mass production of high-end display modules.
Patent Information
- Application Number
- CN202611457511.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing UV-OCA production processes are cumbersome, costly, inefficient, and suffer from solvent residue leading to poor terminal quality. The isocyanate grafting system also exhibits poor stability, limited performance, and is not adjustable, failing to meet the demands of large-scale production of high-end display modules.
A solvent-free optical adhesive with adjustable damping in two stages is adopted. Through the design of prepolymer components and post-polymer components, the combination of acid-free acrylate main monomer, branching regulator, high-temperature damping modified monomer and interface wetting modified monomer is used. Combined with oxygen-free coating and staged UV curing, solvent residue and acid corrosion are avoided, so as to achieve both high fluidity and curing stability of the adhesive.
It has achieved efficient and stable film preparation, solved the problems of high production cost, low efficiency and poor terminal quality, improved the chemical stability and optical durability of the film, and met the needs of large-scale mass production of high-end display modules.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention relates to the field of optical pressure-sensitive adhesive materials technology, and in particular to a solvent-free optical adhesive with adjustable dual-stage damping, a solvent-free optical adhesive film with adjustable dual-stage damping, its preparation method and application. Background Technology
[0002] Currently, the mainstream manufacturing process for UV-OCA used in blind hole bonding in the industry generally adopts a production route of solvothermal polymerization + grafting modification with isocyanate-modified monomers with double bonds + solvent coating and drying. The OCA prepared by this process can achieve an acid-free system, secondary UV curing, and zero gel fraction, which can meet the basic blind hole bonding requirements. However, in actual production and end-use applications, there are many unavoidable technical defects and process bottlenecks, as follows: (1) The production process is complicated and the mass production cost is high. Traditional processes require multiple steps such as solvothermal polymerization, NCO-OH grafting to introduce UV double bonds, high temperature vacuum desolventizing, secondary dilution and compounding of solvent, and long-distance oven segmented solvent removal. The production steps are complicated, the investment in special equipment is large, the production line occupies a large area, and the overall energy consumption is relatively high.
[0003] (2) Coating mass production efficiency is extremely low. The coating speed of solvent-based OCA is strictly limited by the solvent evaporation rate. The mass production speed of solvent-based OCA with a thickness of 100μm in the industry is generally <5m / min, which cannot meet the needs of large-scale and high-efficiency mass production of high-end display modules, resulting in a prominent capacity bottleneck.
[0004] (3) Solvent residue causes terminal defects. The solvent inside the thick OCA adhesive film is difficult to dry and remove completely. The residual solvent will slowly precipitate under high temperature and high humidity conditions, causing quality problems such as micro bubbles at the blind hole bonding interface, increased screen haze, and film delamination, which greatly reduces the product's service life.
[0005] (4) The stability of the isocyanate grafting system is poor. The mainstream isocyanate modified monomers with double bonds are expensive and extremely sensitive to the humidity of the production environment. Even a small amount of moisture can trigger side reactions to generate impurities, which directly leads to a decrease in the light transmittance of the film, an increase in the appearance defect rate, and difficulty in controlling the production yield.
[0006] (5) Single and unadjustable performance, poor adaptability to blind holes. In order to maintain dimensional stability, traditional solvent-based OCA has a low high-temperature loss factor and strict requirements for degassing temperature, pressure and time. Moreover, it is easy to have low yield in one degassing and colloidal shrinkage and bubble rebound problems in high-temperature environment.
[0007] Meanwhile, the industry has long held fixed technical biases, generally believing that solvent-free bulk polymerization has problems such as easy explosive polymerization, high gelation, and uncontrollable molecular branching, making it impossible to achieve high filling performance of blind holes. Therefore, the industry has long relied on solvent polymerization grafting routes.
[0008] In view of this, the present invention is hereby proposed. Summary of the Invention
[0009] One of the objectives of this invention is to provide a solvent-free optical adhesive with adjustable two-stage damping, so as to at least solve one of the technical problems existing in the prior art.
[0010] The second objective of this invention is to provide a solvent-free optical film with adjustable two-stage damping.
[0011] The third objective of this invention is to provide a method for preparing the above-mentioned solvent-free optical film with adjustable two-stage damping.
[0012] The fourth objective of this invention is to provide the application of the above-mentioned solvent-free optical adhesive or solvent-free optical adhesive film with adjustable dual-stage damping.
[0013] In order to achieve the above-mentioned objectives of the present invention, the following technical solution is adopted: This invention provides a solvent-free optical adhesive with adjustable two-stage damping, wherein the raw materials of the solvent-free optical adhesive include a prepolymer component and a post-polymer component; The prepolymer components include an acid-free acrylate main monomer, a branching regulator, a high-temperature damping modified monomer, an interface wetting modified monomer, and a bulk polymerization initiator. The post-formulation components include UV crosslinking monomers and photoinitiators; The solvent-free optical adhesive contains no acidic carboxyl monomers and no solvents.
[0014] Furthermore, the Ubbelohde viscosity IV value of the prepolymer component is 1.7 to 2.2.
[0015] Furthermore, the acid-free acrylate main monomer includes at least two of isooctyl acrylate, isooctyl methacrylate, butyl acrylate, hydroxyethyl acrylate, and acrylamide; Preferably, the branching regulator includes Showa PE1 resin, and more preferably pentaerythritol tetra(3-mercaptobutyrate); Preferably, the high-temperature damping modifying monomer includes at least one of hexyl acrylate, lauryl acrylate, and tert-butyl acrylate; Preferably, the interface wetting modifying monomer includes at least one of N-vinylpyrrolidone and N-vinylformamide; Preferably, the bulk polymerization initiator includes at least one selected from 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, and α,α-dimethoxy-α-phenylacetophenone; Preferably, the UV crosslinking monomer includes at least one of 1,9-nonanediol diacrylate, 6-hexanediol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, and pentaerythritol triacrylate. Preferably, the photoinitiator comprises at least one selected from 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, and α,α-dimethoxy-α-phenylacetophenone; Furthermore, the solvent-free optical adhesive also includes functional additives; Preferably, the functional additives include leveling agents and antioxidants.
[0016] Furthermore, it includes the following raw materials in parts by weight: The composition includes 80-90 parts of acid-free acrylate main monomer, 0.5-2.0 parts of branching regulator, 5 parts of high-temperature damping modified monomer, 0.2-1.0 parts of interface wetting modified monomer, 0.1-0.5 parts of bulk polymerization initiator, 0.1-0.5 parts of UV crosslinking monomer, 0.1-0.4 parts of photoinitiator, and 0.1-0.6 parts of functional additives.
[0017] The present invention also provides a solvent-free optical film with adjustable dual-stage damping, which is prepared from the above-mentioned solvent-free optical film with adjustable dual-stage damping.
[0018] The present invention also provides a method for preparing the above-mentioned solvent-free optical film with adjustable dual-stage damping, the method comprising the following steps: (a) The acid-free acrylate main monomer, the high-temperature damping modified monomer, the interface wetting modified monomer and the branching regulator are homogenized and mixed to obtain a solvent-free mixed monomer system; (b) Add the bulk polymerization initiator to the solvent-free mixed monomer system to carry out a bulk prepolymerization reaction, and terminate the bulk prepolymerization reaction when the monomer double bond conversion rate reaches a preset conversion rate threshold to obtain the prepolymer component; (c) The UV crosslinking monomer and the photoinitiator are added to the prepolymer component and mixed to obtain the solvent-free optical adhesive with adjustable two-stage damping; (d) The solvent-free optical adhesive with adjustable damping in two stages is coated with oxygen-free material and subjected to first radiation curing during the coating process to obtain the solvent-free optical adhesive film with adjustable damping in two stages.
[0019] Furthermore, the homogeneous mixing is carried out under nitrogen protection; Preferably, the reaction temperature of the bulk prepolymerization reaction is 50~60℃ and the time is 25~35min; Preferably, the preset conversion rate threshold is 15%~25%; Preferably, the coating speed of the oxygen-free coating is greater than or equal to 15 m / min; Preferably, the coating thickness of the oxygen-free coating is 70~150μm; Preferably, the oxygen-free coating adopts a slot coating method, and an oxygen-free environment is constructed by double-sided coating with a release film during the coating process.
[0020] Preferably, the radiation energy of the first radiation curing is 500~1500 mJ / cm². 2 .
[0021] Furthermore, the present invention also provides the application of the above-mentioned solvent-free optical adhesive with adjustable dual-stage damping or solvent-free optical adhesive film with adjustable dual-stage damping, or solvent-free optical adhesive film with adjustable dual-stage damping prepared by the above-mentioned preparation method, in the bonding of display modules.
[0022] Furthermore, the solvent-free optical film with adjustable dual-stage damping is bonded between the cover plate and the polarizer of the display module, and the bonded solvent-free optical film is subjected to debubbling treatment under preset temperature and preset pressure conditions.
[0023] Furthermore, the degassing treatment is performed at a temperature of 55~65℃, a pressure of 0.4~0.6MPa, and a time of 15~30min; Preferably, the degassing treatment further includes: subjecting the dual-stage damping adjustable solvent-free optical film to a second radiation curing process. The second radiation curing process uses a UV-LED light source with a radiation wavelength of 365nm and a radiation energy of 2500mJ / cm² or higher, so that the loss factor of the cured film is less than or equal to 0.3 under the test conditions of 80℃ and 1Hz.
[0024] Compared with the prior art, the present invention has the following beneficial effects: This invention designs the raw materials as a two-stage system of prepolymer components and post-polymer components, and uses an acid-free acrylate main monomer in combination with a branching regulator, a high-temperature damping modified monomer, and an interface wetting modified monomer. Solvents and acidic carboxyl monomers are excluded throughout the process, ensuring that the prepolymer component is free of acidic monomers. This fundamentally avoids corrosion of the ITO electrode and the risk of screen yellowing, improving the chemical stability and optical durability of the film. Simultaneously, the branching regulator and the high-temperature damping modified monomer work synergistically in the prepolymer stage, enabling the construction of a low-branching, highly linear prepolymer structure even under solvent-free conditions, endowing the colloid with initial high creep and high-temperature flowability. Furthermore, the UV crosslinking monomer and photoinitiator are introduced as post-polymer components before coating, ensuring the inertness of double bond reactions during storage and coating, thereby maintaining high fluidity and process stability, and providing a structural basis for subsequent controllable two-stage UV curing.
[0025] The preparation method provided by this invention utilizes a phased process of prepolymerization and post-polymerization to enable the colloid to maintain flow characteristics suitable for coating processing in the early stage and achieve cross-linking stability in the later stage, thereby achieving phased controllability of damping performance. At the same time, the solvent-free system eliminates the solvent removal process, avoids oxygen inhibition during radiation curing in an oxygen-free environment, and avoids the risk of acid corrosion through the acid-free raw material system. Detailed Implementation
[0026] Unless otherwise defined herein, the scientific and technical terms used in conjunction with this invention shall have the meanings commonly understood by one of ordinary skill in the art. The meaning and scope of terms shall be clear; however, in any case of potential ambiguity, the definitions provided herein shall prevail over any dictionary or foreign definitions. In this application, unless otherwise stated, the use of "or" means "and / or". Furthermore, the use of the term "comprising" and other forms is non-limiting.
[0027] According to one aspect of the present invention, a solvent-free optical adhesive with adjustable damping in two stages is provided, wherein the raw materials of the solvent-free optical adhesive include a prepolymer component and a post-polymer component; The prepolymer components include an acid-free acrylate main monomer, a branching regulator, a high-temperature damping modified monomer, an interface wetting modified monomer, and a bulk polymerization initiator. The post-formulation components include UV crosslinking monomers and photoinitiators; The solvent-free optical adhesive contains no acidic carboxyl monomers and no solvents.
[0028] By designing the raw materials as a two-stage system of prepolymer components and post-polymer components, and using acid-free acrylate main monomers in combination with branching regulators, high-temperature damping modified monomers, and interface wetting modified monomers, while eliminating solvents and acidic carboxyl monomers throughout the process, the optical adhesive maintains high damping flow characteristics in the first processing stage by relying on the prepolymer system to fully wet and fill the micro-segment differences of blind holes. After the post-polymer UV crosslinking component participates in the secondary curing, it switches to a low-damping stable state to lock the colloidal form. Thus, while avoiding the risks of solvent residue and acid corrosion, it effectively solves the technical contradiction of the optical adhesive's filling flowability and curing stability.
[0029] In some preferred embodiments, the Ubbelohde viscosity IV value of the prepolymer component is 1.7 to 2.2.
[0030] This specific value directly ensures that the prepolymer has a suitable molecular weight and narrow distribution characteristics: an IV value < 1.7 indicates insufficient molecular weight or excessive branching, which easily leads to poor colloidal strength and uncontrolled high-temperature creep; an IV value > 2.2 indicates a large molecular weight or the presence of microgels, which will significantly increase coating viscosity, deteriorate leveling properties, and hinder blind hole filling; while precisely controlling the IV value within this range allows for simultaneous consideration of the prepolymer's solution processability, chain segment mobility, and structural regularity in a solvent-free system, thereby achieving mass-producible high-consistency film preparation without relying on solvent dilution.
[0031] In some preferred embodiments, the acid-free acrylate main monomer includes at least two of isooctyl acrylate (2EHA), isooctyl methacrylate (EHMA), butyl acrylate (BA), hydroxyethyl acrylate (HEA), and acrylamide (AM).
[0032] The amount of acrylamide added is strictly controlled between 2 and 8 parts by weight. 2EHA is the core flexible monomer, which lowers the glass transition temperature of the film and improves adhesion creep resistance; EHMA is a heat-resistant modifying monomer, which improves the rigidity of the colloidal backbone and its high-temperature anti-rebound performance; BA optimizes coating flowability and film uniformity; HEA improves the polarity of the system and interfacial adhesion; and acrylamide enhances the cohesion of the film and its resistance to humid heat aging.
[0033] In some preferred embodiments, the branching regulator includes Showa PE1 resin; preferably pentaerythritol tetra(3-mercaptobutyrate).
[0034] Showa PE1 resin has dual functions of chain transfer and branching regulation, which can precisely intervene in the free radical polymerization chain growth behavior, inhibit excessive branching of molecular chains, regulate the linear structure of polymers, and stabilize the IV viscosity value of prepolymers in the range of 1.7 to 2.2.
[0035] In some preferred embodiments, the high-temperature damping modifying monomer includes at least one of hexyl acrylate, lauryl acrylate, and tert-butyl acrylate; High-temperature damping modified monomers are used to improve the high-temperature damping stability and micro-segment wettability of adhesive films, enhance the flow and filling ability of adhesives under high-temperature bonding conditions, and avoid the problem of incomplete filling caused by rapid setting of adhesives.
[0036] In some preferred embodiments, the interface wetting modifier includes at least one of N-vinylpyrrolidone and N-vinylformamide; Interface wetting modifiers can improve the wettability, interfacial adhesion and film transmittance of the system. The dosage is strictly limited to 1.0 part. Excessive dosage will lead to film embrittlement and increased shrinkage, while insufficient dosage will result in insufficient adhesion.
[0037] In some preferred embodiments, the bulk polymerization initiator includes at least one selected from 1-hydroxycyclohexylphenyl ketone (184), 2-hydroxy-2-methyl-1-phenylpropanone (1173), and α,α-dimethoxy-α-phenylacetophenone (651). The bulk polymerization initiator is used to gently initiate solvent-free bulk polymerization, avoiding burst polymerization and gelation defects, and ensuring a stable and controllable polymerization process.
[0038] Preferably, the UV crosslinking monomer includes at least one selected from 1,9-nonanediol diacrylate (NDDA), 6-hexanediol diacrylate (HDDA), tripropylene glycol diacrylate (TPGDA), trimethylolpropane triacrylate (TMPTA), and pentaerythritol triacrylate (PETA). Preferably, the photoinitiator includes at least one of 1-hydroxycyclohexylphenyl ketone (184), 2-hydroxy-2-methyl-1-phenylpropanone (1173), and α,α-dimethoxy-α-phenylacetophenone (651).
[0039] In some preferred embodiments, the solvent-free optical adhesive further includes functional additives, such as leveling agents and antioxidants, to optimize the coating appearance and improve the film's resistance to aging and yellowing.
[0040] In some preferred embodiments, the solvent-free optical adhesive with adjustable two-stage damping comprises the following raw materials in parts by weight: The composition includes: 80-90 parts of acid-free acrylate main monomer (e.g., but not limited to 80, 82, 85, 88, or 90 parts), 0.5-2.0 parts of branching regulator (e.g., but not limited to 0.5, 0.8, 1, 1.2, 1.5, 1.8, or 2.0 parts), 5 parts of high-temperature damping modifier monomer, 0.2-1.0 parts of interface wetting modifier monomer (e.g., but not limited to 0.2, 0.5, 0.8, or 1.0 parts), and 0.1-0.5 parts of bulk polymerization initiator (e.g., but not limited to 80, 82, 85, 88, or 90 parts). The following components are included: (but not limited to) 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts or 0.5 parts, UV crosslinking monomer 0.1 to 0.5 parts (e.g., but not limited to 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts or 0.5 parts), photoinitiator 0.1 to 0.4 parts (e.g., but not limited to 0.1 parts, 0.2 parts, 0.3 parts or 0.4 parts), and functional additives 0.1 to 0.6 parts (e.g., but not limited to 0.1 parts, 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts or 0.6 parts).
[0041] According to a second aspect of the present invention, a solvent-free optical film with adjustable dual-stage damping is provided, which is prepared from the above-described solvent-free optical film with adjustable dual-stage damping.
[0042] According to a third aspect of the present invention, a method for preparing the above-described two-stage damping adjustable solvent-free optical film is provided, the method comprising the following steps: (a) The acid-free acrylate main monomer, the high-temperature damping modified monomer, the interface wetting modified monomer and the branching regulator are homogenized and mixed to obtain a solvent-free mixed monomer system; (b) Add the bulk polymerization initiator to the solvent-free mixed monomer system to carry out a bulk prepolymerization reaction, and terminate the bulk prepolymerization reaction when the monomer double bond conversion rate reaches a preset conversion rate threshold to obtain the prepolymer component; (c) The UV crosslinking monomer and the photoinitiator are added to the prepolymer component and mixed to obtain the solvent-free optical adhesive with adjustable two-stage damping; (d) The solvent-free optical adhesive with adjustable damping in two stages is coated with oxygen-free material and subjected to first radiation curing during the coating process to obtain the solvent-free optical adhesive film with adjustable damping in two stages.
[0043] In this process, steps (a) and (b) ensure that the branching regulator fully participates in the free radical chain growth process in the solvent-free system, effectively suppressing side reactions and forming a prepolymer with a narrow molecular weight distribution and high linearity. In step (c), the UV crosslinking monomer and photoinitiator are added after the prepolymerization is completed to avoid their premature participation in polymerization, which would lead to the premature introduction of crosslinking points and lock the chain segment mobility. In step (d), coating and first radiation curing are completed simultaneously in an oxygen-free environment, which not only eliminates the inhibitory effect of oxygen on free radical polymerization to ensure that the degree of semi-curing crosslinking is controllable, but also enables the film to obtain an adjustable damping state at the moment of film formation. Thus, without introducing solvents or isocyanates, the synergy of prepolymer structural stability, coating process feasibility and initial damping functionality is directly achieved.
[0044] In some preferred embodiments, the homogenization is carried out under nitrogen protection.
[0045] Mixing is completed in a nitrogen atmosphere, ensuring that the monomer system is in a low-oxygen state before the bulk polymerization initiator is added. This ensures the controllability and repeatability of the subsequent prepolymerization reaction initiation and avoids polymerization rate fluctuations or micro-gel point formation caused by local oxygen residue.
[0046] In some preferred embodiments, the reaction temperature of the bulk prepolymerization reaction is 50~60°C, for example, but not limited to 50°C, 52°C, 55°C, 58°C or 60°C, and the reaction time is 25~35 min, for example, but not limited to 25 min, 28 min, 30 min, 32 min or 35 min.
[0047] In some preferred embodiments, the preset conversion rate threshold is 15% to 25%, for example, but not limited to 15%, 18%, 20%, 22% or 25%.
[0048] When the conversion rate is below 15%, the degree of polymerization is insufficient, the molecular weight of the prepolymer is too low, and it is difficult to form effective chain entanglement and the colloidal damping properties required for subsequent processing. When the conversion rate is above 25%, the free radical lifetime is prolonged, the probability of chain transfer and coupling termination increases, and branching is easily induced, local crosslinking or microgel formation is induced, resulting in a sudden increase in viscosity and rheological instability. However, by strictly controlling the conversion rate within this range, it is possible to ensure that the prepolymer has a moderate degree of polymerization, low degree of branching and high chain end activity under solvent-free conditions, thereby simultaneously meeting the basic requirements of coating flowability, storage stability and subsequent semi-curing responsiveness without introducing crosslinking monomers.
[0049] In some preferred embodiments, the coating speed of the oxygen-free coating is greater than or equal to 15 m / min.
[0050] Traditional coating speeds are limited by solvent evaporation rates or the shear stability of high-viscosity systems. However, this embodiment achieves such high-speed coating under anaerobic conditions, indicating that the adhesive composed of the prepolymer component and the post-polymer component has excellent low shear viscosity, high ductility, and anti-firing properties.
[0051] In some preferred embodiments, the coating thickness of the oxygen-free coating is 70~150μm, for example, but not limited to 70μm, 80μm, 100μm, 120μm or 150μm.
[0052] In some preferred embodiments, the oxygen-free coating is performed using a slot coating method, and an oxygen-free environment is constructed by double-sided coating with a release film during the coating process.
[0053] The slit die provides high-precision thickness control and a stable shear field, ensuring repeatable rheological behavior of the adhesive during the extrusion-film formation transient process. The double-sided release film coating not only physically isolates the diffusion of ambient oxygen to the upper and lower surfaces of the adhesive, but also maintains a millisecond-level response sealed atmosphere under dynamic conditions with a coating line speed ≥15 m / min. This ensures that the free radical active centers are not quenched during the first radiation curing, allowing the semi-cured crosslinking degree to be uniformly established along the film thickness direction. This avoids stress gradients and interface defects caused by low surface conversion and high inner crosslinking due to surface oxidation, ultimately supporting the continuous preparation of high-smoothness and high-consistency adhesive films.
[0054] In some preferred embodiments, the radiation energy of the first radiation curing is 500~1500 mJ / cm². 2 For example, it can be, but is not limited to, 500 mJ / cm 2 800 mJ / cm2 1000 mJ / cm 2 1200 mJ / cm 2 Or 1500 mJ / cm 2 .
[0055] Energy below 500 mJ / cm 2 At times, insufficient photoinitiation efficiency and excessively high residual double bond density result in low initial film strength and poor dimensional stability, making it unable to support deformation constraints in subsequent degassing processes; energy levels exceeding 1500 mJ / cm 2 When the free radical concentration is too high and the reaction is too violent, it is easy to cause local over-crosslinking or chain breakage, destroying the original linear structural advantages of the prepolymer and weakening the chain segment mobility and damping characteristics at high temperatures. However, within this energy range, the photoinitiator can be fully activated under anaerobic conditions, selectively triggering partial double bond crosslinking to form a primary network of appropriate density. This provides the film with the necessary mechanical support to maintain the coating morphology and transfer accuracy, while retaining a sufficient number of residual double bonds and chain end activity, reserving sufficient reaction space for the final curing in the second stage.
[0056] According to a fourth aspect of the present invention, the application of the above-described two-stage damping adjustable solvent-free optical adhesive, or the two-stage damping adjustable solvent-free optical adhesive film, or the two-stage damping adjustable solvent-free optical adhesive prepared by the above-described preparation method, in display module bonding is provided.
[0057] In some preferred embodiments, the solvent-free optical film with adjustable dual-stage damping is bonded between the cover plate and the polarizer of the display module, and the bonded solvent-free optical film is subjected to debubbling treatment under preset temperature and preset pressure conditions.
[0058] This embodiment utilizes the specific rheological state of the adhesive film after the first radiation curing, enabling it to spontaneously fill micron-level gaps and expel trapped air under interfacial stress. This process does not rely on the internal mass transfer driving force generated by solvent evaporation, but purely on the synergistic effect of the intrinsic high-temperature damping properties (high tanδ) of the adhesive film and the applied mechanical energy (pressure), thereby achieving the physical elimination of interfacial defects without VOC release or thermal degradation risk, ensuring the integrity and reliability of optical bonding.
[0059] In some preferred embodiments, the degassing treatment temperature is 55~65°C, for example, but not limited to 55°C, 58°C, 60°C, 62°C or 65°C; the pressure is 0.4~0.6 MPa, for example, but not limited to 0.4 MPa, 0.5 MPa or 0.6 MPa; and the time is 15~30 min, for example, but not limited to 15 min, 18 min, 20 min, 22 min, 25 min, 28 min or 30 min.
[0060] In some preferred embodiments, the degassing treatment further includes: subjecting the two-stage damping adjustable solvent-free optical film to a second radiation curing process. The second radiation curing process uses a UV-LED light source with a radiation wavelength of 365nm and a radiation energy of 2500 mJ / cm² or higher, so that the loss factor of the cured film is less than or equal to 0.3 under the test conditions of 80°C and 1Hz.
[0061] The residual double bonds retained by the first radiation curing are fully activated in the second stage and form a dense three-dimensional cross-linked network, which systematically suppresses the mobility of molecular chain segments. The loss factor, as a key parameter characterizing the proportion of energy dissipation in viscoelasticity, drops to 0.3 or below, indicating that the film has irreversibly transformed from the high-damping flow dynamics (tanδ≥0.8) required in the degassing stage to a stable state dominated by elastic response and significantly enhanced resistance to creep and deformation rebound. This effectively suppresses colloidal shrinkage, interfacial debonding, and bubble rebound in blind pore regions in high-temperature service environments, achieving the final shaping of the structure and function.
[0062] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise specified, the materials in the embodiments are prepared according to existing methods or purchased directly from the market.
[0063]
[0064] The above embodiments and comparative examples also contain 0.1 parts of bulk polymerization initiator 1-hydroxycyclohexylphenyl ketone (184), 0.05 parts of leveling agent MYSD UV 3720, and 0.05 parts of antioxidant BHT.
[0065] The solvent-free optical films with adjustable dual-stage damping provided in Examples 1-14, 17 and 18 and Comparative Examples 1-6 were prepared by the following method: S1. Homogenization: The formula amount of main monomer, hexyl acrylate, NVP, and Showa PE1 resin are put into a light-proof and sealed reactor. Nitrogen is used to replace oxygen and the mixture is stirred and homogenized to obtain a solvent-free mixed monomer system.
[0066] S2. Temperature- and conversion-controlled bulk prepolymerization: A bulk polymerization initiator is added to the solvent-free mixed monomer system, and polymerization is initiated by light initiation at room temperature of 23±2℃. Utilizing the system's self-heating effect, the system temperature is kept constant at 55℃ by a temperature control system, and the constant temperature dark reaction is maintained for 30 min. The conversion rate of monomer double bonds is monitored in real time using the weight loss method. The polymerization is terminated immediately when the conversion rate reaches 20%, resulting in a low-branched, highly linear prepolymer.
[0067] Note: Example 4 has the same formulation as Example 1, except that the monomer double bond conversion rate is 24.9% when the bulk prepolymerization reaction is terminated; Example 5 has the same formulation as Example 1, except that the bulk prepolymerization reaction temperature is 60°C.
[0068] S3. Adding functional components: After the prepolymer is naturally cooled to room temperature, add UV crosslinking monomers and suitable UV photoinitiators (HDDA 184, TMPTA 184, NDDA 1173, all in a 1:1 ratio), stir at low speed (200 RPM) in the dark until homogeneous, and prepare a solvent-free optical adhesive with adjustable damping in two stages.
[0069] S4. Oxygen-free UV semi-curing coating: The slot die coating process is adopted to precisely control the dry film thickness to 100μm; the coating process uses a release film to fully cover both sides, creating a closed oxygen-free environment to prevent oxygen from inhibiting polymerization; the UV coating curing energy is controlled at 1000mj / cm², and the first curing is completed by low-energy UV to obtain a solvent-free optical film with adjustable damping in two stages.
[0070] The solvent-free optical film with adjustable dual-stage damping provided in Example 15 above was prepared by the following method: S1. Homogenization: The formula amount of main monomer, hexyl acrylate, NVP, and Showa PE1 resin are put into a light-proof and sealed reactor. Nitrogen is used to replace oxygen and the mixture is stirred and homogenized to obtain a solvent-free mixed monomer system.
[0071] S2. Temperature- and conversion-controlled bulk prepolymerization: A bulk polymerization initiator is added to the solvent-free mixed monomer system, and polymerization is initiated by light initiation at room temperature of 23±2℃. Utilizing the system's self-heating effect, the system temperature is kept constant at 50℃ by a temperature control system, and the reaction is carried out in the dark for 30 minutes. The conversion rate of monomer double bonds is monitored in real time using the weight loss method. When the conversion rate reaches 25% (the specific conversion rates for each example are shown in the table below), the polymerization is immediately terminated to obtain a low-branched, highly linear prepolymer.
[0072] S3. Post-concentration functional components: After the prepolymer is naturally cooled to room temperature, UV crosslinking monomers and suitable UV photoinitiators are added and stirred at low speed (200 RPM) in the dark to prepare a solvent-free optical adhesive with adjustable damping in two stages.
[0073] S4. Oxygen-free UV semi-curing coating: The slot die coating process is adopted to precisely control the dry film thickness to 100μm; the coating process uses a release film to fully cover both sides, creating a closed oxygen-free environment to prevent oxygen from inhibiting polymerization; the UV coating curing energy is controlled at 500mj / cm², and the first curing is completed by low-energy UV to obtain a solvent-free optical film with adjustable damping in two stages.
[0074] The solvent-free optical film with adjustable dual-stage damping provided in Example 16 above was prepared by the following method: S1. Homogenization: The formula amount of main monomer, hexyl acrylate, NVP, and Showa PE1 resin are put into a light-proof and sealed reactor. Nitrogen is used to replace oxygen and the mixture is stirred and homogenized to obtain a solvent-free mixed monomer system.
[0075] S2. Temperature- and conversion-controlled bulk prepolymerization: A bulk polymerization initiator is added to the solvent-free mixed monomer system, and polymerization is initiated by micro-light initiation at room temperature of 23±2℃. Utilizing the system's self-heating effect, the system temperature is kept constant within the 60℃ range by a temperature control system, and the constant temperature dark reaction is maintained for 30 min. The conversion rate of monomer double bonds is monitored in real time using the weight loss method. The polymerization is terminated immediately when the conversion rate reaches 15%, resulting in a low-branched, highly linear prepolymer.
[0076] S3. Post-concentration functional components: After the prepolymer is naturally cooled to room temperature, UV crosslinking monomers and suitable UV photoinitiators are added and stirred at low speed (200 RPM) in the dark to prepare a solvent-free optical adhesive with adjustable damping in two stages.
[0077] S4. Oxygen-free UV semi-curing coating: The slot die coating process is adopted to precisely control the dry film thickness to 100μm; the coating process uses a release film to fully cover both sides, creating a closed oxygen-free environment to prevent oxygen from inhibiting polymerization; the UV coating curing energy is controlled at 1500mj / cm², and the first curing is completed by low-energy UV to obtain a solvent-free optical film with adjustable damping in two stages.
[0078] The solvent-free optical film with adjustable two-stage damping provided in Comparative Example 7 was prepared by the following method: S1. Homogenization: The formula amount of main monomer, hexyl acrylate, NVP, and Showa PE1 resin are put into a light-proof and sealed reactor. Nitrogen is used to replace oxygen and the mixture is stirred and homogenized to obtain a solvent-free mixed monomer system.
[0079] S2. Temperature- and conversion-controlled bulk prepolymerization: A bulk polymerization initiator is added to the solvent-free mixed monomer system, and polymerization is initiated by micro-light initiation at room temperature of 23±2℃. Utilizing the system's self-heating effect, the system temperature is kept constant at 70℃ by a temperature control system, and the constant-temperature dark reaction is maintained for 30 min. The conversion rate of monomer double bonds is monitored in real time using the weight loss method. When the conversion rate reaches 30%, the polymerization is immediately terminated to obtain a low-branched, highly linear prepolymer.
[0080] S3. Post-concentration functional components: After the prepolymer is naturally cooled to room temperature, UV crosslinking monomers and suitable UV photoinitiators are added and stirred at low speed (200 RPM) in the dark to prepare a solvent-free optical adhesive with adjustable damping in two stages.
[0081] S4. Oxygen-free UV semi-curing coating: The slot die coating process is adopted to precisely control the dry film thickness to 100μm; the coating process uses a release film to fully cover both sides, creating a closed oxygen-free environment to prevent oxygen from inhibiting polymerization; the UV coating curing energy is controlled at 400mj / cm², and the first curing is completed by low-energy UV to obtain a solvent-free optical film with adjustable damping in two stages.
[0082] Test case To verify the product performance, the solvent-free optical films with adjustable dual-stage damping prepared in Examples 1-18 and Comparative Examples 1-7 were used respectively by the following methods: s1. Debubbling of blind hole bonding: The solvent-free optical adhesive with adjustable dual-stage damping is bonded between the Glass cover plate of the blind hole display module and the perforated polarizer. Debubbling is performed for 15~30 minutes at 60℃ and 0.5MPa. The adhesive fully wets the blind hole step, achieving a blind hole filling rate of >70%, with no bubbles and no dead corners.
[0083] s2. Second radiation curing: After bonding, the adhesive film is deeply cross-linked and cured using a UV-LED light source with a radiation wavelength of 365nm and a radiation energy of more than 2500 mJ / cm², so that the loss factor of the cured adhesive film is ≤0.3 under the test conditions of 80℃ and 1Hz.
[0084] The used products were then tested according to the following standards: (1) Ubbelohde viscosity IV value: 0.6mm Ubbelohde viscometer, constant temperature test at 25℃, unit is dL / g; (2) Monomer conversion rate: determined by weight loss method; (3) Coating viscosity: Brookfield rotational viscometer, 25°C, 20 rpm; (4) Peeling force (adhesion): According to GB / T 2792-2014, the glass cover was tested at 180° peel and 300mm / min. The actual adhesion of the finished product of this invention can reach >20N / 25mm. (5) Loss factor: Tested with a TA rheometer HR10 at 1Hz and 80℃; (6) Blind hole filling rate: 100μm OCA bonded to 70μm blind hole polarizer module, debubbling at 60℃ and 0.5MPa for 15~30min, the filling rate is judged to be >70% if there are no bubbles, and ≤70% if there are defects; (7) Reliability: 1000h damp heat and 500 cycles of hot and cold cycling test; (8) UV curing energy: The energy of the first radiation curing UV coating is controlled at 500~1500mj / cm²; (9) Coating speed: The coating speed of traditional solvent-based 100μm thick OCA is usually <5m / min. The solvent-free formulation system of this invention can stably achieve high-speed coating mass production of more than 15m / min.
[0085] The test results are as follows:
[0086] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A solvent-free optical adhesive with adjustable dual-stage damping, characterized in that, The raw materials of the solvent-free optical adhesive include prepolymer components and post-polymer components; The prepolymer components include an acid-free acrylate main monomer, a branching regulator, a high-temperature damping modified monomer, an interface wetting modified monomer, and a bulk polymerization initiator. The post-formulation components include UV crosslinking monomers and photoinitiators; The solvent-free optical adhesive contains no acidic carboxyl monomers and no solvents.
2. The solvent-free optical adhesive with adjustable dual-stage damping according to claim 1, characterized in that, The Ubbelohde viscosity IV value of the prepolymer component is 1.7~2.
2.
3. The solvent-free optical adhesive with adjustable dual-stage damping according to claim 1, characterized in that, The acid-free acrylate main monomer includes at least two of isooctyl acrylate, isooctyl methacrylate, butyl acrylate, hydroxyethyl acrylate, and acrylamide; Preferably, the branching regulator includes Showa PE1 resin, and more preferably pentaerythritol tetra(3-mercaptobutyrate); Preferably, the high-temperature damping modifying monomer includes at least one of hexyl acrylate, lauryl acrylate, and tert-butyl acrylate; Preferably, the interface wetting modifying monomer includes at least one of N-vinylpyrrolidone and N-vinylformamide; Preferably, the bulk polymerization initiator includes at least one selected from 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, and α,α-dimethoxy-α-phenylacetophenone; Preferably, the UV crosslinking monomer includes at least one of 1,9-nonanediol diacrylate, 6-hexanediol diacrylate, tripropylene glycol diacrylate, trimethylolpropane triacrylate, and pentaerythritol triacrylate. Preferably, the photoinitiator comprises at least one selected from 1-hydroxycyclohexylphenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, and α,α-dimethoxy-α-phenylacetophenone; Preferably, the solvent-free optical adhesive further includes functional additives; Preferably, the functional additives include leveling agents and antioxidants.
4. The solvent-free optical adhesive with adjustable dual-stage damping according to any one of claims 1 to 3, characterized in that, The ingredients include the following parts by weight: The composition includes 80-90 parts of acid-free acrylate main monomer, 0.5-2.0 parts of branching regulator, 5 parts of high-temperature damping modified monomer, 0.2-1.0 parts of interface wetting modified monomer, 0.1-0.5 parts of bulk polymerization initiator, 0.1-0.5 parts of UV crosslinking monomer, 0.1-0.4 parts of photoinitiator, and 0.1-0.6 parts of functional additives.
5. A solvent-free optical film with adjustable dual-stage damping, characterized in that, It is prepared from the solvent-free optical adhesive with adjustable dual-stage damping as described in any one of claims 1-4.
6. The method for preparing the solvent-free optical film with adjustable dual-stage damping as described in claim 5, characterized in that, The preparation method includes the following steps: (a) The acid-free acrylate main monomer, the high-temperature damping modified monomer, the interface wetting modified monomer and the branching regulator are homogenized and mixed to obtain a solvent-free mixed monomer system; (b) Add the bulk polymerization initiator to the solvent-free mixed monomer system to carry out a bulk prepolymerization reaction, and terminate the bulk prepolymerization reaction when the monomer double bond conversion rate reaches a preset conversion rate threshold to obtain the prepolymer component; (c) The UV crosslinking monomer and the photoinitiator are added to the prepolymer component and mixed to obtain the solvent-free optical adhesive with adjustable two-stage damping; (d) The solvent-free optical adhesive with adjustable damping in two stages is coated with oxygen-free material and subjected to first radiation curing during the coating process to obtain the solvent-free optical adhesive film with adjustable damping in two stages.
7. The preparation method according to claim 6, characterized in that, The homogeneous mixing was carried out under nitrogen protection; Preferably, the reaction temperature of the bulk prepolymerization reaction is 50~60℃ and the time is 25~35min; Preferably, the preset conversion rate threshold is 15%~25%; Preferably, the coating speed of the oxygen-free coating is greater than or equal to 15 m / min; Preferably, the coating thickness of the oxygen-free coating is 70~150μm; Preferably, the oxygen-free coating adopts a slot coating method, and an oxygen-free environment is constructed by double-sided coating with a release film during the coating process; Preferably, the radiation energy of the first radiation curing is 500~1500 mJ / cm². 2 .
8. The application of a solvent-free optical adhesive with adjustable dual-stage damping as described in any one of claims 1 to 4, or a solvent-free optical adhesive film with adjustable dual-stage damping as described in claim 5, or a solvent-free optical adhesive film with adjustable dual-stage damping prepared by the preparation method described in claim 6 or 7, in the bonding of display modules.
9. The application according to claim 8, characterized in that, The solvent-free optical film with adjustable dual-stage damping is bonded between the cover plate and the polarizer of the display module, and the bonded solvent-free optical film is subjected to debubbling treatment under preset temperature and preset pressure conditions.
10. The application according to claim 9, characterized in that, The degassing treatment is performed at a temperature of 55~65℃, a pressure of 0.4~0.6MPa, and a time of 15~30min. Preferably, the degassing treatment further includes: subjecting the dual-stage damping adjustable solvent-free optical film to a second radiation curing process. The second radiation curing process uses a UV-LED light source with a radiation wavelength of 365nm and a radiation energy of 2500 mJ / cm² or higher, so that the loss factor of the cured film is less than or equal to 0.3 under the test conditions of 80℃ and 1Hz.