A dual-mode electroresponsive nanocomposite ionic pressure-sensitive adhesive, its preparation method and application
By introducing silanized modified metal oxide nanoparticles into pressure-sensitive adhesives, the viscoelasticity and ion transport properties of the adhesive layer are regulated, solving the problem of the difficulty in simultaneously achieving adhesion and ion transport in electro-tack reducing pressure-sensitive adhesives. This enables rapid electro-tack reduction and strain sensing functions, making it suitable for flexible electronics and wearable devices.
Patent Information
- Application Number
- CN202611526803.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing electro-tack pressure-sensitive adhesives suffer from problems such as high stimulation voltage or long stimulation time, making it difficult to balance adhesion and ion transport performance, and they also lack strain sensing functionality.
By introducing silanized metal oxide nanoparticles into an ion-modified pressure-sensitive adhesive system, and adjusting the type, grafting density, and addition amount of nanoparticles and silane coupling agents, the viscoelasticity and ion transport properties of the adhesive layer can be controlled, thereby achieving rapid electro-tack reduction and strain sensing functions.
It achieves strain sensing response at low test voltage and rapid electro-adhesion reduction at high stimulation voltage, while possessing both good adhesion and ion transport properties, making it suitable for flexible electronic devices and wearable devices.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of pressure-sensitive adhesive materials technology, specifically relating to a dual-mode electroresponsive nanocomposite ionic pressure-sensitive adhesive, its preparation method, and its application. Background Technology
[0002] Pressure-sensitive adhesives (PSAs) are crucial basic materials in electronics, medical, automotive, construction, and packaging industries, and their performance directly affects the performance and reliability of end products. However, traditional PSAs rely on mechanical force for peeling, which can easily lead to adhesive residue and substrate deformation or damage. With the increasing emphasis on rapid and sustainable development in fields such as flexible electronic devices, removable batteries, and wafer fabrication, the difficulty of achieving rapid and controllable peeling with traditional PSAs is becoming increasingly prominent. Therefore, there is an urgent need to develop PSAs that combine stable adhesion with rapid detack reduction properties.
[0003] Introducing ionic liquids and / or conductive salts as ionic conductive components into electro-adhesive systems allows ions to migrate to the electrode interface and undergo electrochemical reactions under an applied electric field, thereby weakening the interfacial adhesion between the adhesive layer and the substrate. Compared to thermally responsive or photoresponsive anti-adhesive systems, electro-adhesive systems offer advantages such as easy implementation and control of electrical stimulation, fast response speed, no limitation on the size and transparency of the adhered device, and reduced likelihood of false triggering.
[0004] In the prior art, patent CN116574453B discloses a method for preparing an electrically removable, on-demand pressure-sensitive adhesive coating, which uses a polymerizable ionic liquid copolymerized with various acrylate monomers to obtain an electrically detack-reducing pressure-sensitive adhesive. In Example 1 of this patent, the peel strength is 0.78 N / mm, and after stimulation with a 150 V voltage for 10 min, the peel strength decreases by approximately 71.8%. Patent CN118389082A discloses a reusable, high-shear-strength electrically detack-reducing tape and its preparation method. This electrically detack-reducing tape is prepared from acrylate or olefin monomers, esters containing methoxy polyethylene glycol, acrylics, salts, and functional monomers, etc. After stimulation with a 30 V voltage for 30 s, the peel strength decreases from 2518 g / 25 mm to 26 g / 25 mm. While the above technologies can achieve electrically detack reduction through an external electric field, they still suffer from problems such as high stimulation voltage or long stimulation time.
[0005] The stimulation voltage and response time required for electro-tack reduction are related to the ion transport properties of the pressure-sensitive adhesive (PSA), while the adhesive properties are mainly affected by the viscoelasticity of the PSA. Both ion transport properties and viscoelasticity are closely related to chain segment mobility. Increasing the amount of ionic liquid usually benefits ion migration, but its plasticizing effect reduces the modulus and cohesive force of the adhesive layer, thus affecting the peel strength. Increasing the amount of polar monomer or improving the degree of crosslinking can improve the cohesive force of the adhesive layer, but it restricts chain segment mobility, which is not conducive to ion transport. Therefore, it is usually difficult to achieve both adhesive properties and ion transport properties in electro-tack reduction PSAs.
[0006] Adding nanofillers is a common method for adjusting the adhesive properties of pressure-sensitive adhesives (PSAs). However, the influence of nanoparticles on the properties of PSAs is closely related to factors such as their type, surface properties, and dosage. For systems containing ionic conductive components, nanoparticles also affect the chain mobility of polymers and the dissociation and migration of ionic liquids, thus influencing ion transport and electro-thickness reduction properties. Therefore, how to achieve good ion transport properties and rapid electro-thickness reduction response while maintaining good adhesive properties through the rational design and surface modification of nanoparticles remains a problem that needs to be solved in nanocomposite ionic PSAs.
[0007] Furthermore, flexible electronics and wearable devices not only require stable adhesion during use but also necessitate monitoring device deformation or human motion. Existing ionic strain sensing materials and electro-adhesive pressure-sensitive adhesives are typically designed separately for strain sensing and electro-adhesive reduction functions. Technical solutions for achieving dual-mode electrical response of the same ionic pressure-sensitive adhesive under different voltage conditions are still relatively rare. Therefore, how to integrate strain sensing and electro-adhesive reduction functions into the same adhesive material to meet the different functional requirements of stable adhesion, condition monitoring, and rapid de-adhesion remains to be solved. Summary of the Invention
[0008] The purpose of this invention is to provide a dual-mode electroresponsive nanocomposite ionic pressure-sensitive adhesive, its preparation method, and its applications, to improve the problem of the difficulty in simultaneously achieving both adhesive performance and ion transport performance in existing electro-tack reducing pressure-sensitive adhesives, and to further meet the functional requirements of strain monitoring. This invention introduces silanized modified metal oxide nanoparticles into the ionic pressure-sensitive adhesive system. By adjusting the types of nanoparticles and silane coupling agents, the grafting density of the silanized nanoparticles, and the amount added, the viscoelasticity and ion transport performance of the adhesive layer are controlled, thereby enabling the pressure-sensitive adhesive to maintain good adhesive performance while also possessing rapid electro-tack reducing and strain sensing functions.
[0009] To achieve the above objectives, the present invention adopts the following technical solution.
[0010] This invention first provides a method for preparing a dual-mode electroresponsive nanocomposite ionic pressure-sensitive adhesive, which includes the following steps:
[0011] S1. Silanization modification of nanoparticles: Metal oxide nanoparticles with Lewis acid sites are mixed with water and ethanol and dispersed by ultrasonication to obtain a dispersion. A silane coupling agent that can be polymerized by free radicals is dissolved in ethanol and added dropwise to the above dispersion for silanization modification. After the reaction is completed, the nanoparticles are obtained by centrifugation, washing and drying.
[0012] S2. Preparation of prepolymer solution: By weight, 50-90 parts of soft monomer, 10-50 parts of polar monomer, 0.05-0.5 parts of photoinitiator, 0.05-0.3 parts of crosslinking agent, 1-10 parts of ionic liquid and 100-200 parts of organic solvent are mixed to obtain a mixture; prepolymerization is initiated by ultraviolet light under inert gas protection, and then organic solvent is added to adjust the solid content to obtain the prepolymer solution;
[0013] S3. Preparation of nanocomposite ionic pressure-sensitive adhesive: The prepolymer adhesive solution, the silanized nanoparticles and the thermal initiator are mixed evenly. The resulting nanocomposite ionic pressure-sensitive adhesive solution is coated on the surface of the release film. After removing the solvent, thermally initiated free radical polymerization is carried out. During the free radical polymerization of the free radical polymerizable organosilane component, it participates in the formation of acrylate copolymer to obtain the nanocomposite ionic pressure-sensitive adhesive.
[0014] According to a preferred embodiment of the present invention, by weight, in step S1, the metal oxide nanoparticles are 5-15 parts, the dispersion contains 200-400 parts water, 400-600 parts ethanol, 0.1-5 parts silane coupling agent, and 1-50 parts ethanol for dissolving the silane coupling agent.
[0015] More preferably, step S1 can be carried out according to the following process: by weight, 10 parts of metal oxide nanoparticles are mixed with 300 parts of water and 500 parts of ethanol, and after ultrasonic dispersion, 0.1 to 5 parts of silane coupling agent are dissolved in 1 to 50 parts of ethanol and added dropwise to the above dispersion for silanization modification. After the reaction is completed, the mixture is centrifuged, washed and dried to obtain silanized nanoparticles.
[0016] Further, in step S3, the amount of silanized nanoparticles is 0.01 to 5 parts by weight per 100 parts by weight of the prepolymer adhesive, and the amount of thermal initiator is 0.05 to 0.5 parts by weight.
[0017] Furthermore, the nanoparticles are one or more of the following metal oxide nanoparticles with Lewis acidic sites: zinc oxide, titanium dioxide, zirconium oxide, aluminum oxide, cerium oxide, etc., with a particle size of 10 to 100 nm.
[0018] Furthermore, the silane coupling agent is a free radical polymerizable silane coupling agent, selected from one or more of 3-(methacryloyloxy)propyltrimethoxysilane, 3-(methacryloyloxy)propyltriethoxysilane, 3-acryloyloxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, etc.
[0019] Furthermore, the soft monomer is one or more of the alkyl acrylate monomers such as isooctyl acrylate, butyl acrylate, ethyl acrylate, lauryl acrylate, and n-hexyl acrylate.
[0020] Furthermore, the polar monomer is a free radical polymerizable monomer containing carboxyl, hydroxyl, amide ether bonds or nitrogen-containing heterocyclic structures, selected from one or more of acrylic acid, hydroxyethyl acrylate, 2-carboxyethyl acrylate, N,N-dimethylacrylamide, 2-methoxyethyl acrylate, N-vinylpyrrolidone, etc.
[0021] Furthermore, the ionic liquid is one or more of the imidazolium-based ionic liquids.
[0022] Furthermore, the crosslinking agent is one or more of multifunctional acrylate crosslinking agents;
[0023] Further, the photoinitiator is one or more of 2-hydroxy-2-methylphenylacetone, 1-hydroxycyclohexylphenyl ketone, 2,2-dimethoxy-2-phenylacetophenone, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide;
[0024] Further, the organic solvent is one or more selected from ethyl acetate, butyl acetate, isopropyl acetate, methyl ethyl ketone, acetone, and propylene glycol methyl ether acetate;
[0025] Furthermore, the thermal initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, and benzoyl peroxide.
[0026] Furthermore, the solid content of the prepolymer solution in S2 is 8~12wt%, more preferably 10wt%.
[0027] The present invention also provides a nanocomposite ionic pressure-sensitive adhesive, comprising an acrylate copolymer, an ionic liquid, and silanized nanoparticles dispersed in the acrylate copolymer; wherein the silanized nanoparticles are metal oxide nanoparticles having Lewis acid sites, and their surfaces are grafted with organosilane components that can be polymerized by free radicals, wherein the organosilane components participate in the formation of the acrylate copolymer during the free radical polymerization process.
[0028] The nanocomposite ionic pressure-sensitive adhesive described in this invention can generate a strain sensing response through the resistance change caused by deformation at a low test voltage (0.1~3 V), and weaken the interfacial adhesion between the adhesive layer and the substrate through electrical stimulation at a higher stimulation voltage (8~36 V), thereby achieving a rapid electro-tack reduction response.
[0029] Further, in a preferred embodiment, the test voltage is 0.5 V and the stimulation voltage is 8 V.
[0030] The present invention also provides the application of the nanocomposite ionic pressure-sensitive adhesive in the fields of flexible electronic devices, wearable devices, soft robots, removable batteries or wafer processing, the application including one or more of bonding, strain monitoring and electro-adhesion reduction.
[0031] By adopting the above technical solution, the present invention has the following beneficial effects:
[0032] First, this invention modifies metal oxide nanoparticles with Lewis acidic sites by silanizing them with a free-radical polymerizable silane coupling agent. This allows the silane coupling agent to be grafted onto the nanoparticle surface and participate in the formation of the acrylate copolymer during subsequent free-radical polymerization. By adjusting the type of nanoparticles, the type of silane coupling agent, the grafting density of the silanized nanoparticles, and the amount added, the viscoelasticity of the copolymer can be adjusted, thereby affecting the adhesive properties of the pressure-sensitive adhesive.
[0033] Secondly, this invention introduces ionic liquids into the pressure-sensitive adhesive system, enabling the adhesive layer to possess ion transport capabilities and achieve electro-tack reduction under an applied electric field. By selecting the type of metal oxide nanoparticles, the type of silane coupling agent, and the grafting density and amount of silanized nanoparticles, the ion transport performance of the adhesive layer can be improved, thereby enhancing the electro-tack reduction performance of the pressure-sensitive adhesive.
[0034] Third, the nanocomposite ionic pressure-sensitive adhesive described in this invention can generate a strain sensing response through the change in resistance caused by deformation at a low test voltage (e.g., 0.5V); at a higher stimulation voltage (e.g., 8V), the interfacial adhesion between the adhesive layer and the substrate is weakened, achieving rapid electro-tack reduction. Thus, the same pressure-sensitive adhesive can have the functions of adhesion, strain sensing, and electro-tack reduction.
[0035] Fourth, the present invention employs processes such as silanization, free radical polymerization, nanoparticle dispersion, and coating film formation. The preparation process is relatively simple, the raw materials are readily available, and it is suitable for conventional pressure-sensitive adhesive processing processes such as coating, drying, and lamination. It has good prospects for large-scale preparation and industrial application. Detailed Implementation
[0036] The present invention will be further described and illustrated below with reference to specific embodiments. The embodiments described are merely examples of the content of this disclosure and do not limit the scope of the invention. The technical features of each embodiment in the present invention can be combined accordingly, provided that there is no mutual conflict.
[0037] The present invention will be further described below with reference to specific embodiments. It should be understood that the following embodiments are for illustrative purposes only and do not constitute a limitation on the content and scope of protection of the present invention.
[0038] Example 1
[0039] This embodiment provides a method for preparing silanized zinc oxide nanoparticles and their nanocomposite ionic pressure-sensitive adhesive, including the following steps:
[0040] S1. Preparation of silanized nanoparticles: 10 parts by weight of zinc oxide nanoparticles with a particle size of 50 nm were vacuum dried at 80 °C to constant weight. Then, they were added to a mixture of 500 parts ethanol and 300 parts deionized water and ultrasonically dispersed for 30 min. 0.5 parts of 3-(methacryloyloxy)propyltrimethoxysilane were dissolved in 5 parts ethanol and slowly added dropwise to the above dispersion at 60 °C, with stirring for 4 h. After the reaction was completed, the nanoparticles were centrifuged, washed several times with ethanol, and then vacuum dried at 80 °C to constant weight to obtain silanized zinc oxide nanoparticles.
[0041] S2. Preparation of the prepolymer solution: By weight, 80 parts of isooctyl acrylate, 20 parts of N-vinylpyrrolidone, 0.5 parts of 2-hydroxy-2-methylphenylacetone, 0.1 parts of 1,6-hexanediol diacrylate, 5 parts of the ionic liquid 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide, and 150 parts of ethyl acetate were stirred and mixed to obtain a mixture. The mixture was added to a reaction vessel equipped with a mechanical stirrer, and nitrogen gas was purged for 30 min to remove oxygen. Prepolymerization was carried out under 50 mW / cm² ultraviolet light for 60 s. Ethyl acetate was added to adjust the solid content to about 10 wt% to obtain the prepolymer solution.
[0042] S3. Preparation of nanocomposite ionic pressure-sensitive adhesive: Take 100 parts by weight of the prepolymer adhesive solution, add 0.1 parts of the above-mentioned silanized zinc oxide nanoparticles and 0.05 parts of azobisisobutyronitrile, stir and mix and ultrasonically disperse for 30 min, coat the obtained nanocomposite ionic pressure-sensitive adhesive solution on the surface of the release film, remove the solvent at 50°C, and carry out thermally initiated free radical polymerization at 70°C to obtain nanocomposite ionic pressure-sensitive adhesive.
[0043] The activation index of silanized zinc oxide nanoparticles was determined according to the group standard T-CSTM 01202—2024. The grafting density of the silanized zinc oxide nanoparticles was calculated based on the difference in thermogravimetric loss of the nanoparticles before and after silanization and the specific surface area of the nanoparticles. The activation index of the silanized zinc oxide nanoparticles obtained in step S1 was determined to be 95.42%, and the grafting density was 2.55 μmol / m².
[0044] Example 2
[0045] This embodiment provides a method for preparing silanized alumina nanoparticles and their nanocomposite ionic pressure-sensitive adhesives, including the following steps:
[0046] Except for the following differences, the raw material composition and preparation conditions are the same as in Example 1. The difference is that the zinc oxide nanoparticles with a particle size of 50 nm are replaced with alumina nanoparticles with a particle size of 50 nm.
[0047] In step S3, based on 100 parts of prepolymer adhesive, the amount of silanized alumina nanoparticles added is still 0.1 parts.
[0048] The activation index of the silanized alumina nanoparticles obtained in step S1 was determined to be 96.97%, and the grafting density was 3.06 μmol / m².
[0049] Example 3
[0050] This embodiment provides a method for preparing silanized titanium dioxide nanoparticles and their nanocomposite ionic pressure-sensitive adhesive, comprising the following steps:
[0051] Except for the following differences, the raw material composition and preparation conditions are the same as in Example 1. The difference is that the zinc oxide nanoparticles with a particle size of 50 nm are replaced with titanium dioxide nanoparticles with a particle size of 50 nm.
[0052] In step S3, based on 100 parts of prepolymer adhesive, the amount of silanized titanium dioxide nanoparticles added is still 0.1 parts.
[0053] The activation index of the silanized titanium dioxide nanoparticles obtained in step S1 was determined to be 97.18%, and the grafting density was 2.76 μmol / m².
[0054] Example 4
[0055] This embodiment provides a method for preparing vinylsilane-modified zinc oxide nanoparticles and their nanocomposite ionic pressure-sensitive adhesive, comprising the following steps:
[0056] Except for the following differences, the composition of the raw materials and the preparation conditions are the same as in Example 1. The difference is that 3-(methacryloyloxy)propyltrimethoxysilane in step S1 is replaced with an equal mass of vinyltrimethoxysilane.
[0057] In step S3, based on 100 parts of prepolymer adhesive, the amount of silanized zinc oxide nanoparticles added is still 0.1 parts.
[0058] The activation index of the silanized zinc oxide nanoparticles obtained in step S1 was determined to be 95.98%, and the grafting density was 3.19 μmol / m².
[0059] Example 5
[0060] This embodiment provides a method for preparing high-graft-density silanized zinc oxide nanoparticles and their nanocomposite ionic pressure-sensitive adhesive, comprising the following steps:
[0061] Except for the following differences, the composition of raw materials and preparation conditions are the same as in Example 1. The difference is that the amount of 3-(methacryloyloxy)propyltrimethoxysilane in step S1 is increased from 0.5 parts to 1 part.
[0062] In step S3, based on 100 parts of prepolymer adhesive, the amount of silanized zinc oxide nanoparticles added is still 0.1 parts.
[0063] The activation index of the silanized zinc oxide nanoparticles obtained in step S1 was determined to be 97.36%, and the grafting density was 10.29 μmol / m².
[0064] Example 6
[0065] This embodiment provides a method for preparing high-content silanized zinc oxide nanoparticles and their nanocomposite ionic pressure-sensitive adhesive, comprising the following steps:
[0066] Except for the following differences, the composition of raw materials and preparation conditions are the same as in Example 1. The difference is that, based on 100 parts of prepolymer solution, the amount of silanized zinc oxide nanoparticles added in step S3 is increased from 0.1 parts to 0.4 parts.
[0067] Example 7
[0068] This embodiment provides a method for preparing silanized zinc oxide nanoparticles and their nanocomposite ionic pressure-sensitive adhesive, including the following steps:
[0069] Except for the following differences, the composition of the raw materials and the preparation conditions are the same as in Example 1. The difference is that in step S2, the soft monomer is butyl acrylate and the polar monomer is 2-methoxyethyl acrylate. By weight, the addition amounts of the soft monomer and the polar monomer are 70 parts and 30 parts, respectively.
[0070] Example 8
[0071] This embodiment provides a method for preparing silanized zinc oxide nanoparticles and their nanocomposite ionic pressure-sensitive adhesive, including the following steps:
[0072] Except for the following differences, the composition of the raw materials and the preparation conditions are the same as in Example 1. The difference is that in step S2, the ionic liquid is 1-butyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt, and the amount added is 10 parts by weight.
[0073] Comparative Example 1
[0074] This comparative example provides a formulation and preparation method for a pressure-sensitive adhesive without the addition of ionic liquids and nanoparticles, including the following steps:
[0075] Except for the following differences, the composition of raw materials and preparation conditions are the same as in Example 1. The difference is that 1-ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide and silanized zinc oxide nanoparticles are not added.
[0076] Comparative Example 2
[0077] This comparative example provides a method for preparing an ionic pressure-sensitive adhesive without adding nanoparticles, comprising the following steps:
[0078] Except for the following differences, the composition of raw materials and preparation conditions are the same as in Example 1. The difference is that no nanoparticles are added.
[0079] Comparative Example 3
[0080] This comparative example provides a method for preparing a nanocomposite ionic pressure-sensitive adhesive with added hydrophobic silica nanoparticles, comprising the following steps:
[0081] Except for the following differences, the composition of raw materials and preparation conditions are the same as in Example 1. The difference is that in step S3, the silanized zinc oxide nanoparticles are replaced with hydrophobic silica nanoparticles with a particle size of 50 nm. The hydrophobic silica nanoparticles are not silanized using the method described in step S1. Based on 100 parts of prepolymer solution, the amount of hydrophobic silica nanoparticles added is still 0.1 parts.
[0082] Comparative Example 4
[0083] This comparative example provides a method for preparing a nanocomposite ionic pressure-sensitive adhesive with added unmodified zinc oxide nanoparticles, comprising the following steps:
[0084] Except for the following differences, the composition of raw materials and preparation conditions are the same as in Example 1. The difference is that in step S3, the silanized zinc oxide nanoparticles are replaced with unmodified commercially available zinc oxide nanoparticles (particle size of 50 nm), and the addition amount is still 0.1 parts based on 100 parts of prepolymer solution.
[0085] Performance testing
[0086] To further verify the influence of key components and structural design in the nanocomposite ionic pressure-sensitive adhesive of this invention on ion transport performance, adhesion performance, electro-tack reduction performance, and strain sensing performance, this invention uses a nanocomposite ionic pressure-sensitive adhesive containing silanized nanoparticles as an example, and sets up systems without ionic liquid, without nanoparticles, with hydrophobic silica nanoparticles, and with unmodified zinc oxide nanoparticles as comparative examples. Through the above comparisons, the effects of ionic liquid composition, nanoparticle type, silane coupling agent type, grafting density of silanized nanoparticles, and addition amount on the ion transport performance, adhesion performance, electro-tack reduction performance, and strain sensing performance of the ionic pressure-sensitive adhesive were investigated.
[0087] The following performance tests were performed on Examples 1-6 and Comparative Examples 1-4:
[0088] (1) Ionic conductivity test: Samples with length, width, and thickness of 20 mm, 10 mm, and 50 μm respectively were tightly bonded between a 20 μm thick stainless steel foil and a special steel plate for peel force testing. Using an electrochemical workstation (Chenhua, CHI 660E), the samples were tested at an amplitude of 10 mV in a two-electrode configuration from 0.01 Hz to 10 mV. 6 Electrochemical impedance spectroscopy in the Hz range was performed, and an equivalent circuit was constructed to calculate the ionic conductivity of the sample.
[0089] (2) 180° peel strength test: The 180° peel strength of the sample was determined according to standard GB / T 2792-2014. A single-sided tape was prepared using a 20 μm thick stainless steel foil as a backing. A 50 μm thick, 25 mm × 150 mm single-sided tape was laminated onto a special steel plate for peel strength testing. The tape was rolled back and forth 3 times with a 2 kg roller and left at room temperature for 20 min. The 180° peel test was then performed on an electronic multi-testing machine at a speed of 300 mm / min.
[0090] (3) Electro-adhesion reduction efficiency test: The sample specifications are consistent with those of the 180° peel strength test. The test steel plate is connected to the negative terminal of the DC regulated power supply, and the stainless steel foil is connected to the positive terminal. The DC regulated power supply (MAISHENG MS1520C) is used to apply an 8 V voltage to the sample. After stimulation for 15 s, the 180° peel strength test is performed immediately. The electro-adhesion reduction efficiency is calculated as follows: electro-adhesion reduction efficiency = (peel strength before energization - peel strength after energization) / peel strength before energization × 100%.
[0091] (4) Strain coefficient test: A rectangular strip of 20 mm × 10 mm × 1 mm was used for uniaxial tension at a tension rate of 1.67% / s. The resistance change of the sample was recorded in real time using a two-wire resistance mode under a test voltage of 0.5 V. The slope of the curve fitting between the relative resistance change and the strain in the strain range of 0 to 100% was used as the strain coefficient.
[0092] Furthermore, gesture recognition testing was conducted on the preferred embodiment 1:
[0093] (5) Gesture recognition test: Five identical splines from Example 1 were fixed to five fingers respectively, and five-channel resistance response signals were collected simultaneously. Five gestures were set, and 120 sets of data were collected for each gesture, for a total of 600 sets of samples. The multi-channel relative resistance change time-series signal was used as input, and a one-dimensional convolutional neural network was used for classification. The classification accuracy of the test set was used to evaluate the gesture recognition performance.
[0094] The test results are shown in Table 1.
[0095] Table 1. Ion transport, adhesion, electro-adhesion reduction, and strain sensing performance of the examples and comparative examples.
[0096]
[0097] Note: " / " indicates that no valid electroviscosity reduction or strain sensing performance data were obtained under the corresponding conditions.
[0098] As shown in Table 1, neither Comparative Example 1 nor Comparative Example 2 contained nanoparticles. Comparative Example 1, a pressure-sensitive adhesive without ionic liquid or nanoparticles, exhibited extremely low ionic conductivity, showing neither electro-adhesion reduction nor strain sensing response. This indicates that the ionic transport properties provided by the ionic liquid are the basis for generating electro-adhesion reduction and strain sensing responses. While Comparative Example 2, after introducing ionic liquid, possessed ionic conductivity and electro-adhesion reduction responses, its peel strength and strain coefficient were significantly lower than the system containing silanized nanoparticles. This demonstrates that the introduction of silanized nanoparticles substantially contributes to improving adhesion and strain sensing performance. Comparing Example 1 and Comparative Example 4, it can be seen that the unmodified nanoparticles are only physically dispersed in the adhesive layer and cannot be anchored to the polymer network through chemical bonds, thus having limited improvement on the adhesive properties. After silanization modification, the zinc oxide nanoparticles in Example 1 participate in the formation of acrylate copolymers during free radical polymerization, thereby chemically bonding the nanoparticles to the polymer network. The 180° peel strength, electro-tack reduction efficiency, and strain coefficient of the sample are all improved, indicating that silanization modification is beneficial to improving the adhesive and strain sensing properties of the sample, while maintaining good ion transport and electro-tack reduction properties.
[0099] Based on this, further changes in the type of nanoparticles, the type of silane coupling agent, the grafting density and addition amount of silanized nanoparticles altered the ion transport, adhesion, electro-tack reduction, and strain sensing properties of the samples. Comparative Example 3 used hydrophobic silica nanoparticles that lacked Lewis acid sites and were not silanized, thus failing to participate in polymer network formation. Its ionic conductivity, peel strength, electro-tack reduction efficiency, and strain coefficient were all lower than those of Example 1. A comparison of Comparative Example 3 and Examples 1-4 shows that different metal oxide nanoparticles containing Lewis acid sites and different free-radical polymerizable silane coupling agents can all be used to prepare nanocomposite ionic pressure-sensitive adhesives with good adhesion, electro-tack reduction, and strain sensing properties. A comparison of Examples 1, 5-8 shows that by changing the grafting density or addition amount of silanized zinc oxide nanoparticles, the type or addition amount of soft monomers and polar monomers, and the type or addition amount of ionic liquids, the adhesion, electro-tack reduction, and strain sensing properties of nanocomposite ionic pressure-sensitive adhesives can be controlled. In summary, Example 1 demonstrates a good balance between ion transport, adhesion, and electro-de-adhesion properties. Further strain sensing tests on Example 1 showed that it exhibited a stable resistance response within the strain range of 0–550% at a test voltage of 0.5 V, and maintained a stable response even after 500 cycles of stretching at 100% strain. Example 1 was further applied to five-finger multi-channel gesture recognition, combined with a one-dimensional convolutional neural network, achieving a recognition accuracy of 98.67% for five types of gestures. These results indicate that this preferred embodiment possesses good adhesion properties, enables strain monitoring at a test voltage of 0.5 V, and achieves rapid electro-de-adhesion after 15 seconds of stimulation with an 8 V voltage.
[0100] The specific monomers, initiators, crosslinking agents, ionic liquids, nanoparticles, and silane coupling agents listed in the above embodiments are merely preferred examples and not intended to limit the scope of protection of this invention. Those skilled in the art can make adjustments within the scope defined by the claims of this invention according to the application scenario, substrate type, coating process, and target peel strength. All changes, modifications, substitutions, and variations made without departing from the principles and spirit of this invention should fall within the scope of protection of this invention.
Claims
1. A method for preparing a dual-mode electrically responsive nanocomposite ionic pressure sensitive adhesive, characterized in that, Includes the following steps: S1. Silanization modification of nanoparticles: Metal oxide nanoparticles with Lewis acid sites are mixed with water and ethanol and dispersed by ultrasonication to obtain a dispersion. A silane coupling agent that can be polymerized by free radicals is dissolved in ethanol and added dropwise to the above dispersion for silanization modification. After the reaction is completed, the nanoparticles are obtained by centrifugation, washing and drying. S2. Preparation of prepolymer solution: By weight, 50-90 parts of soft monomer, 10-50 parts of polar monomer, 0.05-0.5 parts of photoinitiator, 0.05-0.3 parts of crosslinking agent, 1-10 parts of ionic liquid and 100-200 parts of organic solvent are mixed to obtain a mixture; prepolymerization is initiated by ultraviolet light under inert gas protection, and then organic solvent is added to adjust the solid content to obtain the prepolymer solution; S3. Preparation of nanocomposite ionic pressure-sensitive adhesive: The prepolymer adhesive solution, the silanized nanoparticles and the thermal initiator are mixed evenly. The resulting nanocomposite ionic pressure-sensitive adhesive solution is coated on the surface of the release film. After removing the solvent, thermally initiated free radical polymerization is carried out. During the free radical polymerization process, the free radical polymerizable organosilane component participates in the formation of the acrylate copolymer to obtain the nanocomposite ionic pressure-sensitive adhesive.
2. The method of claim 1, wherein the method is characterized by, By weight, in step S1, the metal oxide nanoparticles are 5-15 parts, the dispersion contains 200-400 parts water, 400-600 parts ethanol, 0.1-5 parts silane coupling agent, and 1-50 parts ethanol to dissolve the silane coupling agent.
3. The preparation method of the nanocomposite ionic pressure-sensitive adhesive according to claim 1, characterized in that: The metal oxide nanoparticles with Lewis acidic sites are one or more of zinc oxide, titanium dioxide, zirconium oxide, aluminum oxide, and cerium oxide, with a particle size of 10–100 nm. The free radical polymerizable silane coupling agent is selected from one or more of 3-(methacryloyloxy)propyltrimethoxysilane, 3-(methacryloyloxy)propyltriethoxysilane, 3-acryloyloxypropyltrimethoxysilane, vinyltrimethoxysilane, and vinyltriethoxysilane.
4. The preparation method of the nanocomposite ionic pressure-sensitive adhesive according to claim 1, characterized in that: The soft monomer is one or more selected from isooctyl acrylate, butyl acrylate, ethyl acrylate, lauryl acrylate, and n-hexyl acrylate; The polar monomer is a free radical polymerizable monomer containing carboxyl, hydroxyl, amide, ether bond or nitrogen-containing heterocyclic structure, selected from one or more of acrylic acid, hydroxyethyl acrylate, 2-carboxyethyl acrylate, N,N-dimethylacrylamide, 2-methoxyethyl acrylate, and N-vinylpyrrolidone. The ionic liquid is one or more of the imidazolonium ionic liquids; The crosslinking agent is one or more of the multifunctional acrylate crosslinking agents; The photoinitiator is one or more of 2-hydroxy-2-methylphenylacetone, 1-hydroxycyclohexylphenyl ketone, 2,2-dimethoxy-2-phenylacetophenone, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, and diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide; The organic solvent is one or more of ethyl acetate, butyl acetate, isopropyl acetate, methyl ethyl ketone, acetone, and propylene glycol methyl ether acetate.
5. The method of claim 1, wherein the method is characterized by: The light intensity for initiating the prepolymerization by ultraviolet light is 20-100 mW / cm 2 , the polymerization time is 10-600 s, the temperature is 15-45℃; and the solid content of the prepolymer glue solution in S2 is 8-12wt%.
6. The method of claim 1, wherein the method is characterized by: In step S3, the amount of silanized nanoparticles is 0.01-5 parts by weight per 100 parts of prepolymer solution, and the amount of thermal initiator is 0.05-0.5 parts by weight; the thermal initiator is one or more of azobisisobutyronitrile, azobisisoheptanenitrile, and benzoyl peroxide; the free radical polymerization time is 0.5-5 h, and the temperature is 50-90℃.
7. A pre-polymer glue solution nanocomposite ionic pressure sensitive adhesive, characterized in that: The preparation method according to any one of claims 1 to 6 is used to obtain the acrylate copolymer, the ionic liquid and the silanized nanoparticles dispersed in the acrylate copolymer; The silanized nanoparticles are metal oxide nanoparticles with Lewis acid sites, and their surfaces are grafted with organosilane components that can be free radical polymerized. The organosilane components participate in the copolymerization of acrylate monomers during the free radical polymerization process.
8. The nanocomposite ionomeric pressure sensitive adhesive of claim 7, wherein: The nanocomposite ionic pressure-sensitive adhesive generates a strain sensing response through the resistance change caused by deformation under test voltage conditions, and weakens the interfacial adhesion between the adhesive layer and the substrate through electrical stimulation under stimulation voltage conditions, thereby achieving rapid electro-tack reduction.
9. The nanocomposite ionic pressure-sensitive adhesive according to claim 8, characterized in that: The test voltage is 0.1~3V, and the stimulation voltage is 8~36V.
10. The application of the nanocomposite ionic pressure-sensitive adhesive according to any one of claims 7 to 9 in flexible electronic devices, wearable devices, soft robots, removable batteries, or wafer processing, characterized in that: The nanocomposite ionic pressure-sensitive adhesive is used for one or more of the following: bonding, strain monitoring, and electro-adhesion reduction.
Citation Information
Patent Citations
Reusable power-on viscosity-reducing adhesive tape with high shear strength and preparation method thereof
CN118389082A