Optical adhesives, optical adhesive films, and display devices

By using acrylate prepolymer and polyurethane prepolymer to form a crosslinked network in optical adhesive, the problem of insufficient bending resistance of optical adhesive was solved, and the bending resistance of display devices was improved.

CN123107586APending Publication Date: 2026-11-17YANTAI BOE MATERIAL TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611584414.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing optical adhesives are not strong enough to withstand bending in foldable or rollable display devices, and are prone to delamination or creases.

Method used

Using acrylate prepolymer and polyurethane prepolymer as raw materials, the side chains of the acrylate prepolymer have hydroxyl and/or carboxylic acid groups, and the end groups of each polyether polyurethane prepolymer are isocyanate groups. By compounding, a cross-linked network is formed, which, combined with the polyether flexible segment structure, improves the bending resistance of the optical adhesive.

Benefits of technology

It significantly improves the bending resistance of optical adhesives, balancing flexibility and cross-linking density, and solves the problem of delamination or creases caused by bending in display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107586A_ABST
    Figure CN123107586A_ABST
Patent Text Reader

Abstract

This application discloses an optical adhesive, an optical adhesive film, and a display device, belonging to the field of optical adhesive technology. The raw materials of the optical adhesive include the following components in parts by weight: 100 parts of acrylate prepolymer and 10-25 parts of polyurethane prepolymer; wherein the side chains of the acrylate prepolymer have hydroxyl and / or carboxylic acid groups; the polyurethane prepolymer is formed by compounding at least two polyether polyurethane prepolymers with different functionalities, and the end groups of each polyether polyurethane prepolymer are isocyanate groups. This application uses acrylate prepolymer and polyurethane prepolymer in the raw materials of the optical adhesive. The polyether polyurethane prepolymer can react with the acrylate prepolymer to form a crosslinked network. The polyether polyurethane prepolymer has a polyether flexible segment structure, which can improve the bending resistance of the optical adhesive. The polyurethane prepolymer can contain polyether polyurethane prepolymers with various structures such as linear and branched structures, improving the flexibility and crosslinking density of the optical adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of optical adhesive technology, and in particular to an optical adhesive, an optical adhesive film, and a display device. Background Technology

[0002] Against the backdrop of rapid development in display technology, foldable or rollable display devices have begun to be widely used, such as in smartphones, automotive pop-up screens, and curved displays.

[0003] The display modules of these display devices are bonded to the protective cover with optical adhesive. Currently, the optical adhesive is prone to delamination or creases when the display device is bent, and its bending resistance is insufficient. Summary of the Invention

[0004] This application provides an optical adhesive, an optical adhesive film, and a display device. It solves the problem of insufficient bending resistance in existing optical adhesives. The technical solution is as follows: On one hand, an optical adhesive is provided, wherein the raw material of the optical adhesive comprises the following components in parts by weight: 100 parts of acrylate prepolymer and 10-25 parts of polyurethane prepolymer; The acrylate prepolymer has hydroxyl and / or carboxylic acid groups on its side chains; the polyurethane prepolymer is formed by compounding at least two polyether polyurethane prepolymers with different functionalities, and the end groups of each polyether polyurethane prepolymer are isocyanate groups.

[0005] Optionally, the polyurethane prepolymer includes: a first polyether polyurethane prepolymer and a second polyether polyurethane prepolymer; The first polyether polyurethane prepolymer is a linear polyether polyurethane prepolymer, and the second polyether polyurethane prepolymer is a branched polyether polyurethane prepolymer; the first polyether polyurethane prepolymer and the second polyether polyurethane prepolymer have different functionalities.

[0006] Optionally, the functionality of the first polyether polyurethane prepolymer is less than that of the second polyether polyurethane prepolymer. The mass ratio of the first polyether polyurethane prepolymer to the second polyether polyurethane prepolymer is 1:2-2:1.

[0007] Optionally, the raw materials for the first polyether polyurethane prepolymer include the following components: The polyether diol and the polyisocyanate, wherein the molar ratio of the isocyanate group of the polyisocyanate to the hydroxyl group of the polyether diol is greater than or equal to 2:1.

[0008] Optionally, the number average molecular weight of the polyether diol is 1000-4000; and / or, the polyisocyanate includes: alicyclic diisocyanate.

[0009] Optionally, the polyether diol includes at least one of polypropylene glycol and polytetrahydrofuran ether diol; And / or, the alicyclic diisocyanate includes at least one of isophorone diisocyanate and dicyclohexylmethane diisocyanate.

[0010] Optionally, the raw materials for the first polyether polyurethane prepolymer further include the following components: The polycarbonate diol and disulfide chain extender are present, wherein the polycarbonate diol accounts for 15%-35% of the total hydroxyl equivalent in the first polyether polyurethane prepolymer, and the disulfide chain extender accounts for 1%-8% of the total hydroxyl equivalent in the first polyether polyurethane prepolymer.

[0011] Optionally, the polycarbonate diol has a number average molecular weight of 1500 to 2500, and / or the disulfide chain extender includes 2,2′-dithiodiethanol.

[0012] Optionally, the raw materials for the second polyether polyurethane prepolymer include the following components: The polyether triol and the polyisocyanate; the molar ratio of the isocyanate group of the polyisocyanate to the hydroxyl group of the polyether triol is greater than or equal to 2:1.

[0013] Optionally, the number average molecular weight of the polyether triol is 1000-4000; and / or, the polyisocyanate includes: alicyclic diisocyanate.

[0014] Optionally, the polyether triol includes: polypropylene oxide triol; And / or, the alicyclic diisocyanate includes at least one of isophorone diisocyanate and dicyclohexylmethane diisocyanate.

[0015] Optionally, the raw materials for the acrylate prepolymer include the following components: Acrylate functional monomers containing hydroxyl and / or carboxylic acid groups.

[0016] Optionally, the raw materials for the acrylate prepolymer may further include the following components: The acrylate soft monomer and the acrylate hard monomer, wherein the mass fraction of the acrylate soft monomer is greater than the mass fraction of the acrylate hard monomer, and the mass fraction of the acrylate hard monomer is greater than the mass fraction of the acrylate functional monomer.

[0017] On the other hand, an optical adhesive film is provided, the optical adhesive film comprising: an optical adhesive layer, and a first release film and a second release film adhered to both sides of the optical adhesive layer; the optical adhesive layer is prepared from any of the optical adhesives described above.

[0018] In another aspect, a display device is provided, the display device comprising: a display module and a protective cover plate, and an optical adhesive layer located between the display module and the protective cover plate; the optical adhesive layer is prepared from any of the optical adhesives described above, or the optical adhesive layer comprises the optical adhesive layer in the optical adhesive film described above.

[0019] The beneficial effects of the technical solutions provided in this application are: By using acrylate prepolymers and polyurethane prepolymers in the raw materials of optical adhesives, the acrylate prepolymers have hydroxyl and / or carboxylic acid groups on their side chains, while the end groups of each polyether polyurethane prepolymer are isocyanate groups. The polyether polyurethane prepolymers can react with the acrylate prepolymers to form a crosslinked network. The polyether polyurethane prepolymers have a polyether flexible segment structure, which can improve the bending resistance of the optical adhesive. The polyurethane prepolymers are formed by compounding at least two polyether polyurethane prepolymers with different functionalities, providing polyether polyurethane prepolymers with various structures such as linear and branched types. This not only improves the flexibility of the optical adhesive but also increases the crosslinking density. Attached Figure Description

[0020] To more clearly illustrate the technical solutions in the embodiments of this application, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 This is a schematic diagram of the film layers of the optical adhesive film according to an embodiment of this application; Figure 2 This is a schematic diagram of the structure of the display device according to an embodiment of this application; Figure 3 This is another schematic diagram of the display device according to an embodiment of this application. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of this application clearer, the embodiments of this application will be described in further detail below with reference to the accompanying drawings.

[0023] This application provides an optical adhesive, the raw materials of which may include the following components in parts by weight: 100 parts of acrylate prepolymer and 10-25 parts of polyurethane prepolymer; The acrylate prepolymer has hydroxyl and / or carboxylic acid groups on its side chains; the polyurethane prepolymer is formed by compounding at least two polyether polyurethane prepolymers with different functionalities, and the end groups of each polyether polyurethane prepolymer are isocyanate groups.

[0024] For example, the side chains of the acrylate prepolymer have hydroxyl and / or carboxylic acid groups, both of which can react with isocyanate groups to form a crosslinked network. The polyurethane prepolymer is formed by compounding at least two polyether polyurethane prepolymers with different functionalities. By adjusting the proportion of polyether polyurethane prepolymers with different functionalities, the average functionality of the polyurethane prepolymer can be adjusted, thereby forming a controlled crosslinked network. The polyether polyurethane prepolymer has long-chain flexible segments, which can avoid the optical adhesive having excessively short chain segments, resulting in a high modulus. The difunctional polyether polyurethane prepolymer can have a linear structure, while the polyether polyurethane prepolymer with more than two functionalities can have a branched structure. The polyurethane prepolymer formed by compounding can simultaneously adjust the crosslinking density, chain segment relaxation, and hygrothermal stability of the optical adhesive.

[0025] For example, the ether bond structure in polyether polyurethane prepolymers can enhance the hydrolytic stability and weather resistance of optical adhesives. The polyether segments can improve the flexibility and low-temperature flexibility of the optical adhesives.

[0026] After the polyether polyurethane prepolymer reacts with the acrylate prepolymer, the polyether soft segments are chemically bonded into the acrylate crosslinking network, forming a "soft segment-hard segment" microphase separation structure. The polyurethane segments act as stress dissipation centers, absorbing energy through segmental movement when subjected to external forces, preventing stress concentration, and thus significantly improving the bending resistance of the film.

[0027] In this embodiment, by using acrylate prepolymers and polyurethane prepolymers in the raw materials of the optical adhesive, the side chains of the acrylate prepolymers have hydroxyl and / or carboxylic acid groups, and the end groups of each polyether polyurethane prepolymer are isocyanate groups. The polyether polyurethane prepolymers can react with the acrylate prepolymers to form a crosslinked network. The polyether polyurethane prepolymers have a polyether flexible segment structure, which can improve the bending resistance of the optical adhesive. The polyurethane prepolymers are formed by compounding at least two polyether polyurethane prepolymers with different functionalities, which can provide polyether polyurethane prepolymers with various structures such as linear and branched types, which can not only improve the flexibility of the optical adhesive but also increase the crosslinking density.

[0028] The following is a description of the raw materials in the optical adhesive: In the embodiments of this application, the mass fraction of the polyurethane prepolymer can range from 10 parts to 25 parts. The mass fraction of the polyurethane prepolymer can include the endpoints of the corresponding range, for example, the mass fraction of the polyurethane prepolymer can be 10 parts, 15 parts, 20 parts, 25 parts, etc. The proportion or ratio of other raw materials can also include the endpoints of the corresponding range, and will not be repeated here.

[0029] In some possible implementations, the polyurethane prepolymer may include: a first polyether polyurethane prepolymer and a second polyether polyurethane prepolymer.

[0030] The first polyether polyurethane prepolymer is a linear polyether polyurethane prepolymer, and the second polyether polyurethane prepolymer is a branched polyether polyurethane prepolymer; the first polyether polyurethane prepolymer and the second polyether polyurethane prepolymer have different functionalities.

[0031] For example, the raw material of the first polyether polyurethane prepolymer may include polyether diol, thereby forming a linear polyether polyurethane prepolymer. The linear first polyether polyurethane prepolymer can provide a soft segment structure for the polyurethane prepolymer, improve the flexibility of the optical adhesive, and thus improve the bending resistance.

[0032] For example, the raw material of the second polyether polyurethane prepolymer may include polyether polyol, thereby forming a branched polyether polyurethane prepolymer. In addition to retaining the flexible structure of the polyether segments, the branched second polyether polyurethane prepolymer can also form branched connections with the acrylate prepolymer, increasing the effective crosslinking connection points and improving the gel content and cohesive strength.

[0033] In this embodiment, a polyurethane prepolymer can be obtained by compounding a first polyether polyurethane prepolymer with a second polyether polyurethane prepolymer of different functionalities. Unlike conventional small-molecule difunctional or trifunctional isocyanate curing agents, this embodiment uses an isocyanate-terminated polyurethane prepolymer as a crosslinking curing agent. The polyurethane prepolymer itself has a polyether soft segment structure. After being mixed with the acrylate prepolymer, its terminal isocyanate groups react with the hydroxyl or carboxylic acid groups of the acrylate prepolymer side chains to form a chemical crosslinking network.

[0034] In some possible implementations, the functionality of the first polyether polyurethane prepolymer is less than that of the second polyether polyurethane prepolymer.

[0035] The mass ratio of the first polyether polyurethane prepolymer to the second polyether polyurethane prepolymer is 1:2-2:1.

[0036] In the embodiments of this application, the average functionality of the polyurethane prepolymer can be adjusted by adjusting the mass ratio of the first polyether polyurethane prepolymer to the second polyether polyurethane prepolymer. This allows for adjustment of the density of the crosslinked network of the final optical adhesive, the storage modulus of the optical adhesive, and the degree of chain segment relaxation, thereby improving the flexibility and bending resistance of the optical adhesive.

[0037] For example, the mass ratio of the first polyether polyurethane prepolymer to the second polyether polyurethane prepolymer can be 1:1. This allows for a balance between the crosslinking density, modulus, and cohesive strength of the optical adhesive.

[0038] In some possible implementations, the raw materials for the first polyether polyurethane prepolymer may include the following components: The molar ratio of the isocyanate group of the polyether diol to the hydroxyl group of the polyether diol is greater than or equal to 2:1.

[0039] In this embodiment, a first polyether polyurethane prepolymer can be formed by polycondensation of polyether diol and polyisocyanate, thereby obtaining an isocyanate-terminated first polyether polyurethane prepolymer. Since polyether diol is used as the raw material, the first polyether polyurethane prepolymer can be a linear polyether polyurethane prepolymer. By controlling the molar ratio of polyether diol to polyisocyanate, it can be ensured that the end groups of the first polyether polyurethane prepolymer are isocyanate groups.

[0040] For example, the polyether diol may include at least one of polypropylene glycol (PPG) and polytetrahydrofuran ether diol (PTMEG). The polyisocyanate may include at least one of isophorone diisocyanate (IPDI), dicyclohexylmethane diisocyanate (HMDI), hexamethylene diisocyanate (HDI), and HDI trimer.

[0041] In some possible implementations, the number average molecular weight of the polyether diol is 1000-4000; and / or, the polyisocyanate may include: alicyclic diisocyanate.

[0042] In the embodiments of this application, by adjusting the molecular weight, functionality, and type of polyether polyol, precise control over the segment length, flexibility, and functionality of the polyurethane prepolymer can be achieved. For example, using difunctional polyether polyols (such as PPG and PTMEG) to synthesize a linear first polyether polyurethane prepolymer can act as a chain extender to introduce flexible segments into the crosslinking network.

[0043] The polyisocyanate may include: alicyclic diisocyanate, for example, at least one of isophorone diisocyanate (IPDI) and dicyclohexylmethane diisocyanate (HMDI), such that the ratio of the isocyanate group (NCO) of the polyisocyanate to the hydroxyl group (OH) of the polyether diol is greater than or equal to 2:1, thereby forming a linear first polyether polyurethane prepolymer having isocyanate group end caps.

[0044] In some possible implementations, the raw materials for the first polyether polyurethane prepolymer may also include the following components: Polycarbonate diol and disulfide chain extender: polycarbonate diol accounts for 15%-35% of the total hydroxyl equivalent in the first polyether polyurethane prepolymer, and disulfide chain extender accounts for 1%-8% of the total hydroxyl equivalent in the first polyether polyurethane prepolymer.

[0045] In this embodiment, by adding polycarbonate diol, the composite soft segment of polyether diol and polycarbonate diol avoids the problem of excessively short chain segments between crosslinking points leading to a sharp increase in modulus. Compared with conventional polyether soft segments, polycarbonate diol contains ether bonds and carbonate bonds, which can introduce carbonate groups (-O-CO-O-) into the molecular chain. This retains the flexibility of the polyether chain segments and enhances intermolecular interactions through the polarity of the carbonate groups, thereby improving cohesive strength and hygrothermal stability. The polycarbonate diol accounts for 15% to 35% of the total hydroxyl equivalent of the first polyether polyurethane prepolymer, for example, 20% to 30%, and the number average molecular weight of the polycarbonate diol can be 1500 to 2500.

[0046] Disulfide bonds are embedded in the main chain of the first polyether polyurethane prepolymer in a low proportion (e.g., 1%–8% of the total hydroxyl equivalent), rather than as end groups or UV-polymerizable groups. This embedded design places the disulfide bonds in the chain segments between the connection points in the crosslinking network, providing stress dissipation pathways through the dynamic exchange of disulfide bonds under stress, thus delaying the accumulation of fatigue damage. Simultaneously, the low proportion of disulfide bonds avoids the impact of excessive sulfur on optical transparency.

[0047] For example, the disulfide chain extender may include 2,2′-dithiodiethanol (HEDS), accounting for 1% to 8% of the total hydroxyl equivalent, for example 2% to 5%.

[0048] The above describes the raw materials for the first polyether polyurethane prepolymer. The following describes the raw materials for the second polyether polyurethane prepolymer.

[0049] In some possible implementations, the raw materials for the second polyether polyurethane prepolymer may include the following components: Polyether triol and polyisocyanate; the molar ratio of the isocyanate group to the hydroxyl group of the polyether triol is greater than or equal to 2:1.

[0050] In the embodiments of this application, the branched second polyether polyurethane prepolymer can provide high-functionality linkage sites and can be formed by polycondensation of polyether triol and polyisocyanate. For example, the molar ratio of isocyanate groups (NCO) of the polyisocyanate to hydroxyl groups (OH) of the polyether triol is 2.1:1. By controlling the molar ratio of polyether triol to polyisocyanate, it can be ensured that the end groups of the second polyether polyurethane prepolymer are isocyanate groups.

[0051] Polyisocyanates may include at least one of isophorone diisocyanate (IPDI), dicyclohexylmethane diisocyanate (HMDI), hexamethylene diisocyanate (HDI), and HDI trimer.

[0052] For example, the number average molecular weight of the polyether triol can be 1000-4000; and / or, the polyisocyanate can include: alicyclic diisocyanate.

[0053] For example, the number average molecular weight of the polyether triol is about 3000 and the hydroxyl value is about 56 mgKOH / g. For example, the polyether triol may include: polypropylene oxide triol. The polyisocyanate may include: alicyclic diisocyanate, for example, it may include at least one of isophorone diisocyanate (IPDI) and dicyclohexylmethane diisocyanate (HMDI).

[0054] The above describes the raw materials for polyurethane prepolymers; the following describes the raw materials for acrylate prepolymers.

[0055] In some possible implementations, the raw materials for the acrylate prepolymer may include the following components: Acrylate functional monomers containing hydroxyl and / or carboxylic acid groups.

[0056] In the embodiments of this application, the acrylate prepolymer can be a copolymer or a homopolymer. The prepolymer formed by using acrylate and having hydroxyl or carboxylic acid groups on the side chains can react with the isocyanate groups at the ends of the polyurethane prepolymer.

[0057] In some possible implementations, the raw materials for the acrylate prepolymer may also include the following components: acrylate soft monomers and acrylate hard monomers, with the mass fraction of acrylate soft monomers being greater than that of acrylate hard monomers, and the mass fraction of acrylate hard monomers being greater than that of acrylate functional monomers.

[0058] For example, the raw materials for acrylate prepolymers may include the following components in parts by weight: 60 to 85 parts of soft acrylate monomers, 10 to 30 parts of hard acrylate monomers, and 2 to 10 parts of functional acrylate monomers; and may also include: 0.1 to 0.5 parts of initiator and 100 to 200 parts of solvent.

[0059] For example, acrylate prepolymers can be acrylate copolymers to balance pressure sensitivity and cohesive strength. The raw materials for acrylate prepolymers may include soft monomers, hard monomers, functional monomers, and initiators.

[0060] The acrylate soft monomer may include at least one of the following: butyl acrylate, isooctyl acrylate, isobutyl acrylate, ethyl acrylate, and n-propyl acrylate.

[0061] The acrylate hard monomers may include at least one of the following: n-butyl methacrylate, methyl acrylate, ethyl methacrylate, methyl methacrylate, and ethoxyethyl acrylate.

[0062] Acrylic ester functional monomers may include: acrylate monomers containing hydroxyl or carboxylic acid groups, (meth)acrylic acid 2 Hydroxyethyl ester, (meth)acrylic acid 2 Hydroxypropyl ester, (meth)acrylic acid 2 Hydroxybutyl ester, phenyl glycidyl ether acrylate, 2 hydroxyl 3 Phenoxypropyl acrylate, polyethylene glycol monomethacrylate, (meth)acrylic acid, β-methacrylate At least one of acryloyloxypropionic acid, itaconic acid, and isobutoxymethylene acrylic acid.

[0063] The initiator may include at least one of the following: azobisisobutyronitrile, benzoyl peroxide, tert-butyl peroxide terephthalate, azobisisoheptanenitrile, and azobisisovalerate.

[0064] For example, the raw materials for the above-mentioned acrylate prepolymer can be polymerized using a solvent method, and the solvent may include at least one of ethyl acetate, toluene, and methyl ethyl ketone.

[0065] This application also provides a method for preparing an optical adhesive, used to prepare the optical adhesive described in any of the above embodiments. The method may include the following steps: Step 1: Synthesize acrylate prepolymer using a solvent method. The acrylate prepolymer is denoted as component A.

[0066] For example, under nitrogen protection, soft monomers, hard monomers, functional monomers, and a portion of the solvent are added to a reactor. Nitrogen is purged for 30 minutes to maintain the nitrogen atmosphere, and the temperature is raised to 65°C–68°C. Then, one-third of the free radical initiator is added, and the reaction is carried out at 65–68°C for 1–3 hours. Another one-third of the free radical initiator is added, and the temperature is raised to 73°C–76°C, then maintained for 1–4 hours. Finally, the remaining one-third of the free radical initiator is added dropwise, the temperature is raised to above 77°C, and then maintained for 1–2 hours. After the reaction is complete, the temperature is cooled to below 60°C, and the remaining solvent is added. After stirring and mixing thoroughly, an acrylate prepolymer is obtained, with a solid content controlled at 30%–50%.

[0067] Step 2: First polyether polyurethane prepolymer and second polyether polyurethane prepolymer are synthesized separately and compounded according to a preset ratio to obtain polyurethane prepolymer. The polyurethane prepolymer is denoted as component B, the first polyether polyurethane prepolymer is denoted as component B1, and the second polyether polyurethane prepolymer is denoted as component B2.

[0068] For example, polyether diol, polycarbonate diol, antioxidant, and disulfide bond extender are added to a reaction vessel and vacuum dehydrated at 120℃~145℃ for 2 to 3 hours; the temperature is then lowered to 80~100℃, polyisocyanate is added, and the reaction is carried out at 110℃~125℃ for 1 to 3 hours under nitrogen protection. The isocyanate group content in the reaction system is monitored until it reaches a preset value, yielding a linear first polyether polyurethane prepolymer, which is then discharged and vacuum-sealed for storage.

[0069] In the first polyether polyurethane prepolymer, the disulfide-bonded diol structure is HO-CH2CH2-SS-CH2CH2-OH. After reacting with NCO, it exists as an embedded structure "-NH-CO-O-CH2CH2-SS-CH2CH2-O-CO-NH-" in the main chain of component B1. The disulfide bond is located inside the B1 main chain rather than as an end group and does not participate in the UV polymerization reaction.

[0070] The first polyether polyurethane prepolymer provides flexible connections and stress dissipation paths through long-chain composite soft segments formed by polyether diol and polycarbonate diol and a low proportion of embedded disulfide bonds, thereby improving the bending resistance of the optical adhesive.

[0071] In the second polyether polyurethane prepolymer, polyether triol with a number average molecular weight of approximately 3000 is vacuum dehydrated at 110℃~140℃ for 2 to 3 hours (vacuum degree ≤ -0.095MPa). The temperature is then lowered to 80℃~100℃, and dicyclohexylmethane diisocyanate (H12MDI) is added to achieve a NCO / OH molar ratio of 2.1:1 in the second polyether polyurethane prepolymer. The reaction is carried out under nitrogen protection at 110℃~125℃ for 2 to 4 hours. The NCO content is monitored until it reaches a preset value, then the material is cooled, discharged, and vacuum-sealed for storage to obtain the second polyether polyurethane prepolymer.

[0072] The second polyether polyurethane prepolymer provides branched connections while maintaining the flexible segments of aliphatic polyurethane, increasing effective crosslinking points and improving gel content and cohesive strength.

[0073] The first polyether polyurethane prepolymer and the second polyether polyurethane prepolymer are mixed in a preset ratio to obtain a polyurethane prepolymer.

[0074] Step 3: Mix the acrylate prepolymer and the polyurethane prepolymer to react and obtain the optical adhesive.

[0075] Mix component A obtained in step one with component B obtained in step two in a certain proportion, add silane coupling agent and antioxidant, and add solvent to adjust the solid content to 25% to 45%, stir evenly, and degas under vacuum to obtain optical adhesive composition.

[0076] During heat treatment, the side chain hydroxyl or carboxylic acid groups of component A react with the terminal NCO groups of components B1 / B2 to form a covalently cross-linked network connected by flexible polyether segments. The reaction is illustrated as follows: A-OH + OCN-B-NCO → AO-CO-NH-B-NH-CO-OA.

[0077] Step 4: Preparation of optical adhesive film.

[0078] The optical adhesive composition obtained in step three is coated onto the first release film, dried in an oven to remove the solvent, and then heat-cured at a temperature of 80℃ to 120℃ for 1 minute to 10 minutes. After heat curing, a second release film is applied and cured at 25℃ to 70℃ for 1 day to 7 days to obtain the optical adhesive film.

[0079] In this embodiment, unlike conventional small-molecule difunctional or trifunctional isocyanate curing agents, an isocyanate-terminated polyurethane prepolymer is used as a crosslinking curing agent. This prepolymer itself has a polyether soft segment structure. After mixing with the acrylate prepolymer, the isocyanate groups at its ends react with the hydroxyl or carboxylic acid groups of the acrylate prepolymer side chains to form a chemical crosslinking network.

[0080] Component A is an acrylate copolymer containing side-chain hydroxyl groups, providing a pressure-sensitive adhesive matrix. The hydroxyl groups in the side chains can react with NCO groups. Component B is a polyether-type polyurethane macromolecular crosslinker, free of acrylate end-capping groups, using NCO end-capping to provide flexible polyether segments and controlled crosslinking points. This ensures that the segment lengths between crosslinking points in the optical adhesive's crosslinking network are neither too short nor too high, balancing the requirements for low modulus and cohesive strength. Adjusting the ratio of components B1 to B2 in component B allows for adjustment of the average functionality of component B, enabling the adjustment of crosslinking density and segment flexibility according to the application scenario.

[0081] Compared to small-molecule multifunctional NCO curing agents, both components B1 and B2 are terminal NCO macromolecular crosslinking agents with long-chain flexible segments. The PPG / polycarbonate diol composite soft segment of component B1 avoids the problem of excessively short chain segments between crosslinking points leading to a sharp increase in modulus; the low proportion of disulfide bonds acts as a chain extension structure embedded in the B1 backbone and does not undertake UV polymerization functions. Component B2 provides branched connections while maintaining the flexible segments of aliphatic polyurethane. When combined, the crosslinking density, chain segment relaxation, and hygrothermal stability can be adjusted simultaneously.

[0082] The coated film is first thermo-cured at 80℃~120℃, allowing the isocyanate groups and hydroxyl groups to react rapidly and form a preliminary cross-linked network. It is then cured at room temperature or slightly above room temperature, allowing the remaining isocyanate groups to continue reacting, while simultaneously promoting chain rearrangement and stress relaxation, resulting in a uniform and stable cross-linked structure. Therefore, a UV curing process is not required, and there is no issue of insufficient curing uniformity due to the thickness of the optical film or other light-absorbing or light-blocking structures.

[0083] In the embodiments of this application, the performance of the optical adhesive can be precisely controlled by adjusting the following parameters: 1. The proportion of polycarbonate diol in component B1 (e.g., 15%–35%) can adjust the polarity, compatibility, and hygrothermal stability of the optical adhesive.

[0084] 2. The amount of disulfide bond extender (e.g., 1% to 8%) can adjust the stress dissipation ability and flexibility of the optical adhesive.

[0085] 3. The mixing ratio of B1 / B2 components (e.g., 1:2-2:1) can adjust the balance of crosslinking density, modulus and cohesive strength of optical adhesive.

[0086] 4. The total amount of component B (e.g., 10% to 25%) can adjust the overall crosslinking density of the optical adhesive.

[0087] In summary, the raw materials for the optical adhesive provided in this application embodiment may include the following components in parts by weight: 100 parts of acrylate prepolymer and 10-25 parts of polyurethane prepolymer. By using acrylate prepolymer and polyurethane prepolymer in the raw materials of the optical adhesive, the side chains of the acrylate prepolymer have hydroxyl and / or carboxylic acid groups, and the end groups of each polyether polyurethane prepolymer are isocyanate groups. The polyether polyurethane prepolymer can react with the acrylate prepolymer to form a crosslinked network. The polyether polyurethane prepolymer has a polyether flexible segment structure, which can improve the bending resistance of the optical adhesive. The polyurethane prepolymer is formed by compounding at least two polyether polyurethane prepolymers with different functionalities, which can provide polyether polyurethane prepolymers with various structures such as linear and branched types, which can not only improve the flexibility of the optical adhesive but also increase the crosslinking density.

[0088] Below, this application provides some specific embodiments for comparison and illustration to demonstrate the feasibility of the optical adhesive provided in the above embodiments.

[0089] First, the basic raw materials are synthesized.

[0090] The first raw material is used for the synthesis of acrylate prepolymer, denoted as component A.

[0091] In a 1L reactor equipped with a stirrer, thermometer, condenser, and nitrogen inlet pipe, 700g of butyl acrylate, 200g of methyl acrylate, 50g of hydroxyethyl acrylate, 30g of acrylic acid, 500g of ethyl acetate, and 40g of toluene were added. Nitrogen gas was purged for 30 minutes to maintain the nitrogen atmosphere, and the mixture was heated to a constant temperature of 66℃~68℃. 0.3g of azobisisobutyronitrile (AIBN) was added, and the reaction was carried out at 65~68℃ for 2 hours. Another 0.3g of AIBN was added, and the temperature was raised to 73~76℃ and held for 2 hours. Finally, the remaining 0.3g of AIBN was added dropwise, and the temperature was raised to above 77℃ and held for 1.5 hours. After the reaction was complete, the mixture was cooled to below 60℃, and the remaining solvent was added. After stirring until homogeneous, the mixture was discharged to obtain the acrylate prepolymer.

[0092] According to gel permeation chromatography (GPC), the number average molecular weight (Mn) of the acrylate prepolymer was 108,000, the molecular weight distribution (PDI) was 4.1, and the solid content was 35%.

[0093] The second raw material is used to synthesize the first type of polyether polyurethane prepolymer. The B1 component of this type can be referred to as the B1-0 component.

[0094] Under dry nitrogen protection, 600g of polypropylene glycol (PPG-2000) with a number average molecular weight of 2000 was added to the reactor, and the mixture was heated to 110℃ and vacuum dehydrated for 2 hours (vacuum degree ≤ -0.095MPa). The temperature was then lowered to 80℃, and 160g of H12MDI (dicyclohexylmethane diisocyanate) was added. The temperature was slowly raised to 120±2℃, and the reaction was carried out for 2 hours. The NCO content in the system was monitored until it reached the preset value (approximately 3.3%). The mixture was then cooled, discharged, and sealed for storage to obtain the first polyether polyurethane prepolymer, i.e., component B1-0, which does not contain polycarbonate glycol or disulfide chain extender.

[0095] The third raw material is used to synthesize the second type of first polyether polyurethane prepolymer. This type of B1 component can be referred to as the B1-DS component.

[0096] Under dry nitrogen protection, 450g of polypropylene glycol (PPG) and 150g of polycarbonate glycol (Mn approximately 2000) were separately dehydrated and then mixed (polycarbonate glycol accounted for 25% of the total hydroxyl equivalent of the B1 soft segment); 1.39g of 2,2′-dithiodiethanol (HEDS) (equivalent to 3% of the total hydroxyl equivalent of PPG / polycarbonate glycol) was added, and the mixture was vacuum dehydrated at 110℃ for 2 hours (vacuum degree ≤ -0.095MPa). The mixture was then cooled to 80℃, and approximately 162g of H12MDI (total NCO / OH approximately 2.0:1) was added. The mixture was reacted at 120±2℃ for 3 hours under nitrogen protection, with the final NCO content controlled to 3.0~3.6% using the dibutylamine back-dropping method. After the reaction was completed, the mixture was cooled and discharged, then vacuum-sealed for storage to obtain the first polyether polyurethane prepolymer B1-DS.

[0097] The fourth raw material is used to synthesize the second polyether polyurethane prepolymer, denoted as component B2.

[0098] Under dry nitrogen protection, 600g of polypropylene triol (hydroxyl value 56mgKOH / g, functionality 3) with a number average molecular weight of approximately 3000 was added to the reactor, and the mixture was heated to 110℃ and vacuum dehydrated for 2 hours (vacuum degree ≤ -0.095MPa). The temperature was then lowered to 80℃, and HMDI (NCO / OH molar ratio 2.1:1) was added. The temperature was slowly raised to 120±2℃, and the reaction was carried out for 2-3 hours. The NCO content was monitored until it reached the preset value, then the mixture was cooled, discharged, and sealed for storage to obtain the second polyether polyurethane prepolymer.

[0099] Then, the four raw materials mentioned above were combined to obtain various embodiments.

[0100] Example 1 Take 1000g of component A (containing 350g of solids), add 52.5g of component B1-0 (equivalent to 15% of the solids of component A), add 1.5g of antioxidant, add an appropriate amount of ethyl acetate to dilute to a viscosity suitable for coating, stir evenly, and vacuum degas for 15 minutes to obtain the optical adhesive composition.

[0101] The composition was coated on a release film with a thickness of 50 micrometers, and the dry adhesive thickness was controlled to be 100 micrometers. It was then heat-cured in a forced-air oven at 120°C for 5 minutes. After heat curing, another release film was covered and cured at 55°C for 3 days to obtain an optical adhesive film. The resulting sample was denoted as S1.

[0102] Example 2 Take 1000g of component A (containing 350g of solids), add 35.0g of component B1-0 (equivalent to 10% of the solids in component A), add 1.5g of antioxidant, and dilute with an appropriate amount of ethyl acetate to a viscosity suitable for coating. Stir evenly and degas under vacuum for 15 minutes to obtain the optical adhesive composition. The film-forming conditions are the same as in Example 1, and the resulting sample is designated as S2.

[0103] Example 3 Take 1000g of component A (containing 350g of solids), add 87.5g of component B1-0 (equivalent to 25% of the solids in component A), add 1.5g of antioxidant, and dilute with an appropriate amount of ethyl acetate to a viscosity suitable for coating. Stir evenly and degas under vacuum for 15 minutes to obtain the optical adhesive composition. The film-forming conditions are the same as in Example 1, and the resulting sample is designated as S3.

[0104] In other words, the optical molds of samples S1 to S3 all contain component A and component B1-0, but do not contain component B2, and the proportion of component B1-0 is different.

[0105] Example 4 Take 1000g of component A (containing 350g of solids), add 52.5g of component B2 (equivalent to 15% of the solids in component A), add 1.5g of antioxidant, and dilute with an appropriate amount of ethyl acetate to a viscosity suitable for coating. Stir evenly and degas under vacuum for 15 minutes to obtain the optical adhesive composition. The film-forming conditions are the same as in Example 1, and the resulting sample is designated as S4. That is, the optical adhesive of sample S4 contains components A and B2, but does not contain component B1.

[0106] Example 5 Take 1000g of component A (containing 350g of solids), add 26.25g of component B1-0 and 26.25g of component B2 (B1-0 / B2 = 1:1, the total amount added is equivalent to 15% of the solids in component A), add 1.5g of antioxidant, and dilute with an appropriate amount of ethyl acetate to a viscosity suitable for coating. Stir evenly and degas under vacuum for 15 minutes to obtain the optical adhesive composition. The film-forming conditions are the same as in Example 1, and the resulting sample is designated as S5. That is, the optical adhesive of sample S5 contains component A, component B1-0, and component B2.

[0107] Example 6 (S6: B1-DS / B2 = 1:1 compound, total amount 15%, optimal example) Take 1000g of component A (containing 350g of solids), add 26.25g of component B1-DS and 26.25g of component B2 (B1-DS / B2 = 1:1, the total amount added is equivalent to 15% of the solids in component A), add 1.5g of antioxidant, and dilute with an appropriate amount of ethyl acetate to a viscosity suitable for coating. Stir evenly and degas under vacuum for 15 minutes to obtain the optical adhesive composition. The film-forming conditions are the same as in Example 1, and the resulting sample is designated as S6. That is, the optical adhesive of sample S6 contains component A, component B1-DS, and component B2. The difference from sample S5 is that component B1-DS contains polycarbonate diol and disulfide chain extender.

[0108] Comparative Example 1 Take 1000g of component A (containing 350g of solids), without adding components B1 / B2, add 1.5g of antioxidant, and dilute with an appropriate amount of ethyl acetate to a viscosity suitable for coating. Stir evenly and degas under vacuum for 15 minutes to obtain the optical adhesive composition. The film-forming conditions are the same as in Example 1, and the resulting sample is designated as D1.

[0109] Comparative Example 2 Take 1000g of component A (containing 350g of solids), replace component B1-0 with a small molecule isocyanate curing agent (HMDI, added in the same molar amount of NCO as in Example 1) with the same NCO equivalent, add 1.5g of antioxidant, and dilute with an appropriate amount of ethyl acetate to a viscosity suitable for coating. Stir evenly and degas under vacuum for 15 minutes to obtain the optical adhesive composition. The film-forming conditions are the same as in Example 1, and the resulting sample is designated as D2.

[0110] Comparative Example 3 When synthesizing the acrylate prepolymer, no functional monomers containing hydroxyl / carboxylic acid groups were added (i.e., only 750g of butyl acrylate and 230g of methyl acrylate were polymerized, with other conditions the same as the synthesis steps of component A above). Then, 1000g of this prepolymer (containing 350g of solids) was taken, and 52.5g of component B1-0 (equivalent to 15% of the solids) was added. 1.5g of antioxidant was added, and an appropriate amount of ethyl acetate was added to dilute to a viscosity suitable for coating. The mixture was stirred evenly, vacuum degassed for 15 minutes, and then coated and cured under the same film-forming conditions as in Example 1. The resulting sample was designated D3.

[0111] Comparative Example 4 An existing general-purpose optical adhesive (acrylate-based, suitable for rigid displays) was selected as a comparison sample and denoted as D4.

[0112] Various performance tests were conducted on the samples S1 to S6 and D1 to D4, including optical properties, adhesive properties, gel content, dynamic mechanical properties, flexural strength, and aging resistance.

[0113] For example, the following testing standards can be used: 1. Optical performance Transmittance and haze: According to ASTM D1003 standard, haze meter was used for testing. The sample size was 50mm×50mm, and it was tested on a glass slide. The average value of 3 tests was taken.

[0114] Yellowing index: According to ASTM E313 standard, the initial b value and the b value after aging are tested using a colorimeter, and Δb is calculated.

[0115] 2. Adhesive performance 180° peel strength: According to GB / T 2792-2014 standard, the optical film was adhered to a clean glass plate and pressed back and forth three times with a 2kg roller. After 24 hours, it was tested with a universal testing machine at a peel speed of 300mm / min and a sample width of 25mm. The average value of the three tests was taken.

[0116] Initial tack: Tested using the inclined plane rolling ball method according to GB / T 4852-2002 standard.

[0117] Holding power: Tested according to GB / T 4851-2014 standard at 40℃ and 1kg load, and the time for sample slippage and detachment was recorded.

[0118] 3. Gel content test Weigh a certain mass (W1) of optical film, wrap it in filter paper, place it in a Soxhlet extractor, reflux extract it with toluene as solvent for 12 hours, take out the residue and dry it to constant weight (W2), and calculate the gel content = W2 / W1×100%.

[0119] 4. Dynamic mechanical properties Energy storage modulus: The energy storage modulus of the film at 25℃ was tested using a dynamic mechanical analyzer in tensile mode, with a temperature range of -60℃ to 100℃, a heating rate of 3℃ / min, and a frequency of 1Hz.

[0120] 5. Bending resistance Dynamic bending test: The optical adhesive film is bonded to a 50μm thick transparent polyimide (CPI) film to make a 5cm×10cm test strip. The inward bending test is carried out using a folding life tester under the conditions of R=3mm and frequency of 30 times / minute. The appearance of the sample is observed every 50,000 times, and the number of bends when creases or delamination occur is recorded.

[0121] 6. Aging resistance High temperature and high humidity aging: According to JIS K5600-7-7 standard, the sample was placed in a constant temperature and humidity chamber of 85℃ / 85% RH. After 500 hours, the sample was taken out and the appearance changes were observed. The optical properties and peel strength retention rate were tested.

[0122] Thermal shock test: According to IEC 60068-2-14 standard, maintain the temperature at -40℃ to 85℃ for 30 minutes each, cycle 100 times, and observe the changes in the appearance of the sample.

[0123] It should be noted that the above testing standards are provided as examples. In the embodiments of this application, the following test data tables can be obtained through the above testing methods. Table 1 contains four test data items: optical performance, adhesive performance, gel content test, and dynamic mechanical performance. Table 2 contains aging resistance data, and Table 3 contains bending resistance data.

[0124]

[0125]

[0126]

[0127] Based on the above test data, the performance of the photoresist provided in this application embodiment is related to the following parameters.

[0128] Firstly, the effect of the amount of the first polyether polyurethane prepolymer on the performance of the optical adhesive can be seen by referring to the test data of samples S1, S2 and S3.

[0129] As the amount of component B1-0 increased from 10% (S2) to 15% (S1) and then to 25% (S3), the gel content increased from 78.6% to 85.3% and then to 92.1%, and the storage modulus increased from 5.6 × 10⁻⁶. 4 Pa rose to 8.2 × 10 4Pa then increased to 1.6 × 10 5 Pa allows for a wide range of modulus control from low to medium. In terms of bending resistance, S3 is the best (no abnormalities after 250,000 cycles, slight creases after 300,000 cycles), followed by S1 (no abnormalities after 200,000 cycles), while S2 shows creases after 150,000 cycles.

[0130] Secondly, the influence of the functionality of polyurethane prepolymer B on the performance of optical adhesives can be seen by referring to the test data of samples S1, S4 and S5.

[0131] Gel content: S4 (91.5%) > S5 (89.3%) > S1 (85.3%); Storage modulus: S4 (1.8 × 10⁻⁶) > S5 (89.3%) > S1 (85.3%); 5 Pa) > S5 (1.2×10 5 Pa) > S1 (8.2×10 4 Pa).

[0132] In terms of bending resistance, S5 is the best (no abnormalities after 250,000 cycles, slight creases after 300,000 cycles). It can be seen that the polyurethane prepolymer B obtained by compounding the first polyether polyurethane prepolymer B1 with the second polyether polyurethane prepolymer B1 has a functionality between 2 and 3, achieving the best balance between crosslinking density and chain segment flexibility.

[0133] Thirdly, the influence of polycarbonate diol and disulfide bond extender in polyurethane prepolymer B on the performance of optical adhesive can be seen by referring to the test data of samples S3, S5 and S6.

[0134] The energy storage modulus of S6 at 25℃ is 1.6×10⁻⁶. 5 Pa, and S3 (1.6×10 5 The value is comparable to that of S5 (1.2 × 10 Pa), and higher than that of S5 (1.2 × 10 Pa). 5 Pa). The reasons are: (1) The carbon group (-O-CO-O-) of the polycarbonate diol chain segment is more polar, the intermolecular interaction is increased, and the chain segment movement is restricted; (2) The disulfide bond chain extender increases the chain segment density in the cross-linked network.

[0135] Therefore, the introduction of polycarbonate diol did not reduce the modulus; its core function was to improve hygrothermal stability and cohesive strength, rather than reduce the modulus. Modulus control was mainly achieved through the B1 / B2 self-ignition blending ratio and total dosage.

[0136] Compared to sample S5, S6, despite an increased modulus, still achieved a 10.1% increase in peel strength, a 50,000-cycle extension in flexural strength, a 3.0% improvement in damp heat aging retention, and a 42.9% reduction in yellowing. This demonstrates that the limited introduction of polycarbonate glycol and disulfide chain extender (25% polycarbonate glycol, 3% disulfide) improves cohesive strength, damp heat stability, and stress dissipation capacity without compromising flexural performance, even with a moderate increase in modulus. Component B of S6, at a low dosage of 15%, achieved superior flexural life and damp heat stability compared to S3 (25% high dosage) at the same modulus. The chemical structure design of the polycarbonate glycol / disulfide chain extender is more efficient than simply increasing the dosage of component B.

[0137] In sample S6, the polycarbonate diol content was 25%, which significantly improved hygrothermal stability and maintained controllable modulus. Testing showed that when the polycarbonate diol content exceeded 30%, the carbonate groups became excessively dense, leading to a sharp increase in modulus and a decrease in flexibility. A disulfide bond content of 3% resulted in sufficient stress dissipation and controllable yellowing (Δb). =0.4). Tests showed that when the disulfide bond content was higher than 5%, the sulfur content in the system increased, and the yellowing worsened after high-temperature and high-humidity aging.

[0138] As can be seen from samples S1 to S5, the optical adhesive using the B1-0 / B2=1:1 compound has better performance than the optical adhesive using only component B1 or component B2, which proves the synergistic effect of hierarchical macromolecular cross-linking topology. Sample S5 achieved 250,000 cycles without abnormalities and 300,000 cycles with slight creases at a low dosage.

[0139] Compared to sample S5, sample S6, based on the combination of components B1 and B2, improves the hygrothermal stability and cohesive strength by adding polycarbonate diol to component B1, and provides dynamic stress dissipation through disulfide chain extender, achieving a bending life of 350,000 cycles.

[0140] Excessive content of polycarbonate diol and disulfide chain extender can negatively impact the performance of optical adhesives. The recommended content range for polycarbonate diol is 20%–30%, and for disulfide chain extender, it is 2%–5%. Exceeding these ranges can lead to excessively high modulus or worsened yellowing, which will negate any potential gains.

[0141] In summary, the optical adhesives provided in this application, such as samples S5 and S6 above, utilize a polyether-type polyurethane prepolymer as a macromolecular crosslinking agent. This polyether soft segment can lower the glass transition temperature of the optical adhesive film, thereby improving its flexibility. The tensile modulus of the optical adhesive film can reach 5 × 10⁻⁶. 4 ~1.6×10 5 With adjustable pressure within the Pa range, it showed no delamination or creases after 200,000 dynamic bending tests, meeting the durability requirements of flexible display devices such as foldable screen phones.

[0142] The intrinsic optical advantages of the polyacrylate backbone are preserved, and the polyether segments exhibit good compatibility with acrylate, avoiding light scattering caused by microphase separation. The resulting optical film has a total light transmittance of ≥92% and a haze of ≤0.5%, meeting the optical requirements of high-end display devices.

[0143] The polyether segment exhibits superior hydrolytic stability compared to the polyester segment, and the choice of aliphatic or alicyclic isocyanate avoids yellowing issues. After 500 hours of high-temperature and high-humidity aging at 85℃ / 85% RH, the resulting product retains >90% of its optical and adhesive properties, with a yellowing index Δb. <1.0.

[0144] It adopts a step-by-step synthesis-blending-thermal curing process, which is compatible with existing coating production lines, requires no special equipment modification, and is easy to industrialize.

[0145] This application also provides an optical adhesive film, please refer to... Figure 1 , Figure 1 This is a schematic diagram of the film layers of the optical adhesive film according to an embodiment of this application. The optical adhesive film 100 may include: an optical adhesive layer 103, and a first release film 101 and a second release film 102 adhered to both sides of the optical adhesive layer; the optical adhesive layer 103 is prepared from the optical adhesive described in any of the above embodiments.

[0146] The optical adhesive provided in the above embodiments can be an optical adhesive liquid, and the optical adhesive layer 103 can be an optical adhesive layer obtained by curing the optical adhesive provided in the above embodiments.

[0147] The optical adhesive layer 103 is in the form of double-sided adhesive. By providing a first release film 101 and a second release film 102 on its opposite bonding surfaces, the bonding surfaces of the optical adhesive layer 103 can be protected by the first release film 101 and the second release film 102. This facilitates the storage of the optical adhesive layer 103 and ensures that it always maintains stable adhesion performance.

[0148] This application also provides a display device, please refer to... Figure 2 , Figure 2 This is a schematic diagram of the structure of a display device according to an embodiment of this application. The display device 200 may include: a display module 201 and a protective cover plate 202, and an optical adhesive layer 103 located between the display module 201 and the protective cover plate 202. The optical adhesive layer 103 is prepared by the optical adhesive described in any of the above embodiments, or the optical adhesive layer 103 may include the optical adhesive layer 103 in the optical adhesive film 100 described in the above embodiments.

[0149] Please refer to some possible implementation methods. Figure 3 , Figure 3This is another structural schematic diagram of the display device according to an embodiment of this application. The display device 200 may further include: a functional film layer 203, and an optical adhesive layer 103 may also be used for bonding any two adjacent structures among the display module 201, the protective cover plate 202, and the functional film layer 203. The functional film layer includes, but is not limited to: a touch module, a polarizer, etc. Since the optical adhesive layer 103 has good adaptability to micro-step structures, the optical adhesive layer 103 can fill the micro-steps present at the edge of the touch module, ensuring that the optical adhesive layer 103 is fully adhered, avoiding the generation of optical shadows or bubbles, thereby improving the display stability of the display device 200.

[0150] In some possible implementations, the protective cover 202 may also be a cover with an integrated functional film layer. For example, the protective cover 202 may include a glass cover and a touch layer located on one side of the glass cover, so that the protective cover 202 can integrate touch functionality.

[0151] In the embodiments of this application, it should be noted that the display panel of the display module provided in this application can be an organic light-emitting diode (OLED) display panel, or it can be a QLED display panel that uses quantum dot light-emitting diodes (QLED) to achieve the display function, or it can be a QD-OLED display panel that uses quantum dot organic light-emitting diodes (QD-OLED) to achieve the display function, or it can be a liquid crystal display (LCD) display panel. This application does not impose any restrictions on this.

[0152] For example, when the display panel of the display module 201 is a foldable or rollable display panel, the protective cover 202 is a flexible protective cover.

[0153] In this embodiment, the optical adhesive significantly reduces its modulus by introducing polyether-type polyurethane segments, thereby improving the flexibility and bending resistance of the optical adhesive film while maintaining high light transmittance and low haze. The optical adhesive exhibits stable performance over a wide temperature range of -40℃ to 85℃, making it particularly suitable for bonding and assembling flexible display devices such as foldable screen phones and rollable screen TVs. This solves the problem of existing optical adhesives easily developing creases and delamination during dynamic bending.

[0154] The display device can be a screen in a display device such as a mobile phone, tablet computer, laptop computer, monitor, or smart TV. Since the display device can have essentially the same technical effects as the optical adhesive described in the previous embodiments, for the sake of brevity, the technical effects of the display device will not be repeated here.

[0155] In this application, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance. The term "multiple" refers to two or more unless otherwise expressly defined.

[0156] In readable storage media, the aforementioned storage media can be read-only memory, disk, or optical disk, etc.

[0157] The above description is merely an optional embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.

Claims

1. An optical adhesive, characterized in that, The raw material of the optical adhesive comprises the following components in parts by weight: 100 parts of acrylate prepolymer and 10-25 parts of polyurethane prepolymer; The acrylate prepolymer has hydroxyl and / or carboxylic acid groups on its side chains; the polyurethane prepolymer is formed by compounding at least two polyether polyurethane prepolymers with different functionalities, and the end groups of each polyether polyurethane prepolymer are isocyanate groups.

2. The optical adhesive according to claim 1, characterized in that, The polyurethane prepolymer comprises: a first polyether polyurethane prepolymer and a second polyether polyurethane prepolymer; The first polyether polyurethane prepolymer is a linear polyether polyurethane prepolymer, and the second polyether polyurethane prepolymer is a branched polyether polyurethane prepolymer; the first polyether polyurethane prepolymer and the second polyether polyurethane prepolymer have different functionalities.

3. The optical adhesive according to claim 2, characterized in that, The functionality of the first polyether polyurethane prepolymer is less than that of the second polyether polyurethane prepolymer; The mass ratio of the first polyether polyurethane prepolymer to the second polyether polyurethane prepolymer is 1:2-2:

1.

4. The optical adhesive according to claim 3, characterized in that, The raw materials for the first polyether polyurethane prepolymer include the following components: The polyether diol and the polyisocyanate, wherein the molar ratio of the isocyanate group of the polyisocyanate to the hydroxyl group of the polyether diol is greater than or equal to 2:

1.

5. The optical adhesive according to claim 4, characterized in that, The number average molecular weight of the polyether diol is 1000-4000; and / or, the polyisocyanate includes: alicyclic diisocyanate.

6. The optical adhesive according to claim 5, characterized in that, The polyether diol includes at least one of polypropylene glycol and polytetrahydrofuran ether diol; And / or, the alicyclic diisocyanate includes at least one of isophorone diisocyanate and dicyclohexylmethane diisocyanate.

7. The optical adhesive according to claim 4, characterized in that, The raw materials for the first polyether polyurethane prepolymer also include the following components: The polycarbonate diol and disulfide chain extender are present, wherein the polycarbonate diol accounts for 15%-35% of the total hydroxyl equivalent in the first polyether polyurethane prepolymer, and the disulfide chain extender accounts for 1%-8% of the total hydroxyl equivalent in the first polyether polyurethane prepolymer.

8. The optical adhesive according to claim 7, characterized in that, The polycarbonate diol has a number average molecular weight of 1500 to 2500, and / or the disulfide chain extender includes 2,2′-dithiodiethanol.

9. The optical adhesive according to any one of claims 2-8, characterized in that, The raw materials for the second polyether polyurethane prepolymer include the following components: The polyether triol and the polyisocyanate; the molar ratio of the isocyanate group of the polyisocyanate to the hydroxyl group of the polyether triol is greater than or equal to 2:

1.

10. The optical adhesive according to claim 9, characterized in that, The number average molecular weight of the polyether triol is 1000-4000; and / or, the polyisocyanate includes: alicyclic diisocyanate.

11. The optical adhesive according to claim 10, characterized in that, The polyether triol includes: polypropylene oxide triol; And / or, the alicyclic diisocyanate includes at least one of isophorone diisocyanate and dicyclohexylmethane diisocyanate.

12. The optical adhesive according to any one of claims 1-8 and 10-11, characterized in that, The raw materials for the acrylate prepolymer include the following components: Acrylate functional monomers containing hydroxyl and / or carboxylic acid groups.

13. The optical adhesive according to claim 12, characterized in that, The raw materials for the acrylate prepolymer also include the following components: The acrylate soft monomer and the acrylate hard monomer, wherein the mass fraction of the acrylate soft monomer is greater than the mass fraction of the acrylate hard monomer, and the mass fraction of the acrylate hard monomer is greater than the mass fraction of the acrylate functional monomer.

14. An optical adhesive film, characterized in that, The optical adhesive film comprises: an optical adhesive layer, and a first release film and a second release film adhered to both sides of the optical adhesive layer; the optical adhesive layer is prepared from the optical adhesive according to any one of claims 1-13.

15. A display device, characterized in that, The display device includes: a display module and a protective cover plate, and an optical adhesive layer located between the display module and the protective cover plate; the optical adhesive layer is prepared from the optical adhesive of any one of claims 1-13, or the optical adhesive layer includes the optical adhesive layer in the optical adhesive film of claim 14.