A cationic photocurable epoxy adhesive, its preparation method and application

By combining a specific structure of bis(3-glycidoxy-2-hydroxypropyl) linear fatty ester and a chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate) titanium(IV) metal adhesive, the problems of poor adhesion to metal substrates and poor high-temperature and low-temperature reliability of traditional cationic photocurable epoxy adhesives are solved, achieving high-strength multi-substrate adhesion and improved impact resistance.

CN123107599APending Publication Date: 2026-11-17XIAMEN WELDTONE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611526002.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional cationic photocurable epoxy adhesives have poor adhesion to metal substrates such as stainless steel, copper, and aluminum, cannot adapt to multi-substrate bonding, and have poor bonding reliability under high and low temperature environments, easily leading to interface delamination and bonding failure.

Method used

A cationic photocurable epoxy adhesive is formed by combining a specific structure of bis(3-glycidoxy-2-hydroxypropyl) linear fatty ester and chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate) titanium(IV) metal adhesive with alicyclic epoxy resin, core-shell rubber toughening particles, polyol, cationic photoinitiator, photosensitizer, and silane coupling agent. This combination enhances the adhesion of metal substrates and the adaptability to multiple substrates, and improves the resistance to high and low temperature cyclic impact.

Benefits of technology

It significantly improves the bonding strength to metal substrates and the bonding effect of multiple substrates, has excellent resistance to high and low temperature cycling impact, quickly establishes initial bonding strength, reduces internal stress, and adapts to high and low temperature environmental changes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_6
    Figure SMS_6
Patent Text Reader

Abstract

This invention belongs to the field of epoxy adhesive technology, specifically relating to a cationic photocurable epoxy adhesive, its preparation method, and its application. The cationic photocurable epoxy adhesive comprises: an alicyclic epoxy resin, a bis(3-glycidoxy-2-hydroxypropyl) linear fatty diacid ester as shown in formula (I), core-shell rubber toughening particles, a polyol, an inorganic filler, a cationic photoinitiator, a photosensitizer, a chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate) titanium (IV) as shown in formula (II), and a silane coupling agent. This invention innovatively introduces a compound of bis(3-glycidoxy-2-hydroxypropyl) linear fatty diacid ester, chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate) titanium (IV), and a core-shell rubber toughening agent, providing a cationic photocurable epoxy adhesive suitable for multiple substrates, exhibiting high adhesion and good high and low temperature cycling reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of epoxy adhesive technology, specifically relating to a cationic photocurable epoxy adhesive, its preparation method, and its application. Background Technology

[0002] Cationic photocurable epoxy adhesives offer advantages such as low curing shrinkage and good bonding stability, making them widely used in electronic device bonding, optoelectronic packaging, and other fields. With the continuous updating of electronic device packaging structures, the requirements for adhesives are also constantly increasing: the need for bonding between different substrate materials; and high bonding reliability to withstand high-temperature and low-temperature environmental changes. However, traditional cationic photocurable epoxy adhesives have significant drawbacks: firstly, poor bonding performance to metal substrates such as stainless steel, copper, and aluminum, leading to unsatisfactory results when bonding structures involving multiple substrate types; secondly, high internal stress after curing results in poor reliability under high / low temperature cycling, easily leading to interface delamination and bonding failure. Existing solutions to this problem generally involve adding core-shell rubber for toughening, but this can only be physically dispersed in the resin, with limited addition amounts and low toughening efficiency. Excessive addition can lead to high adhesive viscosity and the risk of phase separation, severely affecting the application process performance. Therefore, the industry urgently needs to develop a cationic photocurable epoxy adhesive with high metal bonding strength, adaptability to multi-substrate bonding, and good resistance to thermal shock. Summary of the Invention

[0003] One of the objectives of this invention is to address the problems of existing cationic photocurable epoxy adhesives, such as poor adhesion to metal substrates, inability to adapt to multi-substrate bonding, and poor bonding reliability under high-temperature and low-temperature environments. This invention provides a cationic photocurable epoxy adhesive to overcome these problems.

[0004] Specifically, the raw material components of the cationic epoxy adhesive include: alicyclic epoxy resin, bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, core-shell rubber toughening particles, polyol, inorganic filler, cationic photoinitiator, photosensitizer, chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) metal adhesive, and silane coupling agent; the cationic photoinitiator is a ferrocene salt compound and an onium salt compound; The bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester has the structure shown in formula (I): Formula (I), In equation (I), n is an integer from 2 to 12; The chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) has the structure shown in formula (II): Ti(OR1)2(OOC-Ar-COO-R2-EPO)2 formula (II), In formula (II), R1 is a C1~C4 alkyl group, Ar is a phenylene group, R2 is a C2~C6 alkylene group, EPO represents a group structure of -O-R3-CH(O)CH2, and R3 is a C1~C4 alkylene group.

[0005] The second objective of this invention is to provide a method for preparing the aforementioned cationic photocurable epoxy adhesive. The preparation method includes: mixing an alicyclic epoxy resin, bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, core-shell rubber toughening particles, a polyol, an inorganic filler, a cationic photoinitiator, a photosensitizer, a chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) metal adhesive, and a silane coupling agent; the resulting mixture is the cationic photocurable epoxy adhesive.

[0006] A third objective of this invention is to provide the application of the above-mentioned cationic photocurable epoxy adhesive in the bonding of electronic device structures, the encapsulation of optoelectronic components, and the composite bonding of ink or metal substrates with plastic substrates.

[0007] Beneficial effects: The key to this invention lies in the creative introduction of a bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester with a specific structure and a chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate) titanium(IV) metal adhesive, which is then combined with alicyclic epoxy resin, core-shell rubber toughening particles, polyol, cationic photoinitiator, photosensitizer, and silane coupling agent. The resulting cationic photocurable epoxy adhesive has significantly enhanced adhesion to metal substrates and is suitable for bonding multiple substrates. It also exhibits excellent high-low temperature cycling impact resistance after curing. The main reasons are as follows: Firstly, the molecular skeleton of bis(3-glycidoxy-2-hydroxypropyl) linear fatty diacid ester contains multiple methylene flexible segments, which can work together with core-shell rubber toughening particles to improve the toughening effect, rapidly increase the elongation at break of the cured colloid, effectively reduce the crosslinking internal stress of the cationic photocurable adhesive layer, and improve the resistance to high-low temperature cycling impact. At the same time, because its molecular chain contains two secondary hydroxyl groups, the hydroxyl groups can act as proton donors to accelerate the ring-opening polymerization of cationic epoxy and increase the photocuring rate. Moreover, bis(3-glycidoxy-2-hydroxypropyl) linear fatty diacid ester does not contain aromatic benzene ring structures, and has the advantage of low yellowing when used in UV cationic epoxy photocurable adhesives. Secondly, compared with ordinary titanate coupling agents on the market, the chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate) titanium(IV) provided by this invention has epoxy groups, which can covalently bond and The epoxy crosslinking network is incorporated, and its structure also introduces aromatic rings and ether bonds and alkyl chains between the aromatic rings and epoxy groups. The aromatic rings enhance thermal stability and adhesive strength, the ether bonds improve resin compatibility and participate in cationic curing, and the alkyl chains reduce epoxy steric hindrance and buffer interfacial stress, achieving covalent bridging between the filler and the resin matrix. This improves the heat resistance, moisture resistance, and adhesive performance of the UV-curable adhesive. Combined with the role of Ti sites in anchoring the metal substrate, an organic matrix-titanium coordination layer-metal substrate transition layer is formed, which is beneficial to significantly improve the adhesive strength of epoxy adhesives on metal substrates such as copper and aluminum. In addition, the cationic photoinitiator, which is a compound of ferrocene salts and onium salts, can significantly improve the responsiveness of the adhesive to long-wavelength light sources of 400~600nm. It can trigger a highly efficient cationic ring-opening polymerization reaction under low energy conditions, greatly improving the curing reaction rate and achieving rapid establishment of high initial adhesive strength after UV irradiation, while achieving complete surface drying. In summary, the cationic photocurable epoxy adhesive provided by this invention, through the synergistic effect of bis(3-glycidoxy-2-hydroxypropyl) linear fatty ester, core-shell rubber toughening particles, and chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate) titanium(IV), endows the adhesive with high toughness and high bonding strength, achieving high adhesion to multiple substrates such as inks and metals, and exhibiting excellent high and low temperature cycling reliability. Detailed Implementation

[0008] The embodiments of the present invention are described in detail below. The embodiments described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. Furthermore, unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of the present invention.

[0009] The raw material components of the cationic photocurable epoxy adhesive provided by this invention include: alicyclic epoxy resin, bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, core-shell rubber toughening particles, polyol, inorganic filler, cationic photoinitiator, photosensitizer, chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) metal adhesive, and silane coupling agent; wherein the cationic photoinitiator is a ferrocene salt compound and an onium salt compound.

[0010] The bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester has the structure shown in formula (I): Formula (I), In equation (I), n is an integer from 2 to 12. Specifically, n can be 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12.

[0011] The chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) has the structure shown in formula (II): Ti(OR1)2(OOC-Ar-COO-R2-EPO)2 formula (II), In formula (II), R1 is a C1-C4 alkyl group, Ar is a phenylene group, R2 is a C2-C6 alkylene group, EPO represents the group structure -O-R3-CH(O)CH2, and R3 is a C1-C4 alkylene group. The C1-C4 alkyl group can be any one of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, or tert-butyl. A phenylene group is a divalent phenyl group, meaning it has two sites on its structure that can form bonds with other groups. The phenylene group can be ortho-phenylene, meta-phenylene, or para-phenylene. The C2-C6 alkylene group can be any one of methylene, ethylene, propylene, butylene, pentylene, or hexylene. The C1-C4 alkylene group can be any one of methylene, ethylene, propylene, or butylene.

[0012] In this invention, the content of the alicyclic epoxy resin is preferably 30-50 wt%, such as 30 wt%, 32 wt%, 35 wt%, 38 wt%, 40 wt%, 42 wt%, 45 wt%, 48 wt%, 50 wt%, or any value between them. The content of the bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester is preferably 5-20 wt%, such as 5 wt%, 8 wt%, 10 wt%, 12 wt%, 15 wt%, 18 wt%, 20 wt%, or any value between them. The content of the core-shell rubber toughening particles is preferably 5-20 wt%, such as 5 wt%, 8 wt%, 10 wt%, 12 wt%, 15 wt%, 18 wt%, 20 wt%, or any value between them. The content of the polyol is preferably 5-15 wt%, such as 5 wt%, 8 wt%, 10 wt%, 12 wt%, 15 wt%, or any value between them. The content of the inorganic filler is preferably 5-15 wt%, such as 5 wt%, 8 wt%, 10 wt%, 12 wt%, 15 wt%, or any value between them. The content of the cationic photoinitiator is preferably 1-5 wt%, such as 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, or any value between them. The content of the photosensitizer is preferably 1-5 wt%, such as 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, or any value between them. The content of the chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) metal adhesive is preferably 0.1-5 wt%, such as 0.1 wt%, 0.5 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, or any value between them. The content of the silane coupling agent is preferably 0.1-5 wt%, such as 0.1 wt%, 0.5 wt%, 1 wt%, 2 wt%, 3 wt%, 4 wt%, 5 wt%, or any value between them.

[0013] In this invention, there are no particular restrictions on the specific structure and source of the alicyclic epoxy resin. It can be a commercially available product or a product prepared by existing methods. Specific examples can be selected from any one or more of the following products: CELLOXIDE 2021P (Daicel Ltd., Japan), TDE-85 (4,5-epoxycyclohexane-1,2-dicarboxylic acid diglycidyl ester), Dow CYRACURE™ UVR-6128 (from Dow Chemical), UVR-6110 (3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexylcarboxylate), and EHPE 3150 (Daicel Ltd., Japan).

[0014] In this invention, the bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester is preferably prepared by the following method: S1. Glycerol was mixed with halopropylene oxide and subjected to a ring-opening etherification reaction in the presence of catalyst I. The resulting intermediate product was subjected to a ring-closing epoxidation reaction under phase transfer catalyst and alkaline conditions. The resulting reaction mixture was purified to obtain intermediate product I with the structure shown in formula (III). S2. The intermediate reaction product I obtained in step S1 is purified after esterification with a straight-chain fatty diacid ester compound in the presence of catalyst II. The resulting reaction product is a di(3-glycidoxy-2-hydroxypropyl) straight-chain fatty diacid ester with the structure shown in formula (I). The halo-propane oxide is 3-chloro-1,2-propane oxide and / or 3-bromo-1,2-propane oxide. Formula (Ⅲ); The general formula of the straight-chain fatty acid ester compound is HOOC-(CH2). n -COOH, where n is an integer from 2 to 12.

[0015] In the above-described preparation of bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, in step S1, the molar ratio between glycerol and halopropylene oxide is preferably 1:(1.1~1.4), such as 1:1.1, 1:1.2, 1:1.3, 1:1.4, or any ratio therebetween. This improves the yield of intermediate product I shown in formula (III).

[0016] In the above-described preparation of bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, in step S1, catalyst I is preferably a Lewis acid catalyst. The Lewis acid catalyst may be selected from at least one of boron trifluoride diethyl ether complex, boron trifluoride tetrahydrofuran complex, tin tetrachloride, and aluminum trichloride.

[0017] In the above-described process for preparing di(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, in step S1, the phase transfer catalyst may be selected from at least one of tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate, and benzyltriethylammonium chloride.

[0018] In the above-described preparation of bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, in step S1, the alkaline conditions are preferably provided in the form of an alkaline solution. The alkaline substance in the alkaline solution can be sodium hydroxide and / or potassium hydroxide.

[0019] In the above-described process for preparing di(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, the ring-opening etherification reaction conditions in step S1 preferably include: a temperature of 40~55℃, such as 40℃, 45℃, 50℃, 55℃ or any value between them; and a time of 3~6h, such as 3h, 4h, 5h, 6h or any value between them.

[0020] In the above-described process for preparing di(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, the epoxidation reaction conditions in step S1 preferably include: a temperature of 40~55℃, such as 40℃, 45℃, 50℃, 55℃ or any value between them; and a time of 3~6h, such as 3h, 4h, 5h, 6h or any value between them.

[0021] In the above-described preparation of bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, in step S2, the molar ratio between the intermediate reaction product I and the linear fatty acid ester compound is preferably (2.05~2.20):1, such as 2.05:1, 2.1:10, 2.15:1, 2.20:1, or any ratio therebetween. In the above-described process for preparing bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, in step S2, the linear fatty acid ester compound only needs to have HOOC-(CH2) content. n Compounds with the general formula -COOH are acceptable, where n is an integer from 2 to 12. Specific examples of the straight-chain fatty acid ester compounds include, but are not limited to, any one or more of oxalic acid, succinic acid, glutaric acid, adipic acid, octanoic acid, azelaic acid, sebacic acid, and dodecanoic acid.

[0022] In the above-described preparation of bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, in step S2, the catalyst II can be any existing catalyst capable of catalyzing the esterification reaction between carboxyl and hydroxyl groups, preferably an organotin catalyst. Specific examples of organotin catalysts include, but are not limited to, any one or more of monobutyltin oxide, dibutyltin oxide, dibutyltin dilaurate, and stannous octoate.

[0023] In the above-described process for preparing di(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, the esterification reaction conditions in step S2 preferably include: below 130°C, specifically 110~125°C, such as 110°C, 115°C, 120°C, 125°C or any value between them; the reaction time is defined as the reaction endpoint when the acid value of the system is ≤2 mgKOH / g.

[0024] The chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) is preferably prepared by the following method: H1. An aromatic ring dicarbonyl compound is mixed with a glycidyl alcohol compound having the structure shown in formula (IV) and then subjected to a ring-opening monoesterification reaction to obtain intermediate product II having the structure shown in formula (V); H2. The intermediate reaction product II obtained in step H1 is purified by coordination chelation reaction with a titanate compound, and the resulting reaction product is a chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium (IV) with the structure shown in formula (II). Formula (IV), Equation (V), In formulas (IV) and (V), R2 is a C2-C6 alkylene group, R3 is a C1-C4 alkylene group, and Ar is a phenylene group.

[0025] The aromatic ring dicarbonyl compound is selected from at least one of phthalic anhydride, isophthalic acid, and terephthalic acid.

[0026] In the above-described preparation of chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium (IV), in step H1, the molar ratio between the aromatic ring dicarbonyl compound and the glycidyl alcohol compound is preferably 1:(0.95~1), such as 1:0.95, 1:0.96, 1:0.97, 1:0.98, 1:0.99, 1:1, or any ratio between them. The preferred conditions for the ring-opening monoesterification reaction include: being carried out under anhydrous and oxygen-free conditions; and a temperature of 80~90℃, such as 80℃, 82℃, 85℃, 88℃, 90℃, or any value between them. There is no particular limitation on the time of the ring-opening monoesterification reaction, as long as the acid anhydride in the system has essentially completed ring-opening. Infrared spectroscopy can be performed on samples to confirm whether the characteristic peaks of the acid anhydride have disappeared. Specifically, the time for the ring-opening monoesterification reaction can be 4 to 5 hours, such as 4 hours, 4.5 hours, 5 hours, or any value between them.

[0027] In the above-described preparation of chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium (IV), in step H2, the molar ratio between the intermediate reaction product II and the titanate compound is preferably 1:(0.45~0.5), such as 1:0.45, 1:0.46, 1:0.47, 1:0.48, 1:0.49, 1:0.5, or any value between them. The conditions for the coordination chelation reaction preferably include: a temperature of 40~55℃, such as 40℃, 45℃, 50℃, 55℃, or any value between them; and a time of 3~6h, such as 3h, 4h, 5h, 6h, or any value between them.

[0028] In the above-described preparation of chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium (IV), the glycidol compound can be any compound satisfying the structure shown in formula (IV). As a preferred example, the glycidol compound can be selected from at least one of 3-(ethylene oxide-2-methoxy)prop-1-ol (CAS: 73642-99-6), 6-[(ethylene oxide-2-yl)methoxy]hex-1-ol (CAS: 21813-06-9), and 4-(ethylene oxide-2-methoxy)-1-butanol (CAS: 4711-95-9). The titanate compound can be any compound satisfying the general formula Ti(OR1), wherein R1 is a C1-C4 alkyl group. As a preferred example, the titanate compound can be selected from at least one of tetraisopropyl titanate, tetrabutyl titanate, tetraethyl titanate, and tetramethyltetrazine (IV).

[0029] In this invention, the core-shell toughened rubber particles refer to core-shell structured materials with an organic rubber core and a polymer material as the shell. There are no particular limitations on the specific materials of the organic rubber and polymer material. For example, the organic rubber can be styrene-butadiene rubber, nitrile rubber, chloroprene rubber, ethylene propylene rubber, etc., and the polymer material can be polymethyl methacrylate, polyacrylate, epoxy resin, etc. As a preferred example, the core-shell toughened rubber particles can be selected from any one or more commercially available products such as Kaneka MZ-120 (Kaneka Chemicals, Japan), Clearstrength® XT151 (Arkema, France), Kaneka MX-553 (Kaneka Chemicals, Japan), and YT-2125 (Fujian Jinghan New Materials).

[0030] In this invention, the polyol is preferably selected from at least one of polyether polyols, polyester polyols, polycarbonate polyols, and hyperbranched polyols. As a preferred example, the polyol may be selected from any one or more of the following products: CELLOXIDE Placcel205 (DAICEL, Japan), UNIPOL210 (Xiamen Juyou), PTMG650 (Asahi Kasei), T-5650E, and other commercially available products. Further, the number-average molecular weight (Mn) of the polyol is preferably 200-2100 g / mol, such as 200 g / mol, 500 g / mol, 800 g / mol, 1000 g / mol, 1500 g / mol, 2000 g / mol, 2100 g / mol, or any value between them.

[0031] In this invention, the inorganic filler can be selected from any one or more of fumed silica, spherical silica, alumina, talc, mica powder, kaolin, calcium carbonate, aluminum hydroxide, magnesium hydroxide, and boron nitride.

[0032] In this invention, the cationic photoinitiator is a ferrocene salt compound and an onium salt compound. Further, the preferred mass ratio of the ferrocene salt compound to the onium salt compound is (0.01~5):1, such as 0.01:1, 0.05:1, 0.1:1, 0.5:1, 1:1, 2:1, 3:1, 4:1, 5:1, or any ratio therebetween. By adjusting the mass ratio of the ferrocene salt compound to the onium salt compound within the above-mentioned preferred range, the responsiveness of the cationic epoxy adhesive to long-wavelength light sources is further improved, achieving complete surface drying with low energy loss while simultaneously establishing high initial bond strength.

[0033] Furthermore, the onium salt compound is preferably a thioonium salt compound and / or an iodonium salt compound. In addition, the present invention does not particularly limit the specific types and sources of the ferrocene salt compound, thioonium salt compound, and iodonium salt compound, and these can be conventional choices in the art. The ferrocene salt compound can be η 3 - Isopropylbenzene ferrocene hexafluorophosphate (Irgacure261, Uyracure261) and / or η 6- Irgacure ferrocene hexafluoroantimonate (Irgacure 262, Uyracure 262). The thioonium salt compound can be selected from any one or more of UVI-6976 (CAS: 71449-78-0), UVI-6992 (CAS: 68156-13-8), and di[4-diphenylthiophenyl]thioether dihexafluoroantimonate. The iodonium salt compound can be selected from any one or more of photoinitiator 250 (CAS: 344562-80-7), Irgacure 250 (BASF), and Uyracure 160 (Shenzhen Youyang Technology).

[0034] In this invention, the photosensitizer is preferably a peroxide, and specific examples include, but are not limited to, any one or more of the following: tert-butyl hydroperoxide, cumene hydroperoxide, benzoyl peroxide, 1,1-di-tert-butylcyclohexane peroxide, and tert-butyl peroxypentanoate.

[0035] In this invention, the silane coupling agent is preferably an epoxy siloxane compound, and specific examples include, but are not limited to, any one or more of the following: (3-glycidyl etheroxypropyl)methyldimethoxysilane, (3-glycidyl etheroxypropyl)methyldiethoxysilane, 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane, bis[2-(3,4-epoxycyclohexyl)ethyl]-1,1,3,3-tetramethyldisiloxane, 1,3-bis(3-glycidyl etheroxypropyl)-1,1,3,3-tetramethyldisiloxane, Shin-Etsu KR-470, (3-glycidyl etheroxypropyl)trimethoxysilane, and (3-glycidyl etheroxypropyl)triethoxysilane.

[0036] In one specific embodiment, the preparation method of the cationic photocurable epoxy adhesive provided by the present invention can be as follows: (1) Add the alicyclic epoxy resin, bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, core-shell rubber toughening particles, polyol, cationic photoinitiator, photosensitizer, chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate) titanium(IV) metal adhesive and silane coupling agent to the stirred tank in sequence. Stir for 1-3 hours at room temperature and pressure, and then turn on the temperature control device to quickly cool down to room temperature. (2) Add the inorganic filler into the mixing vessel, turn on the temperature control device, and stir for 0.5~1.5h at room temperature and under vacuum. Then it can be removed from the vessel and sealed for packaging.

[0037] This invention provides the application of the above-mentioned cationic photocurable epoxy adhesive in the bonding of electronic device structures, the encapsulation of optoelectronic components, and the composite bonding of ink or metal substrates with plastic substrates. In specific applications, the photocuring wavelength of the cationic photocurable epoxy adhesive can be 400~600nm, for example, 400nm, 450nm, 500nm, 550nm, 600nm, or any value or wavelength range therebetween; the photocuring intensity can be 0.5~25J / cm². 2 It can be 0.5 J / cm 2 1J / cm 2 2J / cm 2 5J / cm 2 8J / cm 2 10J / cm 2 12J / cm 2 15J / cm 2 18J / cm 2 20J / cm 2 25J / cm 2 Or any value between them.

[0038] The present invention will be described in detail below through specific embodiments. These embodiments are intended to explain the invention and should not be construed as limiting it. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in the art or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.

[0039] In the following examples and comparative examples, all parts refer to parts by weight.

[0040] Synthesis example 1 The preparation of a bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester is illustrated by the following steps and reaction process: S1. Equip a 2000mL four-necked reaction flask with a mechanical stirrer, dropping funnel, and thermometer; add 138.2g (1.2mol) glycerol, stir and heat to 50℃, then maintain the temperature. Slowly add 141.2g (1.53mol) epichlorohydrin dropwise over 2.5h; after the addition is complete, add 3.15g boron trifluoride-ethyl ether complex, and maintain the reaction at 50℃ for 3.2h to obtain a chlorohydrin ring-opening intermediate; maintain the system temperature at 50℃, and add... Add 9.6 g of tetrabutylammonium bromide and slowly add 206.2 g of sodium hydroxide aqueous solution (32 wt%) over 2 hours. After the addition is complete, continue the reaction at 50 °C for 4 hours to close the ring. After the reaction is complete, allow the mixture to stand and separate the layers, discarding the lower aqueous phase. Wash the organic phase three times with saturated brine (150 g each time) until the pH of the aqueous phase is close to neutral. Perform high-vacuum distillation on the washed organic phase and collect the main fraction to obtain 202.4 g of glycerol monoglycidyl ether. The structure of glycerol monoglycidyl ether is shown in formula (III). The epoxy value was measured to be 0.532 mol / 100 g, which meets the requirement of ≥0.52 mol / 100 g for use.

[0041] S2. Equip a 1000mL four-necked flask with a mechanical stirrer, water separator, condenser, and thermometer; add 154.97g (1.046mol) glycerol monoglycidyl ether, 101.1g (0.5mol) sebacic acid, 160.0g toluene, and 1.2g monobutyltin oxide; under nitrogen protection, stir, heat, and reflux to separate water, controlling the flask temperature ≤130℃, continuously separating the water generated in the reaction; monitor the acid value of the system, the reaction endpoint is defined as acid value ≤2mgKOH / g, and the reaction time is 8±1h. After the reaction is complete, remove the toluene solvent under reduced pressure; filter the crude product to remove trace solid impurities, obtaining a pale yellow transparent viscous liquid, which is di(3-glycidoxy-2-hydroxypropyl) sebacic acid.

[0042]

[0043] Synthesis example 2 The preparation of a bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester is illustrated by the following steps: The method of Synthesis Example 1 was followed, except that the same molar amount of oxalic acid was used instead of sebacic acid in step S2, and the other conditions were the same as in Synthesis Example 1. Thus, di(3-glycidoxy-2-hydroxypropyl) oxalate was prepared, which has the structure shown in formula (I), where n is 2.

[0044] Synthesis example 3 The preparation of a bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester is illustrated by the following steps: The method of Synthesis Example 1 was followed, except that the same molar amount of glutaric acid was used instead of sebacic acid in step S2, and all other conditions were the same as in Synthesis Example 1. Thus, di(3-glycidoxy-2-hydroxypropyl) glutarate was prepared, which has the structure shown in formula (I), and n is 5.

[0045] Synthesis example 4 The preparation of a chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) is illustrated below, with specific steps and reaction procedures as follows: H1. In a 500 mL four-necked reaction flask equipped with a mechanical stirrer, a reflux condenser, a constant-pressure dropping funnel, a nitrogen delivery tube, and a thermometer, dry nitrogen was introduced to replace the air in the system, maintaining a slight positive pressure nitrogen protection throughout the process. 200 mL of anhydrous toluene was added to the reaction flask, followed by 74.0 g (0.50 mol) of phthalic anhydride and 66.08 g (0.50 mol) of 3-(ethylene oxide-2-methoxy)prop-1-ol. Stirring was started, and the temperature was raised to 85 °C and maintained for 5 h to carry out the ring-opening monoesterification of the anhydride. Infrared spectroscopy was performed, and the characteristic peak of the anhydride disappeared, yielding a toluene solution containing 0.50 mol of mono-(3-glycidoxypropyl) phthalic acid ester with a theoretical mass of 140.14 g.

[0046] H2. Cool the system after the above reaction to 45℃, strictly controlling the system temperature to not exceed 60℃. Slowly add 71.06g (0.25mol) of tetraisopropyl titanate through a constant pressure dropping funnel over 2 hours. After the addition is complete, continue stirring at 45℃ for 3 hours to allow ligand exchange chelation between the carboxyl group and the titanium atom, removing isopropanol. After the reaction is complete, start vacuum distillation, controlling the system temperature to be below 65℃, and gradually increase the vacuum to -0.095MPa to remove the solvent toluene and free isopropanol until no fraction flows out. Cool to room temperature to obtain a pale yellow viscous transparent liquid product, which is the target product, diisopropoxy-bis[mono(3-glycidoxypropyl)phthalate]titanium(IV) metal binder.

[0047]

[0048] Synthesis example 5 The preparation of a chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) is illustrated below, with specific steps and reaction procedures as follows: The method of Synthesis Example 4 was followed, except that in step H1, the same molar amount of terephthalic acid was used instead of phthalic anhydride, and the same molar amount of 6-[(ethylene oxide-2-yl)methoxy]hex-1-ol was used instead of 3-(ethylene oxide-2-methoxy)prop-1-ol. All other conditions were the same as in Synthesis Example 4. Thus, diisopropoxy-bis[terephthalic acid mono(3-glycidoxyhexyl)ester]titanium (IV) was prepared, and its structure is shown below.

[0049]

[0050] Comparative Synthesis Example 1 The preparation of a bis(3-glycidoxypropyl) linear fatty acid ester is illustrated by the following steps: The method of Synthesis Example 1 was followed, except that the same molar amount of propylene glycol was used instead of glycerol in step S1, and all other conditions were the same as in Synthesis Example 1. Thus, di(3-glycidoxy-propyl) sebacate was prepared, the structure of which is shown below.

[0051]

[0052] Comparative Synthesis Example 2 The preparation of a chelated dialkoxy-bis(glycidoxyalkyl)titanium (IV) is illustrated by the following specific steps and reaction process: In a 500 mL four-necked reaction flask equipped with a mechanical stirrer, a reflux condenser, a constant-pressure dropping funnel, a nitrogen delivery tube, and a thermometer, dry nitrogen was introduced to replace the air in the system, maintaining a slight positive pressure nitrogen protection throughout the process. 200 mL of anhydrous toluene was added to the reaction flask, followed by 66.08 g (0.50 mol) of 3-(ethylene oxide-2-methoxy)prop-1-ol. The stirring was started and the temperature was raised to 45 °C, with the system temperature strictly controlled not to exceed 60 °C. 71.06 g (0.25 mol) of tetraisopropyl titanate was slowly added dropwise through the constant-pressure dropping funnel over a period of 2 hours. After the addition was complete, the reaction was continued at 45 °C with stirring for 3 hours, resulting in ligand exchange chelation between the hydroxyl group and the titanium atom, thus removing the isopropanol. After the reaction was completed, vacuum distillation was started, the system temperature was controlled below 65℃, and the vacuum degree was gradually increased to -0.095MPa to remove the solvent toluene and free isopropanol until no distillate flowed out; cooled to room temperature, a pale yellow viscous transparent liquid product was obtained, which is diisopropoxy-bis[3-glycidoxypropyl)ester]titanium(IV) metal binder, the structure of which is shown below.

[0053]

[0054] Example 1 The preparation process of a cationic photocurable epoxy adhesive is illustrated below: (1) 42 parts of alicyclic epoxy resin CELLOXIDE 2021P, 12 parts of di(3-glycidoxy-2-hydroxypropyl) sebacate from Synthesis Example 1, 15 parts of core-shell rubber toughening particles Kaneka MZ-120, 10 parts of polyol CELLOXIDEPlaccel205, 1 part of ferrocene salt photoinitiator Irgacure 261, 1 part of iodonium salt photoinitiator 250, 3 parts of photosensitizer (tert-butyl hydrogen peroxide), 3 parts of diisopropoxy-bis[mono(3-glycidoxypropyl) phthalate]titanium(IV) metal adhesive from Synthesis Example 4, and 3 parts of (3-glycidoxypropyl)methyldimethoxysilane were added to a stirred tank in sequence. After stirring for 2 hours at room temperature and pressure, the temperature control device was turned on to quickly lower the temperature to room temperature. (2) Add 10 parts of spherical silica to the mixing vessel, turn on the temperature control device, and stir for 1 hour at room temperature and under vacuum. Then, remove the mixture from the vessel and seal it in a package to obtain cationic photocurable epoxy adhesive.

[0055] Example 2 The preparation process of a cationic photocurable epoxy adhesive is illustrated below: (1) 50 parts of alicyclic epoxy resin Dow CYRACURE™ UVR-6128, 20 parts of di(3-glycidoxy-2-hydroxypropyl) sebacate from Synthesis Example 1, 6 parts of core-shell rubber toughening particles Clearstrength® XT151, 6 parts of polyol UNIPOL210, 1.6 parts of ferrocene salt photoinitiator Irgacure 262, 0.4 parts of iodonium salt photoinitiator Uyracure160, 3 parts of photosensitizer (cumene hydroperoxide), 1 part of diisopropoxy-bis[mono(3-glycidoxypropyl) phthalate]titanium(IV) metal adhesive from Synthesis Example 4, and 5 parts of 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane were added to a stirred tank in sequence. After stirring for 2 hours at room temperature and pressure, the temperature control device was turned on to quickly lower the temperature to room temperature. (2) Add 7 parts of alumina to the mixing tank, turn on the temperature control device, and stir for 1 hour at room temperature and under vacuum. Then, remove the mixture from the tank and seal it in a package to obtain the cationic photocurable epoxy adhesive.

[0056] Example 3 The preparation process of a cationic photocurable epoxy adhesive is illustrated below: (1) 32 parts of alicyclic epoxy resin UVR-6110, 5 parts of di(3-glycidoxy-2-hydroxypropyl) sebacate from Synthesis Example 1, 20 parts of core-shell rubber toughening particles YT-2125, 15 parts of polyol PTMG 650, 0.2 parts of ferrocene salt photoinitiator Uyracure261, 1.8 parts of thionium salt photoinitiator UVI-6976, 3 parts of photosensitizer (benzoyl peroxide), 5 parts of diisopropoxy-bis[mono(3-glycidoxypropyl) phthalate]titanium(IV) metal adhesive from Synthesis Example 4, and 3 parts of 1,3-bis(3-glycidoxypropyl)-1,1,3,3-tetramethyldisiloxane were added to a stirred tank in sequence. After stirring for 2 hours at room temperature and pressure, the temperature control device was turned on to quickly lower the temperature to room temperature. (2) Add 15 parts of spherical silica to the mixing vessel, turn on the temperature control device, and stir for 1 hour at room temperature and under vacuum. Then, remove the mixture from the vessel and seal it in a package to obtain the cationic photocurable epoxy adhesive.

[0057] Example 4 The preparation process of a cationic photocurable epoxy adhesive is illustrated below: The cationic photocurable epoxy adhesive was prepared according to the method of Example 1, except that the same parts by weight of di(3-glycidoxy-2-hydroxypropyl) oxalate from Synthesis Example 2 was used instead of di(3-glycidoxy-2-hydroxypropyl) sebacate from Synthesis Example 1, and all other conditions were the same as in Example 1.

[0058] Example 5 The preparation process of a cationic photocurable epoxy adhesive is illustrated below: The cationic photocurable epoxy adhesive was prepared according to the method of Example 1, except that the same parts by weight of self-synthesized Example 3 di(3-glycidoxy-2-hydroxypropyl) glutarate was used instead of the di(3-glycidoxy-2-hydroxypropyl) sebacate from Example 1, and all other conditions were the same as in Example 1.

[0059] Example 6 The preparation process of a cationic photocurable epoxy adhesive is illustrated below: Prepared according to the method of Example 1, except that the same parts by weight of diisopropoxy-bis[mono(3-glycidoxypropyl) phthalate]titanium(IV) from Synthesis Example 5 were used instead of the diisopropoxy-bis[mono(3-glycidoxyhexyl) phthalate]titanium(IV) metal adhesive from Synthesis Example 4, and all other conditions were the same as in Example 1, thereby obtaining a cationic photocurable epoxy adhesive.

[0060] Comparative Example 1 The preparation process of a reference cationic photocurable epoxy adhesive is illustrated below: The preparation was carried out according to the method of Example 1, except that the same amount of alicyclic epoxy resin CELLOXIDE 2021P was used instead of di(3-glycidoxy-2-hydroxypropyl) sebacate, and all other conditions were the same as in Example 1, thereby preparing a reference cationic photocurable epoxy adhesive.

[0061] Comparative Example 2 The preparation process of a reference cationic photocurable epoxy adhesive is illustrated below: The preparation was carried out according to the method of Example 1, except that the same amount of di(3-glycidoxy-propyl) sebacate from Comparative Synthesis Example 1 was used instead of di(3-glycidoxy-2-hydroxypropyl) sebacate, and all other conditions were the same as in Example 1, thereby preparing a reference cationic photocurable epoxy adhesive.

[0062] Comparative Example 3 The preparation process of a reference cationic photocurable epoxy adhesive is illustrated below: The preparation was carried out according to the method of Example 1, except that the same amount of glyceryl diglycidyl ether (CAS: 27043-36-3) was used instead of di(3-glycidyloxy-2-hydroxypropyl) sebacate, and the other conditions were the same as in Example 1, thereby preparing a reference cationic photocurable epoxy adhesive.

[0063] Comparative Example 4 The preparation process of a reference cationic photocurable epoxy adhesive is illustrated below: The preparation was carried out according to the method of Example 1, except that the same amount of (3-glycidyl ether oxypropyl)methyl dimethoxysilane was used instead of diisopropoxy-bis[phthalic acid mono(3-glycidyl oxypropyl) ester]titanium(IV), and all other conditions were the same as in Example 1, thereby preparing a reference cationic photocurable epoxy adhesive.

[0064] Comparative Example 5 The preparation process of a reference cationic photocurable epoxy adhesive is illustrated below: The preparation was carried out according to the method of Example 1, except that the same amount of diisopropoxy-bis[mono(3-glycidoxypropyl)phthalate]titanium(IV) from Comparative Synthesis Example 2 was used instead of diisopropoxy-bis[mono(3-glycidoxypropyl)phthalate]titanium(IV), and all other conditions were the same as in Example 1, thereby preparing a reference cationic photocurable epoxy adhesive.

[0065] Test case The cationic photocurable epoxy adhesives prepared in the above examples and comparative examples were tested for surface dryness, initial bond strength on different substrates, steady-state final strength, and resistance to thermal cycling using the following methods. Specific results are shown in Table 1.

[0066] (1) Curing conditions and surface drying status observation: 470nm long-wave LED was used uniformly, and the light curing intensity was 11J / cm. 2 .

[0067] Surface Dryness Test Method: Referring to GB / T 10006-1988, the surface dryness performance of the adhesive layer was quantitatively evaluated using a coefficient of friction meter. The adhesive to be tested was coated onto a clean float glass substrate with a coating thickness of 50 μm and cured according to the set curing process. After curing, the sample was placed in an environment of 23℃ and 50% relative humidity for 1 hour. A 200g stainless steel slider with a contact area of ​​40 cm², a sliding speed of 100 mm / min, and a sliding stroke of 50 mm was used. The test was started after the slider was placed on the adhesive film surface for 30 seconds of pre-contact, and the static coefficient of friction (μ) was collected. s The dynamic friction coefficient μd was measured, and each group underwent 5 parallel tests. After the test, the presence of adhesive transfer on the bottom surface of the slider was observed. Surface dryness evaluation criteria: When the static friction coefficient μd of the adhesive film... s ≤0.45, the frictional displacement curve is smooth, and there is no material transfer on the bottom surface of the slider, which is judged as acceptable for surface drying; static friction coefficient 0.45<μ s ≤0.60, with a small amount of curve burrs and no obvious glue transfer, is judged as critical surface drying; μ s If the value is greater than 0.60, the curve fluctuates violently, and the slider shows adhesive adhesion, indicating that it is not surface-dried.

[0068] (2) Bond strength test: using size 3 3 A 1mm mold was applied to the surface of the substrate to be tested. Adhesive was precisely applied into the mold, avoiding air bubbles that could affect the actual bonding area. Excess adhesive was scraped off and the surface smoothed before applying the LSR material, followed by UV curing. After curing, the substrate was allowed to stand for 10 minutes before demolding. The initial shear strength of the stainless steel, copper, aluminum, and ink-based substrates with the LSR material was tested using a DAGE4000 thrust tester and denoted as T. 0,i .

[0069] After photocuring, the substrates were left at room temperature for 24 hours. The steady-state shear strength of each substrate was then tested using a DAGE4000 thrust tester and denoted as T. 1,i .

[0070] (3) High and low temperature cycle reliability test: After bonding, light curing and 24h of room temperature storage according to the method in (2), the sample was subjected to 100 cycles of thermal shock at -40℃ to 85℃ (30min at -40℃ and 30min at 85℃, with each cycle lasting approximately 61mins). The shear strength at this time was tested and recorded as T. 2,i And calculate the strength retention rate (strength retention rate = T) 2,i / T 1,i 100) and observe the cracking and delamination of the sample.

[0071] Table 1

[0072] As shown in Table 1, compared with Comparative Examples 1 to 5, the cationic photocurable epoxy adhesive provided in this embodiment of the invention has higher initial bond strength and steady-state final strength for bonding to various substrates while ensuring surface dryness. It also maintains higher strength retention and surface condition in thermal cycling tests.

[0073] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention without departing from the principles and spirit of the present invention.

Claims

1. A cationic photocurable epoxy adhesive, characterized in that, The raw material components of the cationic epoxy adhesive include: alicyclic epoxy resin, bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, core-shell rubber toughening particles, polyol, inorganic filler, cationic photoinitiator, photosensitizer, chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) metal adhesive, and silane coupling agent; the cationic photoinitiator is a ferrocene salt compound and an onium salt compound; The bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester has the structure shown in formula (I): Equation (I), In equation (I), n is an integer from 2 to 12; The chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) has the structure shown in formula (II): Ti(OR1)2(OOC-Ar-COO-R2-EPO)2 formula (II), In formula (II), R1 is a C1~C4 alkyl group, Ar is a phenylene group, R2 is a C2~C6 alkylene group, EPO represents a group structure of -O-R3-CH(O)CH2, and R3 is a C1~C4 alkylene group.

2. The cationic photocurable epoxy adhesive according to claim 1, characterized in that, The alicyclic epoxy resin contains 30-50 wt%, the bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester contains 5-20 wt%, the core-shell rubber toughening particles contain 5-20 wt%, the polyol contains 5-15 wt%, the inorganic filler contains 5-15 wt%, the cationic photoinitiator contains 1-5 wt%, the photosensitizer contains 1-5 wt%, the chelated dialkoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) metal adhesive contains 0.1-5 wt%, and the silane coupling agent contains 0.1-5 wt%.

3. The cationic photocurable epoxy adhesive according to claim 1, characterized in that, The bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester was prepared by the following method: S1. Glycerol was mixed with halopropylene oxide and then subjected to a ring-opening etherification reaction in the presence of catalyst I. The resulting intermediate product was subjected to an epoxidation reaction under a phase transfer catalyst and alkaline conditions. The resulting reaction mixture was purified to obtain intermediate product I with the structure shown in formula (III). S2. The intermediate reaction product I obtained in step S1 is purified after esterification with a straight-chain fatty diacid ester compound in the presence of catalyst II. The resulting reaction product is a di(3-glycidoxy-2-hydroxypropyl) straight-chain fatty diacid ester with the structure shown in formula (I). The halo-propane oxide is 3-chloro-1,2-propane oxide and / or 3-bromo-1,2-propane oxide. Formula (Ⅲ); The general formula of the straight-chain fatty acid ester compound is HOOC-(CH2). n -COOH, where n is an integer from 2 to 12.

4. The cationic photocurable epoxy adhesive according to claim 3, characterized in that, In step S1, the molar ratio between glycerol and halopropylene oxide is 1:(1.1~1.4); Preferably, in step S1, the catalyst I is a Lewis acid catalyst, which is selected from at least one of boron trifluoride diethyl ether complex, boron trifluoride tetrahydrofuran complex, tin tetrachloride, and aluminum trichloride. Preferably, in step S1, the phase transfer catalyst is selected from at least one of tetrabutylammonium bromide, tetrabutylammonium hydrogen sulfate, and benzyltriethylammonium chloride; Preferably, in step S1, the alkaline condition is provided in the form of an alkaline solution, wherein the alkaline substance in the alkaline solution is sodium hydroxide and / or potassium hydroxide; Preferably, in step S2, the molar ratio between the intermediate reaction product I and the straight-chain fatty acid ester compound is (2.05~2.20):1; Preferably, in step S2, catalyst II is an organotin catalyst.

5. The cationic photocurable epoxy adhesive according to claim 1, characterized in that, The chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) was prepared by the following method: H1. An aromatic ring dicarbonyl compound is mixed with a glycidyl alcohol compound having the structure shown in formula (IV) and then subjected to a ring-opening monoesterification reaction to obtain intermediate product II having the structure shown in formula (V); H2. The intermediate reaction product II obtained in step H1 is purified by coordination chelation reaction with a titanate compound, and the resulting reaction product is a chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium (IV) with the structure shown in formula (II). Formula (IV), Equation (V), In formulas (IV) and (V), R2 is a C2-C6 alkylene group, R3 is a C1-C4 alkylene group, and Ar is a phenylene group; The aromatic ring dicarbonyl compound is selected from at least one of phthalic anhydride, isophthalic acid, and terephthalic acid.

6. The cationic photocurable epoxy adhesive according to claim 5, characterized in that, In step H1, the molar ratio between the aromatic ring dicarbonyl compound and the glycidyl alcohol compound is 1:(0.95~1); Preferably, in step H1, the conditions for the ring-opening monoesterification reaction include: anhydrous and oxygen-free conditions, and a temperature of 80~90℃; Preferably, in step H2, the molar ratio between the intermediate reaction product II and the titanate compound is 1:(0.45~0.5); Preferably, in step H2, the titanate compound is selected from at least one of tetraisopropyl titanate, tetrabutyl titanate, tetraethyl titanate, and tetramethyltitanic (IV). Preferably, in step H2, the conditions for the coordination chelation reaction include: a temperature of 40~55℃ and a time of 3~6h.

7. The cationic photocurable epoxy adhesive according to claim 1, characterized in that, The mass ratio between the ferrocene salts and the onium salts is (0.01~5):

1.

8. The cationic photocurable epoxy adhesive according to claim 1, characterized in that, The toughening polyol has a number-average molecular weight of 200-2100 g / mol; Preferably, the silane coupling agent is an epoxy siloxane compound.

9. A method for preparing the cationic photocurable epoxy adhesive according to any one of claims 1 to 8, characterized in that, The preparation method includes: mixing alicyclic epoxy resin, bis(3-glycidoxy-2-hydroxypropyl) linear fatty acid ester, core-shell rubber toughening particles, polyol, inorganic filler, cationic photoinitiator, photosensitizer, chelated diekoxy-bis(mono-(ω-glycidoxyalkyl)phthalate)titanium(IV) metal adhesive and silane coupling agent, and the resulting mixture is a cationic photocurable epoxy adhesive.

10. The cationic photocurable epoxy adhesive according to any one of claims 1 to 8 is used in the bonding of electronic device structures, the encapsulation of optoelectronic components, and the composite bonding of ink or metal substrates with plastic substrates.