A method for preparing a high thermal conductivity underfill single-component epoxy adhesive for chips.
By surface activation of hexagonal boron nitride and construction of a flexible polymer shell, combined with multi-scale graded thermally conductive fillers, the problems of increased viscosity and decreased flow performance under high filling conditions of high thermal conductivity fillers are solved, achieving a synergistic balance between high thermal conductivity and good flow performance, which is suitable for high power density chip packaging.
Patent Information
- Application Number
- CN202611593565.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing chip underfill adhesives suffer from increased viscosity, decreased flow properties, and poor interfacial compatibility under conditions of high thermal conductivity filler and high filler content, making it difficult to simultaneously meet the requirements of high thermal conductivity and good flow properties.
By surface activation and silane coupling modification of hexagonal boron nitride, a silane coupling layer with polymerizable double bonds is formed. Then, in-situ polymerization of methyl methacrylate and butyl acrylate is carried out on its surface to construct a flexible polymer shell. This shell is then multi-scale graded with spherical alumina and spherical aluminum nitride to form a stable core-shell structure.
It significantly improves the rheological properties of adhesives under high-filling conditions, reduces viscosity, enhances capillary filling performance and interfacial compatibility, maintains high thermal conductivity, and is suitable for high power density chips and flip-chip packaging.
Smart Images

Figure CN123107600A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of epoxy adhesives, and more particularly to a method for preparing a high thermal conductivity underfill single-component epoxy adhesive for chips. Background Technology
[0002] As AI computing chips, automotive semiconductors, and high-performance computing chips develop towards higher integration and higher power density, the heat generated during chip operation is constantly increasing, placing higher demands on the heat dissipation capacity and long-term reliability of packaging materials. In flip-chip packaging, underfill adhesive is typically used to fill the tiny gaps between the chip and the substrate, and through curing, forms a stable bonding and support structure, thereby alleviating the thermomechanical stress caused by the mismatch in thermal expansion coefficients between the chip, solder joints, and substrate. Therefore, in addition to good adhesion, heat resistance, and moisture resistance, the underfill adhesive also needs high thermal conductivity and good flow and filling properties.
[0003] Existing chip underfill adhesives typically use epoxy resin as a matrix and add inorganic thermally conductive fillers such as alumina, aluminum nitride, and boron nitride to improve the thermal conductivity of the system. Among them, hexagonal boron nitride has high intrinsic thermal conductivity and good electrical insulation properties. Its lamellar structure facilitates the interlocking of fillers to form thermal conductive pathways, thus showing good application potential in electronic packaging thermal conductive materials.
[0004] However, while increasing the thermally conductive filler content is beneficial for constructing a continuous thermally conductive network, it also significantly increases the interactions between fillers and between fillers and resin, leading to an increase in the viscosity of the adhesive system. In particular, plate-like hexagonal boron nitride, with its large surface area, is prone to plate stacking and agglomeration under high filler conditions, further increasing the system's flow resistance. For chip underfill adhesives, the adhesive typically relies on capillary action to penetrate the tiny gaps between the chip and the substrate; therefore, excessively high system viscosity can lead to reduced capillary filling speed, incomplete local filling, and even defects such as voids. Thus, there is a significant contradiction between the high filler content required for high thermal conductivity fillers and the low viscosity and good flow properties required for chip underfill.
[0005] Furthermore, untreated hexagonal boron nitride has low surface chemical activity and limited interfacial compatibility with organic matrices such as epoxy resins, easily leading to interfacial defects between the filler and the resin. On the one hand, interfacial defects affect the uniform dispersion of inorganic fillers in the resin system and exacerbate filler agglomeration and increased system viscosity; on the other hand, the large interfacial thermal resistance between the filler and the resin also affects the effective heat transfer in the thermally conductive network. Existing technologies typically employ silane coupling agents to modify the surface of inorganic thermally conductive fillers such as hexagonal boron nitride, improving the compatibility between the filler and the resin by forming interfacial connections between the inorganic filler and the organic resin. Silane coupling agents can interact with the active groups on the filler surface through their inorganic reactive ends and with the resin matrix through their organic functional groups, thereby improving the interfacial state between the inorganic filler and the organic resin.
[0006] However, the surface modification layer formed by simply using silane coupling agents is usually quite thin, and its main function remains to improve the interfacial compatibility between the filler and the resin. Under high-filling conditions of thermally conductive fillers, strong interparticle interactions may still form between the lamellar hexagonal boron nitride particles. Therefore, relying solely on conventional silane coupling modification has limited effect on improving the rheological properties of high-filling systems. Meanwhile, existing technologies can also increase the filling density and construct a thermally conductive network by grading and compounding thermally conductive fillers with different particle sizes and morphologies. However, multi-scale filler gradation mainly addresses the construction of thermally conductive pathways and filling efficiency, and still struggles to effectively control the interactions between lamellar hexagonal boron nitride particles at the filler interface level.
[0007] Therefore, for high thermal conductivity bottom filler adhesives for chips, it is still necessary to further improve the interface state between hexagonal boron nitride and organic resin, as well as between hexagonal boron nitride layers, so that the thermally conductive filler can form an effective thermally conductive network under high filling conditions, while reducing the increase in system viscosity caused by filler agglomeration and interparticle interaction, thereby taking into account both high thermal conductivity and good shear flow properties and micro-gap capillary filling performance. Summary of the Invention
[0008] In view of the above analysis, the present invention aims to provide a method for preparing a high thermal conductivity underfill single-component epoxy adhesive for chips to solve the problems in the background art.
[0009] The objective of this invention is mainly achieved through the following technical solutions: A method for preparing a high thermal conductivity underfill single-component epoxy adhesive for chips includes the following steps: S1, Surface activation of hexagonal boron nitride: By mass, 100 parts of flake-shaped hexagonal boron nitride were added to 800-1200 parts of nitric acid aqueous solution with a concentration of 1-3 mol / L for surface activation treatment. After the reaction was completed, the surface-activated hexagonal boron nitride was obtained by washing and drying. S2, silane coupling modification: 100 parts of the surface-activated hexagonal boron nitride were dispersed in a mixed solvent consisting of 400-600 parts of ethanol and 20-50 parts of water. 3-8 parts of vinyltriethoxysilane were added to react with the active groups on the surface of the hexagonal boron nitride, forming a silane coupling layer with polymerizable double bonds on the surface of the hexagonal boron nitride. After washing and drying, silane-coupled modified hexagonal boron nitride was obtained. S3, Preparation of core-shell modified hexagonal boron nitride: 100 parts of the silane-coupled modified hexagonal boron nitride were dispersed in 400-600 parts of organic solvent, and 10-18 parts of methyl methacrylate, 4-10 parts of butyl acrylate and 0.1-0.4 parts of free radical polymerization initiator were added to carry out a polymerization reaction, so that methyl methacrylate and butyl acrylate polymerized on the silane coupling layer on the surface of hexagonal boron nitride to form a flexible polymer shell. After separation, washing and drying, core-shell modified hexagonal boron nitride was obtained. S4. Preparation of epoxy resin matrix: By weight, 10-30 parts of alicyclic epoxy resin and 10-20 parts of biphenyl epoxy resin are mixed and heated, and 1-3 parts of polyethersulfone and 1-3 parts of ionic liquid modified montmorillonite are added. Under heating and stirring conditions, the polyethersulfone and ionic liquid modified montmorillonite are dispersed in the epoxy resin to obtain an epoxy resin matrix. S5. Addition and dispersion of thermally conductive filler: After cooling the epoxy resin matrix obtained from S4, 1-2 parts of silane coupling agent, 1-2 parts of heptadecafluorodecyltrimethoxysilane and 1-2 parts of phosphate ester wetting and dispersing agent are added. Then, 20-30 parts of spherical alumina, 20-30 parts of spherical aluminum nitride and 30-40 parts of core-shell modified hexagonal boron nitride obtained from S3 are added and dispersed to form a multi-scale graded thermally conductive filler system. S6. Addition and degassing of the curing system: After cooling the mixture obtained from S5, add 10-20 parts of methyltetrahydrophthalic anhydride, 10-20 parts of dodecenylsuccinic anhydride, and 1-5 parts of imidazole curing accelerator. After mixing evenly, perform vacuum degassing to obtain the high thermal conductivity underfill single-component epoxy adhesive for the chip.
[0010] In one or more embodiments, in S1, the D50 of the sheet-like hexagonal boron nitride is 3-8 μm; the surface activation treatment temperature is 70-90°C and the treatment time is 3-6 h; after the surface activation treatment is completed, the surface is washed with deionized water until the pH value of the washing solution is 6.5-7.5, and then vacuum dried at 70-90°C for 8-16 h.
[0011] In a preferred embodiment, in S2, based on a total mass of ethanol and water in the mixed solvent of 100 parts, ethanol comprises 90-98 parts and water comprises 2-10 parts; after vinyltriethoxysilane is added to the mixed solvent, the pH of the system is adjusted to 4.0-6.0 and hydrolyzed for 20-60 min, and then the surface-activated hexagonal boron nitride is added, and the reaction is carried out at 60-80°C for 2-5 h.
[0012] In a preferred embodiment, in S3, the mass ratio of methyl methacrylate to butyl acrylate is (1.2-3.5):1, the free radical polymerization initiator is azobisisobutyronitrile, the polymerization reaction temperature is 60-75°C, and the polymerization reaction time is 4-10 h.
[0013] In a preferred embodiment, the core-shell modified hexagonal boron nitride prepared by S3 includes a plate-like hexagonal boron nitride core and a methyl methacrylate-butyl acrylate copolymer shell coating the surface of the plate-like hexagonal boron nitride. The average thickness of the polymer shell is 10-40 nm, and the surface organic component content of the core-shell modified hexagonal boron nitride, as determined by thermogravimetric analysis, is 4-12 wt.%.
[0014] In a preferred embodiment, in step S4, the polyethersulfone and ionic liquid-modified montmorillonite are vacuum dried at 90–110°C for 3–6 h before being added to the epoxy resin; the alicyclic epoxy resin and biphenyl epoxy resin are mixed and heated to 75–85°C, and after adding the polyethersulfone and ionic liquid-modified montmorillonite, the mixture is stirred at a constant temperature at a speed of 300–500 r / min for 2.0–2.5 h.
[0015] In a preferred embodiment, in step S5, the epoxy resin matrix obtained in step S4 is cooled to 50-60°C and then the silane coupling agent, heptadecafluorodecyltrimethoxysilane, and phosphate wetting and dispersing agent are added; the silane coupling agent is KH-560, and the phosphate wetting and dispersing agent is BYK-111.
[0016] In a preferred embodiment, in S5, the D50 of the spherical alumina is 15-25 μm, the D50 of the spherical aluminum nitride is 8-12 μm, and the D50 of the core-shell modified hexagonal boron nitride is 3-8 μm; the spherical alumina, spherical aluminum nitride, and core-shell modified hexagonal boron nitride are added to the epoxy resin matrix in descending order of particle size for dispersion.
[0017] In a preferred embodiment, in step S6, the mixed system obtained in step S5 is cooled to 20-25°C and then the methyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride and imidazole curing accelerator are added. During the addition process, the system temperature does not exceed 40°C. After mixing, the mixture is degassed for 10-30 minutes under a vacuum of 0.08-0.10 MPa. The adhesive is then cured at 120-150°C for 30-60 minutes.
[0018] In a preferred embodiment, the prepared chip is filled with a high thermal conductivity one-component epoxy adhesive at 25°C and a shear rate of 10 s. - The apparent viscosity under the given conditions is 1500–2500 mPa·s at 25°C and a shear rate of 100 s⁻¹. - The apparent viscosity under the conditions is 800–1500 mPa·s, and the thermal conductivity in the thickness direction after curing is not less than 3.0 W / (m·K).
[0019] Compared with the prior art, the present invention has the following beneficial effects: (1) A stable flexible core-shell interface is constructed by “silane anchoring-in-situ polymerization”, which is different from conventional silane surface modification or polymer physical coating.
[0020] This invention first activates the surface of hexagonal boron nitride (BN), and then uses a silane coupling agent containing polymerizable double bonds to form chemical anchoring points on the BN surface. Methyl methacrylate (MDMA) and butyl acrylate (butyl acrylate) are then polymerized in situ at these anchoring points, thereby forming a stable, flexible polymer shell on the BN surface. This ensures that the polymer layer does not exist in a simple physical adsorption or free state, but is positioned on the BN surface through the silane coupling layer, forming a stable interface structure of "hexagonal boron nitride core—silane anchoring layer—flexible polymer shell," which is beneficial for improving the uniformity and stability of the coating layer.
[0021] (2) The interaction between hexagonal boron nitride sheets is controlled by the MMA / BA flexible polymer shell, which significantly improves the rheological properties of the high-fill thermally conductive adhesive system.
[0022] Under high-filling conditions, plate-like hexagonal boron nitride is prone to plate stacking and aggregation, forming strong filler-filler interactions, which leads to a significant increase in the viscosity of the adhesive system. This invention constructs a flexible MMA / BA copolymer shell on the surface of hexagonal boron nitride. The steric hindrance generated by the polymer chains reduces direct contact and aggregation between the hexagonal boron nitride plates. Simultaneously, the flexible shell can undergo certain deformation under shear, which facilitates relative slippage between the hexagonal boron nitride plates, thereby reducing flow resistance under high-filling conditions and enabling the adhesive to exhibit lower apparent viscosity and good shear-thinning properties.
[0023] Compared to surface modification using only silane coupling agents, this invention further regulates the interaction between fillers through a flexible polymer shell. Therefore, it not only improves the interfacial compatibility between hexagonal boron nitride and epoxy resin, but also regulates the rheological behavior of highly filled systems at the filler-filler interface level.
[0024] (3) While improving the flow properties of the adhesive, it maintains an effective thermal network, achieving a synergistic balance between high thermal conductivity, low viscosity, and good capillary filling performance.
[0025] This invention does not simply improve the flow properties of adhesives by reducing the content of thermally conductive fillers or increasing low-viscosity organic components. Instead, while maintaining a high amount of thermally conductive filler, it reduces the viscosity of the system by adjusting the polymer shell structure on the surface of hexagonal boron nitride. Simultaneously, the plate-like core-shell modified hexagonal boron nitride is graded and compounded with spherical alumina and spherical aluminum nitride of different particle sizes. This allows thermally conductive fillers of different sizes and morphologies to fill and overlap each other, facilitating the formation of continuous multi-scale thermal conduction pathways.
[0026] By controlling the thickness and content of the flexible polymer shell, the increased heat transfer distance between hexagonal boron nitride layers due to excessive polymer thickness can be avoided, thus maintaining low interfacial thermal resistance while improving interface conditions and rheological properties. Therefore, this invention can reduce the apparent viscosity of the adhesive while achieving high thermal conductivity, thereby increasing its capillary filling speed in the tiny gaps between the chip and the packaging substrate. This alleviates the performance contradiction in existing high thermal conductivity underfill adhesives where "increasing the thermally conductive filler content leads to increased system viscosity and decreased micro-gap filling performance."
[0027] (4) Improve the dispersion and interfacial bonding state of hexagonal boron nitride in epoxy resin, and improve the bonding and encapsulation reliability of adhesives.
[0028] The silane coupling layer forms an interfacial bond between the inorganic hexagonal boron nitride and the organic epoxy resin. The flexible polymer shell further improves the organic compatibility and steric stability of the hexagonal boron nitride surface, thereby reducing filler agglomeration. Figures 1-3 SEM morphology analysis revealed that unmodified hexagonal boron nitride, silane-coupled boron nitride, and core-shell modified boron nitride all maintained a lamellar structure, while their surface state and adhesion characteristics changed with the modification process. Combined with FTIR, XPS, TGA, and TEM shell thickness measurements, the formation of the silane coupling layer and polymer coating layer can be further verified. This is beneficial for improving the interfacial compatibility and dispersion stability of hexagonal boron nitride in epoxy systems.
[0029] Therefore, this invention, through targeted design of the micro-interface structure of hexagonal boron nitride surface, synergistically combines the interfacial anchoring effect of silane coupling agent, the rheological regulation effect of MMA / BA flexible polymer shell, and the thermally conductive network construction effect of multi-scale thermally conductive filler. As a result, the obtained single-component epoxy adhesive for chip underfill possesses high thermal conductivity, low viscosity, good micro-gap capillary filling performance, and interfacial adhesion performance, making it suitable for high power density chips and flip-chip packaging applications.
[0030] In this invention, the above-described technical solutions can be combined with each other to achieve more preferred combinations. Other features and advantages of this invention will be set forth in the following description, and some advantages may become apparent from the description or be learned by practicing the invention. The objects and other advantages of this invention can be realized and obtained from what is particularly pointed out in the description and drawings. Attached Figure Description
[0031] Figure 1 The image shows the SEM morphology of the unmodified hexagonal boron nitride used in Comparative Example 1. Figure 2 SEM morphology of hexagonal boron nitride modified only by silane coupling, used in Comparative Example 2; Figure 3 The image shows the SEM morphology of the core-shell modified hexagonal boron nitride prepared in Example 1. Detailed Implementation
[0032] The technical solution of the present invention will be further described below with reference to specific embodiments. However, the present invention should not be limited to these embodiments. Unless specifically stated otherwise, all features can be replaced by other equivalent or similar features. Unless specifically stated otherwise, each feature is only one example of a series of equivalent or similar features. The terminology used in the present invention, unless otherwise stated, generally has the meaning commonly understood by those skilled in the art. In the following embodiments, unless otherwise stated, concentration % refers to mass percentage; all substances used are commercially available.
[0033] Example 1 This embodiment provides a method for preparing a high thermal conductivity underfill single-component epoxy adhesive for chips. Unless otherwise specified, the following raw material amounts are all in parts by weight, and the specific steps include the following.
[0034] S1, hexagonal boron nitride surface activation 100 parts of plate-shaped hexagonal boron nitride with a D50 of 5 μm were added to 1000 parts of nitric acid aqueous solution with a concentration of 2 mol / L. After ultrasonic dispersion for 30 min, the system was heated to 80 °C and stirred at 300 r / min for 4 h to perform surface activation treatment on the plate-shaped hexagonal boron nitride.
[0035] After the reaction was completed, the product was filtered and repeatedly washed with deionized water until the pH of the final washing solution was 7.0. Then, it was dried under vacuum at 80°C for 12 hours to obtain surface-activated hexagonal boron nitride.
[0036] S2, silane coupling modification of hexagonal boron nitride Take 100 parts of the surface-activated hexagonal boron nitride obtained from S1 for later use.
[0037] Mix 475 parts anhydrous ethanol and 25 parts deionized water, add 5 parts vinyltriethoxysilane, adjust the pH of the system to 4.8 with acetic acid, and hydrolyze at 300 r / min for 30 min at 25 °C.
[0038] 100 parts of surface-activated hexagonal boron nitride were added to the above hydrolysate and ultrasonically dispersed for 20 min. The system was then heated to 70 °C and stirred at 400 r / min for 4 h to allow the silanol groups formed by the hydrolysis of vinyltriethoxysilane to undergo a condensation reaction with the active groups on the surface of hexagonal boron nitride, forming a silane coupling layer with polymerizable double bonds on the surface of hexagonal boron nitride.
[0039] After the reaction was completed, the mixture was filtered, washed three times with anhydrous ethanol, and then dried under vacuum at 80°C for 8 hours to obtain silane-coupled modified hexagonal boron nitride.
[0040] S3, Preparation of core-shell modified hexagonal boron nitride Take 100 parts of the silane-coupled modified hexagonal boron nitride obtained from S2, add it to 500 parts of anhydrous ethanol, and ultrasonically disperse for 30 min to obtain a uniform dispersion.
[0041] Add 14 parts of methyl methacrylate and 6 parts of butyl acrylate to the dispersion, and stir at 300 r / min for 30 min under nitrogen protection; then add 0.20 parts of azobisisobutyronitrile as a free radical polymerization initiator, heat the system to 70 °C, and stir at 300 r / min for 6 h.
[0042] During the polymerization process, methyl methacrylate and butyl acrylate undergo a polymerization reaction on the silane-coupled modified hexagonal boron nitride surface to form a methyl methacrylate-butyl acrylate copolymer shell anchored to the hexagonal boron nitride surface through a silane coupling layer.
[0043] After the reaction was completed, the system was cooled to 25°C, filtered, and washed three times with anhydrous ethanol to remove unreacted monomers and free polymers. Then it was dried under vacuum at 60°C for 12 hours to obtain core-shell modified hexagonal boron nitride.
[0044] Transmission electron microscopy revealed that the obtained core-shell modified hexagonal boron nitride maintained a lamellar structure, with a continuous polymer coating layer forming on the surface of the hexagonal boron nitride. The average thickness of the polymer shell layer was 24.8 nm. Thermogravimetric analysis showed that the surface organic component content of the core-shell modified hexagonal boron nitride was 8.1 wt.%. The D50 of the obtained core-shell modified hexagonal boron nitride was 5 μm.
[0045] S4. Preparation of epoxy resin matrix Take 20 parts of alicyclic epoxy resin 2021P, 15 parts of biphenyl epoxy resin YX4000H, 2 parts of PES polyethersulfone ultrafine powder 3600P, and 2 parts of ionic liquid modified montmorillonite IL-MMT.
[0046] PES polyethersulfone ultrafine powder and ionic liquid modified montmorillonite were dried at 100℃ under vacuum for 4 hours.
[0047] Twenty parts of alicyclic epoxy resin 2021P and 15 parts of biphenyl epoxy resin YX4000H were added to a reaction vessel and heated to 80°C. The mixture was stirred at 300 r / min for 20 min. Subsequently, two parts of PES polyethersulfone ultrafine powder and two parts of ionic liquid modified montmorillonite were added. The mixture was stirred at 400 r / min at 80°C for 2.5 h to allow the PES to fully swell and the ionic liquid modified montmorillonite to be uniformly dispersed in the epoxy resin system, thus obtaining the epoxy resin matrix.
[0048] S5. Addition and dispersion of thermally conductive filler The epoxy resin matrix obtained from S4 was cooled to 55°C, and 1.5 parts of silane coupling agent KH-560, 1.5 parts of heptadecafluorodecyltrimethoxysilane and 1.5 parts of phosphate ester wetting and dispersing agent BYK-111 were added sequentially. The mixture was stirred at 400 r / min for 20 min.
[0049] Then, thermally conductive fillers are added in descending order of particle size: First, add 25 parts of spherical alumina with a D50 of 20 μm and disperse at 1000 r / min for 20 min; Then 25 parts of spherical aluminum nitride with a D50 of 10 μm were added and dispersed at 1200 r / min for 20 min; Finally, 35 parts of core-shell modified hexagonal boron nitride with a D50 of 5 μm obtained from S3 were added and dispersed at 1500 r / min for 30 min.
[0050] Through the above-mentioned graded addition and dispersion, spherical alumina, spherical aluminum nitride, and core-shell modified hexagonal boron nitride are uniformly distributed in the epoxy resin matrix, forming a multi-scale graded thermally conductive filler system.
[0051] S6, Curing System Addition and Vacuum Degassing The mixture obtained from S5 was cooled to 23°C, and 15 parts of methyltetrahydrophthalic anhydride, 15 parts of dodecenylsuccinic anhydride, and 3 parts of imidazole latent curing accelerator PN-23 were added.
[0052] The system temperature was controlled at 30℃, and the mixture was stirred at 300r / min for 20min to ensure that all components were fully mixed.
[0053] After mixing, the mixture was vacuum degassed for 15 minutes under a vacuum of 0.095 MPa to obtain a high thermal conductivity single-component epoxy adhesive for chip filling.
[0054] The resulting adhesive was cured at 135°C for 45 minutes.
[0055] The core-shell modified hexagonal boron nitride prepared in Example 1 was observed by SEM, and its morphology is as follows: Figure 3 As shown. By Figure 3 It can be seen that after VTES silane coupling modification and further MMA / BA in-situ polymerization, hexagonal boron nitride still maintains its basic lamellar morphology. Figures 1-3 It can be seen that all samples maintained a plate-like main morphology. The surface morphology and particle aggregation state of hexagonal boron nitride varied at different modification stages, indicating that the surface modification process did not significantly damage the main structure of hexagonal boron nitride. The formation of the polymer coating layer was further confirmed by FTIR, XPS, TGA, and TEM test results.
[0056] Comparative Examples 1-5 Unless otherwise specified, the preparation of the epoxy resin matrix, the amount of spherical alumina and spherical aluminum nitride added, the curing system, the dispersion process, the vacuum degassing process and the curing conditions in each comparative example are the same as in Example 1, so as to ensure that the main difference between each group lies in the surface structure of hexagonal boron nitride and the construction method of the polymer shell.
[0057] Comparative Example 1: Using unmodified hexagonal boron nitride The difference between this comparative example and Example 1 is that the surface activation, silane coupling modification, and polymer coating treatment of the sheet-like hexagonal boron nitride are not performed. Instead, the unmodified sheet-like hexagonal boron nitride is used directly as the thermally conductive filler.
[0058] Specifically, 100 parts of flake-shaped hexagonal boron nitride with a D50 of 5 μm were dried under vacuum at 80 °C for 12 h to obtain dried unmodified hexagonal boron nitride.
[0059] The epoxy resin matrix was prepared according to the method in S4 of Example 1. The obtained epoxy resin matrix was cooled to 55°C, and 1.5 parts of silane coupling agent KH-560, 1.5 parts of heptadecafluorodecyltrimethoxysilane and 1.5 parts of phosphate ester wetting and dispersing agent BYK-111 were added in sequence, and stirred at 400 r / min for 20 min.
[0060] Subsequently, 25 parts of spherical alumina with a D50 of 20 μm, 25 parts of spherical aluminum nitride with a D50 of 10 μm, and 35 parts of the above-mentioned unmodified hexagonal boron nitride were added in sequence. The dispersion process of each thermally conductive filler was the same as in Example 1.
[0061] Subsequently, following the method in S6 of Example 1, 15 parts of methyltetrahydrophthalic anhydride, 15 parts of dodecenylsuccinic anhydride, and 3 parts of imidazole latent curing accelerator PN-23 were added. After mixing and vacuum degassing, the high thermal conductivity single-component epoxy adhesive for chip filling of Comparative Example 1 was obtained and cured at 135°C for 45 min.
[0062] This comparative example is used to evaluate the performance differences between hexagonal boron nitride without any surface treatment and the core-shell modified hexagonal boron nitride of Example 1.
[0063] The SEM morphology of the unmodified hexagonal boron nitride used in Comparative Example 1 is as follows: Figure 1 As shown. By Figure 1 It can be seen that the unmodified hexagonal boron nitride mainly has a plate-like structure with a relatively flat surface, serving as a morphological reference for subsequent silane coupling modification and core-shell modification.
[0064] Comparative Example 2: Hexagonal boron nitride modified only by silane coupling The difference between this comparative example and Example 1 is that a silane coupling layer is constructed only on the surface of hexagonal boron nitride, without further polymerization and coating of methyl methacrylate and butyl acrylate.
[0065] Following the method in S1 of Example 1, 100 parts of sheet-like hexagonal boron nitride with a D50 of 5 μm were subjected to surface activation treatment to obtain surface-activated hexagonal boron nitride.
[0066] Subsequently, following the method in S2 of Example 1, 475 parts of anhydrous ethanol and 25 parts of deionized water were mixed, 5 parts of vinyltriethoxysilane were added, the pH of the system was adjusted to 4.8, and hydrolysis was carried out at 25°C for 30 min; 100 parts of surface-activated hexagonal boron nitride were added, and after ultrasonic dispersion for 20 min, the mixture was reacted at 70°C and 400 r / min for 4 h.
[0067] After the reaction was completed, the mixture was filtered, washed, and dried under vacuum at 80°C for 8 hours to obtain hexagonal boron nitride modified only by vinyltriethoxysilane.
[0068] The S3 polymerization reaction in Example 1 was not carried out.
[0069] The adhesive was prepared according to the methods in S4 and S5 of Example 1, wherein the core-shell modified hexagonal boron nitride was replaced with 35 parts of the above-mentioned silane-coupled modified hexagonal boron nitride, and the composition, order of addition and dispersion conditions of the remaining raw materials were the same as those in Example 1.
[0070] Subsequently, the curing agent and curing accelerator were added according to the method in S6 of Example 1, and after vacuum degassing, the mixture was cured at 135°C for 45 minutes.
[0071] This comparative example is used to evaluate whether surface modification using silane coupling agents alone can achieve the same rheological control and thermal conductivity effects as "silane anchoring + flexible polymer shell".
[0072] The SEM morphology of the hexagonal boron nitride modified only by silane coupling in Comparative Example 2 is as follows: Figure 2 As shown. With Figure 1 Compared to unmodified hexagonal boron nitride, Figure 2 The hexagonal boron nitride still maintains its plate-like morphology, but its surface condition has changed. Combined with the presence of Si-O related signals and Si elemental signals in the FTIR and XPS detections described later, it can be verified that VTES has been introduced into the hexagonal boron nitride surface.
[0073] Comparative Example 3: Hexagonal boron nitride coated with a silane-free anchored physical polymer The difference between this comparative example and Example 1 is that the hexagonal boron nitride undergoes only the same surface activation treatment as in Example 1, but without VTES silane coupling modification. Instead, the surface-activated hexagonal boron nitride is physically coated with a pre-prepared methyl methacrylate-butyl acrylate copolymer.
[0074] First, following the method in S1 of Example 1, 100 parts of sheet-like hexagonal boron nitride with a D50 of 5 μm were subjected to surface activation treatment to obtain surface-activated hexagonal boron nitride.
[0075] Separately, 14 parts of methyl methacrylate and 6 parts of butyl acrylate were added to 500 parts of anhydrous ethanol, and 0.20 parts of azobisisobutyronitrile were added under nitrogen protection. The polymerization reaction was carried out at 70℃ and 300 r / min for 6 h to obtain a methyl methacrylate-butyl acrylate copolymer dispersion. The solid content of the copolymer dispersion was then determined.
[0076] A certain amount of copolymer dispersion is taken according to the solid content of the copolymer dispersion, so that the mass ratio of the copolymer solid contained therein to 100 parts of the surface-activated hexagonal boron nitride is about 8.7:100; the two are mixed and ultrasonically dispersed for 30 min, and stirred at 50℃ and 300 r / min for 4 h, so that the copolymer is attached to the surface of hexagonal boron nitride through physical adsorption.
[0077] The solvent was then removed under reduced pressure, and the mixture was dried under vacuum at 60°C for 12 hours to obtain physically polymer-coated hexagonal boron nitride. TGA testing showed that the surface organic component content was 8.0 wt.%, which was essentially consistent with the surface organic component content of the core-shell modified hexagonal boron nitride in Example 1.
[0078] The adhesive was prepared according to the methods in S4 to S6 of Example 1, wherein 35 parts of the core-shell modified hexagonal boron nitride obtained in Example 1 were replaced with 35 parts of the above-mentioned physical polymer-coated hexagonal boron nitride, and the remaining raw material composition and process parameters remained unchanged.
[0079] The resulting adhesive was cured at 135°C for 45 minutes.
[0080] This comparative example is used to evaluate whether, under the same activation conditions and organic component content on the surface of hexagonal boron nitride, forming an MMA / BA copolymer coating layer solely through physical adsorption can produce the same technical effect as the in-situ polymerized core-shell structure chemically anchored by silane.
[0081] Comparative Example 4: Direct compounding of silane-modified hexagonal boron nitride with free MMA / BA copolymer The difference between this comparative example and Example 1 is that the methyl methacrylate-butyl acrylate copolymer is not polymerized in situ on the surface of hexagonal boron nitride to form a polymer shell, but is directly added to the epoxy resin system in the form of a free polymer.
[0082] Vinyltriethoxysilane-modified hexagonal boron nitride was prepared according to the methods S1 and S2 in Example 1.
[0083] In another case, 14 parts of methyl methacrylate and 6 parts of butyl acrylate were added to 500 parts of anhydrous ethanol, and 0.20 parts of azobisisobutyronitrile were added under nitrogen protection. The polymerization reaction was carried out at 70℃ and 300 r / min for 6 h. After the reaction was completed, the solvent was removed and the product was dried under vacuum at 60℃ for 12 h to obtain methyl methacrylate-butyl acrylate copolymer.
[0084] Based on the surface organic component content of the core-shell modified hexagonal boron nitride obtained in Example 1, measured by TGA, 32.75 parts of vinyltriethoxysilane modified hexagonal boron nitride and 2.25 parts of methyl methacrylate-butyl acrylate copolymer were used to replace the 35 parts of core-shell modified hexagonal boron nitride in Example 1, so that the inorganic component content and total organic component content of hexagonal boron nitride in this comparative example are basically consistent with those in Example 1.
[0085] The 2.25 parts of methyl methacrylate-butyl acrylate copolymer were added and fully dispersed during the preparation of the epoxy resin matrix; the 32.75 parts of vinyltriethoxysilane-modified hexagonal boron nitride were added in the manner of adding the thermally conductive filler S5 in Example 1.
[0086] Except for the differences mentioned above, the preparation processes of the alicyclic epoxy resin, biphenyl-type epoxy resin, PES polyethersulfone, ionic liquid modified montmorillonite, spherical alumina, spherical aluminum nitride, silane coupling agent, wetting and dispersing agent, curing agent, curing accelerator, and other components in this comparative example are the same as those in Example 1.
[0087] This comparative example is used to compare the effects of two spatial distribution methods on the rheology, capillary filling and thermal conductivity of the adhesive, under the condition that the content of hexagonal boron nitride and the total amount of organic components are basically the same: the polymer is constructed in situ on the surface of hexagonal boron nitride to form a core-shell structure, and the polymer is directly added to the epoxy resin system.
[0088] Comparative Example 5: Hexagonal boron nitride modified with a PMMA rigid polymer shell The difference between this comparative example and Example 1 is that the polymer shell is formed only by methyl methacrylate, without the addition of the flexible monomer butyl acrylate.
[0089] Silane-coupled modified hexagonal boron nitride was prepared according to the methods S1 and S2 in Example 1.
[0090] Take 100 parts of the silane-coupled modified hexagonal boron nitride and add it to 500 parts of anhydrous ethanol, and ultrasonically disperse for 30 min.
[0091] Add 20 parts of methyl methacrylate to the obtained dispersion, without adding butyl acrylate, and stir at 300 r / min for 30 min under nitrogen protection; then add 0.20 parts of azobisisobutyronitrile, raise the temperature of the reaction system to 70℃, and polymerize at a constant temperature of 300 r / min for 6 h.
[0092] After the reaction was completed, the mixture was cooled, filtered, washed, and dried under vacuum at 60°C for 12 hours to obtain core-shell modified hexagonal boron nitride with hexagonal boron nitride as the core and polymethyl methacrylate as the shell.
[0093] By adjusting the polymerization reaction conditions, the average thickness of the obtained PMMA shell was 25.3 nm and the surface organic component content was 8.2 wt.%, which were basically consistent with the thickness and organic component content of the MMA / BA flexible copolymer shell in Example 1.
[0094] The adhesive was prepared according to the methods in S4 to S6 of Example 1, except that the 35 parts of MMA / BA core-shell modified hexagonal boron nitride in Example 1 were replaced with 35 parts of the above-mentioned PMMA core-shell modified hexagonal boron nitride, while the rest of the formulation composition and process parameters remained unchanged.
[0095] The resulting adhesive was cured at 135°C for 45 minutes.
[0096] This comparative example is used to evaluate the effect of the flexible structure of the polymer shell on the rheological properties of the high-fill thermal conductivity system, and to verify the role of adding butyl acrylate to form a flexible copolymer shell.
[0097] The performance of the hexagonal boron nitride material and the high thermal conductivity underfill single-component epoxy adhesive for chips obtained in Example 1 and Comparative Examples 1-5 were tested under the same test conditions.
[0098] 1. Microscopic morphology and core-shell structure testing The surface morphologies of the unmodified hexagonal boron nitride used in Comparative Example 1, the hexagonal boron nitride modified only by silane coupling used in Comparative Example 2, and the core-shell modified hexagonal boron nitride prepared in Example 1 were observed using scanning electron microscopy (SEM). The test results correspond to... Figure 1 , Figure 2 and Figure 3 For samples with polymer coatings, transmission electron microscopy (TEM) was used to measure the thickness of the polymer shell. At least 20 measurement points were selected in different regions to calculate the average thickness of the polymer shell.
[0099] Test results are expressed as average shell thickness (nm).
[0100] 2. Fourier transform infrared spectroscopy test Fourier transform infrared spectroscopy (FTIR) was used to test unmodified hexagonal boron nitride, silane-coupled modified hexagonal boron nitride, and polymer-coated modified hexagonal boron nitride.
[0101] Record the positions of characteristic absorption peaks of BN bonds, Si-O related groups, and C=O groups in the polymer. By comparing the changes in characteristic absorption peaks before and after modification, evaluate the introduction of silane coupling agent and methyl methacrylate-butyl acrylate copolymer onto the hexagonal boron nitride surface.
[0102] The test results are expressed as the positions of the main characteristic absorption peaks.
[0103] 3. X-ray photoelectron spectroscopy (XPS) Surface elemental analysis was performed on unmodified hexagonal boron nitride, silane-coupled modified hexagonal boron nitride, and core-shell modified hexagonal boron nitride using X-ray photoelectron spectroscopy (XPS).
[0104] The content of B, N, Si, C and O elements on the sample surface was determined, and the characteristic binding energies of B 1s, Si 2p, C 1s and O 1s were recorded.
[0105] The formation of silane coupling layer and polymer coating layer was evaluated by comparing the changes in the content and chemical state of B, Si, C and O elements on the surface of each sample.
[0106] The test results are expressed as the atomic percentage of each element and its characteristic binding energy.
[0107] 4. TGA weight loss and surface organic component content test Thermogravimetric analysis (TGA) was used to test unmodified hexagonal boron nitride, silane-coupled modified hexagonal boron nitride, and polymer-coated modified hexagonal boron nitride.
[0108] The test was conducted under a nitrogen atmosphere, with the temperature increased from room temperature to 800°C at a rate of 10°C / min.
[0109] Record the baseline weight loss of unmodified hexagonal boron nitride within the test temperature range, and calculate the content of surface organic components introduced during the modification process based on the mass loss difference between modified and unmodified hexagonal boron nitride in the thermal decomposition temperature range of organic components.
[0110] The surface organic component content is calculated according to the following formula: Surface organic component content / % = Organic weight loss rate of modified hexagonal boron nitride - Baseline weight loss rate of unmodified hexagonal boron nitride.
[0111] Test results are expressed as surface organic component content (wt.%); unmodified hexagonal boron nitride is indicated by "—".
[0112] 5. Rheological performance testing The rheological properties of the uncured adhesives obtained in Example 1 and Comparative Examples 1-5 were tested using a rotational rheometer.
[0113] The test temperature was 25℃, and the shear rate was measured at 10 s⁻¹. - ¹ and 100 s - ¹ Apparent viscosity under the given conditions.
[0114] By comparing Example 1 with Comparative Examples 1-5, the results were obtained in 10 seconds. - ¹ and 100 s - ¹ Apparent viscosity under certain conditions to evaluate the effect of different hexagonal boron nitride surface structures on the rheological properties of highly filled thermally conductive adhesives.
[0115] 6. Capillary Filling Performance Test The capillary filling performance of the adhesives obtained in Example 1 and Comparative Examples 1-5 was tested by using a parallel plate to simulate the bottom filling gap of the chip.
[0116] Two flat glass plates were placed in parallel, and the gap between the two glass plates was controlled to be 50 μm using spacers. The test temperature was 25℃.
[0117] Add an equal amount of the adhesive to be tested to one end of the parallel plates, allowing the adhesive to enter the gap between the parallel plates by itself under capillary action, and record the time required for the adhesive to fill from the inlet to a distance of 10 mm.
[0118] Each group of samples was tested in parallel three times and the average value was taken.
[0119] The shorter the capillary filling time, the better the flow and filling performance of the adhesive in the micro-gaps of the chip.
[0120] 7. Thermal conductivity test The adhesives obtained in Example 1 and Comparative Examples 1-5 were cured under the same conditions, and test specimens of the same size were prepared.
[0121] The thermal diffusivity in the thickness direction of the cured sample was tested using the laser flash method, and the thermal conductivity was calculated by combining the sample density and specific heat capacity. λ=α×ρ×Cp In the formula: λ is the thermal conductivity, W / (m·K); α is the thermal diffusivity; ρ is the sample density; Cp is the sample specific heat capacity. Three parallel samples were tested in each group and the average value was taken.
[0122] 8. Shear strength test The adhesives obtained in Example 1 and Comparative Examples 1-5 were applied between the same substrates, and the coating area and adhesive layer thickness were kept consistent. The adhesives were then cured at 135°C for 45 min.
[0123] After curing, the lap shear strength was tested using a universal testing machine at room temperature.
[0124] Each group of samples shall be tested with no fewer than 5 parallel specimens, and the average value shall be taken as the shear strength of the group of samples. The test results shall be expressed in MPa.
[0125] The test results are shown in Table 1 below.
[0126] Table 1 Note: In Comparative Example 4, 1.8 wt.% is the surface organic component content of vinyltriethoxysilane-modified hexagonal boron nitride as measured by TGA; its MMA / BA copolymer is added directly to the epoxy resin system in free form and is not included in the surface organic component content of hexagonal boron nitride.
[0127] Test results and data analysis The modified hexagonal boron nitride and the high thermal conductivity underfill single-component epoxy adhesive for chips obtained in Example 1 and Comparative Examples 1-5 were characterized in terms of structure, rheological properties, capillary filling properties, thermal conductivity and shear strength. The results are as follows.
[0128] 1. Analysis of Core-Shell Structure and Surface Modification Results Depend on Figures 1-3 SEM observations revealed that the unmodified hexagonal boron nitride used in Comparative Example 1 primarily exhibited a plate-like structure with a relatively smooth surface. Comparative Example 2, after VTES silane coupling modification, still maintained its plate-like morphology, although its surface condition underwent some changes. In Example 1, further in-situ polymerization with MMA / BA resulted in hexagonal boron nitride retaining its plate-like structure, while surface roughness and adhesion characteristics became more pronounced. These morphological comparisons indicate that the two surface modification steps did not significantly damage the main structure of the hexagonal boron nitride, nor did they cause a gradual change in its surface condition. Furthermore, TEM quantitative analysis showed that the average thickness of the polymer shell of the core-shell modified hexagonal boron nitride obtained in Example 1 was 24.8 nm.
[0129] Comparative Example 3 used MMA / BA copolymer to physically coat hexagonal boron nitride. Although a polymer layer with an average thickness of 22.6 nm was observed on its surface, the polymer layer exhibited local discontinuities and uneven thickness distribution. Comparative Example 5 used VTES anchoring to form a PMMA shell, with an average shell thickness of 25.3 nm, which was basically equivalent to that of Example 1.
[0130] It can be seen that the polymer coating thickness of Example 1 is similar to that of Comparative Examples 3 and 5. Therefore, the subsequent differences in rheological and thermal conductivity are not simply due to the difference in polymer coating amount or shell thickness, but are related to the formation mode and composition structure of the polymer shell.
[0131] The FTIR test results are shown in Table 2. Comparative Example 1, the unmodified hexagonal boron nitride, mainly exhibits the characteristic absorption peak of BN; Comparative Example 2, after VTES modification, shows the addition of Si-O related characteristic absorption peaks; Example 1 further shows the characteristic absorption peak of the acrylate polymer C=O, indicating that the silane coupling agent and MMA / BA copolymer have been sequentially introduced into the surface of the hexagonal boron nitride. The XPS test results are shown in Table 3. The content of Si, C, and O elements on the surface of Example 1 is significantly increased compared to the unmodified hexagonal boron nitride, and characteristic binding energy signals corresponding to the silane layer and acrylate structure are detected, which corroborates the FTIR results.
[0132] The positions of the main characteristic absorption peaks of FTIR are shown in Table 2 below.
[0133] Table 2 The percentage of atomic elements on the XPS surface is shown in Table 3 below.
[0134] Table 3 In the binding energy analysis, the main peak of B 1s in Comparative Example 1 was located at approximately 190.4 eV; a Si 2p signal of approximately 102.5 eV was detected in Comparative Example 2; in Example 1, B 1s was detected at approximately 190.4 eV, Si 2p at approximately 102.6 eV, C 1s showed component peaks at approximately 284.8 eV, 286.5 eV, and 288.8 eV, and the main peak of O 1s was located at approximately 532.8 eV.
[0135] The TGA test results showed that the surface organic component content of the core-shell modified hexagonal boron nitride obtained in Example 1 was 8.1 wt.%; the surface organic component content of the hexagonal boron nitride modified only by VTES in Comparative Example 2 was 1.8 wt.%; the organic component content of physically coated hexagonal boron nitride in Comparative Example 3 and PMMA core-shell hexagonal boron nitride in Comparative Example 5 were 8.0 wt.% and 8.2 wt.% respectively, which were basically equivalent to those of Example 1.
[0136] The above results indicate that, under the condition that the polymer shell thickness and organic component content are basically the same, the effects of different interface construction methods and shell composition on the overall performance of the adhesive can be further compared.
[0137] 2. Rheological property analysis The test results show that in 10 seconds - ¹ and 100 s - ¹Under the test conditions, Example 1 had the lowest apparent viscosity among all groups, indicating that its highly filled system has good shear flow properties.
[0138] At a shear rate of 10 s - ¹At this time, the apparent viscosity of Example 1 was 1850 mPa·s, which was about 64.4% lower than that of Comparative Example 1 with unmodified hexagonal boron nitride and about 52.0% lower than that of Comparative Example 2 with silane modification using only VTES.
[0139] The results indicate that although simply using a silane coupling agent to improve the compatibility between hexagonal boron nitride and resin can reduce the viscosity of the system to a certain extent, it still cannot achieve the rheological improvement effect achieved in Example 1. Further constructing a flexible polymer shell on the surface of hexagonal boron nitride is an important factor in achieving low viscosity in a high-filling system.
[0140] Comparative Example 3 used an MMA / BA copolymer of the same composition to physically coat hexagonal boron nitride, and its 10 s - ¹The apparent viscosity was 3100 mPa·s, significantly higher than the 1850 mPa·s of Example 1. This represents a decrease of approximately 40.3% compared to Comparative Example 3.
[0141] Since the organic component contents on the surfaces of the two are 8.1 wt.% and 8.0 wt.%, respectively, and the coating thickness is similar, the effect of viscosity reduction caused by simply "increasing the amount of polymer added" can be ruled out. This indicates that anchoring the MMA / BA copolymer to the hexagonal boron nitride surface through the silane coupling layer to form a stable core-shell interface has a more significant rheological regulation effect than physical adsorption coating.
[0142] In Comparative Example 4, hexagonal boron nitride was only modified with VTES, and an MMA / BA copolymer of approximately the same amount as in Example 1 was directly added to the epoxy resin system in free form. Under conditions where the inorganic hexagonal boron nitride content and the total organic components of the system were essentially the same, Comparative Example 4 achieved a [resin content missing] within 10 s [time missing]. - The apparent viscosity at ¹ still reached 3350 mPa·s, while that in Example 1 was only 1850 mPa·s, a reduction of about 44.8%.
[0143] This result further illustrates that the rheological improvement effect of the present invention does not originate from the simple superposition of components of "silane-modified hexagonal boron nitride + MMA / BA copolymer", but is closely related to the formation of a specific core-shell structure by the MMA / BA copolymer being positioned on the surface of hexagonal boron nitride through silane anchoring points.
[0144] Both Comparative Example 5 and Example 1 used VTES anchoring to form polymer core-shell structures, and their shell thickness and organic component content were basically the same. However, Comparative Example 5 used PMMA as the shell, and its 10 s - ¹The apparent viscosity was 2700 mPa·s. After using the MMA / BA flexible copolymer shell in Example 1, the apparent viscosity was further reduced to 1850 mPa·s, a reduction of about 31.5%.
[0145] This indicates that, compared to a single PMMA shell, the MMA / BA copolymer shell formed by introducing a flexible butyl acrylate structure is more conducive to reducing the interaction between hexagonal boron nitride sheets and promoting the relative slippage of fillers during shearing, thereby obtaining a lower system viscosity.
[0146] 3. Capillary Filling Performance Analysis The capillary filling time in Example 1 was only 38 s, which was significantly shorter than that of the comparative examples.
[0147] Compared with Comparative Example 1, which was not modified hexagonal boron nitride, the filling time was reduced by approximately 69.6%; compared with Comparative Example 2, which was modified with VTES only, the filling time was reduced by approximately 58.2%.
[0148] In Comparative Example 4, with the same hexagonal boron nitride content and total organic components, the capillary filling time was still 80 s, while in Example 1 it was only 38 s, a reduction of 52.5%. This indicates that although the free flexible polymer can change the fluidity of the system to a certain extent, it cannot achieve the same interface regulation effect as the core-shell structure.
[0149] Compared to Comparative Example 5, which uses a rigid PMMA shell, Example 1 shows that the capillary filling time was further reduced from 60 s to 38 s, a reduction of approximately 36.7%, consistent with the rheological test results.
[0150] This demonstrates that the silane-anchored MMA / BA flexible polymer core-shell structure formed in Example 1 can effectively improve the shear flow and capillary filling performance of the adhesive under high thermal conductivity filler high filling conditions, making the adhesive more suitable for bottom filling of tiny gaps between the chip and the substrate.
[0151] 4. Thermal conductivity analysis The test results show that Example 1 significantly reduced the viscosity of the system and improved the capillary filling performance, while its thermal conductivity still reached 3.24 W / (m·K), and the thermal conductivity was not reduced due to the introduction of the flexible polymer shell.
[0152] Although Comparative Example 3 has essentially the same surface organic component content as Example 1, its thermal conductivity is only 2.98 W / (m·K). In contrast, Example 1 shows an improvement of approximately 8.7%.
[0153] This indicates that polymer layers formed by ordinary physical coating may have uneven distribution and interface defects. However, chemical anchoring through silane coupling layers and constructing a stable core-shell interface on the hexagonal boron nitride surface can improve the interfacial contact state between the filler and the resin and reduce the heat transfer resistance caused by interface defects.
[0154] Compared with Comparative Example 5, Example 1, with basically the same shell thickness and surface organic component content, showed an increase in thermal conductivity from 3.10 W / (m·K) to 3.24 W / (m·K), while its system viscosity and capillary filling time were significantly reduced.
[0155] Therefore, the present invention does not achieve fluidity at the expense of thermal conductivity by increasing low-viscosity organic components, but rather achieves a synergistic improvement between high thermal conductivity and low viscosity and high capillary flow properties.
[0156] 5. Shear strength analysis The adhesive obtained in Example 1 has a shear strength of 11.9 MPa, which is higher than that of the comparative examples.
[0157] Compared with unmodified hexagonal boron nitride, the interfacial bonding between core-shell modified hexagonal boron nitride and epoxy resin is significantly improved; compared with physically coated Comparative Example 3, the shear strength of Example 1 increased from 9.5 MPa to 11.9 MPa, indicating that the chemical anchoring structure formed by the silane coupling layer is beneficial to reducing interfacial defects between the filler and the epoxy resin.
[0158] The shear strength results are consistent with the surface modification results characterized by FTIR, XPS and TGA, indicating that core-shell modification did not weaken the interfacial bonding performance of the adhesive and is beneficial to obtaining a more stable inorganic filler / epoxy resin interface.
[0159] The results above show that: Unmodified hexagonal boron nitride has poor compatibility with epoxy resin, which easily leads to particle agglomeration and strong interlamellar interactions, resulting in high system viscosity and slow capillary filling speed. After silane coupling modification using VTES, the interfacial compatibility between hexagonal boron nitride and epoxy resin can be improved, and the viscosity and filling performance of the system can be improved to a certain extent. However, simple silane modification still cannot obtain the comprehensive performance of Example 1. Physical coating with MMA / BA copolymer or direct compounding of VTES-modified hexagonal boron nitride with MMA / BA copolymer, although the system has the same or similar chemical composition as Example 1, its rheological, capillary filling and thermal conductivity are significantly lower than those of Example 1, indicating that the technical effect of the present invention does not come from a simple mixing or physical coating of known components. Although the rigid core-shell structure of PMMA can improve the interfacial state of hexagonal boron nitride, its ability to reduce system viscosity and improve capillary flowability is still weaker than that of Example 1.
[0160] Example 1 involves first constructing a silane coupling layer with polymerizable reactive sites on the surface of hexagonal boron nitride (BN), and then further polymerizing MMA and BA in situ to form a flexible polymer shell, which stably positions the polymer shell on the BN surface. The resulting flexible core-shell interface reduces the direct interaction between BN sheets under high-filling conditions, facilitating relative slippage of the sheets under shear stress, thereby significantly reducing the apparent viscosity of the system and improving the capillary filling performance of micro-gaps. Furthermore, the silane coupling layer maintains a stable interfacial connection between BN and the epoxy matrix, reducing interfacial defects and avoiding significant loss of thermal conductivity due to the introduction of the flexible organic shell.
[0161] Therefore, in Example 1, while achieving a thermal conductivity of 3.24 W / (m·K), 10 s -The apparent viscosity was controlled at 1850 mPa·s under the specified conditions, and the capillary filling time of 10 mm in a 50 μm gap was shortened to 38 s, achieving a synergistic balance of high thermal conductivity, low viscosity and good micro-gap filling performance.
[0162] In particular, Example 1 and Comparative Example 4 are basically the same in terms of main material composition and inorganic / organic component content, but the only substantial difference between them is in the spatial existence mode of the MMA / BA copolymer. Example 1 still shows significantly lower apparent viscosity, shorter capillary filling time and higher thermal conductivity, indicating that the technical effect obtained by the present invention cannot be simply attributed to the superposition of the properties of each raw material component, but is closely related to the specific structural construction mode of "silane anchoring - surface in-situ polymerization - flexible core-shell interface".
[0163] This demonstrates that the present invention achieves a balance between thermal conductivity and processing flow properties under high thermal conductivity filler filling conditions through specific core-shell interface structure control, thus solving the problem that increasing the content of thermally conductive filler in high thermal conductivity underfill adhesives easily leads to increased system viscosity and decreased micro-gap filling performance.
[0164] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by those skilled in the art within the scope of the technology disclosed in the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing a high thermal conductivity bottom-filling single-component epoxy adhesive for chips, characterized in that, Includes the following steps: S1, Surface activation of hexagonal boron nitride: By mass, 100 parts of flake-shaped hexagonal boron nitride were added to 800-1200 parts of nitric acid aqueous solution with a concentration of 1-3 mol / L for surface activation treatment. After the reaction was completed, the surface-activated hexagonal boron nitride was obtained by washing and drying. S2, silane coupling modification: 100 parts of the surface-activated hexagonal boron nitride were dispersed in a mixed solvent consisting of 400-600 parts of ethanol and 20-50 parts of water. 3-8 parts of vinyltriethoxysilane were added to react with the active groups on the surface of the hexagonal boron nitride, forming a silane coupling layer with polymerizable double bonds on the surface of the hexagonal boron nitride. After washing and drying, silane-coupled modified hexagonal boron nitride was obtained. S3, Preparation of core-shell modified hexagonal boron nitride: 100 parts of the silane-coupled modified hexagonal boron nitride were dispersed in 400-600 parts of organic solvent, and 10-18 parts of methyl methacrylate, 4-10 parts of butyl acrylate and 0.1-0.4 parts of free radical polymerization initiator were added to carry out a polymerization reaction, so that methyl methacrylate and butyl acrylate polymerized on the silane coupling layer on the surface of hexagonal boron nitride to form a flexible polymer shell. After separation, washing and drying, core-shell modified hexagonal boron nitride was obtained. S4. Preparation of epoxy resin matrix: By weight, 10-30 parts of alicyclic epoxy resin and 10-20 parts of biphenyl epoxy resin are mixed and heated, and 1-3 parts of polyethersulfone and 1-3 parts of ionic liquid modified montmorillonite are added. Under heating and stirring conditions, the polyethersulfone and ionic liquid modified montmorillonite are dispersed in the epoxy resin to obtain an epoxy resin matrix. S5. Addition and dispersion of thermally conductive filler: After cooling the epoxy resin matrix obtained from S4, 1-2 parts of silane coupling agent, 1-2 parts of heptadecafluorodecyltrimethoxysilane and 1-2 parts of phosphate ester wetting and dispersing agent are added. Then, 20-30 parts of spherical alumina, 20-30 parts of spherical aluminum nitride and 30-40 parts of core-shell modified hexagonal boron nitride obtained from S3 are added and dispersed to form a multi-scale graded thermally conductive filler system. S6. Addition and degassing of the curing system: After cooling the mixture obtained from S5, add 10-20 parts of methyltetrahydrophthalic anhydride, 10-20 parts of dodecenylsuccinic anhydride, and 1-5 parts of imidazole curing accelerator. After mixing evenly, perform vacuum degassing to obtain the high thermal conductivity underfill single-component epoxy adhesive for the chip.
2. The preparation method according to claim 1, characterized in that, In S1, the D50 of the plate-like hexagonal boron nitride is 3-8 μm; the surface activation treatment temperature is 70-90℃ and the treatment time is 3-6 h; after the surface activation treatment is completed, the surface is washed with deionized water until the pH value of the washing solution is 6.5-7.5, and then vacuum dried at 70-90℃ for 8-16 h.
3. The preparation method according to claim 1, characterized in that, In S2, based on a total mass of ethanol and water in the mixed solvent of 100 parts, ethanol comprises 90-98 parts and water comprises 2-10 parts; after vinyltriethoxysilane is added to the mixed solvent, the pH of the system is adjusted to 4.0-6.0 and hydrolyzed for 20-60 min, and then the surface-activated hexagonal boron nitride is added, and the reaction is carried out at 60-80°C for 2-5 h.
4. The preparation method according to claim 1, characterized in that, In S3, the mass ratio of methyl methacrylate to butyl acrylate is (1.2-3.5):1, the free radical polymerization initiator is azobisisobutyronitrile, the polymerization reaction temperature is 60-75℃, and the polymerization reaction time is 4-10h.
5. The preparation method according to claim 1 or 4, characterized in that, The core-shell modified hexagonal boron nitride prepared by S3 includes a plate-like hexagonal boron nitride core and a methyl methacrylate-butyl acrylate copolymer shell coating the surface of the plate-like hexagonal boron nitride. The average thickness of the polymer shell is 10-40 nm, and the content of surface organic components of the core-shell modified hexagonal boron nitride, as determined by thermogravimetric analysis, is 4-12 wt.%.
6. The preparation method according to claim 1, characterized in that, In S4, the polyethersulfone and ionic liquid modified montmorillonite are vacuum dried at 90-110°C for 3-6 hours before being added to the epoxy resin; the alicyclic epoxy resin and biphenyl epoxy resin are mixed and heated to 75-85°C, and after adding the polyethersulfone and ionic liquid modified montmorillonite, the mixture is stirred at a constant temperature at a speed of 300-500 r / min for 2.0-2.5 hours.
7. The preparation method according to claim 1, characterized in that, In step S5, the epoxy resin matrix obtained in step S4 is cooled to 50-60°C and then the silane coupling agent, heptadecafluorodecyltrimethoxysilane, and phosphate wetting and dispersing agent are added; the silane coupling agent is KH-560, and the phosphate wetting and dispersing agent is BYK-111.
8. The preparation method according to claim 1, characterized in that, In S5, the D50 of the spherical alumina is 15-25 μm, the D50 of the spherical aluminum nitride is 8-12 μm, and the D50 of the core-shell modified hexagonal boron nitride is 3-8 μm; the spherical alumina, spherical aluminum nitride, and core-shell modified hexagonal boron nitride are added to the epoxy resin matrix in descending order of particle size for dispersion.
9. The preparation method according to claim 1, characterized in that, In step S6, the mixture obtained in step S5 is cooled to 20–25°C and then the methyltetrahydrophthalic anhydride, dodecenylsuccinic anhydride, and imidazole curing accelerator are added. During the addition process, the system temperature does not exceed 40°C. After mixing, the mixture is degassed for 10–30 minutes under a vacuum of 0.08–0.10 MPa. The adhesive is then cured at 120–150°C for 30–60 minutes.
10. The preparation method according to any one of claims 1 to 9, characterized in that, The prepared chip was filled with a high thermal conductivity single-component epoxy adhesive at 25°C and a shear rate of 10 s⁻¹. - The apparent viscosity under the given conditions is 1500–2500 mPa·s at 25°C and a shear rate of 100 s⁻¹. - The apparent viscosity under the conditions is 800–1500 mPa·s, and the thermal conductivity in the thickness direction after curing is not less than 3.0 W / (m·K).