A flexible epoxy potting compound for bonding low polarity materials and its preparation method
By forming an interpenetrating network structure using ETPB and siloxane tackifiers, the problems of poor adhesion of flexible epoxy potting compounds to low-polarity materials and increased hardness after thermal aging are solved, achieving the effect of high-strength adhesion and low hardness increase.
Patent Information
- Application Number
- CN202611164010.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-03
- Publication Date
- 2026-11-17
AI Technical Summary
Existing flexible epoxy potting compounds have poor adhesion to low-polarity materials such as PP and PE, and their hardness increases significantly after thermal aging, making it impossible to balance low modulus, low hardness, and high thermal aging stability.
Using epoxy-terminated polybutadiene (ETPB) as the main resin, combined with siloxane tackifier and flexible polyamide curing agent, an interpenetrating network structure is formed. The bonding strength is improved through hydrophobic anchoring and molecular chain entanglement, and low hardness growth is maintained during thermal aging.
It achieves high-strength bonding to low-polarity substrates, with a hardness increase rate of less than 10% after thermal aging, while maintaining good flexibility and thermal aging stability.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of electronic potting materials, and more specifically, relates to a flexible epoxy potting compound for bonding low-polarity materials and its preparation method. Background Technology
[0002] With the rapid development of new energy vehicles, electronic modules, and smart sensors, stringent requirements have been placed on potting materials for lightweighting, low stress, and broad-spectrum adhesion. Many electronic housings, controllers, and sensors are increasingly using low-polarity engineering materials such as polypropylene (PP), polyethylene (PE), PP+LGF (long glass fiber reinforced PP), and PP+EPDM / talc to reduce weight and cost. However, these materials have extremely low surface energy (typically below 32 mN / m), making it difficult for traditional epoxy potting compounds to effectively wet and bond to their surfaces. Plasma, flame, or primer treatments are usually required, and even then, the bonding effect of conventional epoxy potting compounds remains unsatisfactory.
[0003] To reduce the internal stress and impart flexibility to epoxy resins, existing technologies typically employ methods such as polyurethane-modified epoxy, polyether polyol glycidyl ether, polyether-modified epoxy resin, or end-epoxy-terminated nitrile butadiene rubber (ETBN) toughening. However, while publicly available flexible epoxy potting compounds exhibit some adhesion to metals, their adhesion strength to PP and PE substrates is almost zero. Some studies have attempted to formulate insulating potting compounds using end-epoxy-terminated polybutadiene (ETPB). Although the non-polarity of the main chain improves compatibility with low-polarity surfaces to some extent, these formulations lack effective interfacial adhesion-enhancing methods. Furthermore, while polyether-modified bisphenol A type epoxy resins (BPA-PO type) such as ADEKAEP-4000 can provide some flexibility, their highly polar polyether main chain results in poor compatibility with low-polarity substrates, and the ether bonds are prone to oxidative degradation at high temperatures, failing to balance adhesion to low-polarity substrates and thermal aging stability.
[0004] Other techniques attempt to add silane coupling agents to improve adhesion to low-polarity materials. However, commonly used epoxy or aminosilane coupling agents, due to their short-chain alkyl structures, cannot form an effective hydrophobic anchoring layer on non-polar surfaces such as PP. Instead, they may weaken the interface due to phase separation. Meanwhile, conventional polyamide or modified amine curing agents continue to react with residual epoxy groups during high-temperature aging, leading to increased crosslinking density, significantly increased hardness, and loss of low-stress protection properties.
[0005] Therefore, it is of great significance to develop a flexible epoxy potting compound that has an ETPB addition amount above the threshold, is combined with a specific tackifier and a suitable curing agent, and has low modulus, low hardness, excellent initial adhesion to low polarity substrates such as PP and high hardness retention after thermal aging. Summary of the Invention
[0006] The purpose of this invention is to provide a flexible epoxy potting compound for bonding low-polarity materials and its preparation method, thereby solving the problems of poor adhesion of existing flexible epoxy compounds to low-polarity substrates such as PP and significant increase in hardness after thermal aging.
[0007] The objective of this invention can be achieved through the following technical solutions: A flexible epoxy potting compound for bonding low-polarity materials, comprising component A and component B in a mass ratio of 1:0.3~1, by weight parts, Component A includes: 40-70 parts of bisphenol A type epoxy resin 30-60 parts of epoxy-terminated polybutadiene, wherein the epoxy-terminated polybutadiene is an oligomer having a polybutadiene backbone and epoxy groups at both ends; 2-8 parts of siloxane tackifier, wherein the siloxane tackifier is an oligomeric siloxane containing hydrophobic long-chain alkyl and alkoxysilane functional groups; Defoamer 0.1~1 part; Component B includes: 40-150 parts of flexible polyamide curing agent; the flexible polyamide curing agent is a low molecular weight polyamide formed by the condensation of dimer acid and polyamine; Wherein, the proportion of terminal epoxy-terminated polybutadiene in the total mass of resin in component A is ≥30%, and the proportion of siloxane tackifier in the total mass of component A is ≥2%; the total mass of resin refers to the sum of the mass of bisphenol A type epoxy resin and terminal epoxy-terminated polybutadiene.
[0008] Furthermore, the epoxy equivalent of the bisphenol A type epoxy resin is 180~200 g / eq.
[0009] Furthermore, the bisphenol A type epoxy resin is selected from at least one of E-51, CYD-128, and Nan Ya NPEL-128 type epoxy resins.
[0010] Furthermore, the epoxy equivalent of the terminally epoxy-terminated polybutadiene is 200~500 g / eq, and the molecular weight is 1500~5000 g / mol.
[0011] Furthermore, the epoxy-terminated polybutadiene is selected from at least one of Nippon Soda JP-100, Cray Valley Poly bd605E, Tianyuan New Materials TY-ETPB, and Daicel EPOLEAD PB4700.
[0012] Among them, the molecular chain of epoxy-terminated polybutadiene (ETPB) contains a flexible polybutadiene backbone and epoxy groups. The epoxy groups can react with primary / secondary amines in polyamide curing agents to form covalent bonds and participate in the curing crosslinking network.
[0013] Preferably, the hydrophobic long-chain alkyl group is C8~C18, and the siloxane thickener is Anric UM998.
[0014] Among them, UM998, a siloxane tackifier, is a siloxane oligomer tackifier containing epoxy functional groups. Its molecular structure contains a siloxane backbone (providing compatibility with low polarity substrates) and epoxy functional groups (participating in the curing reaction), and it has excellent tackifying effect on low polarity substrates such as PE / PP.
[0015] Furthermore, the amine value of the flexible polyamide curing agent is 150~300 mgKOH / g, and the active hydrogen equivalent is 150~250 g / eq.
[0016] Preferably, the dimer acid is C36 dimer acid; the flexible polyamide curing agent is selected from at least one of Evonik Ancamide 910, Evonik Ecflex-01, Gadida XH 463, Gadida XH-351S, and Henster WE-3115.
[0017] This type of curing agent has long aliphatic hydrocarbon segments, which are compatible with the polybutadiene segments of ETPB. After crosslinking, it imparts excellent flexibility and low hardness to the system.
[0018] Preferably, the defoamer is an organosilicon or polymer defoamer, preferably BYK-A530 or BYK-1790.
[0019] Furthermore, component A also contains thermally conductive filler and / or flame retardant; based on the total weight of component A, the amount of thermally conductive filler added is 10-50%, and the amount of flame retardant added is 2-10%.
[0020] Furthermore, the thermally conductive filler is selected from at least one of alumina, boron nitride, and aluminum nitride; the flame retardant is a phosphorus-based flame retardant, a nitrogen-based flame retardant, or a mixture of the two.
[0021] Another aspect of the present invention provides a method for preparing the potting compound as described above, comprising the following steps: S1. Mix and degas the raw materials of component A in a vacuum stirred tank to obtain component A; S2. Mix the raw materials of component B to obtain component B; S3. Mix component A and component B at a mass ratio of 1:0.3~1 and degas to obtain the flexible epoxy potting compound.
[0022] Step S3 is performed during use, where the potting compound mixed and degassed in step S3 is potted and cured.
[0023] Furthermore, the curing conditions of the potting compound are as follows: curing at a temperature below 25°C for 24 to 72 hours, or curing at 25 to 60°C for 2 to 48 hours, or curing at 60 to 80°C for 1 to 8 hours, or a stepped curing process of first low temperature and then high temperature at 20 to 80°C.
[0024] The above-mentioned potting compounds are used in the potting of electronic components with polypropylene substrates, polyethylene substrates, PP+LGF composites, or PP+EPDM / talc modified composites.
[0025] Furthermore, the substrate is subjected to flame treatment or plasma treatment before use.
[0026] The potting compound of this invention can be widely used for potting and protecting polypropylene, polyethylene and their modified composite materials (PP+LGF, PP+EPDM / talc, etc.) housings and components in electric vehicles, electronic modules, sensors and other fields. It is especially suitable for electronic component packaging scenarios with high requirements for long-term thermal aging reliability. After flame or plasma treatment, it can achieve strong adhesion to low polarity substrates and maintain stable low-stress protection characteristics during long-term high-temperature service.
[0027] Compared with the prior art, the present invention has the following beneficial effects: (1) Achieved high-strength bonding to low-polarity substrates This invention uses epoxy-terminated polybutadiene (ETPB) as the main resin component (≥30%), introducing a large number of flexible polybutadiene segments into the cured network. This reduces the polarity of the epoxy cured network, significantly improving its compatibility with low-polarity substrates. Simultaneously, the siloxane segments of the siloxane tackifier (≥2%) can effectively migrate to the colloid / substrate interface, forming physical adsorption and molecular chain entanglement with the surface of low-polarity substrates such as PP and PE through hydrophobic anchoring. The synergistic effect of these two components enhances the tensile shear strength of the encapsulated substrate without requiring any surface pretreatment.
[0028] (2) The critical threshold effect of ETPB was discovered. When end-epoxy polybutadiene (ETPB) accounts for less than 30% of the total resin mass, ETPB exists as a dispersed phase within the continuous bisphenol A epoxy phase. The system remains dominated by a rigid network, lacking flexibility, and the contribution of ETPB segments to adhesion is limited. When the ETPB content is ≥30%, the system transforms into a bicontinuous phase or interpenetrating network structure. The flexible polybutadiene segments become continuous network components, significantly reducing the overall modulus and polarity of the cured product, providing a molecular-level basis for adhesion to low-polarity substrates. This critical threshold effect was discovered through extensive experiments and cannot be extrapolated from existing technologies.
[0029] (3) The critical threshold effect of UM998 was discovered. When the siloxane tackifier UM998 accounts for less than 2% of the total mass of component A, its siloxane segments have insufficient coverage at the colloid / substrate interface, failing to form a continuous hydrophobic anchoring layer, resulting in limited improvement in adhesive strength. When the UM998 content is ≥2%, a dense siloxane anchoring layer is formed at the interface, which works synergistically with the flexible segments of ETPB, leading to a significant increase in adhesive strength.
[0030] (4) Synergistic thickening effect of ETPB+UM998 The synergistic adhesion-enhancing mechanism of epoxy-terminated polybutadiene (ETPB) and the siloxane tackifier UM998 involves two levels: ① Molecular chain entanglement mechanism—the long polybutadiene chains of ETPB and the siloxane segments of UM998 form an entangled structure during curing, enhancing the cohesive strength of the interfacial layer; ② Hydrophobic anchoring mechanism—the siloxane segments of UM998 form hydrophobic adsorption on the low-polarity substrate surface at the interface, while the van der Waals forces between the low-polarity segments of ETPB and the substrate molecular chains further enhance the interfacial bonding. The synergistic effect of these two mechanisms results in an adhesive strength far exceeding the sum of the effects of any single mechanism.
[0031] (5) Excellent overall performance The long-chain aliphatic hydrocarbon structure of component B of this invention—the flexible polyamide curing agent—controls the initial hardness of the cured product within the Shore A range of 50-65. In the ternary system of ETPB+UM998+flexible polyamide, the polybutadiene segments of ETPB and the aliphatic segments of polyamide form an interpenetrating flexible network, which effectively relaxes the internal stress generated during post-curing during 90℃×1000h heat aging, resulting in a hardness increase rate of <10%. In contrast, the heat aging hardness increase rate of traditional amine-based curing systems is typically >20%. Detailed Implementation
[0032] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described below with reference to specific embodiments, but the scope of protection of this invention is not limited thereto. Experimental methods not specifically described in the embodiments are generally performed under conventional conditions or according to the manufacturer's recommendations. Unless otherwise specified, all reagents and materials used are commercially available.
[0033] The main sources of raw materials in the following embodiments and comparative examples are as follows: Bisphenol A type epoxy resin 128 (Nanya NPEL-128); JP-100 (Japanese Soda); Poly bd 605E (Cray Valley); TY-ETPB (Tianyuan New Materials); UM998 (Anric), a siloxane tackifier; Ancamide 910 (Evonik); Ecflex-01 (Shanghai Feimi Technology); XH 463 (Jiadida); XH-351S (Jiadida); Defoamer BYK-A530; Silane coupling agents KH-560 (epoxy group), KH-550 (amino group); Polyetheramine D2000 (Hunsman); Polyetheramine D400 (Hunsman); ETBN (Hunsmann 861340), an epoxy-terminated butadiene-acrylonitrile rubber toughening agent; Polyether-modified epoxy resin (ADEKA EP-4000), polyether-modified bisphenol A type (BPA-PO type), epoxy equivalent 320 g / eq; Thermally conductive filler: spherical alumina (a mixture of 5 μm and 20 μm average particle sizes); Flame retardant: Ammonium polyphosphate / melamine cyanurate compound.
[0034] Examples 1-3 A flexible epoxy potting compound for bonding low-polarity materials comprises the following components:
[0035] In Example 1, ETPB accounts for 30% of the total resin mass = 30 / (70+30)×100% = 30%; The percentage of UM998 in the total mass of component A is approximately 2% (70 + 30 + 2 + 0.5) × 100%.
[0036] In Example 2, ETPB accounts for 40% of the total resin mass = 40 / (60+40)×100% = 40%; UM998 accounts for 2.9% of the total mass of component A = 3 / (60+40+3+0.5)×100% = 2.9%.
[0037] In Example 3, ETPB accounts for 50% of the total resin mass = 50 / (50+50)×100% = 50%; UM998 accounts for 3.8% of the total mass of component A = 4 / (50+50+4+0.5)×100% = 3.8%.
[0038] Example 4 The difference between this embodiment and Example 1 is that Ancamide 910 in component B is replaced with XH-351S, with a mass of 102.5g, and the mass of UM998 in component A is increased to 5g.
[0039] Example 5 The difference between this embodiment and embodiment 2 is that 128.5g of spherical alumina (accounting for about 50% of the total mass of component A), 15g of ammonium polyphosphate and 10g of melamine cyanurate were added to component A in this embodiment, and the amount of UM998 was increased to 6.3g, with UM998 accounting for about 3% of the total mass of component A.
[0040] The preparation methods of Examples 1-5 above are as follows: (1) Preparation of Component A: Bisphenol A type epoxy resin 128 and TY-ETPB were stirred and mixed at 60°C for 30 minutes until uniform and transparent. The mixture was then cooled to 45°C, and UM998 and defoamer were added. The mixture was stirred for 15 minutes to obtain Component A. In Example 5, after adding UM998 and defoamer, spherical alumina, ammonium polyphosphate and melamine cyanurate were added and dispersed at high speed for 30 minutes until uniform to obtain Component A.
[0041] (2) Preparation of component B: Stir the flexible polyamide curing agent until uniform to obtain component B.
[0042] (3) Preparation of potting compound: Mix component A and component B, stir for 3 minutes until uniform, degas under vacuum and pour onto flame-treated PP+LGF standard test piece, cure at 25℃ / 24h + 60℃ / 2h.
[0043] Comparative Example 1 Compared with Example 1, the difference in this comparative example is that in component A of this comparative example, the mass of bisphenol A type epoxy resin 128 is 80g, the mass of TY-ETPB is 20g (ETPB accounts for 20% of the total resin mass, which is lower than the 30% threshold), and the other components, preparation steps and parameters are the same.
[0044] Comparative Example 2 Compared with Example 1, the difference in this comparative example is that in component A of this comparative example, the mass of bisphenol A type epoxy resin 128 is 75g, the mass of TY-ETPB is 25g (ETPB accounts for 25% of the total resin mass, which is lower than the 30% threshold), and the other components, preparation steps and parameters are the same.
[0045] Comparative Example 3 Compared with Example 1, the difference in this comparative example is that the mass of UM998 in component A of this comparative example is 1g (accounting for about 1.0% of the total mass of component A, which is lower than the 2% threshold), while the other components, preparation steps and parameters are the same.
[0046] Comparative Example 4 Compared with Example 2, the difference in this comparative example is that in component A of this comparative example, UM998 is replaced with an equal amount of KH-560 (epoxysilane coupling agent), while the other components, preparation steps and parameters are the same.
[0047] Comparative Example 5 Compared with Example 2, the difference in this comparative example is that 3g of KH-550 was added to component B, while the other components, preparation steps and parameters were the same.
[0048] Comparative Example 6 Compared with Example 2, the difference in this comparative example is that in component B of this comparative example, the flexible polyamide curing agent Ancamide 910 (100g) is replaced with polyetheramine D2000 (80g), while the other components, preparation steps and parameters are the same.
[0049] Comparative Example 7 Compared with Example 2, the difference in this comparative example is that in component B of this comparative example, the flexible polyamide curing agent Ancamide 910 (100g) is replaced with polyetheramine D400 (45g), while the other components, preparation steps and parameters are the same.
[0050] Comparative Example 8 Compared to Example 2, this comparative example differs in that the mass of bisphenol A type epoxy resin 128 in component A is increased to 100g, TY-ETPB is absent, and 30g of ETBN (Hunsmann 861340) is added (as a toughening agent, not the main resin). Meanwhile, the mass of Ancamide 910 in component B is increased to 105g. All other components, preparation steps, and parameters remain the same.
[0051] Comparative Example 9 Compared to Example 2, this comparative example differs in that component A of this comparative example does not contain bisphenol A type epoxy resin 128 and TY-ETPB, but instead contains 100g of polyether modified epoxy resin (ADEKA EP-4000, polyether modified bisphenol A type BPA-POtype). Simultaneously, the amount of Ancamide 910 in component B is reduced to 66g. All other components, preparation steps, and parameters remain the same.
[0052] Performance testing methods (1) Hardness: The Shore A hardness after curing and after heat aging was determined according to GB / T 531.1.
[0053] (2) Tensile shear strength: Using PP+LGF composite sheet as the substrate, the surface of the substrate is flame treated (after wiping with alcohol), the overlap is 25mm×12.5mm, the adhesive layer thickness is 0.2mm, and the tensile rate is 10mm / min according to GB / T 7124.
[0054] (3) Thermal aging: The fully cured sample and overlapping parts were placed in a 90℃ forced-air oven for 1000 hours, then removed and cooled to room temperature to determine hardness and shear strength. The percentage increase in hardness was calculated using the following formula: (4) Hardness growth rate (%) = (hardness after heat aging - initial hardness) / initial hardness × 100%.
[0055] (5) The curing agent obtained in Example 5 was subjected to thermal conductivity and flame retardancy tests. The thermal conductivity was determined using the HotDisk method. The flame retardancy was evaluated according to the UL94 vertical burning method.
[0056] The test results are shown in Table 1.
[0057] Table 1
[0058] As shown in Table 1, the proportion of ETPB in the total mass of component A resin in Examples 1-5 is 30%-50%. After curing, the initial tensile shear strength of the potting compound on the surface-treated PP+LGF substrate reaches 1.8-2.5 MPa. After heat aging at 90℃ for 1000h, the Shore A hardness increases from the initial 52-62 to 55-67, with a hardness growth rate of only 5.8%-8.6%, all remaining within 10%. This indicates that the potting compound of the present invention has excellent hardness retention under long-term heat aging conditions.
[0059] In Comparative Example 1, when the ETPB addition was reduced to 20%, the initial tensile shear strength was only 0.8 MPa, while the hardness increase rate after heat aging was as high as 25.8%, far exceeding the corresponding values of Examples 1-5. Comparing Comparative Examples 1 and 2, it can be seen that when the ETPB addition was increased to 25%, the performance improved, but it was still inferior to Examples 1-5. The above results indicate that there is a critical threshold of 30% for ETPB addition. When the ETPB content is below this threshold, the flexible polybutadiene segments cannot form continuous non-polar microregions in the cured network, and the rigid bisphenol A structure dominates. On the one hand, it is difficult to generate sufficient molecular chain entanglement with the surface of low-polarity substrates, resulting in insufficient interfacial compatibility; on the other hand, the subsequent crosslinking reaction of residual epoxy groups during heat aging leads to a significant increase in crosslinking density and a sharp increase in hardness. Only when the ETPB addition reaches more than 30% can its non-polar backbone form continuous flexible microregions in the cured network, effectively bonding to low-polarity substrates while effectively diluting the rigid structure in the crosslinking network and inhibiting the post-curing crosslinking reaction.
[0060] In Comparative Examples 8 and 9, the initial tensile shear strengths of Comparative Examples 8 and 9 were 0.6 MPa and 0.4 MPa, respectively, with hardness increases of up to 32.7% and 35.3% after heat aging, respectively. The toughening effect of ETBN (Comparative Example 8) depends on the rubber dispersed phase, while that of polyether-modified epoxy (Comparative Example 9) depends on the flexible polyether segments. Both exhibit problems such as toughening phase separation, degradation, or ether bond breakage during heat aging, failing to effectively improve interfacial compatibility with low-polarity substrates or inhibit post-curing crosslinking during heat aging. The above comparison fully demonstrates the unique mechanism of action of ETPB as the main resin rather than a simple toughening agent in this invention.
[0061] In Comparative Example 3, the amount of UM998 added was only 1% (accounting for 1% of the total mass of component A), which is below the critical threshold of 2%. Although the ETPB content reached 30%, its initial tensile shear strength was only 0.9 MPa, far lower than the 2.1 MPa in Example 1. The above results indicate that UM998 also has a critical addition threshold of 2%. The UM998 molecular structure contains C8~C18 hydrophobic long-chain alkyl groups and hydrolyzable alkoxysilane groups. Only when its content in component A reaches more than 2% can it form a continuous and effective hydrophobic anchoring layer on the surface of the low polarity substrate, producing a synergistic effect with the non-polar backbone of ETPB, and achieving a unity of dual physical anchoring and chemical bonding of "molecular chain entanglement + hydrophobic anchoring".
[0062] Comparative Example 4 used the conventional epoxy silane coupling agent KH-560 instead of UM998, and Comparative Example 5 added the conventional amino silane coupling agent KH-550 to component B. The initial tensile shear strengths of both were 0.7 MPa and 0.6 MPa, respectively, both significantly lower than the 2.3 MPa of Example 2. This indicates that even if KH-550 is correctly placed in component B to avoid its active amino groups reacting with the epoxy resin during storage (Comparative Example 5), its short-chain alkyl structure still cannot form an effective hydrophobic anchoring layer on non-polar surfaces such as PP. Therefore, the unique long-chain hydrophobic alkyl structure of UM998 is a key structural feature for achieving effective adhesion to low-polarity substrates, and conventional short-chain silane coupling agents, whether placed in component A or component B, cannot achieve the same tackifying effect as UM998.
[0063] Comparative Examples 6 and 7 used polyetheramine D2000 and D400 curing agents, respectively, to replace the flexible polyamide curing agent of this invention. Although the ETPB and UM998 contents of both reached the critical threshold, their initial tensile shear strengths were 1.5 MPa and 1.3 MPa, respectively, but the hardness growth rates after heat aging were as high as 50.0% and 53.8%, respectively, far exceeding the 7.3% of Example 2. This indicates that although the polyetheramine curing agent can provide a certain degree of flexibility, its terminal amino group has high reactivity, and it is easy to undergo post-curing reaction with the residual epoxy groups in the system during heat aging, resulting in a significant increase in crosslinking density. In contrast, the dimer acid type polyamide curing agent selected in this invention has a long-chain aliphatic hydrocarbon structure, and its active hydrogen reactivity is relatively low. The crosslinking network formed has almost no subsequent crosslinking reaction during heat aging, thus ensuring long-term stability of hardness. In addition, the long-chain aliphatic hydrocarbon segments of the polyamide curing agent have good compatibility with the polybutadiene segments of ETPB, which is beneficial to the formation of a uniform flexible crosslinking network.
[0064] Example 5 added spherical alumina and a phosphorus-nitrogen compound flame retardant to component A. The results showed that the thermal conductivity of the potting compound reached 0.65 W / m·K, the flame retardancy rating reached UL94 V-0, while the PP shear strength remained at 1.8 MPa, and the heat aging hardness increase rate was 8.1%. This indicates that the technical solution of the present invention can still maintain excellent adhesion and heat aging stability after introducing a large number of functional fillers, and has good filler carrying capacity and formulation universality.
[0065] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A flexible epoxy potting adhesive for bonding low polarity materials, characterized by, Includes component A and component B in a mass ratio of 1:0.3~1, by weight parts. Component A includes: 40-70 parts of bisphenol A type epoxy resin 30-60 parts of epoxy-terminated polybutadiene, wherein the epoxy-terminated polybutadiene is an oligomer having a polybutadiene backbone and epoxy groups at both ends; 2-8 parts of siloxane tackifier, wherein the siloxane tackifier is an oligomeric siloxane containing hydrophobic long-chain alkyl and alkoxysilane functional groups; Defoamer 0.1~1 part; Component B includes: 40-150 parts of flexible polyamide curing agent; the flexible polyamide curing agent is a low molecular weight polyamide formed by the condensation of dimer acid and polyamine; Wherein, the proportion of terminal epoxy-terminated polybutadiene in the total mass of resin in component A is ≥30%, and the proportion of siloxane tackifier in the total mass of component A is ≥2%; the total mass of resin refers to the sum of the mass of bisphenol A type epoxy resin and terminal epoxy-terminated polybutadiene.
2. The flexible epoxy potting adhesive for bonding low polarity materials according to claim 1, characterized in that, The epoxy equivalent of the bisphenol A type epoxy resin is 180~200 g / eq; The epoxy equivalent of the terminally epoxy-terminated polybutadiene is 200~500 g / eq, and the molecular weight is 1500~5000 g / mol.
3. The flexible epoxy potting adhesive for bonding low-polarity materials according to claim 1 or 2, characterized in that, The bisphenol A type epoxy resin is selected from at least one of E-51, CYD-128, and Nan Ya NPEL-128 type epoxy resins; The epoxy-terminated polybutadiene is selected from at least one of Nippon Soda JP-100, Cray Valley Poly bd 605E, Tianyuan New Materials TY-ETPB, and Daicel EPOLEAD PB4700.
4. The flexible epoxy potting adhesive for bonding low polarity materials according to claim 1, characterized in that, The hydrophobic long-chain alkyl group is C8~C18, and the siloxane thickener is Anric UM998.
5. The flexible epoxy potting adhesive for bonding low polarity materials according to claim 1, characterized in that, The dimer acid is C36 dimer acid; the flexible polyamide curing agent is selected from at least one of Evonik Ancamide 910, Evonik Ecflex-01, Gadida XH 463, Gadida XH-351S, and Henster WE-3115; The defoamer is an organosilicon or polymer-based defoamer.
6. The flexible epoxy potting adhesive for bonding low polarity materials according to claim 1 or 5, characterized in that, The amine value of the flexible polyamide curing agent is 150~300 mgKOH / g, and the active hydrogen equivalent is 150~250 g / eq; The defoamer is BYK-A530 or BYK-1790.
7. The flexible epoxy potting adhesive for bonding low polarity materials according to claim 1, characterized in that, Component A further comprises thermally conductive filler and / or flame retardant; based on the total weight of component A, the amount of thermally conductive filler added is 10-50%, and the amount of flame retardant added is 2-10%.
8. The flexible epoxy potting adhesive for bonding low polarity materials according to claim 7, characterized in that, The thermally conductive filler is selected from at least one of alumina, boron nitride, and aluminum nitride; the flame retardant is a phosphorus-based flame retardant, a nitrogen-based flame retardant, or a mixture of the two.
9. A process for preparing a flexible epoxy potting compound for bonding low-polarity materials as claimed in any one of claims 1 to 8, characterized in that, The preparation method includes the following steps: S1. Mix and degas the raw materials of component A in a vacuum stirred tank to obtain component A; S2. Mix the raw materials of component B to obtain component B; S3. Mix component A and component B at a mass ratio of 1:0.3~1 and degas to obtain the flexible epoxy potting compound.
10. Use of the potting glue according to claims 1-8 for potting of electronic components on polypropylene substrates, polyethylene substrates, PP+LGF composites or PP+EPDM / talc modified composites.