A conductive adhesive containing multidimensional structure filler and its preparation method
By combining the filler with a three-dimensional/one-dimensional/zero-dimensional "tethered anchor" structure and o-cresyl cyanate resin, the problem of insufficient comprehensive performance of existing conductive fillers in high-end electronic packaging is solved, and the simultaneous optimization of conductivity and mechanical strength is achieved.
Patent Information
- Application Number
- CN202611277135.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing conductive fillers have significant shortcomings in terms of overall performance, cost control, and process adaptability, making it difficult to meet the needs of high-end electronic packaging.
A three-dimensional/one-dimensional/zero-dimensional "tethered anchor" structure filler is designed and combined with o-cresyl formaldehyde cyanate resin to prepare a multi-dimensional conductive adhesive through a multi-step process, including impact crushing, air jet milling, hydrothermal reaction and coupling agent modification, to form a stable core-shell structure.
It significantly improves the conductivity and mechanical properties of conductive adhesive, reduces resistivity, and enhances interfacial bonding strength, making it suitable for large-scale production.
Smart Images

Figure CN123107614A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electronic packaging materials technology, specifically to a conductive adhesive containing multidimensional structure fillers and its preparation method. Background Technology
[0002] With the rapid development of electronic components towards high frequency, high power, high integration, and miniaturization, higher requirements are being placed on electronic packaging and interconnect materials in terms of conductivity, thermal stability, and interface reliability. While traditional metal-based interconnect materials (such as solder) offer excellent conductivity, their high-temperature processing characteristics easily lead to thermal stress concentration and damage to heat-sensitive components, posing a bottleneck in advanced electronic packaging. Polymer-based interconnect materials (such as conductive adhesives), due to their low-temperature processing characteristics, flexible processes, and adaptability to complex interfaces, have become key materials for replacing traditional metal-based interconnect materials. The performance of conductive adhesives is mainly determined by the polymer matrix and conductive fillers: the matrix provides mechanical support and stress buffering; while the conductive fillers form a three-dimensional network through mutual contact, undertaking the core function of current transmission.
[0003] Currently, the research and application of conductive fillers mainly focus on the following categories: metal fillers (such as Ag and Cu), carbon-based fillers (such as carbon nanotubes and graphene), and intrinsically conductive ceramic fillers. Among them, silver powder is the most widely used due to its excellent conductivity, oxidation resistance, and mature processing technology. However, the strong demand from the three pillar industries of photovoltaics, electronics, and automotive electrification has led to a severe shortage of Ag resources, resulting in increased costs for silver-based conductive adhesives and severely restricting their large-scale application. Although copper powder has a lower cost, its surface is prone to oxidation, leading to a surge in contact resistance and a decline in long-term reliability, usually requiring complex surface modification or protection processes. Carbon-based fillers typically have lower intrinsic conductivity than metals and are prone to agglomeration in polymer matrices due to strong van der Waals forces, making it difficult to uniformly disperse and construct efficient and stable conductive pathways. In recent years, MAX phase ceramics, represented by transition metal carbides / nitrides, have attracted attention due to their unique dual metal and ceramic properties (such as good intrinsic conductivity, high melting point, high modulus, and processability) and are considered as potential new conductive fillers. However, undesigned conventional MAX phase particles still face challenges such as high percolation threshold, weak interfacial bonding with polymer matrix, and uneven filler dispersion in the matrix, making it difficult for the conductive adhesive to meet the requirements of high-end electronic packaging in terms of conductivity, mechanical enhancement effect, and overall reliability.
[0004] In summary, existing conductive fillers have significant shortcomings in terms of overall performance, cost control, and process adaptability. Developing a novel conductive filler with a low percolation threshold, high conductivity, and excellent mechanical properties is crucial to overcoming the current performance bottlenecks of conductive adhesives and promoting the development of advanced electronic packaging technologies. Based on this, this invention aims to design a novel conductive adhesive with excellent conductivity, mechanical properties, and reliability by performing multi-dimensional structural design on MAX phase materials and matching them with a high-performance resin matrix. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the technical problem this invention aims to solve is to provide a conductive adhesive containing multidimensional structural fillers and its preparation method. It innovatively designs a three-dimensional / one-dimensional / zero-dimensional "rope anchor" structure filler and selects a suitable o-cresphenolic cyanate resin, with the goal of preparing a novel conductive adhesive with significantly improved conductivity, mechanical properties, and reliability.
[0006] The present invention is achieved through the following technical solutions.
[0007] This invention provides a conductive adhesive containing multidimensional structure fillers. The matrix material of the conductive adhesive is o-crestoform cyanate resin, and the filler is a material with a three-dimensional / one-dimensional / zero-dimensional "bolt-anchor" structure. The "bolt" structure is a three-dimensional MAX phase, the "rope" structure is a one-dimensional "single crystal core@oxide shell" core-shell structure, and the "anchor" structure is a zero-dimensional coupling agent site grafted onto the oxide layer on the surface of a single crystal wire.
[0008] This invention also provides a method for preparing a conductive adhesive containing a multidimensional filler, specifically including the following steps:
[0009] S1: Impact crushing of MAX phase powder to obtain millimeter-sized MAX phase powder;
[0010] S2: The millimeter-scale MAX phase powder is subjected to air jet milling to obtain micron-scale three-dimensional "bolt" structure MAX phase powder;
[0011] S3: Mix the micron-sized MAX phase powder with Lewis acid, perform ultrasonic stirring and low-temperature heat treatment, filter, wash and centrifuge the treated suspension to obtain MAX phase powder pretreated by A-layer isochronization.
[0012] S4: The MAX phase powder after the A layer isochronous pretreatment is mixed with ammonia and ultrapure water and subjected to hydrothermal reaction; the suspension after hydrothermal reaction is filtered, washed and vacuum freeze-dried to obtain powder with a three-dimensional / one-dimensional "tethered rope" structure.
[0013] S5: Use a coupling agent to modify the surface of the powder of the "tethered rope" structure to obtain a filler with a three-dimensional / one-dimensional / zero-dimensional "tethered rope anchor" structure;
[0014] S6: After heating the o-cresol cyanate resin, it is mixed and stirred with diallyl bisphenol A (DBA) to obtain a homogeneous resin matrix;
[0015] S7: After pre-dispersing the "rope anchor" structure filler, add it to the matrix described in S6 and continue stirring and dispersing to obtain a mixture; then stir until the dispersant in the mixture is completely removed, and heat to cure to obtain the conductive adhesive.
[0016] Preferably, in step S1, the impact crushing is performed using an ultrafine vertical impact crusher with an impeller speed of 1000-2000 r / min and a crushing time of 5-10 min, to obtain MAX phase powder with a particle size of 0.5-2 mm.
[0017] Preferably, in step S2, the air jet milling is performed using an all-ceramic, pollution-free fluidized bed air jet mill, with a milling pressure of 0.8-1.0 MPa and a milling time of 20-30 min, to obtain MAX phase powder with a particle size of 20-50 µm.
[0018] Preferably, in step S3, the mass ratio of the micron-sized MAX phase powder to the 1-3 wt.% Lewis acid solution is 1:1, the reaction time is 2 h, and the centrifugal drying speed is 1000-1500 r / min for 30-60 min. The Lewis acid cation selectively acts on the weakly bound A-layer atoms in the MAX phase through coordination, homogenizing the A-layer coordination environment. Any potential A-layer segregation / local clustering / surface oxidation unevenness is homogenized by the Lewis acid, forming a state of homogenized A-layer coordination and pre-activated weak MA bonds. This is referred to in this invention as "A-layer homogenization pretreatment," the purpose of which is to provide a uniform Sn source for the subsequent "rope" structure growth and to achieve stable nucleation density and growth rate.
[0019] Preferably, in step S4, the hydrothermal reaction is carried out in a high-pressure reactor, with ultrapure water accounting for 70% of the reactor volume added. The reaction temperature is 120-160℃, the reaction time is 12-24 h, the pH value of the reaction system is adjusted to 9 by ammonia water, and the vacuum freeze-drying time is 12-24 h to obtain a three-dimensional / one-dimensional "tether" structure powder. The "tether" structure is a single crystal wire grown in situ from the A layer of the "tether" structure. The diameter of the single crystal wire is 0.1-2 µm, the length is 100-200 µm, and the surface of the single crystal wire is coated with an A element oxide layer, which is a "single crystal core@oxide shell" core-shell structure.
[0020] Preferably, step S5 includes: mixing and dispersing the "tethered rope" structure powder and coupling agent in deionized water at a mass ratio of 80-100:1, adjusting the pH value to about 9 with NaOH solution, and stirring the reaction at 25°C for 6-8 h; and obtaining the filler of the "tethered rope anchor" structure by centrifugation, washing, and drying.
[0021] Preferably, in step S6, after adding o-cresol cyanate resin to a water bath at 80°C for 30-60 min, it is mixed with diallyl bisphenol A (DBA) at a mass ratio of 10-15:1 and stirred at a speed of 500-1000 rpm for 1-3 h.
[0022] Preferably, in step S7: the filler of the "rope anchor" structure is ultrasonically dispersed in anhydrous ethanol for 1-2 hours, then added to the matrix at a stirring speed of 550-750 rpm, and the stirring speed is increased to 1500-2000 rpm for further dispersion. After uniform dispersion, the mixture is stirred at 550-750 rpm until the anhydrous ethanol is completely evaporated, then cured at 120-140℃ for 1.5 hours, and then cured at 160-180℃ for 2 hours.
[0023] Compared with the prior art, the present invention has the following technical effects:
[0024] 1. Compared with traditional combined multidimensional fillers, the "bolt-anchor" structure designed in this invention is a type of integrated multidimensional filler. Traditional "combined" fillers generally suffer from problems such as poor dispersion uniformity, weak interfacial bonding, and modulus mismatch, resulting in poor mechanical properties of composite materials and complex processing. In this invention: the three-dimensional "bolt" structure provides effective stress support for the composite material due to its high modulus; the one-dimensional "rope" structure, as a "single crystal core@oxide shell" core-shell nanowire, possesses high conductivity and high modulus, and constructs a long-range, continuous electron transport pathway; the zero-dimensional "anchor" structure significantly enhances interfacial bonding strength and suppresses stress concentration by introducing strong covalent bonds between the filler and the resin matrix.
[0025] 2. Thanks to the unique "rope anchor" structure mentioned above, the conductive adhesive prepared by this invention has a significantly lower resistivity compared to commercial conductive adhesives with the same content of silver filler; and a significantly higher shear strength compared to commercial conductive adhesives with the same content of silver-plated copper balls, thus achieving simultaneous optimization of conductivity and mechanical strength.
[0026] 3. The filler provided by this invention is a multi-dimensional integrated material with high stability and uniformity, and its preparation process is simple, making it suitable for large-scale production. Attached Figure Description
[0027] Figure 1The images show the microstructure of the Ti2SnC "rope anchor" structure filler and its conductive adhesive prepared in Example 1 of this invention; where: (a) is a low-magnification SEM image of the filler; and (b) is a high-magnification SEM image of the filler and EDS element point scanning results.
[0028] Figure 2 The images shown are SEM images and high-magnification images of the conductive adhesive sample prepared in Example 1 of the present invention; wherein: (a) shows the overall morphology of the conductive adhesive; and (b) is a high-magnification image.
[0029] Figure 3 The X-ray diffraction (XRD) patterns of Ti2SnC powder samples before and after Lewis acid treatment in Example 1 of this invention are shown.
[0030] Figure 4 The transmission electron microscope (TEM) characterization results of the "rope structure" (single crystal wire) prepared in Example 1 of the present invention.
[0031] Figure 5 This is a bar chart comparing the volume resistivity of the conductive adhesives prepared in Examples 4, 7-16 and Comparative Examples 3-6 of the present invention.
[0032] Figure 6 The bar chart shows the comparison of the shear properties of the conductive adhesives prepared in Examples 4, 7-16 and Comparative Examples 3-6 of this invention.
[0033] Figure 7 This is a performance curve showing the change in volume resistivity of conductive adhesive with the content of conductive filler.
[0034] Figure 7 (a) is a performance curve of volume resistivity as a function of conductive filler content in Examples 1-6 of the present invention; Figure 7 (b) is a performance curve of volume resistivity as a function of conductive filler content in Comparative Examples 1-3. Detailed Implementation
[0035] The above-mentioned and other technical features and advantages of the present invention will be described in more detail below with reference to the accompanying drawings.
[0036] Example 1
[0037] 100 g of Ti₂SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 1000 r / min, and crushed for 5 min. After discharge, the powder was sieved to obtain millimeter-sized Ti₂SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure set to 0.8 MPa, and crushed for 20 min. This yielded micron-sized Ti₂SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti₂SnC phase powder was weighed and mixed with 20 g of a 1% (w / w) FeCl₃ solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti₂SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1000 r / min for 30 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 120℃ for 12 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain "bolt-rope" structure packing composed of one-dimensional "rope" structures with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which were grown in situ on the surface of the three-dimensional "bolt". 4 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. Prepare 50 ml of anhydrous ethanol solution containing 0.05 g of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and slowly add it dropwise to the above filler dispersion under stirring. Continue stirring at 25 °C for 6 h. Then, adjust the pH of the reaction system to 9 with 0.1 mol / L NaOH solution and continue the reaction for 1 h. After the reaction is complete, centrifuge, wash three times with ethanol, and vacuum dry at 60 °C for 6 h to obtain the three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure filler. Weigh 20 g of o-cresyl aldehyde cyanate resin and heat it in an 80 °C water bath for 30 min to reduce viscosity. Then add 2 g of DBA and mix under mechanical stirring at 500 rpm for 1 h to obtain a homogeneous matrix. Weigh 5 g of the "tethered anchor" structure filler (30 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol, and ultrasonically disperse for 1 h to form a stable slurry. Slowly add this slurry dropwise to the resin matrix under stirring at 550 rpm. After the material is added, increase the stirring speed to 1500 rpm and continue high-speed dispersion for 2 hours to ensure uniform dispersion of the filler.The mixture obtained in S7 was transferred to a shallow dish and stirred continuously at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was then applied to a glass substrate, with a thickness controlled at 100 ± 10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120 °C for 1.5 h, then the temperature was increased to 160 °C and cured for another 2 h. After curing, the mixture was cooled to room temperature in the oven to obtain the final 30 wt.% Ti2SnC “rope anchor” conductive adhesive.
[0038] Figure 1 The microstructure of the Ti2SnC "rope anchor" structure filler and its conductive adhesive prepared in this embodiment is shown. Figure 1 (a) is a low-magnification SEM image of the filler, showing the macroscopic distribution of the "bolts" and "ropes". It can be clearly observed that a large number of slender one-dimensional "ropes" structures are grown in situ on the surface of the micron-scale "bolt" structures. Figure 1 (b) High-magnification SEM image and EDS elemental scanning results of the filler. The figure visually presents the composite morphology of the "bolt" and "rope". EDS analysis results show that the "bolt" structure is mainly composed of Ti (68.75 at.%) and Sn (31.25 at.%), which is consistent with the stoichiometry of the Ti2SnC MAX phase; while the surface of the "rope" structure contains Sn (77.30 at.%) and O (22.70 at.%). This result confirms that the "rope" structure is a one-dimensional "single crystal core@oxide shell" core-shell structure, and the oxide shell provides abundant active sites for subsequent grafting of coupling agents.
[0039] Figure 2 The images shown are SEM images and high-magnification images of the conductive adhesive sample prepared in this embodiment. Figure 2 (a) shows the overall morphology of the conductive adhesive, where the filler is densely distributed in the resin matrix, forming a continuous conductive permeation channel. Figure 2 (b) is a high-magnification image, microscopically showing the interfacial bonding between the "rope anchor" structure and the resin matrix. It is clearly visible that the filler and matrix are tightly bonded, with a blurred interface and no obvious voids or debonding. This indicates that the filler and resin matrix have formed a strong interfacial bond, a key indicator of the excellent conductivity and shear strength of the conductive adhesive.
[0040] Figure 3The X-ray diffraction (XRD) patterns of Ti2SnC powder samples before and after Lewis acid treatment in this embodiment are shown to characterize the evolution of phase composition and crystallinity of Ti2SnC powder samples before and after Lewis acid treatment. As shown in the figure, before Lewis acid treatment (blue curve): the sample peaks are relatively broad, indicating that although the original powder has a certain degree of crystallinity, the internal stress of the crystal lattice is relatively large or there are certain defects, and the overall atomic arrangement homogeneity is at a relatively low level. After Lewis acid treatment (red curve): the sample exhibits a series of sharp and high-intensity characteristic peaks. This indicates that Lewis acid selectively acts on the weakly bonded A-layer atoms in the MAX phase through coordination, homogenizing the A-layer coordination environment. The possible A-layer segregation / local clustering / surface oxidation inhomogeneity is homogenized by Lewis acid, forming a state of uniform A-layer coordination and weak MA bond pre-activation. The sharp diffraction peaks directly prove that the obtained product has high crystallinity, a complete crystal lattice structure, and a highly homogeneous atomic arrangement.
[0041] Figure 4 The transmission electron microscopy (TEM) characterization results of the "rope structure" (single crystal wire) prepared in this embodiment are shown in the figure. As shown, the "rope structure" exhibits a distinct core-shell structure. This microstructure directly demonstrates that the hydrothermal reaction process in S4 of this invention enables the growth of a single crystal wire of element A (such as Sn) at the microscale, and the coating of its surface with a continuous and complete oxide film of element A. This unique "single crystal core@oxide shell" core-shell structure effectively improves the surface activity of the material and optimizes its interfacial wetting and bonding performance with the subsequent resin matrix, which is a key factor supporting the excellent overall performance of the conductive adhesive of this invention.
[0042] Example 2
[0043] 100 g of Ti₂SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 1000 r / min, and crushed for 5 min. After discharge, the powder was sieved to obtain millimeter-sized Ti₂SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure set to 0.8 MPa, and crushed for 20 min. This yielded micron-sized Ti₂SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti₂SnC phase powder was weighed and mixed with 20 g of a 1% (w / w) FeCl₃ solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti₂SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1000 r / min for 30 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 120℃ for 12 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain "bolt-rope" structure packing composed of one-dimensional "rope" structures with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which were grown in situ on the surface of the three-dimensional "bolt". 4 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. A 50 ml anhydrous ethanol solution containing 0.05 g N-(2-aminoethyl)-3-aminopropyltrimethoxysilane was prepared and slowly added dropwise to the above filler dispersion under stirring. The reaction was carried out with stirring at 25 °C for 6 h. Subsequently, the pH of the reaction system was adjusted to 9 with 0.1 mol / L NaOH solution, and the reaction was continued for 1 h. After the reaction was completed, the mixture was centrifuged, washed three times with ethanol, and vacuum dried at 60 °C for 6 h to obtain the filler with a three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure. 20 g of o-cresyl formaldehyde cyanate resin was weighed and heated in an 80 °C water bath for 30 min to reduce viscosity. Then 2 g of DBA was added, and the mixture was stirred mechanically at 500 rpm for 1 h to obtain a homogeneous matrix. 6.7 g of the "tethered anchor" structure filler (accounting for 40 wt.% of the resin mass) was weighed and added to 30 ml of anhydrous ethanol, and ultrasonically dispersed for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm. After the addition was complete, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler.The mixture obtained in S7 was transferred to a shallow dish and stirred continuously at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was applied to a glass substrate, with a thickness controlled at 100 ± 10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120 °C for 1.5 h, then the temperature was increased to 160 °C and cured for another 2 h. After curing, it was cooled to room temperature in the oven to obtain the final 40 wt.% Ti2SnC “rope anchor” conductive adhesive.
[0044] Example 3
[0045] 100 g of Ti₂SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 1000 r / min, and crushed for 5 min. After discharge, the powder was sieved to obtain millimeter-sized Ti₂SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure set to 0.8 MPa, and crushed for 20 min. This yielded micron-sized Ti₂SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti₂SnC phase powder was weighed and mixed with 20 g of a 1% (w / w) FeCl₃ solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti₂SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1000 r / min for 30 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 120℃ for 12 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain "bolt-rope" structure packing composed of one-dimensional "rope" structures with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which were grown in situ on the surface of the three-dimensional "bolt". 4 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. A 50 ml anhydrous ethanol solution containing 0.05 g N-(2-aminoethyl)-3-aminopropyltrimethoxysilane was prepared and slowly added dropwise to the above filler dispersion under stirring. The reaction was carried out with stirring at 25 °C for 6 h. Subsequently, the pH of the reaction system was adjusted to 9 with 0.1 mol / L NaOH solution, and the reaction was continued for 1 h. After the reaction was completed, the mixture was centrifuged, washed three times with ethanol, and vacuum dried at 60 °C for 6 h to obtain the filler with a three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure. 20 g of o-cresyl phenolic cyanate resin was weighed and heated in an 80 °C water bath for 30 min to reduce the viscosity. Then 2 g of DBA was added, and the mixture was stirred mechanically at 500 rpm for 1 h to obtain a homogeneous matrix. 8.3 g of the "tethered anchor" structure filler (accounting for 50 wt.% of the resin mass) was weighed and added to 30 ml of anhydrous ethanol, and ultrasonically dispersed for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm. After the addition was complete, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler.The mixture obtained in S7 was transferred to a shallow dish and stirred continuously at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was applied to a glass substrate, with a thickness controlled at 100 ± 10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120 °C for 1.5 h, then the temperature was increased to 160 °C and cured for another 2 h. After curing, it was cooled to room temperature in the oven to obtain the final 50 wt.% Ti2SnC "rope anchor" conductive adhesive.
[0046] Example 4
[0047] 100 g of Ti₂SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 1000 r / min, and crushed for 5 min. After discharge, the powder was sieved to obtain millimeter-sized Ti₂SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure set to 0.8 MPa, and crushed for 20 min. This yielded micron-sized Ti₂SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti₂SnC phase powder was weighed and mixed with 20 g of a 1% (w / w) FeCl₃ solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti₂SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1000 r / min for 30 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 120℃ for 12 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain "bolt-rope" structure packing composed of one-dimensional "rope" structures with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which were grown in situ on the surface of the three-dimensional "bolt". 4 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. A 50 ml anhydrous ethanol solution containing 0.05 g N-(2-aminoethyl)-3-aminopropyltrimethoxysilane was prepared and slowly added dropwise to the above filler dispersion under stirring. The reaction was carried out with stirring at 25 °C for 6 h. Subsequently, the pH of the reaction system was adjusted to 9 with 0.1 mol / L NaOH solution, and the reaction was continued for 1 h. After the reaction was completed, the mixture was centrifuged, washed three times with ethanol, and vacuum dried at 60 °C for 6 h to obtain the three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure filler. 20 g of o-cresyl formaldehyde cyanate resin was weighed and heated in an 80 °C water bath for 30 min to reduce viscosity. Then 2 g of DBA was added, and the mixture was stirred mechanically at 500 rpm for 1 h to obtain a homogeneous matrix. 10 g of the "tethered anchor" structure filler (accounting for 60 wt.% of the resin mass) was weighed and added to 30 ml of anhydrous ethanol, and ultrasonically dispersed for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm. After the addition was complete, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler.The mixture obtained in S7 was transferred to a shallow dish and stirred continuously at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was applied to a glass substrate, with a thickness controlled at 100 ± 10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120 °C for 1.5 h, then the temperature was increased to 160 °C and cured for another 2 h. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ti2SnC “rope anchor” conductive adhesive.
[0048] Example 5
[0049] 100 g of Ti₂SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 1000 r / min, and crushed for 5 min. After discharge, the powder was sieved to obtain millimeter-sized Ti₂SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure set to 0.8 MPa, and crushed for 20 min. This yielded micron-sized Ti₂SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti₂SnC phase powder was weighed and mixed with 20 g of a 1% (w / w) FeCl₃ solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti₂SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1000 r / min for 30 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 120℃ for 12 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain "bolt-rope" structure packing composed of one-dimensional "rope" structures with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which were grown in situ on the surface of the three-dimensional "bolt". 4 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. A 50 ml anhydrous ethanol solution containing 0.05 g N-(2-aminoethyl)-3-aminopropyltrimethoxysilane was prepared and slowly added dropwise to the above filler dispersion under stirring. The reaction was carried out with stirring at 25 °C for 6 h. Subsequently, the pH of the reaction system was adjusted to 9 with 0.1 mol / L NaOH solution, and the reaction was continued for 1 h. After the reaction was completed, the mixture was centrifuged, washed three times with ethanol, and vacuum dried at 60 °C for 6 h to obtain the filler with a three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure. 20 g of o-cresyl formaldehyde cyanate resin was weighed and heated in an 80 °C water bath for 30 min to reduce the viscosity. Then 2 g of DBA was added, and the mixture was stirred mechanically at 500 rpm for 1 h to obtain a homogeneous matrix. 11.7 g of the "tethered anchor" structure filler (accounting for 70 wt.% of the resin mass) was weighed and added to 30 ml of anhydrous ethanol, and ultrasonically dispersed for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm. After the addition was complete, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler.The mixture obtained in S7 was transferred to a shallow dish and stirred continuously at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was then applied to a glass substrate, with a thickness controlled at 100 ± 10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120 °C for 1.5 h, then the temperature was increased to 160 °C and cured for another 2 h. After curing, the mixture was cooled to room temperature in the oven to obtain the final 70 wt.% Ti2SnC “rope anchor” conductive adhesive.
[0050] Example 6
[0051] 100 g of Ti₂SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 1000 r / min, and crushed for 5 min. After discharge, the powder was sieved to obtain millimeter-sized Ti₂SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure set to 0.8 MPa, and crushed for 20 min. This yielded micron-sized Ti₂SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti₂SnC phase powder was weighed and mixed with 20 g of a 1% (w / w) FeCl₃ solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti₂SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1000 r / min for 30 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 120℃ for 12 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain "bolt-rope" structure packing composed of one-dimensional "rope" structures with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which were grown in situ on the surface of the three-dimensional "bolt". 4 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. A 50 ml anhydrous ethanol solution containing 0.05 g N-(2-aminoethyl)-3-aminopropyltrimethoxysilane was prepared and slowly added dropwise to the above filler dispersion under stirring. The reaction was carried out with stirring at 25 °C for 6 h. Subsequently, the pH of the reaction system was adjusted to 9 with 0.1 mol / L NaOH solution, and the reaction was continued for 1 h. After the reaction was completed, the mixture was centrifuged, washed three times with ethanol, and vacuum dried at 60 °C for 6 h to obtain the filler with a three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure. 20 g of o-cresyl cyanate resin was weighed and heated in an 80 °C water bath for 30 min to reduce viscosity. Then 2 g of DBA was added, and the mixture was stirred mechanically at 500 rpm for 1 h to obtain a homogeneous matrix. 13.3 g of the "tethered anchor" structure filler (accounting for 80 wt.% of the resin mass) was weighed and added to 30 ml of anhydrous ethanol, and ultrasonically dispersed for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm. After the addition was complete, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler.The mixture obtained from S7 was transferred to a shallow dish and stirred continuously at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was then applied to a glass substrate, with a thickness controlled at 100 ± 10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120 °C for 1.5 h, then the temperature was increased to 160 °C and cured for another 2 h. After curing, the mixture was cooled to room temperature in the oven to obtain the final 80 wt.% Ti2SnC “rope anchor” conductive adhesive.
[0052] Example 7
[0053] 100g of Ti2SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 2000 r / min, and crushed for 10 min. After discharge, the powder was sieved to obtain millimeter-sized Ti2SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure of 1.0 MPa, and crushed for 30 min. This yielded micron-sized Ti2SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti2SnC phase powder was weighed and mixed with 20 g of a 3% FeCl3 solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti2SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1500 r / min for 60 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 140℃ for 12 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 24 h to obtain a "bolt-rope" structure packing composed of a one-dimensional "rope" structure with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which was grown in situ on the surface of the three-dimensional "bolt". 5 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. Prepare 50 ml of anhydrous ethanol solution containing 0.05 g of bis-[3-(trimethoxysilylpropyl)]amine, and slowly add it dropwise to the above filler dispersion under stirring. Continue stirring at 25 °C for 7 h. Then, adjust the pH of the reaction system to 9 with 0.1 mol / L NaOH solution and continue the reaction for 1 h. After the reaction is complete, centrifuge, wash three times with ethanol, and vacuum dry at 60 °C for 6 h to obtain the three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure filler. Weigh 20 g of o-cresyl formaldehyde cyanate resin and heat it in an 80 °C water bath for 60 min to reduce viscosity. Then add 2 g of DBA and mix under mechanical stirring at 1000 rpm for 3 h to obtain a homogeneous matrix. Weigh 10 g of the "tethered anchor" structure filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol, and ultrasonically disperse for 2 h to form a stable slurry. Slowly drop this slurry into the resin matrix under stirring at 750 rpm. After the material is added, increase the stirring speed to 2000 rpm and continue high-speed dispersion for 2 hours to ensure uniform dispersion of the filler.The mixture obtained in S7 was transferred to a shallow dish and stirred continuously at a low speed of 750 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was applied to a glass substrate, with a thickness controlled at 100 ± 10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 140 °C for 1.5 h, then the temperature was increased to 180 °C and cured for another 2 h. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ti2SnC “rope anchor” conductive adhesive.
[0054] Example 8
[0055] 100 g of Ti₂SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 2000 r / min, and crushed for 10 min. After discharge, the powder was sieved to obtain millimeter-sized Ti₂SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure of 0.8 MPa, and crushed for 30 min. This yielded micron-sized Ti₂SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti₂SnC phase powder was weighed and mixed with 20 g of 1% FeCl₃ solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti₂SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1500 r / min for 60 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 160℃ for 12 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain a "bolt-rope" structure packing composed of a one-dimensional "rope" structure with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which was grown in situ on the surface of the three-dimensional "bolt". 5 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. Prepare 50 ml of anhydrous ethanol solution containing 0.05 g of bis-[3-(trimethoxysilylpropyl)]amine, and slowly add it dropwise to the above filler dispersion under stirring. Continue stirring at 25 °C for 8 h. Then, adjust the pH of the reaction system to 9 with 0.1 mol / L NaOH solution and continue the reaction for 1 h. After the reaction is complete, centrifuge, wash three times with ethanol, and vacuum dry at 60 °C for 6 h to obtain the three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure filler. Weigh 30 g of o-cresyl formaldehyde cyanate resin and heat it in an 80 °C water bath for 30 min to reduce viscosity. Then add 2 g of DBA and mix under mechanical stirring at 500 rpm for 1 h to obtain a homogeneous matrix. Weigh 10 g of the "tethered anchor" structure filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol, and ultrasonically disperse for 1 h to form a stable slurry. Slowly add this slurry dropwise to the resin matrix under stirring at 550 rpm. After the material is added, increase the stirring speed to 1500 rpm and continue high-speed dispersion for 2 hours to ensure uniform dispersion of the filler.The mixture obtained in S7 was transferred to a shallow dish and stirred continuously at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was applied to a glass substrate, with a thickness controlled at 100 ± 10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120 °C for 1.5 h, then the temperature was increased to 160 °C and cured for another 2 h. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ti2SnC “rope anchor” conductive adhesive.
[0056] Example 9
[0057] 100 g of Ti₂SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 2000 r / min, and crushed for 10 min. After discharge, the powder was sieved to obtain millimeter-sized Ti₂SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure of 0.8 MPa, and crushed for 30 min. This yielded micron-sized Ti₂SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti₂SnC phase powder was weighed and mixed with 20 g of 1% FeCl₃ solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti₂SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1500 r / min for 60 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 120℃ for 24 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain a "bolt-rope" structure packing composed of a one-dimensional "rope" structure with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which was grown in situ on the surface of the three-dimensional "bolt". 5 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. Prepare 50 ml of anhydrous ethanol solution containing 0.05 g of N-(piperazinylethyl)-3-aminopropylmethyldimethoxysilane, and slowly add it dropwise to the above filler dispersion under stirring. Continue stirring at 25 °C for 6 h. Then, adjust the pH of the reaction system to 9 with 0.1 mol / L NaOH solution and continue the reaction for 1 h. After the reaction is complete, centrifuge, wash three times with ethanol, and vacuum dry at 60 °C for 6 h to obtain the three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure filler. Weigh 20 g of o-cresyl formaldehyde cyanate resin and heat it in an 80 °C water bath for 30 min to reduce viscosity. Then add 2 g of DBA and mix under mechanical stirring at 500 rpm for 1 h to obtain a homogeneous matrix. Weigh 10 g of the "tethered anchor" structure filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol, and ultrasonically disperse for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm.After the addition of materials, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler. The mixture obtained from S7 was transferred to a shallow dish and stirred at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was coated onto a glass substrate, with a thickness controlled at 100±10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120℃ for 1.5 hours, and then the temperature was increased to 160℃ for another 2 hours. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ti2SnC "rope anchor" conductive adhesive.
[0058] Example 10
[0059] 100 g of Ti₂SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 2000 r / min, and crushed for 10 min. After discharge, the powder was sieved to obtain millimeter-sized Ti₂SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure of 0.8 MPa, and crushed for 30 min. This yielded micron-sized Ti₂SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti₂SnC phase powder was weighed and mixed with 20 g of 1% FeCl₃ solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti₂SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1500 r / min for 60 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 140℃ for 24 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain a "bolt-rope" structure packing composed of a one-dimensional "rope" structure with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which was grown in situ on the surface of the three-dimensional "bolt". 5 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. A 50 ml anhydrous ethanol solution containing 0.05 g N-(piperazinylethyl)-3-aminopropylmethyldimethoxysilane was prepared and slowly added dropwise to the above filler dispersion under stirring. The reaction was carried out with stirring at 25 °C for 7 h. Subsequently, the pH of the reaction system was adjusted to 9 with 0.1 mol / L NaOH solution, and the reaction was continued for 1 h. After the reaction was completed, the mixture was centrifuged, washed three times with ethanol, and vacuum dried at 60 °C for 6 h to obtain the filler with a three-dimensional / one-dimensional / zero-dimensional "rope anchor" structure. 30 g of o-cresyl formaldehyde cyanate resin was weighed and heated in an 80 °C water bath for 30 min to reduce the viscosity. Then 2 g of DBA was added, and the mixture was stirred mechanically at 500 rpm for 1 h to obtain a homogeneous matrix. 10 g of the "rope anchor" structure filler (accounting for 60 wt.% of the resin mass) was weighed and added to 30 ml of anhydrous ethanol, and ultrasonically dispersed for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm.After the addition of materials, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler. The mixture obtained from S7 was transferred to a shallow dish and stirred at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was coated onto a glass substrate, with a thickness controlled at 100±10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120℃ for 1.5 hours, and then the temperature was increased to 160℃ for another 2 hours. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ti2SnC "rope anchor" conductive adhesive.
[0060] Example 11
[0061] 100 g of Ti₂SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 2000 r / min, and crushed for 10 min. After discharge, the powder was sieved to obtain millimeter-sized Ti₂SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure of 0.8 MPa, and crushed for 30 min. This yielded micron-sized Ti₂SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti₂SnC phase powder was weighed and mixed with 20 g of 1% FeCl₃ solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti₂SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1000 r / min for 60 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 160℃ for 24 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain a "bolt-rope" structure packing composed of a one-dimensional "rope" structure with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which was grown in situ on the surface of the three-dimensional "bolt". 5 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. Prepare 50 ml of anhydrous ethanol solution containing 0.05 g of N-(piperazinylethyl)-3-aminopropylmethyldimethoxysilane, and slowly add it dropwise to the above filler dispersion under stirring. Continue stirring at 25 °C for 8 h. Then, adjust the pH of the reaction system to 9 with 0.1 mol / L NaOH solution and continue the reaction for 1 h. After the reaction is complete, centrifuge, wash three times with ethanol, and vacuum dry at 60 °C for 6 h to obtain the three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure filler. Weigh 30 g of o-cresyl formaldehyde cyanate resin and heat it in an 80 °C water bath for 30 min to reduce viscosity. Then add 2 g of DBA and mix under mechanical stirring at 500 rpm for 1 h to obtain a homogeneous matrix. Weigh 10 g of the "tethered anchor" structure filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol, and ultrasonically disperse for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm.After the addition of materials, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler. The mixture obtained from S7 was transferred to a shallow dish and stirred at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was applied to a glass substrate, with a thickness controlled at 100±10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120℃ for 1.5 hours, and then the temperature was increased to 160℃ for another 2 hours. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ti2SnC “rope anchor” conductive adhesive.
[0062] Example 12
[0063] 100 g of Cr2SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 2000 r / min, and crushed for 10 min. After discharge, the powder was sieved to obtain millimeter-sized Cr2SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure of 0.8 MPa, and crushed for 30 min. This yielded micron-sized Cr2SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Cr2SnC phase powder was weighed and mixed with 20 g of 1% FeCl3 solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Cr2SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1000 r / min for 60 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Cr2SnC phase powder with A-layer homogenization pretreatment. 10 g of the S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 160℃ for 24 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain a "bolt-rope" structure packing composed of a one-dimensional "rope" structure with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which was grown in situ on the surface of the three-dimensional "bolt". 5 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. Prepare 50 ml of anhydrous ethanol solution containing 0.05 g of N-(piperazinylethyl)-3-aminopropylmethyldimethoxysilane, and slowly add it dropwise to the above filler dispersion under stirring. Continue stirring at 25 °C for 8 h. Then, adjust the pH of the reaction system to 9 with 0.1 mol / L NaOH solution and continue the reaction for 1 h. After the reaction is complete, centrifuge, wash three times with ethanol, and vacuum dry at 60 °C for 6 h to obtain the three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure filler. Weigh 30 g of o-cresyl formaldehyde cyanate resin and heat it in an 80 °C water bath for 30 min to reduce viscosity. Then add 2 g of DBA and mix under mechanical stirring at 500 rpm for 1 h to obtain a homogeneous matrix. Weigh 10 g of the "tethered anchor" structure filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol, and ultrasonically disperse for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm.After the addition of materials, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler. The mixture obtained from S7 was transferred to a shallow dish and stirred at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was applied to a glass substrate, with a thickness controlled at 100±10 µm. Curing was then carried out: first, it was cured in a forced-air drying oven at 120℃ for 1.5 hours, and then the temperature was increased to 160℃ for another 2 hours. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Cr2SnC “rope anchor” conductive adhesive.
[0064] Example 13
[0065] 100 g of Zr₂SnC powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 2000 r / min, and crushed for 10 min. After discharge, the powder was sieved to obtain millimeter-sized Zr₂SnC phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure of 0.8 MPa, and crushed for 30 min. This yielded micron-sized Zr₂SnC phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Zr₂SnC phase powder was weighed and mixed with 20 g of 1% FeCl₃ solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Zr₂SnC suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1500 r / min for 60 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Zr2SnC phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 120℃ for 24 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain "bolt-rope" structure packing composed of one-dimensional "rope" structures with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which were grown in situ on the surface of the three-dimensional "bolt". 5 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. Prepare 50 ml of anhydrous ethanol solution containing 0.05 g of N-(piperazinylethyl)-3-aminopropylmethyldimethoxysilane, and slowly add it dropwise to the above filler dispersion under stirring. Continue stirring at 25 °C for 6 h. Then, adjust the pH of the reaction system to 9 with 0.1 mol / L NaOH solution and continue the reaction for 1 h. After the reaction is complete, centrifuge, wash three times with ethanol, and vacuum dry at 60 °C for 6 h to obtain the three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure filler. Weigh 20 g of o-cresyl formaldehyde cyanate resin and heat it in an 80 °C water bath for 30 min to reduce viscosity. Then add 2 g of DBA and mix under mechanical stirring at 500 rpm for 1 h to obtain a homogeneous matrix. Weigh 10 g of the "tethered anchor" structure filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol, and ultrasonically disperse for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm.After the addition of materials, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler. The mixture obtained from S7 was transferred to a shallow dish and stirred at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was applied to a glass substrate, with a thickness controlled at 100±10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120℃ for 1.5 hours, and then the temperature was increased to 160℃ for another 2 hours. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Zr2SnC “rope anchor” conductive adhesive.
[0066] Example 14
[0067] 100 g of Ti3SnC2 powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 2000 r / min, and crushed for 10 min. After discharge, the powder was sieved to obtain millimeter-sized Ti3SnC2 phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure of 0.8 MPa, and crushed for 30 min. This yielded micron-sized Ti3SnC2 phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti3SnC2 phase powder was weighed and mixed with 20 g of a 1% FeCl3 solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti3SnC2 suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1500 r / min for 60 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti3SnC2 phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 160℃ for 24 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain a "bolt-rope" structure packing composed of a one-dimensional "rope" structure with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which was grown in situ on the surface of the three-dimensional "bolt". 5 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. Prepare 50 ml of anhydrous ethanol solution containing 0.05 g of N-(piperazinylethyl)-3-aminopropylmethyldimethoxysilane, and slowly add it dropwise to the above filler dispersion under stirring. Continue stirring at 25 °C for 6 h. Then, adjust the pH of the reaction system to 9 with 0.1 mol / L NaOH solution and continue the reaction for 1 h. After the reaction is complete, centrifuge, wash three times with ethanol, and vacuum dry at 60 °C for 6 h to obtain the three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure filler. Weigh 20 g of o-cresyl formaldehyde cyanate resin and heat it in an 80 °C water bath for 30 min to reduce viscosity. Then add 2 g of DBA and mix under mechanical stirring at 500 rpm for 1 h to obtain a homogeneous matrix. Weigh 10 g of the "tethered anchor" structure filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol, and ultrasonically disperse for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm.After the addition of materials, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler. The mixture obtained from S7 was transferred to a shallow dish and stirred at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was coated onto a glass substrate, with a thickness controlled at 100±10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120℃ for 1.5 hours, and then the temperature was increased to 160℃ for another 2 hours. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ti3SnC2 “rope anchor” conductive adhesive.
[0068] Example 15
[0069] 100 g of Ti3SnC2 powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 2000 r / min, and crushed for 10 min. After discharge, the powder was sieved to obtain millimeter-sized Ti3SnC2 phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure of 0.8 MPa, and crushed for 30 min. This yielded micron-sized Ti3SnC2 phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti3SnC2 phase powder was weighed and mixed with 20 g of a 1% FeCl3 solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti3SnC2 suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1500 r / min for 60 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti3SnC2 phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 120℃ for 12 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain a "bolt-rope" structure packing composed of a one-dimensional "rope" structure with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which was grown in situ on the surface of the three-dimensional "bolt". 5 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. Prepare 50 ml of anhydrous ethanol solution containing 0.05 g of N-(piperazinylethyl)-3-aminopropylmethyldimethoxysilane, and slowly add it dropwise to the above filler dispersion under stirring. Continue stirring at 25 °C for 6 h. Then, adjust the pH of the reaction system to 9 with 0.1 mol / L NaOH solution and continue the reaction for 1 h. After the reaction is complete, centrifuge, wash three times with ethanol, and vacuum dry at 60 °C for 6 h to obtain the three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure filler. Weigh 20 g of o-cresyl formaldehyde cyanate resin and heat it in an 80 °C water bath for 30 min to reduce viscosity. Then add 2 g of DBA and mix under mechanical stirring at 500 rpm for 1 h to obtain a homogeneous matrix. Weigh 10 g of the "tethered anchor" structure filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol, and ultrasonically disperse for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm.After the addition of materials, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler. The mixture obtained from S7 was transferred to a shallow dish and stirred at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was coated onto a glass substrate, with a thickness controlled at 100±10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120℃ for 1.5 hours, and then the temperature was increased to 160℃ for another 2 hours. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ti3SnC2 “rope anchor” conductive adhesive.
[0070] Example 16
[0071] 100 g of Ti3SnC2 powder was placed in an ultrafine vertical impact crusher, with the impeller speed set to 2000 r / min, and crushed for 10 min. After discharge, the powder was sieved to obtain millimeter-sized Ti3SnC2 phase powder with a particle size distribution of 0.5-2 mm. The millimeter-sized powder was then fed into an all-ceramic, pollution-free fluidized bed jet mill, with a crushing pressure of 0.8 MPa, and crushed for 30 min. This yielded micron-sized Ti3SnC2 phase powder with a three-dimensional "bolt" structure and a particle size of approximately 20-50 µm. 20 g of the micron-sized Ti3SnC2 phase powder was weighed and mixed with 20 g of a 1% FeCl3 solution, and placed in a beaker. The mixture was treated in a 50℃ water bath under ultrasonic power of 300 W and mechanical stirring speed of 300 rpm for 2 h to obtain a Ti3SnC2 suspension that was slightly etched and homogenized. The suspension was filtered and washed with deionized water until the filtrate was neutral. The filter cake was redispersed in deionized water and centrifuged at 1500 r / min for 60 min. The precipitate was dried in a vacuum drying oven at 80℃ for 12 h to obtain Ti3SnC2 phase powder with A-layer homogenization pretreatment. 10 g of the obtained S3 powder was weighed and placed in a 100 ml high-pressure reactor. Ultrapure water was added to fill 70% of the inner liner volume, and then ammonia was added dropwise to adjust the pH of the system to 9. The reactor was sealed and placed in an oven at 120℃ for 24 h. After the reactor cooled naturally, the product suspension was removed, filtered, and washed three times alternately with deionized water and anhydrous ethanol. It was then freeze-dried under vacuum for 12 h to obtain a "bolt-rope" structure packing composed of a one-dimensional "rope" structure with a diameter of 0.1-2 µm and a length of 100-200 µm, and coated with a Sn oxide layer, which was grown in situ on the surface of the three-dimensional "bolt". 5 g of the "bolt-rope" structure packing was dispersed in 200 ml of deionized water. Prepare 50 ml of anhydrous ethanol solution containing 0.05 g of N-(piperazinylethyl)-3-aminopropylmethyldimethoxysilane, and slowly add it dropwise to the above filler dispersion under stirring. Continue stirring at 25 °C for 6 h. Then, adjust the pH of the reaction system to 9 with 0.1 mol / L NaOH solution and continue the reaction for 1 h. After the reaction is complete, centrifuge, wash three times with ethanol, and vacuum dry at 60 °C for 6 h to obtain the three-dimensional / one-dimensional / zero-dimensional "tethered anchor" structure filler. Weigh 20 g of o-cresyl formaldehyde cyanate resin and heat it in an 80 °C water bath for 30 min to reduce viscosity. Then add 2 g of DBA and mix under mechanical stirring at 500 rpm for 1 h to obtain a homogeneous matrix. Weigh 10 g of the "tethered anchor" structure filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol, and ultrasonically disperse for 1 h to form a stable slurry. The slurry was slowly added dropwise to the resin matrix at a stirring speed of 550 rpm.After the addition of materials, the stirring speed was increased to 1500 rpm, and high-speed dispersion was maintained for 2 hours to ensure uniform dispersion of the filler. The mixture obtained from S7 was transferred to a shallow dish and stirred at a low speed of 550 rpm in a fume hood until the anhydrous ethanol was completely evaporated, resulting in a viscous conductive paste. The paste was coated onto a glass substrate, with a thickness controlled at 100±10 µm. Curing was then performed: first, it was cured in a forced-air drying oven at 120℃ for 1.5 hours, and then the temperature was increased to 160℃ for another 2 hours. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ti3SnC2 “rope anchor” conductive adhesive.
[0072] Comparative Example 1
[0073] Weigh 20 g of epoxy resin and heat it in an 80℃ water bath for 30 min to reduce its viscosity. Then add 2 g of DDS curing agent and mix for 1 h under mechanical stirring at 500 rpm to obtain a homogeneous matrix. Weigh 6.7 g of micron-sized Ag ball filler (40 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol. Disperse the mixture ultrasonically for 1 h to form a stable slurry. Slowly add the slurry dropwise to the resin matrix while stirring at 550 rpm. After the addition is complete, increase the stirring speed to 1500 rpm and continue high-speed dispersion for 2 h to ensure uniform dispersion of the filler. Transfer the mixture obtained in S7 to a shallow dish and stir continuously at low speed of 550 rpm in a fume hood until the anhydrous ethanol is completely evaporated to obtain a viscous conductive paste. Apply the paste to a glass substrate, controlling the thickness to be 100±10 µm. Curing was then carried out: first, it was cured in a forced-air drying oven at 120℃ for 1.5 h, and then the temperature was raised to 160℃ for another 2 h. After curing, it was cooled to room temperature in the oven to obtain the final 40 wt.% Ag ball conductive adhesive.
[0074] Comparative Example 2
[0075] Weigh 20 g of epoxy resin and heat it in an 80℃ water bath for 30 min to reduce its viscosity. Then add 2 g of DDS curing agent and mix for 1 h under mechanical stirring at 500 rpm to obtain a homogeneous matrix. Weigh 8.3 g of micron-sized Ag ball filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol. Disperse the mixture ultrasonically for 1 h to form a stable slurry. Slowly add the slurry dropwise to the resin matrix while stirring at 550 rpm. After the addition is complete, increase the stirring speed to 1500 rpm and continue high-speed dispersion for 2 h to ensure uniform dispersion of the filler. Transfer the mixture obtained in S7 to a shallow dish and stir continuously at low speed of 550 rpm in a fume hood until the anhydrous ethanol is completely evaporated to obtain a viscous conductive paste. Apply the paste to a glass substrate, controlling the thickness to be 100±10 µm. Curing was then carried out: first, it was cured in a forced-air drying oven at 120°C for 1.5 h, and then the temperature was raised to 160°C for another 2 h. After curing, it was cooled to room temperature in the oven to obtain the final 50 wt.% Ag ball conductive adhesive.
[0076] Comparative Example 3
[0077] Weigh 20 g of epoxy resin and heat it in an 80℃ water bath for 30 min to reduce its viscosity. Then add 2 g of DDS curing agent and mix for 1 h with mechanical stirring at 500 rpm to obtain a homogeneous matrix. Weigh 10 g of micron-sized Ag ball filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol. Disperse the mixture ultrasonically for 1 h to form a stable slurry. Slowly add the slurry dropwise to the resin matrix while stirring at 550 rpm. After the addition is complete, increase the stirring speed to 1500 rpm and continue high-speed dispersion for 2 h to ensure uniform dispersion of the filler. Transfer the mixture obtained in S7 to a shallow dish and stir continuously at low speed of 550 rpm in a fume hood until the anhydrous ethanol is completely evaporated to obtain a viscous conductive paste. Apply the paste to a glass substrate, controlling the thickness to be 100±10 µm. Curing was then carried out: first, it was cured in a forced-air drying oven at 120°C for 1.5 h, and then the temperature was raised to 160°C for another 2 h. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ag ball conductive adhesive.
[0078] Comparative Example 4
[0079] Weigh 20 g of epoxy resin and heat it in an 80℃ water bath for 30 min to reduce its viscosity. Then add 2 g of DDS curing agent and mix for 1 h under mechanical stirring at 500 rpm to obtain a homogeneous matrix. Weigh 10 g of micron-sized Ag sheet filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol. Disperse the filler ultrasonically for 1 h to form a stable slurry. Slowly add the slurry dropwise to the resin matrix while stirring at 550 rpm. After the addition is complete, increase the stirring speed to 1500 rpm and continue high-speed dispersion for 2 h to ensure uniform dispersion of the filler. Transfer the mixture obtained in S7 to a shallow dish and stir continuously at low speed of 550 rpm in a fume hood until the anhydrous ethanol is completely evaporated to obtain a viscous conductive paste. Apply the paste to a glass substrate, controlling the thickness to be 100±10 µm. Curing was then carried out: first, it was cured in a forced-air drying oven at 120°C for 1.5 h, and then the temperature was raised to 160°C for another 2 h. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ag sheet conductive adhesive.
[0080] Comparative Example 5
[0081] Weigh 20 g of epoxy resin and heat it in an 80℃ water bath for 30 min to reduce its viscosity. Then add 2 g of DDS curing agent and mix for 1 h under mechanical stirring at 500 rpm to obtain a homogeneous matrix. Weigh 10 g of micron-sized Ag nanowire filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol. Disperse the filler ultrasonically for 1 h to form a stable slurry. Slowly add the slurry dropwise to the resin matrix while stirring at 550 rpm. After the addition is complete, increase the stirring speed to 1500 rpm and continue high-speed dispersion for 2 h to ensure uniform dispersion of the filler. Transfer the mixture obtained in S7 to a shallow dish and stir continuously at a low speed of 550 rpm in a fume hood until the anhydrous ethanol is completely evaporated to obtain a viscous conductive paste. Apply the paste to a glass substrate, controlling the thickness to be 100±10 µm. Curing was then carried out: first, it was cured in a forced-air drying oven at 120℃ for 1.5 h, and then the temperature was raised to 160℃ for another 2 h. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% Ag nanowire conductive adhesive.
[0082] Comparative Example 6
[0083] Weigh 20 g of epoxy resin and heat it in an 80℃ water bath for 30 min to reduce its viscosity. Then add 2 g of DDS curing agent and mix for 1 h under mechanical stirring at 500 rpm to obtain a homogeneous matrix. Weigh 10 g of micron-sized Cu@Ag ball filler (60 wt.% of the resin mass) and add it to 30 ml of anhydrous ethanol. Disperse the mixture ultrasonically for 1 h to form a stable slurry. Slowly add the slurry dropwise to the resin matrix while stirring at 550 rpm. After the addition is complete, increase the stirring speed to 1500 rpm and continue high-speed dispersion for 2 h to ensure uniform dispersion of the filler. Transfer the mixture obtained in S7 to a shallow dish and stir continuously at low speed of 550 rpm in a fume hood until the anhydrous ethanol is completely evaporated to obtain a viscous conductive paste. Apply the paste to a glass substrate, controlling the thickness to be 100±10 µm. Curing was then carried out: first, it was cured in a forced-air drying oven at 120℃ for 1.5 h, and then the temperature was raised to 160℃ for another 2 h. After curing, it was cooled to room temperature in the oven to obtain the final 60 wt.% silver-plated copper ball conductive adhesive.
[0084] The conductive adhesive prepared above was subjected to performance tests according to GB / T 33362-2022 General Technical Conditions for Conductive Adhesives. The performance data are shown in Table 1.
[0085] Table 1 Performance test results of conductive adhesive
[0086] Resistivity (Ω·cm) Shear properties (MPa) Example 1 insulation 19.8 Example 2 <![CDATA[2.5×10 5 ]]> 19.2 Example 3 <![CDATA[8.9×10 -2 ]]> 18.2 Example 4 <![CDATA[5.9×10 -5 ]]> 17.3 Example 5 <![CDATA[6.4×10 -5 ]]> 15.9 Example 6 <![CDATA[2.9×10 -4 ]]> 12.1 Example 7 <![CDATA[5.7×10 -5 ]]> 16.5 Example 8 <![CDATA[5.2×10 -5 ]]> 16.9 Example 9 <![CDATA[5.5×10 -5 ]]> 16.6 Example 10 <![CDATA[5.1×10 -5 ]]> 17.2 Example 11 <![CDATA[5.0×10 -5 ]]> 17.5 Example 12 <![CDATA[5.3×10 -5 ]]> 16.7 Example 13 <![CDATA[6.0×10 -5 ]]> 16.6 Example 14 <![CDATA[5.3×10 -5 ]]> 16.9 Example 15 <![CDATA[5.9×10 -5 ]]> 16.7 Example 16 <![CDATA[5.3×10 -5 ]]> 16.5 Comparative Example 1 / Ag Ball insulation 15.3 Comparative Example 2 / Ag Ball <![CDATA[2.7×10 4 ]]> 14.6 Comparative Example 3 / Ag Ball <![CDATA[5.3×10 -4 ]]> 12.3 Comparative Example 4 / Ag Tablets <![CDATA[7.1×10 -5 ]]> 16.1 Comparative Example 5 / Ag Line <![CDATA[3.5×10 -4 ]]> 13.3 Comparative Example 6 / Cu@Ag Ball <![CDATA[6.2×10 -4 ]]> 10.7
[0087] pass Figure 5 It can be concluded that, compared with conductive adhesives containing multidimensional "rope anchor" structure fillers prepared in this invention, the actual resistivity range measured in Examples 4, 7-16 of Ag spheres, Ag sheets, Ag wires, and Cu@Ag spheres is 5.0-6.0 × 10⁻⁶. -5 Ω·cm. Comparative Example 4 (7.1 × 10⁻⁶) -5 Based on Ω·cm, Example 11 (5.0×10 -5 The resistivity of Ω·cm decreased by approximately 29.6% [i.e., (7.1-5.0) / 7.1×100%]; compared to Comparative Example 6 (6.2×10 -4 Based on Ω·cm, Example 13 (6.0×10) -5 The resistivity (Ω·cm) was reduced by approximately 90.3% [i.e., (62.0-6.0) / 62.0×100%]; overall, compared to the aforementioned comparative materials, the resistivity of the present invention achieved a reduction of 29.6%-90.3%.
[0088] pass Figure 6It can be concluded that, compared with Ag spheres, Ag sheets, Ag wires, and Cu@Ag sphere conductive adhesives, the actual shear performance of the conductive adhesive containing multidimensional "tethered anchor" structure filler prepared in this invention ranges from 16.5 to 17.5 MPa, as measured in Examples 4, 7-16. Based on Comparative Example 4 (16.1 MPa), the shear performance of Example 11 (17.5 MPa) is improved by approximately 8.7% [i.e., (17.5-16.1) / 16.1×100%]; based on Comparative Example 6 (10.7 MPa), the shear performance of Example 7 (16.5 MPa) is improved by approximately 54.2% [i.e., (16.5-10.7) / 10.7×100%]; overall, compared with the above comparative materials, the shear performance of this invention achieves an improvement of 8.7%-54.2%.
[0089] like Figure 7 As shown, the multidimensional "tethered anchor" structure conductive adhesive prepared by this invention exhibits significantly superior conductive network construction efficiency. Specifically, as... Figure 7 As shown in (a), with the increase of the multidimensional "rope anchor" filler content, the resistivity of the conductive colloid exhibits typical percolation characteristics: a sharp percolation transition occurs in the 30-40 wt.% range; when the filler content reaches 60 wt.%, the volume resistivity decreases to 5.9 × 10⁻⁶. -5 Ω·cm indicates the formation of a dense and efficient conductive path. In contrast, such as Figure 7 As shown in (b), a sharp seepage transition occurred in the 40-50 wt.% range in Comparative Examples 1-3; the volume resistivity of pure Ag sphere packing at a filling amount of 60 wt.% was 5.3 × 10⁻⁶. -4 Ω·cm. The above data shows that the multidimensional "bolt-rope anchor" structure packing of the present invention has a lower seepage threshold; under the same filling amount, the multidimensional "bolt-rope anchor" structure packing of the present invention, with the supporting effect of the three-dimensional "bolt" structure and the high aspect ratio overlap effect of the one-dimensional "rope" structure, reduces the resistivity by an order of magnitude compared with the traditional spherical Ag packing, and achieves superior low-resistance conductivity.
[0090] The above description is merely a preferred embodiment of the present invention and is illustrative rather than restrictive. Those skilled in the art will understand that many changes, modifications, and even equivalents can be made within the spirit and scope defined by the claims of the present invention, all of which will fall within the protection scope of the present invention.
Claims
1. A conductive adhesive containing a multidimensional structure filler, characterized in that, The conductive adhesive matrix is o-cresol formaldehyde cyanate resin, and the filler is a material with a "rope anchor" structure. The "rope anchor" structure is as follows: The bolt structure is a three-dimensional MAX phase; The rope structure is a one-dimensional "single crystal core@oxide shell" core-shell nanowire; Anchor structure, which is a coupling agent site grafted onto the oxide shell on the surface of a one-dimensional single crystal wire; The MAX phase material is selected from any one of Ti2SnC, Ti3SnC2, Cr2SnC and Zr2SnC; The coupling agent is selected from any one of N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, bis-[3-(trimethoxysilylpropyl)]amine, and N-(piperazinylethyl)-3-aminopropylmethyldimethoxysilane.
2. A method for preparing the conductive adhesive as described in claim 1, characterized in that... Includes the following steps: S1: Impact crushing of MAX phase powder to obtain millimeter-sized MAX phase powder; S2: The millimeter-scale MAX phase powder is subjected to airflow pulverization to obtain micron-scale three-dimensional "bolt" structure MAX phase powder; S3: Mix the micron-sized MAX phase powder with Lewis acid, perform ultrasonic stirring and low-temperature heat treatment, filter, wash and centrifuge the treated suspension to obtain MAX phase powder pretreated by A-layer isochronization. S4: The MAX phase powder after the A layer isochronous pretreatment is mixed with ammonia and ultrapure water and subjected to hydrothermal reaction; the suspension after hydrothermal reaction is filtered, washed and vacuum freeze-dried to obtain powder with a three-dimensional / one-dimensional "tethered rope" structure. S5: The powder of the "tethered rope" structure is surface modified with a coupling agent to obtain a filler with a three-dimensional / one-dimensional / zero-dimensional "tethered rope anchor" structure; S6: After heating the o-cresol cyanate resin, it is mixed and stirred with diallyl bisphenol A to obtain a homogeneous resin matrix; S7: After pre-dispersing the "rope anchor" structure filler, add it to the matrix described in S6 and continue stirring and dispersing to obtain a mixture; then stir until the dispersant in the mixture is completely removed, and heat to cure to obtain the conductive adhesive.
3. The method for preparing conductive adhesive as described in claim 2, characterized in that, In step S1, the impact crushing adopts an ultrafine vertical impact crusher with an impeller speed of 1000-2000 r / min and a crushing time of 5-10 min, to obtain MAX phase powder with a particle size of 0.5-2 mm.
4. The method for preparing conductive adhesive as described in claim 2, characterized in that, In step S2, the air jet milling is performed using an all-ceramic, pollution-free fluidized bed air jet mill with a milling pressure of 0.8-1.0 MPa and a crushing time of 20-30 min, to obtain MAX phase powder with a particle size of 20-50 µm.
5. The method for preparing conductive adhesive as described in claim 2, characterized in that, In step S3, the mass ratio of the micron-sized MAX phase powder to the 1-3 wt.% Lewis acid solution is 1:1, the reaction time is 2 h, the centrifugal drying speed is 1000-1500 r / min, and the time is 30-60 min, to obtain MAX phase powder with a homogenized A-layer coordination environment and a weakly activated MA bond state.
6. The method for preparing conductive adhesive according to claim 2, characterized in that, In step S4, the hydrothermal reaction is carried out in a high-pressure reactor, with 70% of the reactor volume filled with ultrapure water. The reaction temperature is 120-160℃, the reaction time is 12-24h, the pH value of the reaction system is adjusted to 9 with ammonia, and the vacuum freeze-drying time is 12-24h to obtain a three-dimensional / one-dimensional "tethered rope" structure powder.
7. The method for preparing conductive adhesive according to claim 2, characterized in that, Step S5 includes: mixing and dispersing the "tethered rope" structure powder and coupling agent in deionized water at a mass ratio of 80-100:1, adjusting the pH value to about 9 with NaOH solution, and stirring the reaction at 25°C for 6-8 hours; after centrifugation, washing, and drying, the filler of the "tethered rope anchor" structure is obtained.
8. The method for preparing conductive adhesive as described in claim 2, characterized in that, In step S6, after the o-cresol cyanate resin is heated in a water bath at 80°C for 30-60 min, it is mixed with diallyl bisphenol A at a mass ratio of 10-15:1 and stirred at a speed of 500-1000 rpm for 1-3 h.
9. The method for preparing conductive adhesive according to claim 2, characterized in that, Step S7 includes: ultrasonically dispersing the filler of the "rope anchor" structure in anhydrous ethanol for 1-2 h, then adding it to the matrix at a stirring speed of 550-750 rpm, and then increasing the stirring speed to 1500-2000 rpm for dispersion; after uniform dispersion, stirring the mixture at a speed of 550-750 rpm until the anhydrous ethanol is completely evaporated, then curing at 120-140℃ for 1.5 h, and then curing at 160-180℃ for 2 h.