An amine polymer inhibitor for drilling fluid and its preparation method

The prepared drilling fluid amine polymer inhibitor utilizes a polymer skeleton formed by the specific reaction of polyhydroxy and amine structures to solve the problem of insufficient wellbore stability under high temperature, high salt and calcium and magnesium ion environments. It achieves stable adsorption and coating of the inhibitor on the clay surface, reduces shale hydration swelling, and improves wellbore stability.

CN123107639APending Publication Date: 2026-11-17SHANDONG DESHUNYUAN PETROLEUM SCI&TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611629090.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing drilling fluid amine polymer inhibitors are susceptible to interference from ionic environment and molecular conformation changes in complex environments such as high temperature, high salinity, and coexistence of calcium and magnesium ions. This results in insufficient wellbore stability and difficulty in effectively controlling shale hydration expansion and dispersion.

Method used

An amine polymer inhibitor for drilling fluid was prepared by reacting glycerol diglycidyl ether in additive A with 2-amino-1,3-propanediol to form a multi-hydroxyl linkage structure, which was then combined with polyether diamine. After introducing methyl acrylate reaction sites, the mixture underwent hydroxyoxime treatment to form an amine-rich polymer backbone. Additive B was treated with viscous esterification to form a composite powder with a multi-hydroxyl structure, which underwent limited ammonolysis with low-molecular-weight polyether diamine to form multi-hydroxyl segments, thereby enhancing the adsorption and coating capacity of clay surfaces.

Benefits of technology

Under conditions of high temperature, high salinity, and calcium and magnesium ion contamination, the stability of the inhibitor was significantly improved, the degree of shale hydration swelling and dispersion was reduced, the stabilizing effect of the drilling fluid on the wellbore was enhanced, and the risk of wellbore instability was mitigated.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107639A_ABST
    Figure CN123107639A_ABST
Patent Text Reader

Abstract

This invention relates to the field of oil and gas drilling engineering technology, specifically to an amine polymer inhibitor for drilling fluids and its preparation method, comprising the following raw materials in parts by weight: 25-35 parts low molecular weight polyether diamine, 8-14 parts additive A, 6-12 parts additive B, 3-6 parts glycerol, 1-2 parts lactic acid, and 45-60 parts deionized water. In this invention, glycerol diglycidyl ether in additive A reacts with 2-amino-1,3-propanediol to form a first linking structure containing multiple hydroxyl groups. This multiple hydroxyl structure helps maintain the dispersion state of the polymer in the aqueous phase and improves the adsorption stability of the inhibitor under high temperature, high salt, and shear conditions. The viscous acid in additive B undergoes esterification treatment to form a composite powder containing multiple hydroxyl groups, which helps regulate the hydration state and spatial conformation of polymer segments and reduces polymer chain shrinkage and aggregation under high salinity conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of oil and gas drilling engineering technology, specifically to an amine polymer inhibitor for drilling fluid and its preparation method. Background Technology

[0002] In oil and gas drilling, water-based drilling fluids are widely used due to their relatively low cost, ease of construction and maintenance, and wide applicability. However, when drilling into water-sensitive formations such as shale and mudstone, water in the drilling fluid can easily enter the clay interlayer, causing clay mineral hydration, swelling, and dispersion, thus affecting wellbore stability. Therefore, it is usually necessary to add inhibitors to water-based drilling fluids to reduce the interaction between clay and shale and the aqueous phase. Amine polymer inhibitors contain amine functional groups that can interact with the surface of negatively charged clay. They can inhibit clay hydration and dispersion through adsorption, coating, and other methods, and are currently a commonly used class of treatment agents in drilling fluid inhibition systems.

[0003] In the prior art, Chinese patent CN109694473B discloses a polyetheramine shale inhibitor for drilling fluid, its preparation method, and the drilling fluid. The polyetheramine shale inhibitor is prepared by reacting glycol compounds, water, chlorinated epoxides, acidic catalysts, polyethylene polyamines, and ethanolamines. It utilizes the interaction between the polyetheramine structure and clay minerals to improve shale inhibition and clay stability, while also taking into account the lubrication performance of the drilling fluid. This technology uses a polyetheramine structure as the main inhibitory structure, relying primarily on the interaction between the amine groups and clay minerals, as well as the effect of the polyether segments on the clay interlayer, to achieve the inhibitory effect. However, in complex drilling fluid environments characterized by high temperature, high salinity, and the coexistence of multivalent ions such as calcium and magnesium, the interaction state between the inhibitor molecules and clay minerals is easily affected by changes in the ionic environment and molecular conformation. Further regulation of the polymer structure to balance high-temperature and high-salt stability, resistance to calcium and magnesium contamination, and shale inhibition performance still has room for improvement. Furthermore, Chinese patent CN111718698B discloses a hyperbranched polyetheramine environmentally friendly shale inhibitor, its preparation method, and a water-based drilling fluid. By constructing a hyperbranched polyetheramine structure, it increases the number of interaction sites and improves the inhibition performance in the drilling fluid system. However, this technology mainly improves performance by increasing the degree of molecular branching, and still has shortcomings in regulating the polymer hydration state and improving long-term coating stability under complex mineralization environments. Therefore, this invention provides an amine polymer inhibitor for drilling fluids and its preparation method. Summary of the Invention

[0004] The purpose of this invention is to provide an amine polymer inhibitor for drilling fluid and its preparation method. The amine polymer inhibitor for drilling fluid prepared by this invention not only has good shale inhibition performance under high temperature and high salinity conditions, but also has good inhibition stability under calcium and magnesium ion contamination conditions. It can effectively reduce the hydration expansion and dispersion of shale and improve the stabilizing effect of drilling fluid on the wellbore.

[0005] To achieve the above objectives, the present invention provides the following technical solution: In a first aspect, the present invention provides an amine polymer inhibitor for drilling fluids, comprising the following raw materials in parts by weight: 25-35 parts of low molecular weight polyether diamine, 8-14 parts of additive A, 6-12 parts of additive B, 3-6 parts of glycerol, 1-2 parts of lactic acid, and 45-60 parts of deionized water; wherein the low molecular weight polyether diamine has a number average molecular weight of 200-400. Additive A is an amine-based composite material obtained by modifying polyether diamine with a binder containing a multi-hydroxyl linkage structure, followed by reaction with methyl acrylate and hydroxylamine hydrochloride hydroxyoxime treatment. Additive B is a polyhydroxyamine-based composite material obtained by dispersing the composite powder obtained by esterification of viscous acid with anhydrous ethanol and then reacting it with low molecular weight polyether diamine.

[0006] Further, the additive A is prepared by the following method: an amine solution is mixed with 4-6 times its mass of deionized water, stirred at 25-35°C and 300-500 rpm for 20-30 minutes, methyl acrylate (MCA) accounting for 5-9% of the total mass of non-aqueous components in the amine solution is added, and the mixture is stirred at 30-40°C and 400-600 rpm for 2-3 hours. Hydroxylamine hydrochloride (hydroxylamine hydrochloride) accounting for 85-105% of the mass of methyl acrylate is added, and sodium bicarbonate is added to adjust the pH to [the desired concentration]. 7.5-8.5, stir at 35-45℃ and 400-600rpm for 3-5h, cool to 25-35℃, adjust pH to 6.5-7.5 with lactic acid, add anhydrous ethanol to make the volume fraction of ethanol 70-80%, let stand for 1-2h and then centrifuge. Wash the precipitate twice with 75% ethanol aqueous solution and once with deionized water. Dry at 50-60℃ for 6-8h, pulverize and pass through a 200-mesh sieve to obtain additive A.

[0007] The obtained additive A was characterized by infrared spectroscopy. Figure 2 It can be seen that additive A is at approximately 3300 cm. -1 A broad absorption band appears at 2930 cm⁻¹, indicating the stretching vibrations of hydroxyl and amino groups. -1 The vicinity shows an absorption peak of aliphatic C-H stretching vibration; approximately 1660 cm⁻¹. -1 An absorption peak for carbonyl stretching vibration appears at approximately 1590 cm⁻¹. -1 An absorption peak for the bending vibration of nitrogen-containing groups appears at approximately 1460 cm⁻¹.-1 An absorption peak for the methylene bending vibration appears at approximately 1100 cm⁻¹. -1 An absorption peak for the stretching vibration of the ether bond carbon-oxygen-carbon structure appears at approximately 940 cm⁻¹. -1 The absorption peaks at the specified locations are assigned according to the N-O stretching vibration. The above characteristic peaks indicate that the obtained additive A has formed and retained structures such as polyhydroxyl groups, nitrogen-containing groups, carbonyl groups, and ether bonds, which correspond to the polyhydroxyl linkage structure, polyether segments, and hydroxyoxime structure introduced during its preparation process.

[0008] Further, the amine-based liquid is prepared by the following method: a polyether diamine with a number average molecular weight of 200-400 is mixed with 2-4 times its mass of deionized water, stirred at 25-35°C and 300-500 rpm for 20-30 min, a first connecting liquid accounting for 4-8% of the mass of the polyether diamine is added, and stirred at 35-45°C and 400-600 rpm for 2-4 h, and then cooled to obtain the amine-based liquid.

[0009] Further, the first connecting liquid is prepared by the following method: glycerol diglycidyl ether is mixed with 1-2 times its mass of deionized water, 18-25% of 2-amino-1,3-propanediol is added, and the mixture is stirred at 25-35°C and 300-500 rpm for 1-2 hours. The temperature is then raised to 40-50°C and stirring is continued for 1-2 hours. After cooling, the first connecting liquid is obtained.

[0010] Further, the additive B is prepared by the following method: low molecular weight polyether diamine is mixed with 2-4 times its mass of deionized water, stirred at 30-40℃ and 300-500rpm for 20-30min, a second connecting liquid accounting for 8-15% of the mass of polyether diamine is added, stirred at 65-80℃ and 400-600rpm for 3-5h, cooled, and anhydrous ethanol is added to make the ethanol volume fraction reach 70-80%, allowed to stand, centrifuged, and the resulting solid is washed twice with 75% ethanol aqueous solution and once with deionized water, dried at 50-60℃ for 6-8h, pulverized, and additive B is obtained.

[0011] Among them, the obtained additive B was characterized by infrared spectroscopy. Figure 3 It can be seen that additive B is at approximately 3370 cm. -1 A broad absorption band for O-H / N-H stretching vibrations appears at 2930 cm⁻¹. -1 The vicinity exhibits aliphatic C-H stretching vibrations; 1720 cm -1 The vicinity is near the C=O stretching vibration of the ester group; approximately 1650 cm. -1 An absorption peak corresponding to the carbonyl stretching vibration of the amide I band appears at approximately 1550 cm⁻¹. -1An absorption peak corresponding to the N-H bending and C-N stretching vibrations of the amide II band appears at approximately 1460 cm⁻¹; an absorption peak of the methylene bending vibration appears at approximately 1100 cm⁻¹. -1 An absorption peak for the stretching vibration of the ether bond carbon-oxygen-carbon structure appears at approximately 940 cm⁻¹. -1 A C-O structure-related absorption peak appears. These characteristic peaks indicate that the obtained additive B retains both the ester group structure and forms an amide structure, while also possessing structures such as polyhydroxyl groups, nitrogen-containing groups, and ether bonds. This corresponds to the preparation process in which the ester group in the composite powder undergoes limited ammonolysis with the low-molecular-weight polyether diamine.

[0012] Further, the second connecting liquid is prepared by the following method: the composite powder is added to anhydrous ethanol at 4-6 times its mass, and stirred at 35-45℃ and 300-500rpm for 20-30min to obtain the second connecting liquid.

[0013] Further, the composite powder is prepared by the following method: viscous acid and methanol are mixed at a mass ratio of 1:(8-12), stirred at 20-30℃ and 300-500rpm for 20-30min, sulfuric acid of 95% by mass (1-2% of the viscous acid mass) is added, a reflux condenser is installed, the temperature is raised to 60-68℃ at 2-4℃ / min, and refluxed at 300-500rpm for 4-6h. After the reaction is completed, the mixture is cooled to 10-20℃ and allowed to stand for 1-2h, filtered, and the resulting solid is washed twice with a 65% methanol aqueous solution, then washed once with deionized water, dried at 50-60℃ for 6-8h, and ground through a 200-mesh sieve to obtain the composite powder.

[0014] Secondly, a method for preparing an amine polymer inhibitor for drilling fluids includes the following steps: S1: Preparation of base solution: Add low molecular weight polyether diamine and glycerol to deionized water, and stir at 25-35℃ and 300-500rpm for 20-30min to obtain base solution; S2: Introduction of polyhydroxy structure: Additive B is added to the base solution and stirred at 35-45℃ and 400-600rpm for 20-30min to obtain the first composite solution; S3: Introduction of anchoring structure: Add additive A to the first composite liquid and stir at 35-45℃ and 400-600rpm for 30-45min to obtain the second composite liquid; S4: System adjustment: Under the conditions of stirring at 25-35℃ and 300-500rpm, lactic acid is added to the second composite solution to adjust the pH to 7.0-8.0, and stirring is continued for 30-45min to obtain the amine polymer inhibitor for drilling fluid.

[0015] Furthermore, when the drilling fluid amine polymer inhibitor is used in water-based drilling fluid, the amount added is 0.8-2.0% of the mass of the water-based drilling fluid, and after addition, it is stirred at 600-800 rpm for 20-30 min.

[0016] When the drilling fluid amine polymer inhibitor is used in water-based drilling fluid, the amount added is 0.8-2.0% of the mass of the water-based drilling fluid, and after addition, it is stirred at 600-800 rpm for 20-30 minutes.

[0017] Compared with the prior art, the beneficial effects of the present invention are: 1. In this invention, glycerol diglycidyl ether in additive A reacts with 2-amino-1,3-propanediol to form a first linking structure containing multiple hydroxyl groups. This structure is then combined with polyether diamine to form a polymer skeleton rich in amine groups. After introducing reaction sites via methyl acrylate, hydroxylamine hydrochloride is used for hydroxyoximation, further introducing hydroxyoxime acid-like interaction sites into the polyether diamine composite structure while retaining amine group interaction sites. The amine groups can adsorb onto the negatively charged clay surface, the hydroxyoxime acid-like interaction sites enhance the interaction between the polymer and the shale mineral surface, and the multiple hydroxyl structure helps maintain the dispersion state of the polymer in the aqueous phase. This improves the adsorption stability of the inhibitor under high temperature, high salinity, and shear conditions, reduces water penetration into the clay interlayer, reduces shale hydration swelling and dispersion, and enhances the stabilizing effect of drilling fluid on the wellbore.

[0018] 2. In this invention, the viscous acid in additive B is esterified to form a composite powder with a multi-hydroxyl structure. After dispersion with anhydrous ethanol, it is directly subjected to limited ammonolysis with an excess of low-molecular-weight polyether diamine, introducing amino group interaction sites and a multi-hydroxyl limited chain extension structure into the polymer chain segments. The polyether diamine segments can adsorb onto the surface of clay and shale, and the multi-hydroxyl segments help regulate the hydration state and spatial conformation of the polymer chains, reducing polymer cluster shrinkage and aggregation under high salinity conditions, and improving the polymer's coverage and coating retention capacity on the shale surface. This improves the inhibition stability of the drilling fluid in the presence of salt and calcium / magnesium ions, reducing the risk of shale water absorption and dispersion and wellbore instability. Attached Figure Description

[0019] Figure 1 This invention provides a flowchart of an amine polymer inhibitor for drilling fluids and its preparation method. Figure 2 The infrared spectrum of additive A. Figure 3 Infrared spectrum of additive B. Detailed Implementation

[0020] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0021] It should be noted that the raw materials used in the following embodiments are all commercially available.

[0022] Example 1

[0023] Preparation of the first connecting liquid: Glycerol diglycidyl ether was mixed with deionized water at a mass of 1, and 2-amino-1,3-propanediol at a mass of 18% of glycerol diglycidyl ether was added. The mixture was stirred at 25°C and 300 rpm for 1 h, then heated to 40°C and stirred for another 1 h. After cooling, the first connecting liquid was obtained.

[0024] Preparation of amine-based liquid: Polyether diamine with a number average molecular weight of 200 was mixed with twice the mass of deionized water and stirred at 25°C and 300 rpm for 20 min. Then, a first connecting liquid accounting for 4% of the mass of polyether diamine was added and stirred at 35°C and 400 rpm for 2 h. After cooling, the amine-based liquid was obtained.

[0025] Preparation of Additive A: The amine solution was mixed with 4 times its mass of deionized water and stirred at 25°C and 300 rpm for 20 min. Methyl acrylate, accounting for 5% of the total mass of non-aqueous components in the amine solution, was added and stirred at 30°C and 400 rpm for 2 h. Hydroxylamine hydrochloride, accounting for 85% of the mass of methyl acrylate, was added and sodium bicarbonate was added to adjust the pH to 7.5. The mixture was stirred at 35°C and 400 rpm for 3 h, then cooled to 25°C. The pH was adjusted to 6.5 with lactic acid. Anhydrous ethanol was added to make the volume fraction of ethanol 70%. After standing for 1 h, the mixture was centrifuged. The resulting precipitate was washed twice with a 75% volume fraction ethanol aqueous solution and once with deionized water. It was dried at 50°C for 6 h and then pulverized through a 200-mesh sieve to obtain Additive A.

[0026] Preparation of composite powder: Viscous acid and methanol were mixed at a mass ratio of 1:8 and stirred at 20℃ and 300rpm for 20min. 95% sulfuric acid (1% by mass of viscous acid) was added. A reflux condenser was installed, and the temperature was raised to 60℃ at 2℃ / min. The mixture was refluxed at 300rpm for 4h. After the reaction was completed, the mixture was cooled to 10℃ and allowed to stand for 1h. The mixture was filtered, and the resulting solid was washed twice with a 65% methanol aqueous solution and once with deionized water. The solid was dried at 50℃ for 6h and then ground through a 200-mesh sieve to obtain the composite powder.

[0027] Preparation of the second connecting liquid: The composite powder was added to anhydrous ethanol at 4 times its mass and stirred at 35°C and 300 rpm for 20 min to obtain the second connecting liquid.

[0028] Preparation of Additive B: Low molecular weight polyether diamine was mixed with twice its mass of deionized water and stirred at 30°C and 300 rpm for 20 min. Then, a second connecting liquid accounting for 8% of the mass of polyether diamine was added and stirred at 65°C and 400 rpm for 3 h. After cooling, anhydrous ethanol was added to make the ethanol volume fraction reach 70%. The mixture was allowed to stand and centrifuged. The resulting solid was washed twice with 75% ethanol aqueous solution and once with deionized water. It was dried at 50°C for 6 h and then pulverized to obtain Additive B.

[0029] Raw material preparation: 25 parts low molecular weight polyether diamine, 8 parts additive A, 6 parts additive B, 3 parts glycerol, 1 part lactic acid and 45 parts deionized water; the number average molecular weight of the low molecular weight polyether diamine is 200.

[0030] Preparation of amine polymer inhibitors for drilling fluids: S1: Preparation of base solution: Add low molecular weight polyether diamine and glycerol to deionized water and stir at 25°C and 300 rpm for 20 min to obtain base solution; S2: Introduction of polyhydroxy structure: Additive B is added to the base solution and stirred at 35℃ and 400rpm for 20min to obtain the first composite solution; S3: Introduction of anchoring structure: Additive A is added to the first composite liquid and stirred at 35℃ and 400rpm for 30min to obtain the second composite liquid; S4: System adjustment: Under the conditions of stirring at 25℃ and 300rpm, lactic acid was added to the second composite solution to adjust the pH to 7.0, and stirring was continued for 30min to obtain the amine polymer inhibitor for drilling fluid.

[0031] When the drilling fluid amine polymer inhibitor is used in water-based drilling fluid, the amount added is 0.8% of the mass of the water-based drilling fluid, and after addition, it is stirred at 600 rpm for 20 minutes.

[0032] Example 2

[0033] Preparation of the first connecting liquid: Glyceryl glycerol diglycidyl ether was mixed with 1.5 times its mass of deionized water, and 2-amino-1,3-propanediol, accounting for 22% of the mass of glycerol diglycidyl ether, was added. The mixture was stirred at 32°C and 400 rpm for 1.5 h, then heated to 46°C and stirred for another 1.5 h. After cooling, the first connecting liquid was obtained.

[0034] Preparation of amine-based liquid: Polyether diamine with a number average molecular weight of 300 was mixed with three times its mass of deionized water and stirred at 31°C and 450 rpm for 26 min. Then, a first connecting liquid accounting for 5.5% of the mass of polyether diamine was added and stirred at 42°C and 550 rpm for 3 h. After cooling, the amine-based liquid was obtained.

[0035] Preparation of Additive A: The amine solution was mixed with 5 times its mass of deionized water and stirred at 31°C and 400 rpm for 26 min. Methyl acrylate, accounting for 7% of the total mass of non-aqueous components in the amine solution, was added and stirred at 37°C and 550 rpm for 2.5 h. Hydroxylamine hydrochloride, accounting for 95% of the mass of methyl acrylate, was added and sodium bicarbonate was added to adjust the pH to 8.0. The mixture was stirred at 42°C and 550 rpm for 4 h, then cooled to 32°C. The pH was adjusted to 7.0 with lactic acid. Anhydrous ethanol was added to make the volume fraction of ethanol 76%. After standing for 1.5 h, the mixture was centrifuged. The resulting precipitate was washed twice with a 75% volume fraction ethanol aqueous solution and once with deionized water. It was dried at 56°C for 7 h and then pulverized through a 200-mesh sieve to obtain Additive A.

[0036] Preparation of composite powder: Viscous acid and methanol were mixed at a mass ratio of 1:10.5 and stirred at 26℃ and 450 rpm for 27 min. 95% sulfuric acid (1.5% by mass of viscous acid) was added. A reflux condenser was installed, and the temperature was raised to 65℃ at 3℃ / min. The mixture was refluxed at 400 rpm for 5 h. After the reaction was completed, the mixture was cooled to 16℃ and allowed to stand for 1.5 h. The mixture was then filtered. The resulting solid was washed twice with 65% methanol aqueous solution and once with deionized water. It was dried at 57℃ for 7 h and then ground through a 200-mesh sieve to obtain the composite powder.

[0037] Preparation of the second connecting liquid: The composite powder was added to anhydrous ethanol at 5 times its mass and stirred at 41°C and 450 rpm for 27 min to obtain the second connecting liquid.

[0038] Preparation of Additive B: Low molecular weight polyether diamine was mixed with three times its mass of deionized water and stirred at 36°C and 400 rpm for 27 min. A second connecting liquid accounting for 12% of the mass of polyether diamine was added and stirred at 75°C and 500 rpm for 4 h. After cooling, anhydrous ethanol was added to make the ethanol volume fraction reach 76%. The mixture was allowed to stand and centrifuged. The resulting solid was washed twice with a 75% ethanol aqueous solution and once with deionized water. It was dried at 55°C for 7 h and then pulverized to obtain Additive B.

[0039] Raw material preparation: 31 parts low molecular weight polyether diamine, 11 parts additive A, 9 parts additive B, 4.5 parts glycerol, 1.5 parts lactic acid and 55 parts deionized water; the number average molecular weight of the low molecular weight polyether diamine is 300.

[0040] Preparation of amine polymer inhibitors for drilling fluids: S1: Preparation of base solution: Add low molecular weight polyether diamine and glycerol to deionized water and stir at 31°C and 450 rpm for 27 min to obtain base solution; S2: Introduction of polyhydroxy structure: Additive B is added to the base solution and stirred at 42℃ and 550rpm for 27min to obtain the first composite solution; S3: Introduction of anchoring structure: Additive A to the first composite liquid and stir at 41℃ and 550rpm for 35min to obtain the second composite liquid; S4: System adjustment: Under the conditions of stirring at 32℃ and 450rpm, lactic acid was added to the second composite solution to adjust the pH to 7.5, and stirring was continued for 35min to obtain the amine polymer inhibitor for drilling fluid.

[0041] When the drilling fluid amine polymer inhibitor is used in water-based drilling fluid, the amount added is 1.5% of the mass of the water-based drilling fluid, and after addition, it is stirred at 700 rpm for 27 min.

[0042] Example 3

[0043] Preparation of the first connecting liquid: Glycerol diglycidyl ether was mixed with twice the mass of deionized water, and 2-amino-1,3-propanediol, accounting for 25% of the mass of glycerol diglycidyl ether, was added. The mixture was stirred at 35°C and 500 rpm for 2 hours, then heated to 50°C and stirred for another 2 hours. After cooling, the first connecting liquid was obtained.

[0044] Preparation of amine-based liquid: Polyether diamine with a number average molecular weight of 400 was mixed with 4 times its mass of deionized water and stirred at 35°C and 500 rpm for 30 min. Then, a first connecting liquid accounting for 8% of the mass of polyether diamine was added and stirred at 45°C and 600 rpm for 4 h. After cooling, the amine-based liquid was obtained.

[0045] Preparation of Additive A: The amine solution was mixed with 6 times its mass of deionized water and stirred at 35°C and 500 rpm for 30 min. Methyl acrylate, accounting for 9% of the total mass of non-aqueous components in the amine solution, was added and stirred at 40°C and 600 rpm for 3 h. Hydroxylamine hydrochloride, accounting for 105% of the mass of methyl acrylate, was added and sodium bicarbonate was added to adjust the pH to 8.5. After stirring at 45°C and 600 rpm for 5 h, the mixture was cooled to 35°C and the pH was adjusted to 7.5 with lactic acid. Anhydrous ethanol was added to make the volume fraction of ethanol 80%. After standing for 2 h, the mixture was centrifuged. The resulting precipitate was washed twice with a 75% volume fraction ethanol aqueous solution and once with deionized water. It was dried at 60°C for 8 h and then pulverized through a 200-mesh sieve to obtain Additive A.

[0046] Preparation of composite powder: Viscous acid and methanol were mixed at a mass ratio of 1:12 and stirred at 30℃ and 500rpm for 30min. 2% by mass of 95% sulfuric acid was added. A reflux condenser was installed, and the temperature was raised to 68℃ at 4℃ / min. The mixture was refluxed at 500rpm for 6h. After the reaction was completed, the mixture was cooled to 20℃ and allowed to stand for 2h. The mixture was filtered, and the resulting solid was washed twice with a 65% methanol aqueous solution and once with deionized water. The solid was dried at 60℃ for 8h and then ground through a 200-mesh sieve to obtain the composite powder.

[0047] Preparation of the second connecting liquid: The composite powder was added to anhydrous ethanol at 6 times its mass and stirred at 45°C and 500 rpm for 30 min to obtain the second connecting liquid.

[0048] Preparation of Additive B: Low molecular weight polyether diamine was mixed with 4 times its mass of deionized water and stirred at 40°C and 500 rpm for 30 min. A second connecting liquid accounting for 15% of the mass of polyether diamine was added and stirred at 80°C and 600 rpm for 5 h. After cooling, anhydrous ethanol was added to make the ethanol volume fraction reach 80%. The mixture was allowed to stand and centrifuged. The resulting solid was washed twice with 75% ethanol aqueous solution and once with deionized water. It was dried at 60°C for 8 h and then pulverized to obtain Additive B.

[0049] Raw material preparation: 35 parts low molecular weight polyether diamine, 14 parts additive A, 12 parts additive B, 6 parts glycerol, 2 parts lactic acid and 60 parts deionized water; the number average molecular weight of the low molecular weight polyether diamine is 400.

[0050] Preparation of amine polymer inhibitors for drilling fluids: S1: Preparation of base solution: Add low molecular weight polyether diamine and glycerol to deionized water and stir at 35°C and 500 rpm for 30 min to obtain base solution; S2: Introduction of polyhydroxy structure: Additive B is added to the base solution and stirred at 45℃ and 600rpm for 30min to obtain the first composite solution; S3: Introduction of anchoring structure: Additive A is added to the first composite liquid and stirred at 45℃ and 600rpm for 45min to obtain the second composite liquid; S4: System adjustment: Under the conditions of 35℃ and 500rpm stirring, lactic acid was added to the second composite solution to adjust the pH to 8.0, and stirring was continued for 45min to obtain the amine polymer inhibitor for drilling fluid.

[0051] When the drilling fluid amine polymer inhibitor is used in water-based drilling fluid, the amount added is 2.0% of the mass of the water-based drilling fluid, and after addition, it is stirred at 800 rpm for 30 min.

[0052] Comparative Example 1: This comparative example differs from Example 1 in that additive A is not added, and low molecular weight polyether diamine of the same mass as additive A is used as a substitute. The composition of other raw materials and preparation conditions are the same as those in Example 1.

[0053] Comparative Example 2 differs from Example 1 in that: Additive B is not added, and low molecular weight polyether diamine of the same mass as Additive B is used as a substitute. The composition of other raw materials and preparation conditions are the same as those in Example 1.

[0054] Comparative Example 3 differs from Example 1 in that: during the preparation of additive A, after the reaction of the amine liquid and methyl acrylate is completed, hydroxylamine hydrochloride is no longer added for hydroxyoxime treatment. After cooling, lactic acid is directly used to adjust the system and the comparative additive A is prepared according to the precipitation, washing, drying and pulverizing steps of Example 1. All other conditions are the same as in Example 1.

[0055] Comparative Example 4 differs from Example 1 in that: 2-amino-1,3-propanediol is not added during the preparation of the first connecting liquid; instead, glycerol diglycidyl ether is mixed with deionized water to form the first connecting liquid. The subsequent preparation processes of the amine liquid, additive A, and the final product are the same as in Example 1.

[0056] Comparative Example 5 differs from Example 1 in that: limited ammonolysis is omitted, and the composite powder of Example 1 is directly and physically compounded with low molecular weight polyether diamine in the same actual amount without the 60°C, 6h reaction. The preparation conditions of subsequent additive B and the final product are the same as those of Example 1.

[0057] Comparative Example 6 differs from Example 1 in that the viscous acid is not subjected to methanol esterification, but is directly dried, ground and sieved as a composite powder. The preparation methods of the subsequent second connecting liquid, additive B and final product are the same as those in Example 1.

[0058] Comparative Example 7 differs from Example 1 in that the amount of composite powder added relative to low molecular weight polyether diamine is increased from 12% to 35%, while the remaining limited ammonolysis conditions are the same as in Example 1.

[0059] Performance Testing: Performance tests were conducted on the drilling fluid amine polymer inhibitors treated in Examples 1-3 and Comparative Examples 1-7. To avoid the influence of different solid content in the products of each example on the test results, the solid content of each sample was uniformly adjusted to 35% using deionized water before the test. Then, amine polymer inhibitors for drilling fluid were added at 1.5% of the mass of the basic test slurry. The samples were stirred at 700 rpm for 25 minutes before the test. The test data are recorded in the table below: Table 1 Test item High temperature high salt hot roll recovery (%) Calcium and magnesium contamination hot roll recovery (%) Linear expansion rate (%) Example 1 91.2 88.5 17.8 Example 2 93.1 91.0 15.9 Example 3 92.4 90.0 16.6 Comparative Example 1 74.3 72.1 33.8 Comparative Example 2 81.5 64.9 29.4 Comparative Example 3 82.7 79.6 26.7 Comparative Example 4 84.1 81.8 24.5 Comparative Example 5 83.3 72.8 25.7 Comparative Example 6 81.2 69.4 28.6 Comparative Example 7 86.0 77.5 22.9 Preparation of the basic test slurry: **Add 14.0g of sodium bentonite and 0.70g of sodium carbonate to 350mL of deionized water, stir at 10000rpm for 20min, and then cure in a sealed container at 25℃ for 24h to obtain the basic test slurry.** Examples 1-3 and Comparative Examples 1-7 all used the same batch of sodium bentonite and the same batch of basic test slurry to reduce the impact of batch differences in raw materials on the test results.

[0060] In performance testing, the laboratory preparation, temperature control, aging, and basic testing conditions of the testing system can be carried out in accordance with GB / T29170-2012; the general testing conditions for water-based drilling fluids can also be carried out in accordance with GB / T 16783.1-2025, and the shale inhibition performance itself should be specifically referred to the current industry standard NB / T 10121-2018.

[0061] Determination of high-temperature and high-salt hot rolling recovery rate: Take 350 mL of basic test slurry, add 17.5 g of sodium chloride to make the sodium chloride concentration 50 g / L based on the volume of water used in the preparation of the basic test slurry, and stir until uniformly dispersed to obtain high-salt test slurry. Add 1.5% by mass of the amine polymer inhibitor for drilling fluid to be tested to the high-salt test slurry and stir at 700 rpm for 25 min. Select shale from the same batch, crush and screen it to obtain shale particles with a particle size of 2.0-5.0 mm, dry them at 105℃ to constant weight, accurately weigh 50.0 g of each group and add them to the test slurry, transfer them to an aging tank, and hot roll at 150℃ for 16 h. After hot rolling, cool to room temperature, sieve the mixture through a 0.42 mm sieve, slowly wash the shale particles on the sieve with deionized water, and then dry it at 105℃ to constant weight and weigh it. The percentage of the mass of dried shale particles after hot rolling to the mass of shale particles before hot rolling is used as the high-temperature, high-salinity hot rolling recovery rate.

[0062] Determination of the hot rolling recovery rate of calcium and magnesium contamination: Take 350 mL of basic test slurry, add 1.75 g of calcium chloride dihydrate and 1.75 g of magnesium chloride hexahydrate respectively, so that the concentration of both is 5 g / L according to the volumetric water used to prepare the basic test slurry. After thorough stirring, a calcium and magnesium contamination test slurry is obtained. Add 1.5% of the mass of the test slurry to the amine polymer inhibitor for the drilling fluid to be tested, stir at 700 rpm for 25 min, and then add 50.0 g of shale particles with a particle size of 2.0-5.0 mm from the same batch. The mixture is placed in an aging tank and hot rolled at 120℃ for 16 h. After cooling, sieve through a 0.42 mm sieve, wash with deionized water, and dry the remaining shale particles at 105℃ to constant weight and weigh them. The percentage of the mass of the dried shale particles after hot rolling to the mass of the initial shale particles is taken as the calcium and magnesium contamination hot rolling recovery rate.

[0063] Determination of linear expansion rate: Shale from the same source as that used in the hot rolling test was dried, pulverized, and passed through a 100-mesh sieve. 10.0 g of shale powder was weighed each time and placed in a pressing mold, held at 10 MPa for 5 minutes to obtain uniformly sized pressed rock samples. The rock samples were then loaded into a linear expansion tester, and a base test slurry containing 1.5% amine polymer inhibitor for the drilling fluid being tested was added at 25°C to completely submerge the rock samples. The test was conducted continuously for 16 hours, recording the rock sample height at the beginning and end of the test. The linear expansion rate was calculated as the percentage increase in rock sample height relative to the initial height.

[0064] The data obtained from the performance tests show that the amine polymer inhibitors for drilling fluids prepared in Examples 1-3 are generally superior to Comparative Examples 1-7 in terms of high-temperature and high-salt hot rolling recovery rate, calcium and magnesium contamination hot rolling recovery rate, and linear expansion control. In Comparative Example 1, without the addition of additive A, its shale recovery capacity under high-temperature and high-salt conditions significantly decreased. This indicates that the multi-site adsorption system formed by the first connecting structure, polyether diamine, and hydroxylated structure in additive A can enhance the adsorption and anchoring effect of the polymer on the clay and shale surfaces. The multi-hydroxyl structure helps maintain the hydration and dispersion state of the polymer chains, further reducing the adsorption layer detachment caused by high temperature, high salt, and shearing. Comparative Examples 3 and 4 further show that the inhibition performance decreased in both cases without hydroxylated treatment or the multi-hydroxyl connecting structure, indicating that both can synergistically improve the stability of the polymer interfacial adsorption layer, thereby inhibiting water from entering the clay interlayer and reducing shale hydration expansion and dispersion.

[0065] Furthermore, in Comparative Example 2 without the addition of additive B, the shale recovery performance decreased significantly under calcium and magnesium contamination conditions, indicating that additive B plays an important role in improving the stability of the inhibitor in high-mineralization environments. Additive B forms a reactive composite powder through viscose esterification, which then interacts with polyether diamine, introducing the polyhydroxy structure from viscose into the polyether diamine system. This enhances the hydration around the polymer chain segments and maintains a suitable spatial conformation, thereby reducing the shrinkage and aggregation of polymer chains under high-mineralization conditions. In Comparative Examples 5-7, the elimination of limited ammonolysis, the elimination of viscose esterification, and the increase in the amount of composite powder all increased the chain elongation, resulting in varying degrees of decrease in related properties. This further illustrates that the above structure is not a simple superposition of raw materials, but rather a continuous structural construction that collectively improves the polymer's coverage and coating retention ability on the shale surface.

[0066] By comparing and analyzing the relevant data in the table, it can be seen that the amine polymer inhibitor for drilling fluid prepared by this invention has good high-temperature and high-salt inhibition performance and calcium and magnesium pollution stability, which can effectively reduce shale hydration expansion and dispersion, and improve wellbore stability.

[0067] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0068] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to the specific implementations described. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.

Claims

1. An amine polymer inhibitor for drilling fluids, characterized in that, The raw materials include the following parts by weight: 25-35 parts low molecular weight polyether diamine, 8-14 parts additive A, 6-12 parts additive B, 3-6 parts glycerol, 1-2 parts lactic acid and 45-60 parts deionized water; wherein the number average molecular weight of the low molecular weight polyether diamine is 200-400. Additive A is an amine-based composite material obtained by modifying polyether diamine with a binder containing a multi-hydroxyl linkage structure, followed by reaction with methyl acrylate and hydroxylamine hydrochloride hydroxyoxime treatment. Additive B is a polyhydroxyamine-based composite material obtained by dispersing the composite powder obtained by esterification of viscous acid with anhydrous ethanol and then reacting it with low molecular weight polyether diamine.

2. The drilling fluid amine polymer inhibitor according to claim 1, characterized in that, Additive A is prepared by the following method: An amine solution is mixed with 4-6 times its mass of deionized water, stirred at 25-35℃ and 300-500 rpm for 20-30 min, methyl acrylate (MCA) accounting for 5-9% of the total mass of non-aqueous components in the amine solution is added, and the mixture is stirred at 30-40℃ and 400-600 rpm for 2-3 h, hydroxylamine hydrochloride (HHA) accounting for 85-105% of the mass of methyl acrylate is added, and sodium bicarbonate is added to adjust the pH to 7. 5-8.5, stir at 35-45℃ and 400-600rpm for 3-5h, cool to 25-35℃, adjust pH to 6.5-7.5 with lactic acid, add anhydrous ethanol to make the volume fraction of ethanol 70-80%, let stand for 1-2h and then centrifuge. Wash the precipitate twice with 75% ethanol aqueous solution and once with deionized water. Dry at 50-60℃ for 6-8h, pulverize and pass through a 200-mesh sieve to obtain additive A.

3. The drilling fluid amine polymer inhibitor according to claim 2, characterized in that, The amine-based liquid is prepared by the following method: a polyether diamine with a number average molecular weight of 200-400 is mixed with 2-4 times its mass of deionized water, stirred at 25-35℃ and 300-500 rpm for 20-30 min, a first connecting liquid accounting for 4-8% of the mass of the polyether diamine is added, and stirred at 35-45℃ and 400-600 rpm for 2-4 h, and then cooled to obtain the amine-based liquid.

4. The amine polymer inhibitor for drilling fluid according to claim 3, characterized in that, The first connecting liquid is prepared by the following method: glycerol diglycidyl ether is mixed with 1-2 times its mass of deionized water, and 18-25% of 2-amino-1,3-propanediol is added. The mixture is stirred at 25-35°C and 300-500 rpm for 1-2 hours, then heated to 40-50°C and stirred for another 1-2 hours. After cooling, the first connecting liquid is obtained.

5. The drilling fluid amine polymer inhibitor according to claim 1, characterized in that, Additive B is prepared by the following method: low molecular weight polyether diamine is mixed with 2-4 times its mass of deionized water, stirred at 30-40℃ and 300-500rpm for 20-30min, a second connecting liquid accounting for 8-15% of the mass of polyether diamine is added, stirred at 65-80℃ and 400-600rpm for 3-5h, cooled, and anhydrous ethanol is added to make the ethanol volume fraction reach 70-80%, allowed to stand, centrifuged, and the resulting solid is washed twice with 75% ethanol aqueous solution and once with deionized water, dried at 50-60℃ for 6-8h, and pulverized to obtain additive B.

6. The drilling fluid amine polymer inhibitor according to claim 5, characterized in that, The second connecting liquid is prepared by the following method: the composite powder is added to anhydrous ethanol at 4-6 times its mass, and stirred at 35-45℃ and 300-500rpm for 20-30min to obtain the second connecting liquid.

7. The drilling fluid amine polymer inhibitor according to claim 6, characterized in that, The composite powder is prepared by the following method: viscous acid and methanol are mixed at a mass ratio of 1:(8-12), stirred at 20-30℃ and 300-500rpm for 20-30min, sulfuric acid of 95% by mass (1-2% of the viscous acid mass) is added, a reflux condenser is installed, the temperature is raised to 60-68℃ at 2-4℃ / min, and refluxed at 300-500rpm for 4-6h. After the reaction is completed, the mixture is cooled to 10-20℃ and allowed to stand for 1-2h, filtered, and the resulting solid is washed twice with a 65% methanol aqueous solution, then washed once with deionized water, dried at 50-60℃ for 6-8h, and ground through a 200-mesh sieve to obtain the composite powder.

8. A method for preparing an amine polymer inhibitor for drilling fluids as described in any one of claims 1-7, characterized in that, Includes the following steps: S1: Preparation of base solution: Add low molecular weight polyether diamine and glycerol to deionized water, and stir at 25-35℃ and 300-500rpm for 20-30min to obtain base solution; S2: Introduction of polyhydroxy structure: Additive B is added to the base solution and stirred at 35-45℃ and 400-600rpm for 20-30min to obtain the first composite solution; S3: Introduction of anchoring structure: Add additive A to the first composite liquid and stir at 35-45℃ and 400-600rpm for 30-45min to obtain the second composite liquid; S4: System adjustment: Under the conditions of stirring at 25-35℃ and 300-500rpm, lactic acid is added to the second composite solution to adjust the pH to 7.0-8.0, and stirring is continued for 30-45min to obtain the amine polymer inhibitor for drilling fluid.

Citation Information

Patent Citations

  • A polyetheramine shale inhibitor for drilling fluid, its preparation method, and the drilling fluid thereof.

    CN109694473B

  • A hyperbranched polyetheramine environmentally friendly shale inhibitor, its preparation method, and water-based drilling fluid

    CN111718698B