A combined process for producing olefins and aromatics from catalytic cracking gasoline
By fractionating catalytic cracking gasoline into light and heavy fractions and converting them under non-hydrogen-exposed conditions using catalysts such as ZSM-5 molecular sieves, the problems of long processing flow and resource waste in catalytic cracking gasoline have been solved, achieving low-cost and high-efficiency production of olefins and aromatics.
Patent Information
- Application Number
- CN202510618984.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2025-05-14
- Publication Date
- 2026-11-17
Smart Images

Figure CN123107732A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of petrochemical technology, specifically a combined process for producing olefins and aromatics from catalytic cracking of gasoline. Background Technology
[0002] As China accelerates the industrialization process of replacing gasoline-powered vehicles with electric vehicles, the demand for refined oil products has peaked and entered a gradual decline since 2018, while the demand for petrochemical products, represented by olefins, xylenes, and benzenes, has continued to grow rapidly. my country will complete and put into operation several advanced refining and chemical projects, and it is estimated that by 2025, my country's refining capacity will reach 980 million tons, and its total ethylene production capacity will exceed 50 million tons, making it the world's largest producer of refining and ethylene. The "China Energy and Chemical Industry Development Report" indicates that the annual growth rate of demand for ethylene and propylene in my country will reach 5.7% and 6.5%, respectively. Therefore, in the future, refining and chemical companies will focus more on how to reduce the yield of refined oil products and increase the output of chemical products in order to maintain a competitive advantage.
[0003] Domestically and internationally, the main method for producing low-carbon olefins is through steam cracking of light hydrocarbons, primarily using ethane, propane, or light petroleum distillates as feedstock. However, due to the increasing deterioration of crude oil processed by my country's petrochemical enterprises and a severe shortage of light hydrocarbon resources, the development of technologies for producing low-carbon olefins through catalytic cracking of heavy distillate or heavy oil has received significant attention. Among these, technologies such as deep catalytic cracking (DCC), enhanced catalytic cracking DCC-Plus, CPP for ethylene and propylene production, high-efficiency catalytic cracking (RTC), heavy oil contact cracking (HCC), and two-stage riser catalytic cracking for high propylene production (TMP) have been extensively researched and applied, opening up new avenues for low-carbon olefin production in my country.
[0004] However, while catalytic cracking technology yields target products such as ethylene and propylene, the byproduct catalytic cracking gasoline is rich in olefins and aromatics (including a large amount of heavy aromatics), requiring secondary processing before it can be sold as a product.
[0005] Currently, catalytic cracking gasoline is generally produced by catalytic hydrotreating for desulfurization and olefin removal, and then used as a clean gasoline blending component. However, due to the high olefin content of catalytic cracking gasoline, the hydrogen consumption during catalytic hydrotreating is high, resulting in high processing costs. It also wastes valuable olefin and aromatic resources and reduces the gasoline's octane number. The common processing flow for existing catalytic cracking gasoline is shown in the attached figure. Figure 1As shown, catalytic cracking gasoline is separated into fractions below C5, C6-C8, and above C9 by atmospheric distillation. The fraction below C5 can be recycled back to the catalytic cracking unit to further produce low-carbon olefins or used as gasoline fraction. The C6-C8 fraction is refined by hydrotreating, solvent extraction and distillation to produce light aromatics (BTX). The fraction above C9 is hydrogenated and used as a blending component for high-octane gasoline.
[0006] However, this process is lengthy, has high investment and operating costs, requires significant hydrogen consumption for the hydrogenation of large quantities of olefin components, and the non-aromatic components and heavy aromatics extracted by solvent extraction are not ideal blending components for gasoline. With the continuous decrease in gasoline demand and the increasing demand for olefins and aromatics in my country, the construction of heavy oil or crude oil catalytic cracking units will inevitably accelerate, leading to a continuous increase in catalytic cracked gasoline. Therefore, in order to meet market demand and improve the economic efficiency of refining enterprises, how to efficiently convert catalytic cracked gasoline into olefins and aromatics has become an urgent problem to be solved. Summary of the Invention
[0007] The purpose of this invention is to provide a combined process for producing olefins and aromatics from catalytic cracking gasoline. This process can be optimized according to the composition of the catalytic cracking gasoline, and has the advantages of short process flow, low investment, low operating costs, and the ability to produce olefins and aromatics, thereby meeting market demand for chemicals and improving economic efficiency.
[0008] The technical solution adopted by the present invention to achieve the above-mentioned technical objectives is as follows: a combined process for producing olefins and aromatics from catalytic cracking gasoline, wherein the catalytic cracking gasoline is fractionated to form catalytic cracking light fractions ≤C8 and catalytic cracking heavy fractions ≥C9;
[0009] The ≤C8 catalytic cracking light fraction undergoes a light hydrocarbon catalytic cracking reaction. The reaction products are separated into C1-C4 catalytic cracking components and ≥C5 catalytic cracking components. The ≥C5 catalytic cracking components are mixed with the ≥C9 catalytic cracking heavy fraction and then subjected to a dealkylation reaction. The C1-C4 catalytic cracking components undergo a secondary separation to obtain dry gas products, propylene products, propane products, and C4 components. A portion of the C4 components is used as feedstock for steam cracking to produce ethylene or as liquefied petroleum gas (LPG) products, while the other portion of the C4 components is returned and mixed with the ≤C8 catalytic cracking light fraction for a light hydrocarbon catalytic cracking reaction.
[0010] The catalytic cracking heavy fraction of ≥C9 is mixed with the catalytic cracking component of ≥C5 and then subjected to a dealkylation reaction to separate the rich gas component of C1-C4, the light aromatic component of C5-C8, and the heavy aromatic component of ≥C9. Among them, the rich gas component of C1-C4 is combined with the catalytic cracking component of C1-C4 and then subjected to a secondary separation. The light aromatic component of C5-C8 is first separated into C5 components. Then, part of the C5 components is used as a blending component for high octane gasoline, and the other part of the C5 components is returned to the light hydrocarbon catalytic cracking reaction. The remaining C6-C8 components are successively hydrorefined and aromatics extracted to separate aromatics and alkanes. The aromatics are then distilled to produce benzene, toluene, and xylene. Part of the heavy aromatic component of ≥C9 is used as a blending component for high octane gasoline, and the other part is returned to the dealkylation reaction.
[0011] As an optimized scheme for a combined process of catalytic cracking gasoline to produce olefins and aromatics, the light hydrocarbon catalytic cracking reaction is carried out at a reaction temperature of 500-720℃, a system pressure of 0-0.8MPa, and a feed space velocity of 0.5-6.0h. -1 The preferred reaction temperature is 580-660℃, system pressure is 0.1-0.2MPa, and feed space velocity is 1.5-3.5h. -1 .
[0012] As another optimized scheme for the combined process of catalytic cracking of gasoline to produce olefins and aromatics, the active component of the catalyst for the light hydrocarbon catalytic cracking reaction is ZSM-5 molecular sieve, the catalyst support is Al2O3, the modifying element is P2O5, and the contents of ZSM-5 molecular sieve and P2O5 in the catalyst are 50-75% and 1.5-2.5% respectively, with the balance being Al2O3 support.
[0013] As another optimized scheme for the combined process of producing olefins and aromatics from catalytic cracking gasoline, the silicon-aluminum ratio of the ZSM-5 molecular sieve is 60-180, preferably 120-150.
[0014] As another optimized approach to the combined process of catalytic cracking of gasoline to produce olefins and aromatics, the preparation method of the catalyst for the light hydrocarbon catalytic cracking reaction is as follows:
[0015] 1) Weigh out aluminum sol, pseudoboehmite, HZSM-5 molecular sieve and phosphoric acid, and ensure that the ratio of ZSM-5 molecular sieve, Al2O3 and P2O5 in the four materials meets the above requirements.
[0016] 2) Add water and boehmite to the alumina sol while stirring. After stirring thoroughly, add HZSM-5 molecular sieve while stirring, and then stir thoroughly again to form a mixture.
[0017] 3) Under the conditions of temperature 400-450℃, outlet temperature 200-250℃, and spray pressure 4-5MPa, the mixture in step 2) is spray-dried and shaped, and then calcined at 600-700℃ for 4-6 hours.
[0018] 4) The calcined catalyst is saturated with an equal volume of phosphoric acid aqueous solution. The impregnated catalyst is dried at 100-150℃ for 4-6 hours, and then calcined at 600-700℃ for 4-6 hours to obtain the finished catalyst.
[0019] As another optimized approach to the combined process of producing olefins and aromatics from catalytic cracking gasoline, the apparatus used for the dealkylation reaction is a fixed-bed reactor, a moving-bed reactor, or a fluidized-bed reactor, with a fixed-bed reactor being preferred.
[0020] As another optimized approach to the combined process of producing olefins and aromatics from catalytic cracking gasoline, the dealkylation reaction uses an acidic catalyst and is carried out under non-hydrogen-exposed conditions.
[0021] As another optimized scheme for the combined process of producing olefins and aromatics from catalytic cracking gasoline, the dealkylation reaction is carried out at a reaction temperature of 550-650℃, a system pressure of 0-1.0MPa, and a feed space velocity of 0.2-3.0h. -1 Preferably, the reaction temperature is 580-630℃, the system pressure is 0.1-0.3MPa, and the feed space velocity is 0.5-1.0h. -1 .
[0022] As another optimized solution for the combined process of producing olefins and aromatics from catalytic cracking gasoline, the active component of the catalyst for the dealkylation reaction is ZSM-5 molecular sieve, MOR molecular sieve or ZSM-12 molecular sieve, preferably ZSM-5 molecular sieve, with a silicon-to-aluminum ratio of 150-350, and more preferably 250-300.
[0023] As another optimized scheme for the combined process of producing olefins and aromatics from catalytic cracking gasoline, the active component of the catalyst for the dealkylation reaction is ZSM-5 molecular sieve, the catalyst support is Al2O3, and the modifying elements are P2O5 and CeO2. The contents of ZSM-5 molecular sieve, P2O5 and CeO2 in the catalyst are 60-70%, 1.0-2.0% and 2.5-3.5% respectively, with the balance being Al2O3 support.
[0024] The basic principle of this invention is as follows:
[0025] The data shown in Tables 1, 2, 3 and 4 below represent the main properties of a typical catalytic cracking gasoline and its heavy gasoline fraction. Group composition Alkanes Olefins Naphthenes Aromatics Value, % 16.09 40.84 3.82 39.25 Table 1 Composition of Catalytic Cracked Gasoline Carbon number C5 C6 C7 C8 ≥C9 Value, % 33.90 13.66 15.98 17.01 19.45 Table 2 Carbon number distribution of catalytic cracking gasoline Group composition Alkanes Olefins Naphthenes Aromatics Value, % 7.09 0 6.82 86.09 Table 3 Composition of Catalytic Cracking Heavy Gasoline Group composition Propylbenzene Ethylbenzene Trimethylbenzene Indane Others Value, % 4.5 35.4 55.5 7.2 2.4 Table 4. Composition of major aromatic hydrocarbons in catalytic cracking heavy gasoline
[0026] Analysis of the data in the table above shows that the light fraction of catalytic cracking gasoline is rich in olefins, making it a high-quality feedstock for the production of low-carbon olefins through catalytic cracking; the heavy fraction of catalytic cracking gasoline is rich in aromatics, making it a high-quality feedstock for the production of benzene, toluene, and xylene through the lightification of heavy aromatics.
[0027] As shown in Table 1, the olefin content in catalytic cracking gasoline is as high as 40.84%, and the olefin content in the light fraction (≤C8) of catalytic cracking gasoline is even higher. Based on the basic reaction principle of catalytic cracking, gasoline fraction olefins are easily converted to C2-C4 olefins under the action of an acidic catalyst. Simultaneously, C4 olefins are easily converted to ethylene and propylene through reprocessing. Therefore, olefin-rich catalytic cracking gasoline is a suitable feedstock for the production of ethylene and propylene using a dedicated catalyst. Furthermore, some aromatics are also generated during the production of ethylene and propylene from catalytic cracking gasoline; that is, the aromatic content of gasoline components is even higher after further catalytic cracking of catalytic cracking gasoline. As shown in Tables 2, 3, and 4, the heavy fraction (≥C9) of catalytic cracking gasoline accounts for 19.45%, with an aromatic content as high as 86%. Using an acidic catalyst under non-hydrogen-exposed conditions, firstly, heavy aromatics can be dealkylated and converted into lighter aromatics such as benzene, toluene, and xylene; secondly, dealkylation under non-hydrogen-exposed conditions can generate olefins rich in ethylene and propylene, thereby further increasing the yield of ethylene and propylene. Conversely, under hydrogen-exposed conditions, ethylene and propylene form low-value ethane and propane; thirdly, under non-hydrogen-exposed conditions, alkanes and cycloalkanes in the heavy aromatic components can also be converted into aromatics, increasing the aromatic yield. Under hydrogen-exposed conditions, alkanes and cycloalkanes are difficult to dehydrogenate to form aromatics. Therefore, based on the composition of catalytic cracking gasoline, a combination of catalytic cracking technology and heavy aromatic dealkylation technology can achieve the production of ethylene, propylene, and light aromatics from catalytic cracking gasoline, thus realizing the conversion of low-value catalytic cracking gasoline into high-value olefins and aromatics.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] 1) The present invention has broad applicability and can process all kinds of catalytic cracking gasoline, including light distillate oil catalytic cracking gasoline, heavy distillate oil catalytic cracking gasoline, residue oil catalytic cracking gasoline, crude oil catalytic cracking gasoline, etc., all of which can be processed by the method of the present invention, while producing low-carbon olefins and light aromatics.
[0030] 2) The process of the present invention does not require hydrodesulfurization or selective hydrodeolefination. After separation by atmospheric distillation, it can directly enter the catalytic cracking and non-hydrodealkylation reaction. By using proprietary catalysts and process technology, the catalytic cracking of light fraction of gasoline can produce low carbon olefins in the largest amount, and the non-hydrodealkylation of heavy gasoline can produce light aromatics in the largest amount.
[0031] 3) In the process of the present invention, the gaseous hydrocarbons produced by the non-hydrodealkylation reaction are rich in olefins. By returning them to catalytic cracking, more low-carbon olefins can be produced. The reprocessing of heavy aromatics produced by the non-hydrodealkylation reaction can further improve the conversion rate of heavy aromatics to light aromatics and produce more light aromatics.
[0032] 4) The process of this invention is based on the composition of catalytic cracking gasoline and optimizes its processing with existing equipment. The process flow is short, the investment is low, the operating cost is low, and it can achieve the purpose of producing olefins and aromatics, meet the market demand for chemicals, and effectively improve economic benefits. Attached Figure Description
[0033] Figure 1 This refers to the existing processing flow for catalytic cracking gasoline;
[0034] Figure 2 This is a process flow diagram of the present invention. Detailed Implementation
[0035] The method of the present invention will be further described in detail below with reference to specific embodiments. Parts not explained in the following embodiments of the present invention are all considered to be prior art known or should be known by those skilled in the art.
[0036] Example 1
[0037] A combined process for producing olefins and aromatics from catalytic cracking gasoline involves fractionating the catalytic cracking gasoline into ≤C8 catalytic cracking light fractions and ≥C9 catalytic cracking heavy fractions.
[0038] The ≤C8 catalytic cracking light fraction undergoes a light hydrocarbon catalytic cracking reaction. The reaction products are separated into C1-C4 catalytic cracking components and ≥C5 catalytic cracking components. The ≥C5 catalytic cracking components are mixed with the ≥C9 catalytic cracking heavy fraction and then subjected to a dealkylation reaction. The C1-C4 catalytic cracking components undergo a secondary separation to obtain dry gas products, propylene products, propane products, and C4 components. A portion of the C4 components is used as feedstock for steam cracking to produce ethylene or as liquefied petroleum gas (LPG) products, while the other portion of the C4 components is returned and mixed with the ≤C8 catalytic cracking light fraction for a light hydrocarbon catalytic cracking reaction.
[0039] The catalytic cracking heavy fraction of ≥C9 is mixed with the catalytic cracking component of ≥C5 and then subjected to a dealkylation reaction to separate the rich gas component of C1-C4, the light aromatic component of C5-C8, and the heavy aromatic component of ≥C9. Among them, the rich gas component of C1-C4 is combined with the catalytic cracking component of C1-C4 and then subjected to a secondary separation. The light aromatic component of C5-C8 is first separated into C5 components. Then, part of the C5 components is used as a blending component for high-octane gasoline, and the other part of the C5 components is returned to the light hydrocarbon catalytic cracking reaction. The remaining C6-C8 components are successively hydrorefined and aromatics extracted to separate aromatics and alkanes. The aromatics are then distilled to produce benzene, toluene, and xylene. Part of the heavy aromatic component of ≥C9 is used as a blending component for high-octane gasoline, and the other part is returned to the dealkylation reaction.
[0040] In this embodiment, the reaction temperature of the light hydrocarbon catalytic cracking reaction is 500°C, the system pressure is 0.01 MPa, and the feed space velocity is 0.5 h⁻¹. -1 ;
[0041] In this embodiment, the active component of the catalyst for the light hydrocarbon catalytic cracking reaction is ZSM-5 molecular sieve, and the silicon-to-aluminum ratio of ZSM-5 molecular sieve is 60. The catalyst support is Al2O3, the modifying element is P2O5, and the contents of ZSM-5 molecular sieve and P2O5 in the catalyst are 50% and 2.5%, respectively, with the remainder being Al2O3 support.
[0042] In this embodiment, the preparation method of the catalyst for the light hydrocarbon catalytic cracking reaction is as follows:
[0043] 1) Weigh out aluminum sol, pseudoboehmite, HZSM-5 molecular sieve and phosphoric acid, and ensure that the ratio of ZSM-5 molecular sieve, Al2O3 and P2O5 in the four materials meets the above requirements.
[0044] 2) Add water and boehmite to the alumina sol while stirring. After stirring thoroughly, add HZSM-5 molecular sieve while stirring, and then stir thoroughly again to form a mixture.
[0045] 3) The mixture from step 2) was spray-dried and shaped under the conditions of 400℃ temperature, 200℃ outlet temperature and 4MPa spray pressure, and then calcined at 600℃ for 4 hours. 4) The calcined catalyst was impregnated with a 5% phosphoric acid aqueous solution to modify the catalyst. The impregnated catalyst was dried at 100°C for 4 hours and then calcined at 600°C for 4 hours to obtain the finished catalyst.
[0046] In this embodiment, the apparatus used for the dealkylation reaction is a fixed-bed reactor, a moving-bed reactor, or a fluidized-bed reactor;
[0047] In this embodiment, the dealkylation reaction is carried out using an acidic catalyst and under non-hydrogen-exposed conditions;
[0048] In this embodiment, the dealkylation reaction is carried out at a reaction temperature of 550°C, a system pressure of 0.01 MPa, and a feed space velocity of 0.2 h⁻¹. -1 ;
[0049] In this embodiment, the active component of the catalyst for the dealkylation reaction is ZSM-5 molecular sieve, the catalyst support is Al2O3, and the modifying elements are P2O5 and CeO2. The contents of ZSM-5 molecular sieve, P2O5 and CeO2 in the catalyst are 60%, 1.0% and 2.5%, respectively, with the remainder being Al2O3 support.
[0050] In this embodiment, the catalyst for the dealkylation reaction is prepared as follows:
[0051] 1) Weigh out boehmite, HZSM-5 molecular sieve, ammonium dihydrogen phosphate and cerium nitrate, as well as 10% dilute nitric acid, 30% citric acid, Tianqing powder and other auxiliary materials, and ensure that the ratio of ZSM-5 molecular sieve, Al2O3, P2O5 and CeO2 meets the above requirements.
[0052] 2) Mix HZSM-5 molecular sieve and pseudoboehmite evenly, then add dilute nitric acid, citric acid and Tianqing powder, mix and crush, and then extrude into strips;
[0053] 3) Dry at 100℃ for 3 hours, then calcine at 600℃ for 3 hours;
[0054] 4) Dissolve 5% ammonium dihydrogen phosphate and 5% cerium nitrate in water to form a mixed impregnation solution. Then, saturate the calcined catalyst with the mixed impregnation solution in equal volume. After impregnation, dry the catalyst at 100°C for 3 hours and then calcine it at 600°C for 3 hours to obtain the finished catalyst.
[0055] Example 2
[0056] A combined process for producing olefins and aromatics from catalytic cracking gasoline involves fractionating the catalytic cracking gasoline into ≤C8 catalytic cracking light fractions and ≥C9 catalytic cracking heavy fractions.
[0057] The ≤C8 catalytic cracking light fraction undergoes a light hydrocarbon catalytic cracking reaction. The reaction products are separated into C1-C4 catalytic cracking components and ≥C5 catalytic cracking components. The ≥C5 catalytic cracking components are mixed with the ≥C9 catalytic cracking heavy fraction and then subjected to a dealkylation reaction. The C1-C4 catalytic cracking components undergo a secondary separation to obtain dry gas products, propylene products, propane products, and C4 components. A portion of the C4 components is used as feedstock for steam cracking to produce ethylene or as liquefied petroleum gas (LPG) products, while the other portion of the C4 components is returned and mixed with the ≤C8 catalytic cracking light fraction for a light hydrocarbon catalytic cracking reaction.
[0058] The catalytic cracking heavy fraction of ≥C9 is mixed with the catalytic cracking component of ≥C5 and then subjected to a dealkylation reaction to separate the rich gas component of C1-C4, the light aromatic component of C5-C8, and the heavy aromatic component of ≥C9. Among them, the rich gas component of C1-C4 is combined with the catalytic cracking component of C1-C4 and then subjected to a secondary separation. The light aromatic component of C5-C8 is first separated into C5 components. Then, part of the C5 components is used as a blending component for high-octane gasoline, and the other part of the C5 components is returned to the light hydrocarbon catalytic cracking reaction. The remaining C6-C8 components are successively hydrorefined and aromatics extracted to separate aromatics and alkanes. The aromatics are then distilled to produce benzene, toluene, and xylene. Part of the heavy aromatic component of ≥C9 is used as a blending component for high-octane gasoline, and the other part is returned to the dealkylation reaction.
[0059] In this embodiment, the reaction temperature of the light hydrocarbon catalytic cracking reaction is 720°C, the system pressure is 0.8 MPa, and the feed space velocity is 6.0 h⁻¹. -1 ;
[0060] In this embodiment, the active component of the catalyst for the light hydrocarbon catalytic cracking reaction is ZSM-5 molecular sieve, and the silicon-to-aluminum ratio of ZSM-5 molecular sieve is 180. The catalyst support is Al2O3, the modifying element is P2O5, and the contents of ZSM-5 molecular sieve and P2O5 in the catalyst are 75% and 2.5%, respectively, with the remainder being Al2O3 support.
[0061] In this embodiment, the preparation method of the catalyst for the light hydrocarbon catalytic cracking reaction is as follows:
[0062] 1) Weigh out aluminum sol, pseudoboehmite, HZSM-5 molecular sieve and phosphoric acid, and ensure that the ratio of ZSM-5 molecular sieve, Al2O3 and P2O5 in the four materials meets the above requirements.
[0063] 2) Add water and boehmite to the alumina sol while stirring. After stirring thoroughly, add HZSM-5 molecular sieve while stirring, and then stir thoroughly again to form a mixture.
[0064] 3) The mixture from step 2) was spray-dried and shaped under conditions of 450℃, 250℃ outlet temperature and 5MPa spray pressure, and then calcined at 700℃ for 6 hours.
[0065] 4) The calcined catalyst was impregnated with a 5% phosphoric acid aqueous solution to modify the catalyst. The impregnated catalyst was dried at 150°C for 6 hours and then calcined at 700°C for 6 hours to obtain the finished catalyst.
[0066] In this embodiment, the apparatus used for the dealkylation reaction is a fixed-bed reactor, a moving-bed reactor, or a fluidized-bed reactor;
[0067] In this embodiment, the dealkylation reaction is carried out using an acidic catalyst and under non-hydrogen-exposed conditions;
[0068] In this embodiment, the dealkylation reaction is carried out at a reaction temperature of 650°C, a system pressure of 1.0 MPa, and a feed space velocity of 3.0 h⁻¹. -1 ;
[0069] In this embodiment, the active component of the catalyst for the dealkylation reaction is ZSM-5 molecular sieve, the catalyst support is Al2O3, and the modifying elements are P2O5 and CeO2. The contents of ZSM-5 molecular sieve, P2O5 and CeO2 in the catalyst are 70%, 2.0% and 3.5%, respectively, with the remainder being Al2O3 support.
[0070] In this embodiment, the catalyst for the dealkylation reaction is prepared as follows:
[0071] 1) Weigh out boehmite, HZSM-5 molecular sieve, ammonium dihydrogen phosphate and cerium nitrate, as well as 10% dilute nitric acid, 30% citric acid, Tianqing powder and other auxiliary materials, and ensure that the ratio of ZSM-5 molecular sieve, Al2O3, P2O5 and CeO2 meets the above requirements.
[0072] 2) Mix HZSM-5 molecular sieve and pseudoboehmite evenly, then add dilute nitric acid, citric acid and Tianqing powder, mix and crush, and then extrude into strips;
[0073] 3) Dry at 150℃ for 5 hours, then calcine at 700℃ for 5 hours;
[0074] 4) Dissolve 5% ammonium dihydrogen phosphate and 5% cerium nitrate in water to form a mixed impregnation solution. Then, saturate the calcined catalyst with the mixed impregnation solution in equal volume. After impregnation, dry the catalyst at 150°C for 5 hours and then calcine it at 700°C for 5 hours to obtain the finished catalyst.
[0075] Example 3
[0076] A combined process for producing olefins and aromatics from catalytic cracking gasoline involves fractionating the catalytic cracking gasoline into ≤C8 catalytic cracking light fractions and ≥C9 catalytic cracking heavy fractions.
[0077] The ≤C8 catalytic cracking light fraction undergoes a light hydrocarbon catalytic cracking reaction. The reaction products are separated into C1-C4 catalytic cracking components and ≥C5 catalytic cracking components. The ≥C5 catalytic cracking components are mixed with the ≥C9 catalytic cracking heavy fraction and then subjected to a dealkylation reaction. The C1-C4 catalytic cracking components undergo a secondary separation to obtain dry gas products, propylene products, propane products, and C4 components. A portion of the C4 components is used as feedstock for steam cracking to produce ethylene or as liquefied petroleum gas (LPG) products, while the other portion of the C4 components is returned and mixed with the ≤C8 catalytic cracking light fraction for a light hydrocarbon catalytic cracking reaction.
[0078] The catalytic cracking heavy fraction of ≥C9 is mixed with the catalytic cracking component of ≥C5 and then subjected to a dealkylation reaction to separate the rich gas component of C1-C4, the light aromatic component of C5-C8, and the heavy aromatic component of ≥C9. Among them, the rich gas component of C1-C4 is combined with the catalytic cracking component of C1-C4 and then subjected to a secondary separation. The light aromatic component of C5-C8 is first separated into C5 components. Then, part of the C5 components is used as a blending component for high-octane gasoline, and the other part of the C5 components is returned to the light hydrocarbon catalytic cracking reaction. The remaining C6-C8 components are successively hydrorefined and aromatics extracted to separate aromatics and alkanes. The aromatics are then distilled to produce benzene, toluene, and xylene. Part of the heavy aromatic component of ≥C9 is used as a blending component for high-octane gasoline, and the other part is returned to the dealkylation reaction.
[0079] In this embodiment, the reaction temperature of the light hydrocarbon catalytic cracking reaction is 610°C, the system pressure is 0.4 MPa, and the feed space velocity is 3.5 h⁻¹. -1 ;
[0080] In this embodiment, the active component of the catalyst for the light hydrocarbon catalytic cracking reaction is ZSM-5 molecular sieve, and the silicon-to-aluminum ratio of ZSM-5 molecular sieve is 60-180. The catalyst support is Al2O3, the modifying element is P2O5, and the contents of ZSM-5 molecular sieve and P2O5 in the catalyst are 62.5% and 2%, respectively, with the remainder being Al2O3 support.
[0081] In this embodiment, the preparation method of the catalyst for the light hydrocarbon catalytic cracking reaction is as follows:
[0082] 1) Weigh out aluminum sol, pseudoboehmite, HZSM-5 molecular sieve and phosphoric acid, and ensure that the ratio of ZSM-5 molecular sieve, Al2O3 and P2O5 in the four materials meets the above requirements.
[0083] 2) Add water and boehmite to the alumina sol while stirring. After stirring thoroughly, add HZSM-5 molecular sieve while stirring, and then stir thoroughly again to form a mixture.
[0084] 3) The mixture from step 2) was spray-dried and shaped under conditions of 420℃, 230℃ outlet temperature, and 4.5MPa spray pressure, and then calcined at 650℃ for 5 hours.
[0085] 4) The calcined catalyst was impregnated with a 5% concentration of phosphoric acid aqueous solution to modify the catalyst. The impregnated catalyst was dried at 130°C for 5 hours and then calcined at 650°C for 5 hours to obtain the finished catalyst.
[0086] In this embodiment, the apparatus used for the dealkylation reaction is a fixed-bed reactor, a moving-bed reactor, or a fluidized-bed reactor;
[0087] In this embodiment, the dealkylation reaction is carried out using an acidic catalyst and under non-hydrogen-exposed conditions;
[0088] In this embodiment, the dealkylation reaction is carried out at a reaction temperature of 600°C, a system pressure of 0.5 MPa, and a feed space velocity of 1.6 h⁻¹. -1 ;
[0089] In this embodiment, the active component of the catalyst for the dealkylation reaction is ZSM-5 molecular sieve, the catalyst support is Al2O3, and the modifying elements are P2O5 and CeO2. The contents of ZSM-5 molecular sieve, P2O5 and CeO2 in the catalyst are 65%, 1.5% and 3%, respectively, and the balance is Al2O3 support.
[0090] In this embodiment, the catalyst for the dealkylation reaction is prepared as follows:
[0091] 1) Weigh out boehmite, HZSM-5 molecular sieve, ammonium dihydrogen phosphate and cerium nitrate, as well as 10% dilute nitric acid, 30% citric acid, Tianqing powder and other auxiliary materials, and ensure that the ratio of ZSM-5 molecular sieve, Al2O3, P2O5 and CeO2 meets the above requirements.
[0092] 2) Mix HZSM-5 molecular sieve and pseudoboehmite evenly, then add dilute nitric acid, citric acid and Tianqing powder, mix and crush, and then extrude into strips;
[0093] 3) Dry at 130℃ for 4 hours, then calcine at 650℃ for 4 hours;
[0094] 4) Dissolve 5% ammonium dihydrogen phosphate and 5% cerium nitrate in water to form a mixed impregnation solution. Then, saturate the calcined catalyst with the mixed impregnation solution in equal volume. After impregnation, dry the catalyst at 130°C for 4 hours and then calcine it at 650°C for 4 hours to obtain the finished catalyst.
[0095] Experimental Example
[0096] To verify the process method of the present invention, the following experiments were conducted;
[0097] The properties of the catalytic cracking gasoline used in the experiment are shown in Table 1-4; The process method of the present invention is as follows: Figure 2 As shown, catalytic cracking gasoline is fractionated to form ≤C8 catalytic cracking light fraction and ≥C9 catalytic cracking heavy fraction. The catalytic cracking process operating conditions for the light gasoline are a reaction temperature of 620℃ and a feed space velocity of 0.5 h⁻¹. -1 The reaction pressure was 0.1 MPa, and the product distribution after catalytic cracking is shown in Table 5 below. The process operating conditions for the dealkylation reaction were a reaction temperature of 630℃ and a feed space velocity of 0.5 h⁻¹. -1 The reaction pressure was 0.1 MPa. The product distribution of the dealkylation reaction is shown in Table 6. The reprocessing ratio of C4 and C5 produced by catalytic cracking and dealkylation was 0.2 (i.e., the ratio of the total reprocessed amount of C4 and C5 to the feed amount of light gasoline), and the reprocessing ratio of the unconverted ≥C9 fraction from heavy gasoline refining was 0.1 (i.e., the ratio of the unconverted ≥C9 fraction reprocessed to the total feed amount of the dealkylation reaction). The experimental results for the production of olefins and aromatics from catalytic cracking gasoline are shown in Table 7. Table 5. Distribution of catalytic cracking products of gasoline, %
[0098] As shown in Table 5, the C4 component has a relatively high olefin content. This C4 component can be recycled back to the catalytic cracking reactor for further cracking into ethylene and propylene. Therefore, recycling the C4 component is an effective means to produce more ethylene and propylene. In addition, the ≥C5 components have high aromatic and olefin contents. If these components are subjected to a non-hydrogenated heavy aromatics lightening reaction, firstly, the heavy aromatics in the aromatic components will undergo dealkylation to generate light aromatics (BTX), increasing the yield of light aromatics. The removed alkyl groups can also form ethylene and propylene. Secondly, the olefins in the ≥C5 components can be cracked into ethylene and propylene under the action of the high-silicon ZSM-5 catalyst. Dry gas (ethylene) 6.8(3.7) Liquefied gas (propylene) 7.6(3.1) C4 4.2 C5 4.0 C6-C8 68.9 ≥C9 8.5 Table 6. Distribution of Light Aromatic Hydrocarbon Products (%) Dry gas (ethylene) 16.3(9.0) Propylene 23.1 Propane 7.8 C4 10.3 C5 2.5 Benzene 7.1 Toluene 16.2 Xylene (ethylbenzene) 8.3(0.8) Alkanes 3.6 ≥C9 4.8 Table 7 Distribution of Aromatization Products from Catalytic Cracked Gasoline (%)
[0099] As shown in Table 7, the combined process of this invention can produce 22.1% low-carbon olefins (ethylene, propylene) and 31.6% light aromatics (benzene, toluene, xylene) from catalytic cracking gasoline, effectively improving the utilization value of catalytic cracking gasoline. It also achieves the goal of reducing the production of saturated gasoline products and increasing the production of olefins and aromatics products that are in short supply, providing a new way for refining and chemical enterprises to cope with market changes and improve economic efficiency. Furthermore, the ethane, propane, and butane produced by this invention are high-quality feedstocks for steam cracking to produce ethylene, which can further increase the production of ethylene, propylene, and other chemicals. Additionally, the C5, alkanes, and ≥C9 heavy aromatics byproducts of the combined process are also blending components for high-octane gasoline.
Claims
1. A combined process for producing olefins and aromatics from catalytic cracking gasoline, characterized in that: The catalytic cracking gasoline is fractionated to form a catalytic cracking light fraction with ≤C8 and a catalytic cracking heavy fraction with ≥C9; The ≤C8 catalytic cracking light fraction undergoes a light hydrocarbon catalytic cracking reaction. The reaction products are separated into C1-C4 catalytic cracking components and ≥C5 catalytic cracking components. The ≥C5 catalytic cracking components are mixed with the ≥C9 catalytic cracking heavy fraction and then subjected to a dealkylation reaction. The C1-C4 catalytic cracking components undergo a secondary separation to obtain dry gas products, propylene products, propane products, and C4 components. A portion of the C4 components is used as feedstock for steam cracking to produce ethylene or as liquefied petroleum gas (LPG) products, while the other portion of the C4 components is returned and mixed with the ≤C8 catalytic cracking light fraction for a light hydrocarbon catalytic cracking reaction. The catalytic cracking heavy fraction of ≥C9 is mixed with the catalytic cracking component of ≥C5 and then subjected to a dealkylation reaction to separate the rich gas component of C1-C4, the light aromatic component of C5-C8, and the heavy aromatic component of ≥C9. Among them, the rich gas component of C1-C4 is combined with the catalytic cracking component of C1-C4 and then subjected to a secondary separation. The light aromatic component of C5-C8 is first separated into C5 components. Then, part of the C5 components is used as a blending component for high octane gasoline, and the other part of the C5 components is returned to the light hydrocarbon catalytic cracking reaction. The remaining C6-C8 components are successively hydrorefined and aromatics extracted to separate aromatics and alkanes. The aromatics are then distilled to produce benzene, toluene, and xylene. Part of the heavy aromatic component of ≥C9 is used as a blending component for high octane gasoline, and the other part is returned to the dealkylation reaction.
2. The combined process for producing olefins and aromatics from catalytic cracking gasoline according to claim 1, characterized in that: The light hydrocarbon catalytic cracking reaction is carried out at a reaction temperature of 500-720℃, a system pressure of 0-0.8MPa, and a feed space velocity of 0.5-6.0h. -1 .
3. The combined process for producing olefins and aromatics from catalytic cracking gasoline according to claim 1, characterized in that: The active component of the catalyst for the light hydrocarbon catalytic cracking reaction is ZSM-5 molecular sieve, the catalyst support is Al2O3, the modifying element is P2O5, and the contents of ZSM-5 molecular sieve and P2O5 in the catalyst are 50-75% and 1.5-2.5%, respectively, with the remainder being Al2O3 support.
4. The combined process for producing olefins and aromatics from catalytic cracking gasoline according to claim 3, characterized in that: The silicon-aluminum ratio of the ZSM-5 molecular sieve is 60-180.
5. The combined process for producing olefins and aromatics from catalytic cracking gasoline according to claim 3, characterized in that, The preparation method of the catalyst for the light hydrocarbon catalytic cracking reaction is as follows: 1) Weigh out aluminum sol, pseudoboehmite, HZSM-5 molecular sieve and phosphoric acid, and the ratio of ZSM-5 molecular sieve, Al2O3 and P2O5 in the four materials meets the requirements of claim 3; 2) Add water and boehmite to the alumina sol while stirring. After stirring thoroughly, add HZSM-5 molecular sieve while stirring, and then stir thoroughly again to form a mixture. 3) Under the conditions of temperature 400-450℃, outlet temperature 200-250℃, and spray pressure 4-5MPa, the mixture in step 2) is spray-dried and shaped, and then calcined at 600-700℃ for 4-6 hours. 4) The calcined catalyst is saturated with an equal volume of phosphoric acid aqueous solution. The impregnated catalyst is dried at 100-150℃ for 4-6 hours, and then calcined at 600-700℃ for 4-6 hours to obtain the finished catalyst.
6. The combined process for producing olefins and aromatics from catalytic cracking gasoline according to claim 1, characterized in that: The apparatus used for the dealkylation reaction is a fixed-bed reactor, a moving-bed reactor, or a fluidized-bed reactor.
7. The combined process for producing olefins and aromatics from catalytic cracking gasoline according to claim 1, characterized in that: The dealkylation reaction is carried out using an acidic catalyst and under non-hydrogen-exposed conditions.
8. The combined process for producing olefins and aromatics from catalytic cracking gasoline according to claim 1, characterized in that: The dealkylation reaction is carried out at a reaction temperature of 550-650℃, a system pressure of 0-1.0 MPa, and a feed space velocity of 0.2-3.0 h⁻¹. -1 .
9. The combined process for producing olefins and aromatics from catalytic cracking gasoline according to claim 1, characterized in that: The catalyst active component for the dealkylation reaction is ZSM-5 molecular sieve, MOR molecular sieve, or ZSM-12 molecular sieve.
10. A combined process for producing olefins and aromatics from catalytic cracking gasoline according to claim 9, characterized in that: The active component of the catalyst for the dealkylation reaction is ZSM-5 molecular sieve, the catalyst support is Al2O3, and the modifying elements are P2O5 and CeO2. The contents of ZSM-5 molecular sieve, P2O5 and CeO2 in the catalyst are 60-70%, 1.0-2.0% and 2.5-3.5% respectively, and the balance is Al2O3 support.