A method for preparing cement kiln alternative fuel with denitrification function using ammonia-containing waste, and the alternative fuel and its application in cement kilns.

The cement kiln alternative fuel prepared by screening and compounding utilizes ammonia-containing waste to decompose into ammonia gas at high temperatures, solving the problems of high denitrification costs and resource waste in cement production. It realizes the dual function of alternative fuel and resource utilization, and reduces NOx emissions and operating costs.

CN123107744APending Publication Date: 2026-11-17DALIAN DONGTAI INDAL WASTE TREATMENT
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611324150.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing cement production, the SNCR denitrification process relies on purchased ammonia or urea, resulting in high operating costs and safety hazards. Ammonia-containing waste is not effectively utilized, and traditional disposal methods cause resource waste and secondary pollution. Cement kilns have limited alternative fuel functions and fail to achieve synergistic effects of solid waste disposal, energy conservation and emission reduction, and flue gas denitrification.

Method used

Through screening, physicochemical testing, and component blending, a cement kiln alternative fuel with denitrification function is prepared. The ammonia component in ammonia-containing waste is decomposed into ammonia gas at high temperature, which serves as an SNCR denitrification reducing agent and provides heat energy to replace part of the fossil fuel.

Benefits of technology

It achieves the dual function of replacing fuel in cement kilns, reducing denitrification costs, utilizing ammonia-containing waste resources, reducing fossil fuel consumption, reducing NOx emissions, avoiding secondary pollution, and the process is simple and easy to industrialize.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a method for preparing cement kiln alternative fuel with denitrification function using ammonia-containing waste, as well as the alternative fuel and its application, belonging to the field of solid waste resource utilization technology. This method uses ammonia-containing waste as the core raw material. After raw material screening and physicochemical testing, it is compounded with auxiliary waste to control the heavy metals, sulfur, chlorine, fluorine, moisture content, and calorific value of the mixture. Following crushing, screening, and pre-treatment by mixing, a functional alternative fuel meeting the requirements for cement kiln feed is obtained. After being fed into the cement kiln decomposition furnace, this alternative fuel decomposes at 950-1050℃, releasing ammonia gas, which participates in the in-situ SNCR reaction to remove nitrogen oxides. It can partially replace purchased denitrification reducing agents and simultaneously provide heating, replacing fossil fuels. This invention achieves a triple functional coupling of solid waste disposal, energy saving, and denitrification, with a simple process and strong adaptability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of solid waste resource utilization technology, and in particular to a method for preparing cement kiln alternative fuel with denitrification function using ammonia-containing waste, as well as the cement kiln alternative fuel and its application. Background Technology

[0002] The cement industry is a major energy-consuming and air pollutant-emitting industry in my country. The high-temperature calcination process in kilns generates large amounts of nitrogen oxides (NOx). x NO is atmospheric NO x One of the main sources of pollution. Currently, the vast majority of cement production lines in China use SNCR (Selective Non-Catalytic Reduction) technology to control NO in flue gas. x This technology has the advantages of simple structure, low retrofit investment, and stable denitrification efficiency, and its application coverage is extremely high.

[0003] The existing SNCR denitrification process relies on purchased ammonia or urea as chemical reducing agents, which are then sprayed into the high-temperature reaction zone of the kiln through a dedicated injection system to achieve denitrification. This model consumes a large amount of chemical reagents in the long term, significantly increasing the production and operating costs of cement companies. At the same time, ammonia and urea are controlled chemicals, and there are volatilization, leakage, and safety hazards throughout the storage, transportation, and injection process, making operation and maintenance management difficult.

[0004] Meanwhile, industries such as petrochemical production, municipal wastewater treatment, and light manufacturing continuously generate large amounts of ammonia-containing waste. This waste contains a large amount of adsorbed ammonia, ammonium salts, and other usable ammonia resources, and also possesses a certain calorific value. Traditional disposal methods are mostly sanitary landfill and direct incineration, which not only occupy land resources and waste ammonia and calorific value resources, but also easily cause secondary pollution problems such as soil pollution, excessive ammonia nitrogen in water bodies, and odor diffusion. The disposal costs are high and the resource utilization rate is low.

[0005] In existing cement kiln co-processing technologies for solid waste, various solid alternative fuels only utilize the calorific value of the materials to replace fossil fuels such as coal for energy conservation and emission reduction, resulting in a relatively singular functional dimension. Under this model, while the chemical energy in the waste is recovered, the internal active components such as ammonia are not effectively utilized, failing to achieve the synergistic environmental benefits of "treating waste with waste." Therefore, there is an urgent need to develop a new functional alternative fuel technology that can simultaneously achieve synergistic effects in solid waste treatment, energy conservation and emission reduction, and flue gas denitrification. Summary of the Invention

[0006] This invention provides a method for preparing cement kiln alternative fuel with denitrification function using ammonia-containing waste, as well as the cement kiln alternative fuel and its application, to overcome the above-mentioned problems.

[0007] To achieve the above objectives, the technical solution of the present invention is as follows: This invention provides a method for preparing alternative fuel for cement kilns with denitrification function using ammonia-containing waste, comprising the following steps: S1. Raw material screening: Collect ammonia-containing waste as basic raw materials and remove explosive substances, persistent toxic pollutants and large pieces of hard, non-combustible debris. S2. Physical and chemical testing: Physical and chemical indicators of the screened ammonia-containing waste are tested to obtain parameters such as ammonia content, ammonia occurrence form, lower heating value, moisture content, total heavy metals, sulfur, chlorine and fluorine content. S3. Component Co-mixing: Based on the parameters of low heating value, moisture content, and heavy metal, sulfur, chlorine, and fluorine content measured in S2, combined with the control standards for co-processing solid waste in cement kilns and the requirements of SNCR denitrification in decomposition furnaces, the ammonia-containing waste is mixed with one or more auxiliary wastes to synergistically adjust the heavy metal, sulfur, chlorine, fluorine, moisture content, and calorific value in the resulting mixture, so that the indicators of the mixture meet the control requirements for cement kiln feed. S4. Material stabilization pretreatment: The mixture is crushed, screened and mixed in sequence to control the particle size distribution and eliminate the segregation of material components, so as to obtain ammonia-containing alternative fuel with uniform composition, stable properties and dual functions of heating and denitrification, that is, cement kiln alternative fuel with denitrification function.

[0008] Furthermore, in step S3, the moisture content of the mixture is 10%-25%, and the lower heating value is not less than 840 kcal / kg; the limits for heavy metals, sulfur, chlorine, and fluorine in the mixture meet the requirements of HJ662-2013 "Environmental Protection Technical Specification for Co-processing Solid Waste in Cement Kilns".

[0009] Furthermore, the ammonia-containing waste includes one or more of ammonia-containing industrial waste residue, ammonia-containing sludge, and ammonia-containing organic waste; the ammonia in the ammonia-containing waste exists in the form of adsorbed ammonia or ammonium salt.

[0010] Furthermore, in step S4, the purpose of screening is to remove solid impurities with a particle size greater than 20 mm after the mixture is crushed; the mixing time is not less than 10 minutes to ensure that the material has no obvious stratification and the components are uniform.

[0011] Furthermore, in step S3, the auxiliary waste is one or more of combustible industrial solid waste and inorganic conditioning solid waste. The auxiliary waste is used to synergistically adjust the calorific value, moisture content, and content of heavy metals, sulfur, chlorine, and fluorine in the mixture with ammonia-containing waste.

[0012] This invention provides a cement kiln alternative fuel with denitrification function, prepared by the aforementioned method. The cement kiln alternative fuel with denitrification function has ammonia-containing waste as its core functional component. It is stable at room temperature and can stably decompose and release ammonia gas after being put into the high-temperature environment of the cement kiln decomposition furnace. The ammonia gas can act as a reducing agent for SNCR denitrification in cement kilns in situ. At the same time, the alternative fuel can be burned for heating and can partially or completely replace cement kiln denitrification agents and fossil fuels.

[0013] This invention provides the application of the aforementioned cement kiln alternative fuel with denitrification function in cement kiln flue gas SNCR denitrification, harmless disposal of solid waste, and energy-saving cement production.

[0014] Furthermore, the application method is as follows: the cement kiln alternative fuel with denitrification function is added at a fixed point to the high-temperature denitrification zone of the cement kiln decomposition furnace. Under the condition of 950℃-1050℃, the cement kiln alternative fuel with denitrification function decomposes and releases ammonia gas after being heated. The released ammonia gas is used in situ as an SNCR denitrification reducing agent to react with nitrogen oxides in the cement kiln flue gas to reduce the NOx emission concentration of the kiln flue gas and reduce the amount of denitrification agent added. At the same time, the heat released by the combustion of the cement kiln alternative fuel with denitrification function provides thermal energy for the cement kiln system, replacing part of the fossil fuel.

[0015] The beneficial effects of this invention are: 1. The present invention discloses a method for preparing cement kiln alternative fuel with denitrification function using ammonia-containing waste, which breaks through the technical barrier of the single function of traditional alternative fuels: traditional cement alternative fuels only have the function of combustion and heating. The present invention utilizes the ammonia component in ammonia-containing waste to give the alternative fuel in-situ denitrification function, realizing the dual function of "both burning and denitrification" of the fuel, which is fundamentally different from existing conventional alternative fuel technologies.

[0016] 2. Significantly reduce cement denitrification operating costs: The functional fuel prepared by this invention can release ammonia gas autonomously after entering the kiln, which can be used as an SNCR denitrification reducing agent. It can partially replace purchased ammonia water and urea, significantly reducing the costs of purchasing, storing, transporting and maintaining denitrification agents, resulting in outstanding economic benefits.

[0017] 3. Opening up a new path for high-value resource utilization of ammonia-containing waste: This method changes the traditional disposal mode of landfilling and inefficient incineration of ammonia-containing waste, fully recovers ammonia and calorific value resources in the waste, realizes the harmless, reduced and high-value utilization of solid waste, and solves the problem of secondary pollution caused by ammonia-containing solid waste.

[0018] 4. Simple process, strong adaptability and easy industrialization: This method only adopts physical screening, compounding, crushing and mixing pretreatment processes throughout the process. No chemical reaction device is required. It can be directly adapted to existing cement kiln co-processing production lines without large-scale equipment modification. It has low implementation cost and strong promotion.

[0019] 5. Achieving Synergistic Coupling of Multiple Environmental Benefits: This method uses ammonia-containing waste as raw material, and through component compounding and stabilization pretreatment, prepares an alternative fuel with both heating and denitrification functions. After entering the kiln, the combustible components of this fuel release heat upon combustion, replacing some fossil fuels and thus reducing coal consumption and carbon emissions. Simultaneously, the ammonia-containing components decompose upon heating, releasing NH3, which participates in the SNCR denitrification reaction in situ, thereby efficiently reducing NOx emissions. x By reducing the amount of purchased ammonia or urea, waste disposal, energy conservation, and pollution control are integrated into a circular economy model that "treats pollution with waste and turns waste into treasure," which aligns with the development direction of the environmental protection industry. Detailed Implementation

[0020] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0021] Example: Example 1 A method for preparing denitrification functional cement kiln alternative fuel using ammonia-containing industrial sludge includes the following steps: S1. Raw material screening: Select ammonia-containing sludge from industrial wastewater treatment, and remove large hard, non-combustible debris such as stones, metal blocks, and glass fragments, as well as explosive substances and persistent toxic pollutants such as fireworks and firecracker residues and waste oil containing polychlorinated biphenyls through manual and mechanical means. S2. Physicochemical Testing: Obtain the ammonia content and ammonia occurrence form of the screened ammonia-containing waste. Ammonia content is used to assess whether the total amount of reducing agent that can be released from the ammonia-containing waste meets the requirements of SNCR denitrification. Ammonia occurrence form is used to confirm that ammonia can exist as adsorbed ammonia or ammonium salts, which can be thermally decomposed to release NH3 within the temperature range of 950-1050℃ in the decomposition furnace. Both parameters jointly determine the usability of the ammonia-containing waste as an ammonia source for SNCR denitrification, ensuring that the obtained alternative fuel has in-situ denitrification capabilities. Simultaneously, obtain parameters such as lower heating value, moisture content, total heavy metals, sulfur, chlorine, and fluorine content for component synergistic blending in the following steps. The tested sludge showed an ammonia content of 3.2%, a moisture content of 53%, and a lower heating value of 680 kcal / kg, with slight exceedances in some heavy metals and chlorine content. S3. Component Mixture Regulation: Ammonia-containing industrial sludge, oil-containing waste residue, powdered catalyst carrier, and industrial waste resin were mixed in a mass ratio of 4:1:2:3 to synergistically neutralize and regulate harmful element parameters, so that the heavy metal, sulfur, chlorine, fluorine and other harmful element indicators of the mixture all meet the kiln entry standards specified in HJ662-2013 "Technical Specification for Environmental Protection of Solid Waste Co-processing in Cement Kilns". The test results are shown in Table 1. After regulation, the moisture content of the mixture was 21% and the lower heating value was 920 kcal / kg. S4. Stabilization Pretreatment: The mixture is fed into a crusher and crushed to below 20mm. After screening to remove solid impurities with a particle size greater than 20mm after crushing, it is fed into a mixer and mixed at a constant speed for 12 minutes to obtain a cement kiln alternative fuel with uniform composition, stable properties, and denitrification function. Uniform composition means that there is no segregation of fuel components, and stable properties mean that ammonia is not released prematurely at room temperature and the fuel does not clump.

[0022] Kiln Application: The prepared cement kiln alternative fuel with denitrification function is added to the high-temperature denitrification zone of the cement kiln decomposition furnace, and the furnace temperature is controlled at 950-1050℃. The alternative fuel stably releases ammonia gas at high temperature, which participates in the SNCR denitrification reaction.

[0023] Experimental results: Using the method in this embodiment, the denitrification efficiency can reach 55%, the ammonia water dosage is reduced by 38%, and the coal consumption is replaced by 12%, without affecting the quality of cement clinker products.

[0024] Example 2 A method for preparing denitrification functional cement kiln alternative fuel using ammonia-containing chemical waste residue includes the following steps: S1. Raw material screening: Select solid ammonia-containing waste residue from the chemical industry, and remove explosive substances such as ammonium nitrate by-products and peroxide catalyst residues, persistent toxic pollutants such as polychlorinated biphenyl waste catalyst carriers, batches of materials with excessive heavy metal content (such as batches with excessive mercury and cadmium content), as well as large hard non-combustible debris such as metal scraps and ceramic fragments; S2. Physicochemical testing: The ammonia content of the waste residue is 5.8%, the moisture content is 30%, the lower heating value is 1200 kcal / kg, and the sulfur, chlorine and fluorine levels are slightly exceeded. S3. Component Compounding and Control: Ammonia-containing waste residue was compounded with waste dust, oil sludge, and industrial waste resin at a mass ratio of 6:2:3:1 to synergistically neutralize and control harmful element parameters, ensuring that the heavy metal, sulfur, chlorine, fluorine, and other harmful element indicators of the mixture all meet the HJ662-2013 kiln entry standard. The test results are shown in Table 1. After adjustment, the moisture content of the mixture was 24%, and the lower heating value was 960 kcal / kg. S4. Stabilization pretreatment: The mixture is crushed to below 18mm, screened, and continuously mixed for 18 minutes to prepare a cement kiln alternative fuel with denitrification function, namely a uniform and stable functional alternative fuel. Kiln application: The alternative fuel for cement kilns with denitrification function is added to the high-temperature denitrification zone of the cement kiln decomposition furnace at a fixed point. The reaction temperature in the decomposition furnace is maintained at 950-1050℃, and the fuel releases ammonia for denitrification in a stable manner.

[0025] Experimental results: Using the method in this embodiment, the denitrification efficiency can reach 70%, the ammonia water dosage can be reduced by 60%, and the coal consumption can be replaced by 15%, without affecting the quality of cement clinker products.

[0026] Example 3 A method for preparing denitrification functional cement kiln alternative fuel using ammonia-containing organic solid waste includes the following steps: S1. Raw material screening: Select ammonia-containing organic solid waste produced by the chemical industry, and remove batches of materials with excessive levels of explosive substances such as residual low flash point organic solvents (such as ethanol, acetone, ethyl acetate), persistent toxic pollutants (such as batches with excessive levels of antibiotic residues and organochlorine pesticide residues), as well as large hard non-combustible debris such as metal packaging parts, stones, and ceramic fragments; S2. Physicochemical testing: The ammonia content of the waste residue is 4.5%, the moisture content is 25%, the lower heating value is 1000 kcal / kg, and the sulfur, chlorine and fluorine levels are slightly exceeded. S3. Component Mixture Adjustment: Based on the parameters measured in step S2, and combined with the control standards for co-processing solid waste in cement kilns and the SNCR denitrification requirements of the decomposer, ammonia-containing waste residue is mixed with powdered catalyst carrier, filter adsorption medium, and oil sludge at a mass ratio of 5:1:3:2 to synergistically neutralize and adjust harmful element parameters, ensuring that the heavy metal, sulfur, chlorine, fluorine, and other harmful element indicators of the mixture meet the HJ662-2013 kiln entry standard. After adjustment, the moisture content of the mixture is 22%, and the lower heating value is 1020 kcal / kg. S4. Stabilization pretreatment: The mixture is crushed to below 19mm, sieved, and continuously mixed for 10 minutes to prepare a uniform and stable functionalized alternative fuel. Kiln application: The alternative fuel for cement kilns with denitrification function is added to the high-temperature denitrification zone of the cement kiln decomposition furnace at a fixed point, and the temperature of the decomposition furnace is controlled at 950-1050℃, and the fuel releases ammonia for denitrification in a stable manner.

[0027] Experimental results: Using the method in this embodiment, the denitrification efficiency can reach 60%, the ammonia water dosage is reduced by 52%, and the coal consumption is replaced by 13%, without affecting the quality of cement clinker products.

[0028] Verified through trials on multiple industrial cement production lines, the functionalized alternative fuel prepared by this invention exhibits stable physical properties. No abnormal conditions such as scaling, kiln blockage, or deflagration occurred after entering the kiln, and it does not affect product indicators such as clinker compressive strength, boiling stability, and setting time. Compared to traditional production methods, this method can reduce denitrification agent costs by 30%–60%, reduce fossil fuel consumption by 10%–20%, and reduce NO… x Emissions were significantly reduced, while achieving 100% harmless co-processing and resource utilization of ammonia-containing waste, resulting in excellent economic, environmental and social benefits.

[0029] Comparative Example Comparative Example 1: Direct feeding of ammonia-containing sludge into the decomposition furnace (This comparative example corresponds to the existing technology of directly feeding ammonia-containing sludge into the decomposition furnace) S1. Raw material selection: Same as in Example 1; S2. Physicochemical testing: The sludge was found to have an ammonia content of 3.2%, a moisture content of 53%, and a lower heating value of 680 kcal / kg. Some heavy metals and chlorine were found to be slightly above the standard. The test results are shown in Table 1. S3, No component adjustment is performed; S4. Stabilization pretreatment: The sludge is crushed and screened to remove impurities, reducing the particle size to below 20mm. Kiln application: The sludge treated as described above is added to the decomposition furnace of a cement kiln, and the furnace temperature is controlled at 950-1050℃. The high temperature releases ammonia gas to participate in the SNCR denitrification reaction.

[0030] Experimental results: The denitrification efficiency was approximately 40%, reducing ammonia dosage by 25%, but the coal consumption was not significantly reduced, and the content of some heavy metals in the cement clinker slightly exceeded the standard. In this comparative example, no component blending was performed, and the calorific value of the sludge was only 680 kcal / kg, which could not provide stable combustion and heating, thus failing to replace coal. Simultaneously, the sludge contained excessive levels of harmful elements (heavy metals, chlorine), leading to a decline in clinker quality if directly fed into the kiln. Example 1, however, increased the calorific value to 920 kcal / kg through blending and diluted harmful elements, enabling the fuel to stably burn and replace coal while meeting kiln entry standards. Furthermore, the blended material exhibited improved uniformity, facilitating stable ammonia release and enhancing denitrification efficiency. Therefore, component blending is a fundamental condition for achieving the triple goals of compliant kiln entry, efficient ammonia release denitrification, and coal replacement.

[0031] Comparative Example 2: Direct feeding of ammonia-containing waste residue into the decomposition furnace S1. Raw material selection: Same as in Example 2; S2. Physicochemical testing: The waste residue had an ammonia content of 5.8%, a moisture content of 30%, a lower calorific value of 1200 kcal / kg, and slightly exceeded the standards for sulfur, chlorine, and fluorine. The test results are shown in Table 1. S3, Component Combination Regulation: No component adjustment is performed; S4. Stabilization pretreatment: The waste residue is crushed and screened to remove impurities, and the particle size is reduced to below 18mm to obtain alternative fuel; Kiln application: Add alternative fuel to the high-temperature denitrification zone of the cement kiln decomposition furnace, control the decomposition furnace temperature to 950-1050℃, and release ammonia gas at high temperature from the alternative fuel to participate in the SNCR denitrification reaction; Experimental results: The denitrification efficiency reached 67%, reducing ammonia water dosage by 58% and replacing 12% of coal consumption, lower than Example 2. After long-term use, the alternative fuel in this comparative example showed crusting and blockage in the kiln (due to excessive sulfur and chlorine content). The waste residue used in Comparative Example 2 had a high calorific value of 1200 kcal / kg and an ammonia content of 5.8%, thus achieving good denitrification and coal replacement effects even when directly fed into the kiln. However, its excessive sulfur and chlorine content led to crusting and blockage over time. Example 2, by adding waste dust, sludge, and waste resin, diluted harmful elements to within standards while maintaining high calorific value and high ammonia content, thus achieving better denitrification effects and long-term stable operation. This indicates that relying solely on the calorific value and ammonia content of the raw materials is insufficient; it is necessary to regulate harmful elements through compounding to ensure the reliability and sustainability of the system.

[0032] Comparative Example 3: Implementation according to CN103551016A scheme This comparative example was implemented strictly according to the scheme of patent CN103551016A. In the reduction combustion zone of the decomposition furnace using staged combustion technology, waste alternative fuel with an ammonia content ≥3% (using ammonia-containing sludge, moisture 5-30%, 80% passing through a 20-mesh sieve, the physicochemical test results are shown in Table 1) was added and injected via pneumatic conveying at a speed of 10-25 m / s.

[0033] Test results: The denitrification efficiency was approximately 38%, the ammonia water dosage was reduced by 22%, and the coal consumption was not significantly reduced.

[0034] Scheme CN103551016A employs a staged combustion decomposition furnace, adding alternative fuels in the reduction combustion zone. Its denitrification mechanism relies on the reduction of NO by active groups such as CHi / NHi / CN. x Instead of NH3-SNCR, this invention uses a compounding process to enrich the fuel with ammonia components and achieves denitrification via the NH3-SNCR mechanism within the temperature range of 950-1050℃, resulting in higher efficiency. Furthermore, the fuel itself has a high calorific value and can replace some coal. The two technical routes differ fundamentally in their denitrification mechanisms and functional positioning; this invention has significant advantages in both denitrification efficiency and energy substitution.

[0035] Comparative Example 4: The compounded product was added to the low-temperature zone (<950℃) of the decomposition furnace. A method for preparing denitrification functional cement kiln alternative fuel using ammonia-containing industrial sludge includes the following steps: S1. Raw material selection: Same as in Example 1; S2. Physicochemical testing: The sludge was found to have an ammonia content of 3.2%, a moisture content of 53%, a lower heating value of 680 kcal / kg, and some heavy metals and chlorine slightly exceeded the standards. S3. Component compounding and regulation: Ammonia-containing industrial sludge, oil-containing waste residue, powdered catalyst carrier, and industrial waste resin were compounded in a mass ratio of 4:1:2:3. After regulation, the moisture content of the mixture was 21%, the lower heating value was 920 kcal / kg, and the heavy metal, sulfur, chlorine, fluorine and other harmful element indicators of the mixture met the HJ662-2013 cement kiln feed standard. The test results are shown in Table 1. S4. Stabilization pretreatment: The mixture is fed into a crusher and crushed to below 20mm. After being screened to remove impurities, it is fed into a mixer and mixed at a constant speed for 12 minutes to obtain a functional alternative fuel with uniform composition and stable properties. Kiln application: The alternative fuel is added to the C5 preheater outlet temperature zone of the upper part of the cement kiln decomposition furnace, which is 860-920℃. The high-temperature combustion of the fuel releases ammonia gas, which participates in the SNCR denitrification reaction.

[0036] Experimental results: The denitrification efficiency was approximately 49%, with a 30% reduction in ammonia water dosage and an 11% replacement of coal consumption, lower than the data in Example 1. This comparative example used the same compound fuel as Example 1, but the temperature of the addition zone was only 860-920℃, lower than 950℃. At this temperature, the ammonium salt decomposition rate slowed down, the NH3 release was insufficient, and the reaction rate between NH3 and NOx was also significantly reduced, leading to a decrease in denitrification efficiency. Although the coal replacement effect was less affected (because combustion could still occur), the denitrification function was significantly weakened. This indicates that a temperature range of 950-1050℃ is a necessary condition for achieving efficient ammonia release SNCR, and temperatures that are too low will directly damage denitrification performance.

[0037] Comparative Example 5: Functionalized alternative fuel was prepared according to the compounding method of Example 1 and added to the high-temperature zone at the top of the decomposition furnace, with the temperature controlled at 1050-1100°C.

[0038] A method for preparing denitrification functional cement kiln alternative fuel using ammonia-containing industrial sludge includes the following steps: S1. Raw material selection: Same as in Example 1; S2. Physicochemical testing: The sludge was found to have an ammonia content of 3.2%, a moisture content of 53%, a lower heating value of 680 kcal / kg, and some heavy metals and chlorine slightly exceeded the standards. S3. Component compounding and regulation: Ammonia-containing industrial sludge, oil-containing waste residue, powdered catalyst carrier, and industrial waste resin are compounded in a mass ratio of 4:1:2:3. After regulation, the moisture content of the mixture is 21% and the lower heating value is 920 kcal / kg. All indicators meet the HJ662-2013 cement kiln feed standard. S4. Stabilization pretreatment: The mixture is fed into a crusher and crushed to below 20mm. After being screened to remove impurities, it is fed into a mixer and mixed at a constant speed for 12 minutes to obtain a functional alternative fuel with uniform composition and stable properties. Kiln Application: The alternative fuel is added to the kiln tail flue gas chamber at the bottom of the cement kiln's decomposition furnace, where the temperature is between 1060 and 1120°C. The high-temperature combustion of the fuel releases ammonia gas, which participates in the SNCR denitrification reaction. Test results show that the denitrification efficiency is 51%, which can reduce the amount of ammonia water added by 33% and replace 12% of the coal consumption without affecting the quality of cement clinker products.

[0039] Experimental results: The denitrification efficiency was 51%, reducing ammonia dosage by 33% and replacing 12% of coal consumption. The denitrification efficiency and ammonia savings in this comparative example are lower than in Example 1. This comparative example also uses the compound fuel from Example 1, but the temperature in the addition zone is as high as 1060-1120℃, exceeding 1050℃. At this temperature, some NH3 is oxidized to NO (2NH3 + 5 / 2O2 → 2NO + 3H2O), resulting in a reduction in the actual NH3 used for denitrification and a decrease in denitrification efficiency. Simultaneously, high temperatures may accelerate the premature decomposition of ammonia, causing it to be consumed before reaching the optimal reaction zone. Therefore, the upper temperature limit is equally important; excessively high temperatures can weaken the denitrification effect. This demonstrates the necessity of the upper temperature range of 950-1050℃ in this application.

[0040] Comparative Example 6: The raw materials were the same as in Example 1, but the compounding ratio was changed to ammonia-containing sludge: oil-containing waste residue: powdered catalyst carrier: industrial waste resin = 5:1:2:2.

[0041] A method for preparing denitrification functional cement kiln alternative fuel using ammonia-containing industrial sludge includes the following steps: S1. Raw material selection: Same as in Example 1; S2. Physicochemical testing: The sludge was found to have an ammonia content of 3.2%, a moisture content of 53%, a lower heating value of 680 kcal / kg, and some heavy metals and chlorine slightly exceeded the standards. S3. Component compounding and regulation: Ammonia-containing industrial sludge, oil-containing waste residue, powdered catalyst carrier, and industrial waste resin were compounded in a mass ratio of 5:1:2:2. After regulation, the moisture content of the mixture was 26% and the lower heating value was 840 kcal / kg. Except for a slight excess of chlorine, all other indicators met the HJ662-2013 cement kiln feed standard. The test results are shown in Table 1. S4. Stabilization pretreatment: The mixture is fed into a crusher and crushed to below 20mm. After being screened to remove impurities, it is fed into a mixer and mixed at a constant speed for 12 minutes to obtain a functional alternative fuel with uniform composition and stable properties. Kiln application: The alternative fuel is added to the cement kiln decomposition furnace, and the furnace temperature is controlled at 950-1050℃. The high-temperature combustion of the fuel releases ammonia gas, which participates in the SNCR denitrification reaction.

[0042] Experimental results: The denitrification efficiency was 53%, reducing ammonia water dosage by 35%, but only replacing 8% of coal consumption, both lower than in Example 1. After long-term use, slight scaling appeared inside the kiln (caused by high chlorine content). This comparative example demonstrates that a specific compounding ratio is the key factor in achieving synergistic effects and optimal overall results; not all mixtures of ammonia-containing solid waste and auxiliary solid waste in arbitrary proportions can achieve the technical effects of this invention. In this comparative example, the ratio of ammonia-containing sludge to auxiliary waste was changed from 4:1:2:3 to 5:1:2:2, resulting in an increase in the moisture content of the mixture to 26%, a decrease in calorific value to 840 kcal / kg, and a slight exceedance of chlorine content. The decrease in calorific value reduces combustion stability and weakens the coal substitution effect; the excessive chlorine causes scaling inside the kiln. Simultaneously, the increased moisture content of the material affects the uniformity of ammonia release, leading to a slight decrease in denitrification efficiency. This indicates that a specific compounding ratio, through design, allows indicators such as calorific value, moisture content, and harmful elements to synergistically meet standards, while simultaneously achieving optimal denitrification, energy saving, and operational reliability. The proportions in this scheme achieve a balance among the various indicators, resulting in the optimal overall effect.

[0043] Table 1. Detection data of sulfur, chlorine, fluorine and heavy metals in the raw materials or mixtures of the examples and comparative examples.

[0044] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing alternative fuel for cement kilns with denitrification function using ammonia-containing waste, characterized in that, Includes the following steps: S1. Raw material screening: Collect ammonia-containing waste as basic raw materials and remove explosive substances, persistent toxic pollutants and large pieces of hard, non-combustible debris. S2. Physical and chemical testing: Physical and chemical indicators of the screened ammonia-containing waste are tested to obtain parameters such as ammonia content, ammonia occurrence form, lower heating value, moisture content, total heavy metals, sulfur, chlorine and fluorine content. S3. Component Co-mixing: Based on the parameters of low calorific value, moisture content, and heavy metal, sulfur, chlorine, and fluorine content measured in step S2, and combined with the control standards for co-processing solid waste in cement kilns and the requirements of SNCR denitrification in decomposition furnaces, the ammonia-containing waste is mixed with one or more auxiliary wastes to synergistically adjust the heavy metal, sulfur, chlorine, fluorine, moisture content, and calorific value in the resulting mixture, so that the indicators of the mixture meet the control requirements for cement kiln feed. S4. Material stabilization pretreatment: The mixture is crushed, screened and mixed in sequence to control the particle size distribution and eliminate the segregation of material components, so as to obtain a cement kiln alternative fuel with denitrification function.

2. The preparation method according to claim 1, characterized in that, In step S3, the moisture content of the mixture is 10%-25%, and the lower heating value is not less than 840 kcal / kg; the limits for heavy metals, sulfur, chlorine and fluorine in the mixture meet the requirements of HJ662-2013 "Environmental Protection Technical Specification for Co-processing Solid Waste in Cement Kilns".

3. The preparation method according to claim 2, characterized in that, The ammonia-containing waste includes one or more of ammonia-containing industrial waste residue, ammonia-containing sludge, and ammonia-containing organic waste; the ammonia in the ammonia-containing waste exists in the form of adsorbed ammonia or ammonium salt.

4. The preparation method according to claim 3, characterized in that, In step S4, the purpose of screening is to remove solid impurities with a particle size greater than 20 mm after the mixture is crushed; the mixing time is not less than 10 minutes.

5. The preparation method according to claim 1, characterized in that, In step S3, the auxiliary waste is one or more of combustible industrial solid waste and inorganic conditioning solid waste.

6. A cement kiln alternative fuel with denitrification function, characterized in that, It is prepared by the preparation method according to any one of claims 1-5.

7. The application of the cement kiln alternative fuel with denitrification function as described in claim 6 in cement kiln flue gas SNCR denitrification, harmless treatment of solid waste, and energy-saving cement production.

8. The application according to claim 7, characterized in that, The application method is as follows: the cement kiln alternative fuel with denitrification function is added at a fixed point to the high-temperature denitrification zone of the cement kiln decomposition furnace. Under the condition of 950℃-1050℃, the cement kiln alternative fuel with denitrification function decomposes and releases ammonia gas after being heated. The released ammonia gas is used in situ as an SNCR denitrification reducing agent to react with nitrogen oxides in the cement kiln flue gas to reduce NO in the kiln flue gas. x The emission concentration is reduced and the dosage of denitrification agents is decreased; at the same time, the heat released by the combustion of alternative fuels in the cement kiln, which also has denitrification function, provides thermal energy for the cement kiln system, replacing part of the fossil fuels.

Citation Information

Patent Citations

  • Method for reburning denitration of cement kiln by using alternative fuel

    CN103551016A