A production method for improving segregation in high-carbon hard wire steel

By implementing a collaborative process control system, the problems of central carbon segregation and low equiaxed crystal ratio in high-carbon hard wire steel under high casting speeds were solved, thereby improving the internal homogeneity of the billet and stabilizing production efficiency, thus meeting the quality requirements of high-end products.

CN123108232APending Publication Date: 2026-11-17INNER MONGOLIA BAOTOU STEEL UNION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611246324.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing high-carbon hard wire steel production processes are prone to severe central carbon segregation, low equiaxed crystal ratio, and increased solute enrichment due to bulging and suction in the cast billet at high drawing speeds. This results in excessive network cementite in the finished wire rod, failing to meet the quality requirements for raw materials of high-end prestressed steel wire and steel cord.

Method used

The process adopts a collaborative control approach throughout the entire process, including molten iron pretreatment, LF refining, continuous casting, and electromagnetic stirring at the end of solidification. By controlling the superheat, cooling method, and electromagnetic stirring parameters, and in conjunction with dynamic light pressure, the internal homogeneity of the cast billet is improved.

Benefits of technology

It significantly reduces the carbon segregation index at the center of the billet, increases the equiaxed crystal ratio, reduces network cementite, improves the wire breakage rate during finished product drawing, meets the quality requirements of high-end products, and maintains production efficiency.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a production method for improving segregation in high-carbon hard wire rod, belonging to the field of continuous casting production technology in iron and steel metallurgy. The method includes: hot metal pretreatment; LF refining; continuous casting process: electromagnetic stirring in the crystallizer: current 320-360A, frequency 6.5-7.5Hz; segmented cooling in the secondary cooling zone: upper section specific water volume 0.95-1.05L / kg, middle and lower sections 0.60-0.70L / kg; electromagnetic stirring at the end of solidification: installation position 15.2-16.8m from the meniscus, current 260-300A, frequency 5.0-6.0Hz; dynamic light reduction: reduction is implemented in the range of solid fraction Fs = 0.32-0.68, with a total reduction of 9-12mm, evenly distributed in 3 segments, with a single segment reduction of 3-4mm. The purpose of this invention is to significantly reduce the carbon segregation index of the billet, eliminate harmful network cementite in the wire rod, and balance production efficiency with the internal homogeneity of the billet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of continuous casting production technology in iron and steel metallurgy, and particularly relates to a production method for improving segregation in high-carbon hard wire steel. Background Technology

[0002] High-carbon hard wire steel has a carbon mass fraction of 0.60%–0.88%. During solidification, the solute redistribution effect is significant. In high-speed casting of small-section billets, the liquidus cavity elongates and the solidification cooling rate is uneven, easily leading to severe central carbon segregation. Existing conventional production processes have the following drawbacks:

[0003] (1) The superheat control of molten steel is rough, with a conventional superheat of 30-45℃. Under high casting speed, columnar crystals are overdeveloped, and the equiaxed crystal ratio is less than 20%. The molten steel enriched with solute converges along the dendrite channel to the center of the billet, and the segregation index is ≥1.18.

[0004] (2) The parameters of the crystallizer and the end electromagnetic stirring are fixed and not matched to the two-phase region of high pulling speed of 2m / min. The stirring force field cannot break the continuous columnar crystals and the solute channels between dendrites cannot be blocked.

[0005] (3) The light reduction range and reduction amount at the end of solidification are set according to the low casting speed parameters. At a casting speed of 2m / min, the position of the liquid phase end of the billet moves backward, and the original reduction range deviates from the core range of 0.3 to 0.7 solid fraction. The shrinkage compensation is insufficient, and the central porosity and segregation are superimposed.

[0006] (4) The water volume in the secondary cooling zone is evenly distributed throughout the entire area, the temperature difference between the inner and outer arcs of the billet is large, the bulging deformation is aggravated, and the liquid phase suction effect is amplified and segregation occurs.

[0007] During the refining stage, only minor adjustments to the composition were made, without simultaneously reducing the fluctuations in the original solute concentration of the molten steel. This further amplified the macroscopic segregation caused by the fluctuations in the original composition of the billet.

[0008] Existing technologies that optimize any one of the stirring, light pressing, or cooling processes individually cannot adapt to the high drawing speed of 2m / min for 150mm square billets. Segregation defects are inherited to the wire rod, resulting in a network of cementite. The finished product has a high wire breakage rate during drawing, which cannot meet the quality requirements of high-end prestressed steel wire and steel cord raw materials. Summary of the Invention

[0009] To address the technical shortcomings of existing high-carbon hard wire steel 150mm cross-section billets produced at a high casting speed of 2m / min, where single-process control cannot suppress carbon center segregation, low equiaxed crystal ratio, billet bulging and suction exacerbating solute enrichment, and excessive network carbides in finished wire rods, a set of synergistic control technology for the entire process of smelting, refining, and continuous casting is provided. Under the premise of maintaining a stable high production efficiency of 2m / min, this technology significantly reduces the carbon segregation index of the billet, eliminates harmful network cementite in the wire rod, and balances production efficiency with the internal homogeneity of the billet.

[0010] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0011] This invention discloses a production method for improving segregation in high-carbon hard wire steel, comprising:

[0012] Hot metal pretreatment: After desulfurization, the sulfur content of the hot metal is ≤0.008%, and the carbon fluctuation of the hot metal entering the furnace is controlled to be ≤±0.05%;

[0013] LF refining: The superheat of the molten steel at the station is 18-24℃, and the carbon content fluctuation at the refining endpoint is ≤±0.02%; soft blowing argon stirring for 12-16 min, argon flow rate 8-12 L / min;

[0014] Continuous casting process:

[0015] Electromagnetic stirring for crystallizer: current 320-360A, frequency 6.5-7.5Hz;

[0016] The cooling system is divided into two sections: the upper section has a specific water flow rate of 0.95–1.05 L / kg, the middle and lower sections have a specific water flow rate of 0.60–0.70 L / kg, and the difference in cooling water flow rate between the inner and outer arcs is ≤8%.

[0017] Electromagnetic stirring at the end of solidification: installation position 15.2~16.8m from the meniscus, current 260~300A, frequency 5.0~6.0Hz;

[0018] Dynamic light reduction: Reduction is carried out in the range of solid fraction Fs = 0.32 to 0.68, with a total reduction of 9 to 12 mm, and the reduction is evenly distributed in 3 segments with a single segment reduction of 3 to 4 mm.

[0019] Furthermore, the carbon mass fraction of the high-carbon hard wire steel is 0.60% to 0.88%.

[0020] Furthermore, the cross-section of the cast billet is 150mm × 150mm.

[0021] Furthermore, the continuous casting constant speed is 2m / min.

[0022] Furthermore, the chemical composition of the high-carbon hard wire steel by mass percentage is as follows: C: 0.78%~0.85%, Si: 0.20%~0.32%, Mn: 0.50%~0.80%, P≤0.018%, S≤0.008%, Cu+Sn+Pb≤0.15%, with the balance being iron and unavoidable impurities.

[0023] Furthermore, the LF refining soft blowing argon stirring time is 14 min, the argon flow rate is 10 L / min, and the superheat of the molten steel at the station is 20-22℃.

[0024] Furthermore, the total reduction under dynamic light pressure is 10 mm, the reduction in each of the three stages is 3.3 mm, and the solid fraction Fs is controlled within the range of 0.35 to 0.65.

[0025] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0026] (1) The whole process of coordinated carbon control, superheat control, cooling control, dual electromagnetic stirring + precise dynamic light pressure matching 2m / min high casting speed, the equiaxed crystal ratio of the billet is increased to more than 42%, and the carbon segregation index in the center of the billet is stably controlled to ≤1.08, which is far better than the existing process level of 1.18 or above;

[0027] (2) The 150mm×150mm cross section billet maintains a high casting speed of 2m / min, without the need to reduce the speed to improve quality, and the hourly capacity of a single casting machine is not lost, and the production efficiency is stable.

[0028] (3) The inheritance of segregation defects in the billet is significantly suppressed, the grade of network cementite in the rolled wire is ≤1, the wire breakage rate during wire drawing decreases by 75%, and the yield of high-end hard wire products increases by 6%;

[0029] (4) The process only requires adjusting the parameters to match the collaborative logic. No new large-scale metallurgical equipment is needed. It can be implemented by simply modifying the parameters of existing smelting and continuous casting equipment. The modification cost is low and the adaptability is strong.

[0030] (5) Refining with low superheat and long-term soft blowing reduces the uneven heating and cooling of molten steel. Secondary cooling zone cooling reduces the internal and external stress of the billet. The billet cracks and porosity defects are improved simultaneously, and the overall billet qualification rate is increased by 4.5%. Detailed Implementation

[0031] Example 1

[0032] Producing SWRH82B high carbon hard wire steel, with a billet size of 150mm×150mm and a constant drawing speed of 2m / min;

[0033] 1) Hot metal pretreatment: After KR desulfurization, S=0.006%, and the carbon fluctuation of the hot metal entering the furnace is ±0.04%;

[0034] 2) LF refining: The superheat of the molten steel leaving the station is 21℃, the final carbon content is 0.825%, and the composition fluctuation is ±0.015%; soft blowing of argon for 14 min, argon flow rate is 10L / min;

[0035] 3) Continuous casting control: EMS current 340A, frequency 7Hz; water flow rate in the upper section of the secondary cooling system 1.0L / kg, 0.65L / kg in the lower section, water flow rate difference between the inner and outer arcs 6%; F-EMS at the end is 16.0m from the meniscus, current 280A, frequency 5.5Hz; light reduction Fs range 0.35~0.65, total reduction 10mm, evenly distributed in three sections 3.3mm each;

[0036] Test results: The equiaxed crystal ratio of the billet is 45%, the central carbon segregation index is 1.06, the wire rod network cementite is grade 0.5, and the wire breakage rate during drawing is 0.12%.

[0037] Example 2

[0038] Producing SWRH77B high carbon hard wire steel, with a billet size of 150mm×150mm and a drawing speed of 2m / min;

[0039] 1) Desulfurization of molten iron pretreatment: S=0.007%, carbon fluctuation of molten iron ±0.05%;

[0040] 2) LF refining superheat 19℃, final carbon 0.772%, soft blowing argon for 12min, argon flow rate 8L / min;

[0041] 3) Continuous casting: EMS current of 320A and frequency of 6.5Hz in the crystallizer; 0.95L / kg in the upper section and 0.60L / kg in the lower section of the secondary cooling system; EMS current of 260A and frequency of 5Hz at the end; total pressure reduction of 9mm under light pressure.

[0042] Test results: equiaxed crystal ratio 42%, segregation index 1.07, no obvious network cementite in the wire rod.

[0043] Comparative example (existing conventional process)

[0044] For the same specification 150mm billet, casting speed of 2m / min, superheat of 38℃, fixed low current for electromagnetic stirring, water content of 0.85L / kg in the entire secondary cooling range, and low casting speed of 1.4m / min under light pressure;

[0045] Test results: equiaxed crystal ratio 17%, carbon segregation index 1.21, wire mesh cementite grade 4, wire breakage rate 0.48%.

[0046] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A production method for improving segregation of high-carbon hard wire steel, characterized by, include: Hot metal pretreatment: After desulfurization, the sulfur content of the hot metal is ≤0.008%, and the carbon fluctuation of the hot metal entering the furnace is controlled to be ≤±0.05%; LF refining: The superheat of the molten steel at the station is 18-24℃, and the carbon content fluctuation at the refining endpoint is ≤±0.02%; soft blowing argon stirring for 12-16 min, argon flow rate 8-12 L / min; Continuous casting process: Electromagnetic stirring for crystallizer: current 320-360A, frequency 6.5-7.5Hz; The cooling system is divided into two sections: the upper section has a specific water flow rate of 0.95–1.05 L / kg, the middle and lower sections have a specific water flow rate of 0.60–0.70 L / kg, and the difference in cooling water flow rate between the inner and outer arcs is ≤8%. Electromagnetic stirring at the end of solidification: installation position 15.2~16.8m from the meniscus, current 260~300A, frequency 5.0~6.0Hz; Dynamic light reduction: Reduction is carried out in the range of solid fraction Fs = 0.32 to 0.68, with a total reduction of 9 to 12 mm, and the reduction is evenly distributed in 3 segments with a single segment reduction of 3 to 4 mm.

2. The production method for improving segregation of high carbon hard wire steel according to claim 1, characterized by, The carbon mass fraction of the high-carbon hard wire steel is 0.60% to 0.88%.

3. The production method for improving segregation of high carbon hard wire steel according to claim 1, characterized by, The cross-section of the cast billet is 150mm×150mm.

4. The production method for improving segregation in high-carbon hard wire steel according to claim 1, characterized in that, The continuous casting speed is constant at 2 m / min.

5. The production method for improving segregation in high-carbon hard wire steel according to claim 1, characterized in that, The chemical composition of the high-carbon hard wire steel by mass percentage is as follows: C: 0.78%~0.85%, Si: 0.20%~0.32%, Mn: 0.50%~0.80%, P≤0.018%, S≤0.008%, Cu+Sn+Pb≤0.15%, with the balance being iron and unavoidable impurities.

6. The production method for improving segregation in high-carbon hard wire steel according to claim 1, characterized in that, The LF refining soft blowing argon stirring time is 14 min, the argon flow rate is 10 L / min, and the superheat of the molten steel at the station is 20-22℃.

7. The production method for improving segregation in high-carbon hard wire steel according to claim 1, characterized in that, The total reduction under dynamic light pressure is 10 mm, and the reduction in each of the three stages is 3.3 mm. The solid fraction Fs is controlled within the range of 0.35 to 0.65.