A method for low-temperature lithium extraction from spodumene with ultra-high yield
By combining low-temperature roasting of spodumene with reaction with concentrated sulfuric acid, along with mother liquor compounding and low-temperature freezing to remove potassium, the problems of high energy consumption and high cost in spodumene lithium extraction have been solved. This method achieves a high-efficiency and low-cost spodumene lithium extraction process, which is applicable to the efficient lithium extraction of spodumene and lepidolite.
Patent Information
- Application Number
- CN202611224557.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing lithium extraction methods from spodumene suffer from high energy consumption, large sulfuric acid consumption, low lithium extraction efficiency, and high cost. Furthermore, new methods are subject to high costs, complex impurity removal processes, or pressure leaching, which is not conducive to industrial application.
Lithium spodumene and calcination aids were ball-milled and mixed, then calcined at a low temperature of 850-950℃. The mixture was then reacted with concentrated sulfuric acid, with the molar ratio of lithium oxide to concentrated sulfuric acid controlled at 1:1. The pH value was adjusted by combining calcium oxide and other agents for leaching. The mixture was then compounded with mother liquor and subjected to low-temperature freezing to remove potassium. Finally, it was reacted with sodium carbonate to prepare lithium carbonate.
It achieves low-temperature roasting to reduce energy consumption, reduce the amount of concentrated sulfuric acid used, increase the lithium extraction rate to over 96%, simplify the potassium removal process, improve the purity and overall yield of lithium carbonate, and is suitable for efficient lithium extraction from spodumene, lepidolite, etc., reducing production costs and environmental impact.
Smart Images

Figure CN123108316A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium extraction technology from ores, and in particular to a method for low-temperature lithium extraction from spodumene with ultra-high yield. Background Technology
[0002] The main method for extracting lithium from spodumene is the sulfuric acid process, which generally includes roasting, acidification, slurry leaching, purification, and evaporation and concentration to obtain lithium sulfate solution. This lithium sulfate solution can then be used as a raw material for subsequent lithium carbonate or lithium hydroxide production. Therefore, the yield and quality of the lithium sulfate solution directly determine the output and quality of the lithium carbonate or lithium hydroxide products, while the output and quality of the lithium sulfate solution depend on the aforementioned production processes.
[0003] A Chinese invention (title: "Method for Extracting Lithium from Spodumene Ore and Producing Zeolite or Potassium Nepheline as a Byproduct", Publication No.: CN109399672B, Publication Date: 2020-08-07) discloses a method for extracting lithium from spodumene ore and producing zeolite or potassium nepheline as a byproduct. The method involves adding spodumene ore to a reactor and stirring the mixture. Under normal pressure and controlled temperature, spodumene is converted into zeolite or potassium nepheline, while lithium is transferred into the solution, resulting in a lithium-containing solution. Lithium can then be obtained from the solution through chemical precipitation. This method primarily modifies the lithium extraction process by using a large amount of strong alkali such as sodium hydroxide for lithium leaching. This method consumes a significant amount of alkali, which, while saving energy, greatly increases the cost of raw materials, far exceeding existing processes. Furthermore, the lithium extraction rate of this method is only consistently around 93%, which is somewhat different from high-efficiency leaching. Its main focus is on producing zeolite or potassium nepheline using this method to improve the utilization rate of lithium extraction slag.
[0004] Chinese invention application (title: "A Method for High-Efficiency and Green Leaching of Lithium from Spodumene Using an External Field Enhancement", publication number: CN117887978A, publication date: 2024-04-16) discloses a method for high-efficiency and green leaching of lithium from spodumene using an external field enhancement. The method involves mixing and grinding spodumene concentrate with a large amount of strong alkali, followed by microwave calcination, and then ultrasonic leaching in water. After filtration, a primary leaching solution and leaching residue are obtained. The leaching residue is washed with water, dried, ground, and then ultrasonically leached in an acid solution to obtain a secondary leaching solution. This method also modifies some lithium extraction processes, using a large amount of strong alkali to achieve lithium conversion and microwave heating instead of gas heating, thus saving energy to some extent. However, the large amount of strong alkali and the dilute acid used for subsequent neutralization increase costs, hindering its industrial application. Furthermore, in pursuit of slag-free leaching, this method also leaches elements such as silicon and aluminum, adding challenges to the subsequent treatment of the lithium-containing leaching solution.
[0005] A Chinese invention (titled "A Method for Lithium Extraction from Spodumene by Secondary Reverse Leaching with Nitric Acid", announcement number: CN114318008B, announcement date: 2022-09-23) discloses a method for lithium extraction from spodumene by secondary reverse leaching with nitric acid. The method involves ball milling spodumene and then calcining it at 900–1300℃; followed by leaching with water at a liquid-to-solid mass ratio of 2.5–6:1 with nitric acid. After separation, the filter residue is leached again with nitric acid under pressure. This process achieves the recovery of lithium, magnesium, rubidium, cesium, etc., from spodumene. While this method modifies the lithium extraction process by replacing the original acidification and leaching with nitric acid leaching, the addition of a pressure-and-heat process for the secondary nitric acid leaching presents new challenges to the entire lithium extraction industry.
[0006] Traditional sulfuric acid leaching of spodumene suffers from high energy consumption, large sulfuric acid usage, and long extraction time leading to low lithium extraction efficiency. Newly proposed methods, however, face challenges such as high cost, complex impurity removal, or pressure leaching, hindering industrial application. Therefore, it is necessary to research a new, low-cost, high-efficiency method for lithium extraction from spodumene that can be rapidly deployed to production. Summary of the Invention
[0007] The present invention aims to provide a method for low-temperature lithium extraction from spodumene with ultra-high yield, which significantly reduces acid usage, has low energy consumption, low cost, is safe and environmentally friendly, does not introduce other impurities, is highly efficient and can be quickly put into production.
[0008] The technical solution adopted in this invention is:
[0009] A method for low-temperature lithium extraction from spodumene with ultra-high yield includes the following steps:
[0010] Step S1: Spodumene and calcination aids are ball-milled and mixed, then calcined at a low temperature of 850-950℃, and cooled to obtain calcined material; wherein, another calcination aid returned during the lithium extraction process accounts for 0-100 wt% of the total weight of the calcination aids.
[0011] Step S2: Mix the calcined material obtained in step S1 with concentrated sulfuric acid and acidify it at 250~300℃ to obtain acid-cooked material; wherein, the molar ratio of lithium oxide to concentrated sulfuric acid in the calcined material is 1:1.
[0012] Step S3: The acidified material obtained in step S2 is mixed with water and leached. During the leaching process, calcium oxide, calcium hydroxide or calcium carbonate is added to adjust the pH value of the system to 5.0~6.0. Solid-liquid separation is performed to obtain leachate and leach residue.
[0013] Step S4: The leachate obtained in step S3 is mixed with the mother liquor returned from another lithium extraction process, the pH is adjusted to 3-4, aluminum sulfate octadecylhydrate is added and then the mixture is frozen at low temperature to separate the solid and liquid, resulting in filtrate and filter residue. The filtrate is then purified to remove impurities, yielding a lithium sulfate solution. The concentration of potassium ions in the mixed solution of leachate and mother liquor is 5-8 g / L, and the molar ratio of aluminum sulfate octadecylhydrate to potassium ions in the mixed solution is 0.5-3:1. The filter residue after solid-liquid separation is returned to step S1 of another lithium extraction process as a roasting aid.
[0014] Step S5: The lithium sulfate solution obtained in step S4 is mixed with sodium carbonate solution to precipitate lithium, and solid-liquid separation is performed to obtain crude lithium carbonate and filtrate; the crude lithium carbonate is stirred, washed, and dried to obtain battery-grade lithium carbonate; wherein, the filtrate after solid-liquid separation is evaporated and concentrated, and then solid-liquid separation is performed again, the separated filter residue is returned to step S1 of another lithium extraction process as a roasting aid, and the separated mother liquor is returned to step S4 of another lithium extraction process to be mixed with the leachate.
[0015] Furthermore, the calcination aid in step S1 includes alkaline earth metal oxides, alkaline earth metal hydroxides or carbonates, and sulfates.
[0016] Further, in step S1, the weight ratio of spodumene, alkaline earth metal oxide, alkaline earth metal hydroxide or carbonate, and sulfate is 100:(4~20):(0.1~10).
[0017] Furthermore, the alkaline earth metal oxide is one or more of calcium oxide and magnesium oxide;
[0018] The alkaline earth metal hydroxide is one or more of calcium hydroxide and magnesium hydroxide;
[0019] The carbonate is one or more of calcium carbonate and magnesium carbonate;
[0020] The sulfate is one or more of sodium sulfate, potassium sulfate, calcium sulfate, and potassium aluminum sulfate.
[0021] Furthermore, in step S3, the weight ratio of acidified material to water is 1:(2~3).
[0022] Furthermore, in step S1, the ball milling time for mixing spodumene and calcination aid is 2-10 minutes.
[0023] Furthermore, the roasting time during the low-temperature roasting transformation in step S1 is 1~5h.
[0024] Furthermore, the temperature during cryogenic freezing in step S4 is -4 to 8°C.
[0025] Furthermore, in step S4, the molar ratio of aluminum sulfate octahydrate to potassium ions in the compound solution is (0.8~1):1.
[0026] Furthermore, in step S4, during the purification and impurity removal of the filtrate, sodium hydroxide is first added to adjust the pH value to 11-12, then sodium carbonate is added, and finally solid-liquid separation is performed to collect the filtrate.
[0027] The beneficial effects of this invention are:
[0028] 1. In this invention, spodumene and a calcination aid are ball-milled, mixed, and activated before being subjected to low-temperature calcination at 850-950℃, reducing the calcination temperature to below 1000℃ and lowering calcination energy consumption. Simultaneously, the calcination aid of this invention can partially or completely utilize filter residue from another lithium extraction process, achieving resource reuse and helping to reduce production costs.
[0029] 2. Compared to the traditional sulfuric acid method for lithium extraction, which requires the addition of excess sulfuric acid (typically a molar ratio of approximately 1.4:1), the present invention uses a 1:1 molar ratio of lithium oxide to concentrated sulfuric acid in the roasted material, thus reducing the amount of concentrated sulfuric acid required. Furthermore, even with a low concentration of concentrated sulfuric acid, the lithium extraction rate of spodumene after low-temperature roasting and acid leaching remains consistently above 96%, demonstrating ultra-high lithium extraction efficiency.
[0030] 3. In this invention, the acidified leachate is compounded with concentrated mother liquor generated during another lithium extraction process. The concentration of potassium ions in the compounded solution is controlled at 5-8 g / L. After adding an appropriate amount of aluminum sulfate octadechydrate and freezing at low temperature, the compounding potassium removal technology removes most of the potassium ions from the lithium sulfate. The potassium removal process is simple and efficient. This potassium removal technology can also be used to treat mother liquor from the lithium salt production process of spodumene, and is particularly applicable to lithium extraction from lepidolite and brine. Furthermore, the mother liquor and filter residue after potassium removal in this invention can be reused, eliminating the waste treatment process and reducing harm to the natural environment.
[0031] 4. In this invention, potassium is removed by mixing concentrated mother liquor and leachate, thereby achieving the preparation of higher purity lithium carbonate, increasing the overall yield (from lithium concentrate to lithium carbonate product) to over 93%, and the battery-grade lithium carbonate ratio (the proportion of battery-grade lithium carbonate obtained to the total lithium carbonate obtained) to 100%.
[0032] 5. This invention significantly reduces the amount of acid used, by approximately 40%, resulting in low energy consumption, low cost, safety, and environmental friendliness. It does not introduce other impurities, yields high-quality lithium carbonate, and is highly efficient and can be quickly put into production. Furthermore, the method in this invention is not only applicable to the efficient lithium extraction from spodumene, but also provides inspiration for the efficient lithium extraction from lepidolite, lithium aluminum phosphate, and other materials. Attached Figure Description
[0033] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0034] Figure 1 This is a schematic flowchart of a method for low-temperature lithium extraction from spodumene with ultra-high yield, as illustrated in the examples. Detailed Implementation
[0035] The embodiments of the invention will now be described in detail with reference to the accompanying drawings.
[0036] A method for low-temperature lithium extraction from spodumene with ultra-high yield, the process is as follows: Figure 1 As shown in the figure. This method for low-temperature lithium extraction from spodumene with ultra-high yield includes the following steps:
[0037] Step S1: Spodumene and calcination aids are ball-milled and mixed, then calcined at a low temperature of 850-950℃, and cooled to obtain calcined material; wherein, another calcination aid returned during the lithium extraction process accounts for 0-100 wt% of the total weight of the calcination aids.
[0038] Step S2: Mix the calcined material obtained in step S1 with concentrated sulfuric acid and acidify it at 250~300℃ to obtain acid-cooked material; wherein, the molar ratio of lithium oxide to concentrated sulfuric acid in the calcined material is 1:1.
[0039] Step S3: The acid-cooked material obtained in step S2 is mixed with water and leached. During the leaching process, calcium oxide, calcium hydroxide or calcium carbonate is added to adjust the pH value of the system to 5.0~6.0. Solid-liquid separation is performed to obtain leachate and leachate residue. The weight ratio of acid-cooked material to water is 1:(2~3).
[0040] In step S4, the leachate obtained in step S3 is mixed with the mother liquor returned from another lithium extraction process. After adjusting the pH to 3-4, aluminum sulfate octadecylhydrate is added and the mixture is frozen at low temperature to separate the solid and liquid, obtaining filtrate and filter residue. The filtrate is then purified to remove impurities, yielding a lithium sulfate solution. The concentration of potassium ions in the mixed solution of leachate and mother liquor is 5-8 g / L, and the molar ratio of aluminum sulfate octadecylhydrate to potassium ions in the mixed solution is 0.5-3:1. The filter residue after solid-liquid separation is returned to step S1 of another lithium extraction process as a roasting aid.
[0041] Step S5: The lithium sulfate solution obtained in step S4 is mixed with sodium carbonate solution to precipitate lithium, and solid-liquid separation is performed to obtain crude lithium carbonate and filtrate; the crude lithium carbonate is stirred, washed, and dried to obtain battery-grade lithium carbonate; wherein, the filtrate after solid-liquid separation is evaporated and concentrated, and then solid-liquid separation is performed again, the separated filter residue is returned to step S1 of another lithium extraction process as a roasting aid, and the separated mother liquor is returned to step S4 of another lithium extraction process to be mixed with the leachate.
[0042] The following will illustrate this with more specific examples.
[0043] Example 1
[0044] 10 kg of low-grade lithium concentrate (lithium oxide content ≤ 5 wt%) was taken separately. The lithium concentrate, calcium oxide (newly added, not returned), and potassium sulfate (newly added, not returned) were ball-milled and mixed for 5 min according to the formula. Then, the mixture was calcined at 950℃ for 1 h to obtain calcined materials #1 to #5. The crystal transformation rate (from α phase to β phase) of the calcined materials was measured by a flame photometer, and the results are shown in Table 1.
[0045] Table 1 Crystal form conversion rate
[0046]
[0047] As shown in Table 2, after lithium concentrate is ball-milled and mixed with calcium oxide and potassium sulfate for activation, it can achieve crystal transformation at a roasting temperature below 1000℃. However, when lithium concentrate is roasted alone under the same conditions, the crystal transformation rate is only 40.4%, which is not valuable for industrial application.
[0048] Example 2
[0049] The No. 4 roasted material prepared in Example 1 was mixed with concentrated sulfuric acid (98wt%) according to the formula, and acidified at 300℃ for 30 min to obtain acid-cooked material. Then, the acid-cooked material was mixed with water according to the formula for leaching, and calcium carbonate was added during the leaching process to adjust the pH value of the system to 5.0~6.0 for rapid leaching. Finally, the mixture was filtered and separated, and the residue was washed to obtain No. 6~9 leaching solutions, leaching residue, and wash water, respectively. The lithium content (statistically based on lithium oxide) and lithium extraction rate in the leaching solution, leaching residue, and wash water are shown in Table 2.
[0050] Table 2 Lithium content and lithium extraction rate
[0051]
[0052] The data in the table shows that, on the one hand, a high lithium extraction rate is achieved when the molar ratio of lithium oxide to concentrated sulfuric acid in the calcined material is 1:1. On the other hand, in this embodiment, when the amount of concentrated sulfuric acid added increases from a molar ratio of lithium oxide to concentrated sulfuric acid in the calcined material from 1:1 to 1:1.4, the lithium extraction rate does not change significantly. This means that the method in this embodiment can reduce the amount of concentrated sulfuric acid used while still maintaining a high lithium extraction rate.
[0053] Example 3
[0054] Leachate No. 6 (potassium ion concentration of 0.041 g / L) was mixed with mother liquor returned from another lithium extraction process (potassium ion concentration of 26.00 g / L), and the pH was adjusted to 3-4. Then, aluminum sulfate octadecylhydrate was added, and the mixture was frozen at 0°C and filtered to obtain filtrate and filter residue. Sodium hydroxide was first added to the filtrate to adjust the pH to 11, and then sodium carbonate was added to remove impurities such as calcium, magnesium, aluminum, and iron. Finally, the mixture was filtered and the filtrate was collected to achieve purification and impurity removal, yielding lithium sulfate solutions No. 9-16. The lithium content (statistically based on lithium oxide) and potassium ion concentration of the lithium sulfate solutions are shown in Table 3.
[0055] Table 3. Lithium oxide concentration and potassium ion concentration of lithium sulfate solution
[0056]
[0057] The data in the table shows that the potassium content in the leachate is increased after the leachate is compounded with the mother liquor. After adding an appropriate amount of aluminum sulfate octahydrate to the compounded solution, the potassium ion concentration is reduced by freezing.
[0058] Example 4
[0059] Lithium sulfate solution (No. 14) was mixed with sodium carbonate solution (300 g / L, molar ratio of lithium sulfate to sodium carbonate 1:1.02) to precipitate lithium. The mixture was then filtered to obtain crude lithium carbonate and filtrate. The crude lithium carbonate was mixed with water at a weight ratio of 1:4, stirred, filtered, and dried to obtain battery-grade lithium carbonate. The purity of the lithium carbonate was above 99.5%, and the impurity indicators met the YS / T 582-2023 standard for battery-grade lithium carbonate. The overall yield was 93.5%.
[0060] Example 5
[0061] Take 1 kg of high-grade lithium concentrate (lithium oxide ≥ 6 wt%), and mix it with calcium carbonate and potassium aluminum sulfate (directly reuse the potassium-removing slag of aluminum sulfate octahydrate) in a ratio of 100:6:5. Then, calcine the mixture at 950℃ for 1 hour. The crystal conversion rate of the calcined material was measured to be 98.97% using a flame photometer.
[0062] The calcined feedstock contained lithium oxide in a 1:1 molar ratio of concentrated sulfuric acid. The feedstock was mixed with concentrated sulfuric acid (98 wt%) and acidified at 300°C for 30 minutes to obtain an acid-cooked feedstock. This acid-cooked feedstock was then leached with water at a solid-liquid ratio of 1:2.8. Calcium carbonate was added during the leaching process to adjust the pH to 6.0, and leaching was performed rapidly. The leaching was then separated by filtration and the residue was washed, yielding leachate, leachate residue, and wash water. The lithium extraction rates were calculated to be 96.53% (water test) and 96.13% (residue test) based on the lithium content (in terms of lithium oxide) in the leachate, wash water, and leaching residue.
[0063] The leachate (potassium ion concentration of 0.16 g / L) and the mother liquor returned from another lithium extraction process (potassium ion concentration of 20.4 g / L) were mixed together until the potassium ion concentration in the mixed solution was 8.2 g / L. The pH was adjusted to 3-4, and then aluminum sulfate octadecahydrate was added at a molar ratio of 1:1 to potassium ions in the mixed solution. The mixture was frozen at 0°C and filtered to obtain filtrate and filter residue. Sodium hydroxide was first added to the filtrate to adjust the pH to 11, and then sodium carbonate was added to remove impurities such as calcium, magnesium, aluminum, and iron. Finally, solid-liquid separation was performed, and the filtrate was collected to achieve purification and impurity removal, yielding a lithium sulfate solution. The lithium sulfate solution contained 5.3 g / L of lithium and potassium ions.
[0064] Lithium sulfate solution was mixed with sodium carbonate solution (300 g / L, molar ratio of lithium sulfate to sodium carbonate 1:1.02) to precipitate lithium, and the mixture was filtered to obtain crude lithium carbonate and filtrate. The crude lithium carbonate was mixed with water at a weight ratio of 1:4, stirred and washed, filtered, and dried to obtain battery-grade lithium carbonate. The purity of lithium carbonate was above 99.5%, and the impurity indicators met the YS / T 582-2023 standard for battery-grade lithium carbonate, with a comprehensive yield of 93.8%.
[0065] Example 6
[0066] Take 1 kg of high-grade lithium concentrate (lithium oxide ≥ 6 wt%), and mix it with calcium carbonate and potassium sulfate in a ratio of 100:6:0.5 by ball milling for 5 min. Then, calcine the mixture at 950℃ for 1 h. The crystal conversion rate of the calcined material was measured to be 98.75% by flame photometer.
[0067] The calcined feedstock contained lithium oxide in a 1:1 molar ratio of concentrated sulfuric acid. The feedstock was mixed with concentrated sulfuric acid (98 wt%) and acidified at 300°C for 30 minutes to obtain an acid-cooked feedstock. This acid-cooked feedstock was then leached with water at a solid-liquid ratio of 1:2.8. Calcium carbonate was added during the leaching process to adjust the pH to 6.0, and leaching was performed rapidly. The leaching was then separated by filtration and the residue was washed, yielding leachate, leachate residue, and wash water. The lithium extraction rates were calculated to be 98.5% (water test) and 97.57% (residue test) based on the lithium content (in terms of lithium oxide) in the leachate, wash water, and leaching residue.
Claims
1. A method for low-temperature lithium extraction from spodumene with ultra-high yield, characterized in that, Includes the following steps: Step S1: Spodumene and calcination aids are ball-milled and mixed, then calcined at a low temperature of 850-950℃, and cooled to obtain calcined material; wherein, another calcination aid returned during the lithium extraction process accounts for 0-100 wt% of the total weight of the calcination aids. Step S2: Mix the calcined material obtained in step S1 with concentrated sulfuric acid and acidify it at 250~300℃ to obtain acid-cooked material; wherein, the molar ratio of lithium oxide to concentrated sulfuric acid in the calcined material is 1:
1. Step S3: The acidified material obtained in step S2 is mixed with water and leached. During the leaching process, calcium oxide, calcium hydroxide or calcium carbonate is added to adjust the pH value of the system to 5.0~6.
0. Solid-liquid separation is performed to obtain leachate and leach residue. Step S4: The leachate obtained in step S3 is mixed with the mother liquor returned from another lithium extraction process, the pH is adjusted to 3-4, aluminum sulfate octadecylhydrate is added and then the mixture is frozen at low temperature to separate the solid and liquid, resulting in filtrate and filter residue. The filtrate is then purified to remove impurities, yielding a lithium sulfate solution. The concentration of potassium ions in the mixed solution of leachate and mother liquor is 5-8 g / L, and the molar ratio of aluminum sulfate octadecylhydrate to potassium ions in the mixed solution is 0.5-3:
1. The filter residue after solid-liquid separation is returned to step S1 of another lithium extraction process as a roasting aid. Step S5: The lithium sulfate solution obtained in step S4 is mixed with sodium carbonate solution to precipitate lithium, and solid-liquid separation is performed to obtain crude lithium carbonate and filtrate; the crude lithium carbonate is stirred, washed, and dried to obtain battery-grade lithium carbonate; wherein, the filtrate after solid-liquid separation is evaporated and concentrated, and then solid-liquid separation is performed again, the separated filter residue is returned to step S1 of another lithium extraction process as a roasting aid, and the separated mother liquor is returned to step S4 of another lithium extraction process to be mixed with the leachate.
2. The method for low-temperature lithium extraction from spodumene with ultra-high yield according to claim 1, characterized in that, The calcination aids in step S1 include alkaline earth metal oxides, alkaline earth metal hydroxides or carbonates, and sulfates.
3. The method for low-temperature lithium extraction from spodumene with ultra-high yield according to claim 2, characterized in that, In step S1, the weight ratio of spodumene, alkaline earth metal oxides, alkaline earth metal hydroxides or carbonates, and sulfates is 100:(4~20):(0.1~10).
4. The method for low-temperature lithium extraction from spodumene with ultra-high yield according to claim 2 or 3, characterized in that, The alkaline earth metal oxide is one or more of calcium oxide and magnesium oxide; The alkaline earth metal hydroxide is one or more of calcium hydroxide and magnesium hydroxide; The carbonate is one or more of calcium carbonate and magnesium carbonate; The sulfate is one or more of sodium sulfate, potassium sulfate, calcium sulfate, and potassium aluminum sulfate.
5. The method for low-temperature lithium extraction from spodumene with ultra-high yield according to claim 1, characterized in that, In step S3, the weight ratio of acidified material to water is 1:(2~3).
6. The method for low-temperature lithium extraction from spodumene with ultra-high yield according to claim 1, characterized in that, In step S1, the ball milling time for mixing spodumene and calcination aid is 2-10 minutes.
7. The method for low-temperature lithium extraction from spodumene with ultra-high yield according to claim 1, characterized in that, The roasting time during the low-temperature roasting transformation in step S1 is 1~5h.
8. The method for low-temperature lithium extraction from spodumene with ultra-high yield according to claim 1, characterized in that, The temperature during cryogenic freezing in step S4 is -4 to 8°C.
9. The method for low-temperature lithium extraction from spodumene with ultra-high yield according to claim 1, characterized in that, In step S4, the molar ratio of aluminum sulfate octahydrate to potassium ions in the compound solution is (0.8~1):
1.
10. The method for low-temperature lithium extraction from spodumene with ultra-high yield according to claim 1, characterized in that, In step S4, when purifying and removing impurities from the filtrate, sodium hydroxide is first added to adjust the pH value to 11-12, then sodium carbonate is added, and finally solid-liquid separation is performed to collect the filtrate.
Citation Information
Patent Citations
Methods for extracting lithium from spodumene ore and producing zeolite or nepheline as byproducts
CN109399672B
A method for lithium extraction from spodumene by secondary reverse leaching with nitric acid
CN114318008B
Method for efficiently and green leaching lithium from spodumene through external field strengthening
CN117887978A