A nickel-based powder superalloy and its preparation method
Nickel-based powder superalloys were prepared by using a low-Ta, low-Nb, low-Mo, and high-W composition design and a refined process. This solved the problem of insufficient performance and stability of superalloys at an operating temperature of 815℃ in existing technologies. It improved the high-temperature tensile properties, creep resistance, and microstructure stability, making it suitable for components such as turbine disks for aero-engines.
Patent Information
- Application Number
- CN202611370301.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-04
- Publication Date
- 2026-11-17
AI Technical Summary
Existing nickel-based powder superalloys struggle to simultaneously achieve excellent high-temperature tensile properties, creep resistance, and microstructure stability at a service temperature of 815℃. The addition of high Ta and high Nb elements in traditional designs leads to a tendency for topological close-packed phase precipitation, affecting microstructure stability and performance.
By employing a composition design with low Ta, low Nb, low Mo, and high W, and through precise control of the content and ratio of each element, combined with vacuum induction melting, argon atomization, hot isostatic pressing, hot extrusion, isothermal forging, and solution and aging heat treatment processes, a nickel-based powder superalloy was prepared, ensuring the stability of the γ' phase and the uniformity of the microstructure.
At an operating temperature of 815℃, the alloy exhibits excellent high-temperature tensile properties, creep resistance, and microstructural stability, making it suitable for key structural components under high-temperature and high-stress conditions, such as turbine disks for aero-engines, and providing a domestic alternative.
Smart Images

Figure CN123108358A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-temperature alloy technology, and in particular to a nickel-based powder high-temperature alloy and its preparation method. Background Technology
[0002] Nickel-based superalloys are core materials for hot-end components of aero-engines and gas turbines (such as turbine disks, turbine blades, and combustion chambers), accounting for nearly half of the engine's total mass. With the continuous increase in the thrust-to-weight ratio and service temperature of advanced aero-engines, increasingly stringent requirements are being placed on the heat resistance, high-temperature strength, and long-term microstructural stability of superalloys. Traditional cast and forged superalloys, due to inherent defects such as macroscopic segregation of alloying elements and inhomogeneous microstructure, cannot fully meet the service requirements of critical rotating components such as turbine disks in high thrust-to-weight ratio engines. Nickel-based powder metallurgy superalloys, prepared using powder metallurgy processes, can eliminate macroscopic segregation, obtain a fine and uniform grain structure, and possess excellent hot working properties, thus becoming the preferred material for manufacturing critical hot-end components such as turbine disks in advanced aero-engines.
[0003] After decades of development, multiple generations of nickel-based powder superalloy systems have been established both domestically and internationally. In my country, second-generation damage-tolerant powder superalloys, represented by FGH96 and FGH97, have achieved mass production. Europe and the United States have already put third-generation high-strength damage-tolerant alloys, represented by René104 (ME3), into large-scale production. my country's third-generation alloys, such as FGH98 and FGH99, are still in the research and development verification or early application stages. Driven by the demand for higher service temperatures, fourth-generation nickel-based powder superalloys are developing towards increasing operating temperatures. The United States has reported on the ME501 alloy in the ME5 series, while my country's corresponding fourth-generation alloys are still in the research and development stage and have not yet formed mature products and applications.
[0004] For service conditions above 800℃, the art has long generally accepted the need for a design strategy that incorporates high Ta, high Nb, or a high proportion of one of these elements. This strategy aims to enhance the high-temperature stability of the γ′ phase by increasing the total amount of these low-diffusion-coefficient elements, thereby ensuring high-temperature strength and creep resistance. However, during long-term high-temperature service, such high-content designs can also increase the tendency for precipitation of harmful topologically close-packed (TCP) phases, posing a potential risk to microstructure stability and performance maintenance. Furthermore, there is still room for further improvement in high-temperature creep resistance. Therefore, obtaining nickel-based powder superalloys that possess excellent high-temperature tensile properties, creep resistance, and microstructure stability at a service temperature of 815℃, thereby enriching the domestic independent product system of nickel-based powder superalloys, is a technical problem that needs to be solved. Summary of the Invention
[0005] The technical problem to be solved by this invention is how to obtain nickel-based powder superalloys that have excellent high-temperature tensile properties, creep resistance and microstructure stability at a service temperature of 815℃, and the method for efficiently and stably preparing the above-mentioned superalloys, so as to realize the manufacturing of key structural components under high temperature and high stress conditions such as aero-engine turbine disks and gas turbine hot end components, especially suitable for scenarios with stringent requirements for high temperature strength, creep resistance and microstructure stability, and enrich the domestic nickel-based powder superalloy product system.
[0006] To address the above problems, the present invention proposes the following technical solution: In a first aspect, the present invention provides a nickel-based powder superalloy, comprising, by weight percentage: Co: 16.0%–22.0%, Cr: 10.0%–14.0%, Mo: 2.0%–3.0%, W: 4.0%–6.0%, Al: 2.8%–4.0%, Ti: 2.8%–4.0%, Nb: 0.8%–1.8%, Ta: 1.0%–2.5%, Hf: 0.1%–0.3%, Zr: 0.01%–0.1%, C: 0.03%–0.08%, B: 0.02%–0.04%, with the balance being Ni and unavoidable impurities.
[0007] Furthermore, the total content of Al and Ti in the high-temperature alloy is 6.5% to 7.3%, the total content of Nb and Ta is 3.3% to 3.7%, and the total content of Mo and W is 6.7% to 7.7%.
[0008] Furthermore, the mass ratio of Nb to Ta is 3:4, the mass ratio of Mo to W is 1:2, and the mass ratio of Al to Ti is 1:1.
[0009] Furthermore, the high-temperature alloy has a γ' phase mass fraction of 50% to 60% at 800°C, and the complete dissolution temperature of the γ' phase is 1170°C to 1190°C.
[0010] Furthermore, by weight percentage, it includes: Co: 17.0%–20.0%, Cr: 11.0%–13.0%, Mo: 2.0%–2.8%, W: 4.4%–5.4%, Al: 3.1%–3.9%, Ti: 3.0%–3.8%, Nb: 1.2%–1.8%, Ta: 1.7%–2.3%, Hf: 0.15%–0.25%, Zr: 0.02%–0.08%, C: 0.03%–0.08%, B: 0.02%–0.04%, with the balance being Ni and unavoidable impurities.
[0011] Furthermore, by weight percentage, it includes: Co: 18.0%–19.0%, Cr: 11.5%–12.5%, Mo: 2.05%–2.55%, W: 4.65%–5.15%, Al: 3.3%–3.7%, Ti: 3.2%–3.6%, Nb: 1.4%–1.6%, Ta: 1.9%–2.1%, Hf: 0.17%–0.23%, Zr: 0.03%–0.07%, C: 0.04%–0.06%, B: 0.025%–0.035%, with the balance being Ni and unavoidable impurities.
[0012] Secondly, the present invention provides a method for preparing the aforementioned nickel-based powder superalloy, comprising the following steps: (1) Prepare raw materials according to the composition of the high-temperature alloy, and after vacuum induction melting, prepare nickel-based high-temperature alloy powder by argon atomization; (2) After vacuum sealing the high-temperature alloy powder obtained in step (1), hot isostatic pressing is performed to obtain a dense billet; (3) The dense billet obtained in step (2) is hot-extruded to obtain an extruded bar; then the extruded bar is isothermally forged to obtain a forging. (4) The forgings obtained in step (3) are subjected to solution heat treatment and aging heat treatment in sequence to obtain the nickel-based powder high-temperature alloy.
[0013] Furthermore, in step (2), the temperature of the hot isostatic pressing is 1130-1190℃, the pressure is 130-170MPa, and the holding time is 2-6 hours.
[0014] Further, in step (3), the hot extrusion temperature is 1080–1120℃, the extrusion speed is 25–45 mm / s, and the extrusion ratio is not less than 4.0; the isothermal forging temperature is 1070–1120℃, and the strain rate is 0.001–0.01 s. -1 .
[0015] Further, in step (4), the temperature of the solution heat treatment is 1180±30℃ and the holding time is 2 to 8 hours; the aging heat treatment is: holding at 750 to 850℃ for 4 to 10 hours; or graded aging is adopted: holding at 820 to 860℃ for 2 hours, and then holding at 740 to 780℃ for 8 hours.
[0016] Furthermore, in step (4), the solution heat treatment is followed by inert gas cooling, air cooling, or oil cooling.
[0017] Furthermore, the hot-end component is a turbine disk.
[0018] Thirdly, the present invention provides a hot-end component for an aero-engine or gas turbine, the component being made of the nickel-based powder high-temperature alloy described in the first aspect.
[0019] Compared with the prior art, the technical effects achieved by the present invention include: The nickel-based powder superalloy provided by this invention achieves its benefits through precise control of the content range of each element, focusing on optimizing the proportion of low Ta, the synergistic ratio of (Al+Ti) and (Nb+Ta), and the mass ratio and total proportion of Mo and W. In this compositional system, the high W content utilizes the low high-temperature diffusion coefficient of tungsten to suppress atomic diffusion and dislocation climb, hindering grain boundary slip and dislocation movement, effectively enhancing the alloy's high-temperature creep resistance. The low Mo content reduces the precipitation tendency of topologically close-packed phases during long-term high-temperature service, providing compositional assurance for the alloy's microstructure stability. Simultaneously, by controlling the mass ratio of Al and Ti and the total amount of Al+Ti, the alloy possesses sufficient γ' phase volume fraction and suitable γ / γ' phase mismatch at 800℃, compensating for the potential impact of low Nb and low Ta additions on precipitation strengthening effects. The synergistic effect of the above elements enables the alloy to have both excellent high-temperature tensile properties and creep resistance at a service temperature of 815℃, and to maintain the stability of the morphology and size of the γ' phase under long-term high-temperature heat exposure conditions, with no obvious harmful phase precipitation at the grain boundaries, exhibiting good microstructure stability.
[0020] The preparation method provided by this invention employs a process route combining vacuum induction melting with argon atomization powdering, hot isostatic pressing densification, hot extrusion, isothermal forging, and solution and aging heat treatment, which matches the alloy's compositional characteristics of low Ta, low Nb, low Mo, and high W. The combined hot extrusion and isothermal forging process effectively breaks down the original particle boundaries, eliminates internal metallurgical defects, and yields a billet microstructure with uniform and fine grains. Subsequent solution and aging heat treatment can effectively control the precipitation size, morphology, and distribution of the γ' phase. This preparation method has a clear process path, is efficient and easy to implement, has good reproducibility, can effectively control the uniformity of the alloy's microstructure, avoids the precipitation of harmful phases, and further improves the alloy's service reliability.
[0021] The nickel-based powder superalloy provided by this invention is suitable for key structural components under high-temperature and high-stress conditions, such as turbine disks of aero-engines and hot-end components of gas turbines. It can serve as a domestic alternative to imported advanced nickel-based powder superalloys such as ME501. This superalloy exhibits excellent comprehensive mechanical properties at 815℃, providing a high-performance, domestically controllable material option for nickel-based powder superalloys used in hot-end components of high-end equipment, and has promising engineering application prospects. Attached Figure Description
[0022] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the following description of the embodiments will be briefly introduced. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1 This is a schematic flowchart of the method for preparing nickel-based powder superalloys according to the present invention.
[0024] Figure 2 The image shows a metallographic photograph of the nickel-based powder superalloy of Example 1 of the present invention, which shows the grain morphology of the alloy after solution treatment and aging heat treatment.
[0025] Figure 3 The image shown is a metallographic photograph of the nickel-based powder superalloy of Example 2 of the present invention, showing the grain morphology of the alloy after increasing the solid solution cooling rate.
[0026] Figure 4 This is a SEM image of the nickel-based powder superalloy of Example 1 of the present invention, showing the size and distribution characteristics of the γ' phase.
[0027] Figure 5 The image shown is an SEM image of the nickel-based powder superalloy of Example 2 of the present invention, showing the fine γ' phase morphology obtained after increasing the solid solution cooling rate.
[0028] Figure 6 The image shown is a SEM image of the nickel-based powder superalloy of Example 1 of the present invention after being kept at 750°C for 500 hours, showing the morphology retention of the γ' phase under thermal exposure conditions.
[0029] Figure 7 The image shown is a SEM image of the nickel-based powder superalloy of Example 2 of the present invention after being kept at 815°C for 900 hours, showing the morphology retention of the γ' phase under higher temperature and longer heat exposure conditions. Detailed Implementation
[0030] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0031] It should be understood that, when used in this specification and the appended claims, the terms "comprising" and "including" indicate the presence of the described features, integrals, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integrals, steps, operations, elements, components and / or collections thereof.
[0032] It should also be understood that the terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the invention. As used in this specification and the appended claims, the singular forms “a,” “an,” and “the” are intended to include the plural forms unless the context clearly indicates otherwise.
[0033] It should also be further understood that the term "and / or" as used in this specification and the appended claims refers to any combination of one or more of the associated listed items and all possible combinations, and includes such combinations.
[0034] To address the challenge of existing nickel-based powder superalloys failing to simultaneously achieve high-temperature tensile properties, creep resistance, and long-term microstructural stability at an operating temperature of 815°C, this invention provides a nickel-based powder superalloy composed of a nickel (Ni) matrix and alloying elements such as cobalt (Co), chromium (Cr), molybdenum (Mo), tungsten (W), aluminum (Al), titanium (Ti), niobium (Nb), tantalum (Ta), hafnium (Hf), zirconium (Zr), carbon (C), and boron (B), as well as unavoidable impurities. The alloy's composition is designed with low Ta, low Nb, low Mo, and high W as core characteristics. Through the synergistic effect of these elements, the alloy exhibits excellent high-temperature tensile properties, creep resistance, and microstructural stability at an operating temperature of 815°C. The specific compositional elements and their ranges are described below.
[0035] In practice, nickel (Ni), as the matrix element of high-temperature alloys, has a face-centered cubic austenitic structure, which can stably dissolve various alloying elements and maintain high structural stability at high temperatures, providing the alloy with basic plasticity, toughness, and high-temperature load-bearing capacity. The amount of Ni is determined based on the total amount of other alloying elements added, and the balance is made up to 100% while ensuring a reasonable ratio of each element.
[0036] In specific implementations, the cobalt (Co) content is 16.0%–22.0% by mass percentage. Co plays multiple roles in the nickel-based superalloy of this invention. First, an appropriate amount of Co can expand the austenite phase region, offset the phase transformation tendency that may be caused by high W content, suppress the precipitation of harmful phases such as topologically close-packed (TCP), and maintain the stability of the microstructure during long-term high-temperature service. Second, Co can produce a solid solution strengthening effect when dissolved in the γ matrix. Third, Co can regulate the stacking fault energy of the matrix, hinder dislocation cross-slip, thereby improving the strength and creep resistance of the alloy. Fourth, Co can regulate the mismatch degree of the γ / γ' phases, achieving a reasonable balance between the strain strengthening effect of the coherent interface and the stability of the microstructure. When the Co content is below 16.0%, the effect of expanding the austenite phase region is limited, making it difficult to fully offset the TCP phase precipitation tendency caused by high W content, and the effect on reducing stacking fault energy is insufficient; when the Co content is above 22.0%, it increases the precipitation tendency of harmful phases. Preferably, the Co content is 17.0% to 20.0%. More preferably, the Co content is 18.0% to 19.0%. For example, the Co content can be 16.0%, 17.5%, 18.6%, 19.4%, 20.8%, or 22.0%.
[0037] In specific implementations, the chromium (Cr) content is 10.0%–14.0% by mass percentage. Cr is mainly enriched in the γ matrix, and at high temperatures, it can form a dense chromium oxide protective film, improving the alloy's resistance to high-temperature oxidation and hot corrosion. Simultaneously, the atomic radius of Cr differs somewhat from that of Ni, and after dissolving in the matrix, it can cause lattice distortion, playing a role in solid solution strengthening. When the Cr content is below 10.0%, the oxidation and corrosion resistance are insufficient to meet the long-term service requirements at 815℃; when the Cr content is above 14.0%, it promotes the precipitation of σ phase and other TCP phases, impairing the microstructure stability and mechanical properties. Preferably, the Cr content is 11.0%–13.0%. More preferably, the Cr content is 11.5%–12.5%. For example, the Cr content can be 10.0%, 11.2%, 11.8%, 12.4%, 13.1%, or 14.0%.
[0038] In specific implementation, the molybdenum (Mo) content is 2.0%–3.0% by mass percentage, and the tungsten (W) content is 4.0%–6.0%. Mo and W are the main solid solution strengthening elements in the high-temperature alloy of this invention. Both have atomic radii larger than Ni, and their solid solution in the γ matrix can cause significant lattice distortion, hindering dislocation movement and improving the high-temperature strength of the alloy. This scheme adopts a low-Mo, high-W design concept. W has a lower high-temperature diffusion coefficient than Mo, which can more effectively hinder element diffusion and dislocation climb during high-temperature creep, improving the high-temperature creep resistance of the alloy; the Mo content is controlled at a low level to reduce the tendency of TCP phase precipitation, which is beneficial to the long-term microstructure stability at high temperatures. When the Mo content is below 2.0%, the solid solution strengthening effect is insufficient; when the Mo content is above 3.0%, the risk of TCP phase precipitation increases. When the W content is below 4.0%, the improvement in high-temperature creep resistance is not significant; when the W content is above 6.0%, it will significantly reduce the plasticity of the alloy and may promote the formation of harmful phases. Preferably, the Mo content is 2.0% to 2.8%, and the W content is 4.4% to 5.4%. More preferably, the Mo content is 2.05% to 2.55%, and the W content is 4.65% to 5.15%. For example, the Mo content can be 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, or 3.0%. For example, the W content can be 4.0%, 4.5%, 4.9%, 5.2%, 5.7%, or 6.0%.
[0039] In this invention, the mass ratio of Mo to W must be 1:2. This ratio ensures that the solid solution strengthening effect is dominated by W, fully leveraging W's role in enhancing high-temperature creep resistance, while a suitable amount of Mo supplements the solid solution strengthening effect, avoiding the risk of tissue instability caused by excessive Mo content. Furthermore, the total content of Mo and W is controlled at 6.7%–7.7%, within which a reasonable balance is achieved between the solid solution strengthening effect, plasticity, and tissue stability.
[0040] In specific implementation, the aluminum (Al) content is 2.8%–4.0% by mass percentage, and the titanium (Ti) content is 2.8%–4.0%. Al and Ti are the core forming elements of the γ' phase. They combine with Ni to form Ni3(Al,Ti) type precipitation strengthening phases with an L12 ordered structure, which are the main sources of strength for high-temperature alloys. Al can significantly increase the volume fraction of the γ' phase, while Ti can increase the lattice mismatch of the γ / γ' phase, enhance the coherent strain strengthening effect, and improve the high-temperature stability of the γ' phase. This scheme ensures sufficient γ' phase content and high-temperature stability through a reasonable ratio of Al to Ti, without relying on the addition of high Nb or high Ta. When the Al or Ti content is below 2.8%, the volume fraction of the γ' phase is insufficient, and the precipitation strengthening effect decreases; when the Al or Ti content is above 4.0%, the complete dissolution temperature of the γ' phase is too high, which will crowd out the solution heat treatment process window and may reduce the hot working plasticity of the alloy. Preferably, the Al content is 3.1% to 3.9%, and the Ti content is 3.0% to 3.8%. More preferably, the Al content is 3.3% to 3.7%, and the Ti content is 3.2% to 3.6%. For example, the Al content can be 2.8%, 3.1%, 3.5%, 3.7%, 3.9%, or 4.0%. For example, the Ti content can be 2.8%, 3.0%, 3.3%, 3.6%, 3.8%, or 4.0%.
[0041] In practice, the mass ratio of Al to Ti must be 1:1. This ratio optimizes the lattice parameters of the γ' phase and controls the γ / γ' phase mismatch within a suitable range. This provides sufficient coherent strengthening effect while avoiding accelerated coarsening of the γ' phase at high temperatures due to excessive mismatch, thus balancing the strength and microstructure stability of the alloy. Simultaneously, the total content of Al and Ti is controlled at 6.5%–7.3%. Under this total content, the mass fraction of the γ' phase at 800℃ can reach 50%–60%, and the complete dissolution temperature of the γ' phase can be controlled at 1170℃–1190℃. This ensures precipitation strengthening while providing a reasonable operating temperature range for solution heat treatment.
[0042] In specific implementations, the niobium (Nb) content is 0.8%–1.8% by mass, and the tantalum (Ta) content is 1.0%–2.5% by mass. Both Nb and Ta can act as γ' phase forming elements, partially replacing Al and Ti positions in the γ' phase unit cell. Simultaneously, their low high-temperature diffusion rates, upon entering the γ' phase, effectively improve the high-temperature stability of the precipitated phase. This invention breaks with conventional understanding, adopting a low-Nb, low-Ta design approach. By precisely controlling the mass ratio and total amount of these two elements, combined with the synergistic effect of other elements such as Al, Ti, Mo, and W, excellent high-temperature performance at 815℃ is achieved while ensuring the high-temperature stability of the γ' phase. When the Nb content is below 0.8%, its contribution to the stability of the γ' phase is insufficient; when the Nb content is above 1.8%, incompletely dissolved primary carbides or intermetallic compounds may form. When the Ta content is below 1.0%, its effect on improving the high-temperature stability of the γ' phase is limited; when the Ta content is above 2.5%, the cost of the high-temperature alloy increases without a significant performance improvement. Preferably, the Nb content is 1.2% to 1.8%, and the Ta content is 1.7% to 2.3%. More preferably, the Nb content is 1.4% to 1.6%, and the Ta content is 1.9% to 2.1%. For example, the Nb content can be 0.8%, 1.0%, 1.3%, 1.5%, 1.7%, or 1.8%. For example, the Ta content can be 1.0%, 1.5%, 1.9%, 2.1%, 2.4%, or 2.5%.
[0043] In practice, the mass ratio of Nb to Ta must be 3:4. This ratio ensures that the two low-diffusion-rate γ' phase-forming elements achieve a reasonable atomic occupancy in the precipitation-strengthening phase, synergistically improving the high-temperature stability of the γ' phase and compensating for the potential impact of low Nb and low Ta total content design on high-temperature performance. Simultaneously, the total content of Nb and Ta is controlled at 3.3%–3.7%, matching the total content of Al and Ti, ensuring a reasonable overall ratio of γ' phase-forming elements and balancing high-temperature strength and microstructure stability.
[0044] In specific implementations, the hafnium (Hf) content is 0.1% to 0.3% by mass. Hf is a strong carbide-forming element, mainly forming dispersed MC-type carbides in high-temperature alloys. This effectively pins grain boundaries, inhibits excessive grain growth at high temperatures, and improves the high-temperature creep resistance of the alloy. Simultaneously, Hf can improve the morphology of grain boundary carbides, transforming them from continuous thin films to granular forms, increasing grain boundary bonding strength, and delaying the initiation of grain boundary cracks. When the Hf content is below 0.1%, the grain boundary pinning effect is not significant; when the Hf content is above 0.3%, large bulk primary carbides may form, impairing the fatigue performance of the alloy. Preferably, the Hf content is 0.15% to 0.25%. More preferably, the Hf content is 0.17% to 0.23%. For example, the Hf content can be 0.10%, 0.15%, 0.18%, 0.21%, 0.24%, or 0.30%.
[0045] In specific implementations, the zirconium (Zr) content is 0.01% to 0.1% by mass. Zr mainly segregates in grain boundary regions, which can improve grain boundary conditions, increase grain boundary strength and bonding force, delay the formation of grain boundary voids and crack propagation at high temperatures, and positively contribute to the high-temperature creep resistance and anti-creep properties of the alloy. When the Zr content is below 0.01%, the grain boundary strengthening effect is insufficient; when the Zr content is above 0.1%, it may reduce the initial melting temperature of the alloy and narrow the heat treatment process window. Preferably, the Zr content is 0.02% to 0.08%. More preferably, the Zr content is 0.03% to 0.07%. For example, the Zr content can be 0.01%, 0.03%, 0.05%, 0.06%, 0.08%, or 0.10%.
[0046] In specific implementations, the carbon (C) content is 0.03% to 0.08% by mass percentage. C combines with strong carbide-forming elements such as Hf, Ti, and Nb in the alloy, precipitating fine, dispersed MC-type carbides at grain boundaries and within grains. Carbides at grain boundaries effectively pin the grain boundaries, inhibiting grain growth at high temperatures; carbides within grains hinder dislocation movement, improving alloy strength. When the C content is below 0.03%, the amount of carbides is insufficient to effectively control grain size; when the C content is above 0.08%, excessive carbides may form or be distributed in a chain-like pattern along grain boundaries, reducing the plasticity and fatigue properties of the high-temperature alloy. Preferably, the C content is 0.04% to 0.06%. For example, the C content can be 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, or 0.08%.
[0047] In specific implementation, the boron (B) content is 0.02% to 0.04% by mass percentage. B mainly segregates at grain boundaries, filling vacancies and reducing element diffusion rates at grain boundaries. This inhibits grain boundary slip and void formation at high temperatures, significantly improving the alloy's high-temperature creep resistance and stability. When the B content is below 0.02%, the grain boundary strengthening effect is not significant; when the B content is above 0.04%, low-melting-point boride eutectic phases may form at grain boundaries, lowering the initial melting temperature of the high-temperature alloy and hindering subsequent hot working and heat treatment processes. Preferably, the B content is 0.025% to 0.035%. For example, the B content can be 0.020%, 0.025%, 0.029%, 0.032%, 0.036%, or 0.040%.
[0048] It should be noted that the unavoidable impurities in the aforementioned high-temperature alloys refer to trace amounts of unintentionally added elements introduced from raw materials or carried over from the process during the high-temperature alloy smelting and powdering. These mainly include oxygen (O), nitrogen (N), sulfur (S), phosphorus (P), silicon (Si), and manganese (Mn). In nickel-based powder superalloys, the oxygen content has a particularly significant impact on the mechanical properties of the superalloy. Excessive oxygen content can form oxide inclusions in the superalloy, becoming a source of fatigue crack initiation and reducing the low-cycle fatigue life of the superalloy. Therefore, the content of each impurity element must be strictly controlled. By mass percentage, the total content of unavoidable impurities in the superalloy should not exceed 0.15%, and the content of any single impurity element should not exceed 0.03%.
[0049] See Figure 1 This is a schematic flowchart of the preparation method of the nickel-based powder superalloy of the present invention, which includes the following steps: (1) Prepare raw materials according to the composition of high-temperature alloys, and after vacuum induction melting, prepare nickel-based high-temperature alloy powder by argon atomization.
[0050] In specific implementation, step (1) can be carried out by vacuum induction melting process to melt the raw materials, so that the alloying elements can be fully fused in a vacuum environment to obtain a uniformly composed master alloy melt. Then, argon atomization process is used to atomize the master alloy melt with high-purity argon as the atomization medium to obtain nickel-based high-temperature alloy powder. The particle size of the powder is controlled to be -270 mesh, that is, the particle size is not greater than 53μm.
[0051] (2) After vacuum sealing the alloy powder obtained in step (1), hot isostatic pressing is performed to obtain a dense blank.
[0052] In specific implementation, the alloy powder obtained in step (1) is packed into a casing and subjected to vacuum degassing and sealing treatment to remove the gas adsorbed on the surface of the powder particles and the residual gas in the casing, so as to avoid the formation of oxide inclusions or thermally induced pores during the subsequent high-temperature forming process. The packaged casing is then subjected to hot isostatic pressing, so that the powder particles are sintered and densified under the combined action of high temperature and isotropic static pressure to obtain a dense billet.
[0053] The hot isostatic pressing (HIP) of this invention is performed at a temperature of 1130–1190°C, a pressure of 130–170 MPa, and a holding time of 2–6 hours. After holding, the material is cooled to room temperature in the furnace. When the temperature is below 1130°C or the pressure is below 130 MPa, the metallurgical bonding between powder particles is insufficient, and residual pores may exist inside the billet. When the temperature is above 1190°C, excessive grain growth may occur, which is not conducive to the refinement of the microstructure during subsequent hot working. Preferably, the HIP temperature is 1140–1170°C, the pressure is 140–160 MPa, and the holding time is 3–5 hours. For example, the hot isostatic pressing temperature can be 1130℃, 1145℃, 1150℃, 1165℃, 1180℃ or 1190℃; the pressure can be 130MPa, 140MPa, 150MPa, 155MPa, 165MPa or 170MPa; and the holding time can be 2h, 3h, 4h, 5h or 6h.
[0054] (3) The dense billet obtained in step (2) is hot-extruded to obtain an extruded bar; then the extruded bar is isothermally forged to obtain a forging.
[0055] In practice, the dense billet obtained in step (2) is first hot-extruded to obtain extruded bars. The hot extrusion process can apply large plastic deformation to the hot isostatic pressing billet, effectively breaking the original powder particle boundaries, and at the same time, a billet structure with uniform and fine grains is obtained through dynamic recrystallization during the deformation process.
[0056] The extruded bars are then subjected to isothermal forging to obtain forgings. Isothermal forging is a forging deformation performed under the condition that the billet temperature remains constant, which further optimizes the grain structure, improves the density and uniformity of the material, and reduces the differences in mechanical properties between different parts of the forging.
[0057] In this invention, the hot extrusion temperature is 1080–1120°C, the extrusion speed is 25–45 mm / s, and the extrusion ratio is not less than 4.0. When the extrusion temperature is below 1080°C, the alloy's deformation resistance is too high, making extrusion difficult; when the extrusion temperature is above 1120°C, recrystallized grains tend to grow, which is not conducive to microstructure refinement. When the extrusion ratio is less than 4.0, the deformation is insufficient to fully break down the original grain boundaries. Preferably, the hot extrusion temperature is 1090–1110°C, the extrusion speed is 30–40 mm / s, and the extrusion ratio is 4.0–6.0. For example, the hot extrusion temperature can be 1080°C, 1090°C, 1100°C, 1110°C, or 1120°C; the extrusion speed can be 25 mm / s, 30 mm / s, 35 mm / s, 40 mm / s, or 45 mm / s; and the extrusion ratio can be 4.0, 4.5, 4.7, 5.0, 5.5, or 6.0.
[0058] In this invention, the isothermal forging temperature is 1070–1120℃, and the strain rate is 0.001–0.01 s. -1 When the forging temperature is below 1070℃, the alloy lacks sufficient plasticity and is prone to forging cracks; when the forging temperature is above 1120℃, grains tend to grow during forging and subsequent cooling. When the strain rate is below 0.001s... -1 At times, the equipment capacity requirements are too high; when the strain rate exceeds 0.01s... -1 During this process, the deformation heat effect is significant, which may lead to localized temperature rise and abnormal grain growth. Preferably, the isothermal forging temperature is 1090–1110℃, and the strain rate is 0.002–0.008 s⁻¹. -1 For example, the isothermal forging temperature can be 1070℃, 1090℃, 1100℃, 1110℃, or 1120℃; the strain rate can be 0.001s. -1 0.003s -1 0.005s -1 0.007s -1 or 0.010s -1 .
[0059] (4) The forging obtained in step (3) is subjected to solution heat treatment and aging heat treatment to obtain the nickel-based powder high-temperature alloy.
[0060] In specific implementation, the forgings obtained in step (3) are subjected to solution heat treatment and aging heat treatment in sequence. The purpose of solution heat treatment is to redissolve the γ' phase and some carbides in the alloy into the γ matrix to obtain a uniform supersaturated solid solution, which provides microstructure conditions for the full precipitation and reasonable distribution of the γ' phase in the subsequent aging treatment. The solution heat treatment temperature is 1180±30℃, the holding time is 2 to 8 hours, and after holding, it is cooled to room temperature at an appropriate cooling rate. This solution temperature range is above the complete dissolution temperature of the alloy γ' phase, which can ensure that the γ' phase is fully re-dissolved, while avoiding grain coarsening caused by excessive temperature. When the solution temperature is below 1150℃, the γ' phase is not fully re-dissolved, and the undissolved γ' phase remaining in the matrix will affect the uniformity of the precipitated phase after aging treatment; when the solution temperature is above 1210℃, the grain growth trend is obvious, and it may be close to the initial melting temperature of the alloy, which poses a risk of overheating. Preferably, the solution heat treatment temperature is 1180–1190°C, and the holding time is 3–5 hours. For example, the solution heat treatment temperature can be 1150°C, 1160°C, 1175°C, 1185°C, 1195°C, or 1210°C; the holding time can be 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, or 8 hours.
[0061] The purpose of aging heat treatment is to precipitate fine, dispersed, and appropriately sized γ' phases in supersaturated solid solutions, thereby enhancing precipitation strengthening. Simultaneously, aging heat treatment can partially eliminate residual stress caused by material deformation. Aging heat treatment can be performed at 750–850℃ for 4–10 hours; or a staged aging process can be used, first holding at 820–860℃ for 2 hours, then at 740–780℃ for 8 hours. The staged aging process first holds at a higher temperature for a shorter time, allowing the γ' phase to nucleate and initially grow rapidly, followed by holding at a lower temperature for a longer time, allowing the γ' phase to further precipitate and reach a stable size and morphology, ultimately obtaining a γ' phase microstructure of moderate size and uniform distribution. When the aging temperature is below 750℃, the amount of supplemented γ' phase precipitated is small, and its size is too small, making it difficult to reduce residual stress; when the aging temperature is above 850℃, prolonged holding can easily cause excessive growth of the γ' phase, reducing the strengthening effect. Preferably, the temperature for single aging is 800–830℃, and the holding time is 6–8 hours; the process for staged aging involves holding at 830–850℃ for 2 hours, followed by holding at 760–780℃ for 8 hours. For example, the temperature for single aging can be 750℃, 780℃, 800℃, 815℃, 830℃, or 850℃, and the holding time can be 4h, 6h, 8h, or 10h; the high-temperature stage temperature for staged aging can be 820℃, 830℃, 845℃, or 860℃, and the low-temperature stage temperature can be 740℃, 755℃, 770℃, or 780℃.
[0062] The present invention will be further illustrated below through specific embodiments and comparative examples. The raw materials used in the embodiments are all commercially available high-purity metals. The smelting, powdering, forming, extrusion, forging, and heat treatment of the alloys were all performed according to the aforementioned process steps. The resulting alloy samples were characterized by their microstructure and tested for their mechanical properties according to the corresponding standard methods.
[0063] Example 1 The alloy composition of this embodiment, by mass percentage, is as follows: Co 18.67%, Cr 11.72%, Mo 2.35%, W 4.88%, Al 3.62%, Ti 3.35%, Nb 1.57%, Ta 2.09%, Hf 0.21%, Zr 0.048%, C 0.046%, B 0.029%, with the balance being Ni and unavoidable impurities. The total impurity content is ≤0.15%, and the content of a single impurity element is ≤0.03%.
[0064] The preparation process is as follows: Step (1): Prepare metal raw materials according to the above composition, and after vacuum induction melting, use argon atomization to produce alloy powder with a particle size of -270 mesh (particle size ≤53μm).
[0065] Step (2): The obtained powder is put into a sleeve, vacuum degassed and then sealed. Then it is hot isostatic pressing is performed at a temperature of 1150±5℃, a pressure of 150MPa, and a holding time of 4h. It is then cooled to room temperature in the furnace to obtain a dense billet.
[0066] Step (3): The dense billet is hot-extruded at an extrusion temperature of 1100±5℃, an extrusion ratio of 4.7, and an extrusion speed of 30±5mm / s to obtain extruded bars. The extruded bars are then isothermally forged at an isothermal forging temperature of 1110±5℃ and a strain rate of 0.002~0.008s. - ¹, with a total pressing amount of 60% to 75%, a forging is obtained.
[0067] Step (4): Samples were taken from the forgings for heat treatment. Solution heat treatment was performed in a vacuum quenching furnace at a temperature of 1185±5℃, held for 4 hours, and then cooled with a gas pressure of 4 bar. Aging heat treatment was performed at a temperature of 815±5℃, held for 8 hours, and then cooled with a gas pressure of 4 bar.
[0068] Example 2 The alloy composition in this embodiment is the same as that in Example 1.
[0069] Steps (1) to (3) of the preparation process are the same as in Example 1. The difference lies in the heat treatment regime of step (4): the solution heat treatment is carried out in a muffle furnace at a temperature of 1205±5℃, held for 4 hours and then air-cooled; the aging heat treatment is carried out at a temperature of 815±5℃, held for 8 hours and then air-cooled. Compared with Example 1, the cooling rate after solution treatment in this example is significantly improved.
[0070] The alloys prepared in Examples 1 (1#) and 2 (2#) were subjected to microstructure observation, room temperature and high temperature tensile property testing, high temperature creep and endurance testing, low cycle fatigue performance testing, and high temperature long-term microstructure stability evaluation, respectively. The test results are listed in Table 1, and the corresponding microstructure photographs are attached. Figures 2 to 7 .
[0071] Table 1 Performance test results of Example 1 and Example 2
[0072] As can be seen from Table 1 and the accompanying figures, the alloys of Example 1 and Example 2, under the same composition conditions, exhibit differences in performance due to different heat treatment regimes. Regarding microstructure, the average grain size of Example 1 is ASTM grade 8 (…). Figure 2 The average grain size of Example 2 was ASTM grade 6.8. Figure 3 The two have slightly different grain sizes. A more significant difference lies in the size of the γ' phase, such as... Figure 4 (Example 1) and Figure 5 As shown in Example 2, due to the faster cooling rate after solution treatment, the precipitated γ' phase in Example 2 is finer and more dispersed than that in Example 1. In terms of tensile properties, the yield strength and tensile strength of Example 2 at all temperatures are slightly higher than those of Example 1, indicating that the finer γ' phase provides a higher contribution to precipitation strengthening. The improvement in creep and rupture properties is particularly significant in Example 2. At 815℃ / 345MPa, the 0.2% creep time of Example 2 is 472h, more than 3.5 times that of Example 1 (133h); the rupture life is 913h, nearly 70% higher than that of Example 1 (544h). This difference indicates that a faster solution cooling rate allows the γ' phase to precipitate in a finer and more dispersed form after aging treatment. The finer γ' phase can more effectively hinder dislocation climb and bypass during high-temperature creep, thereby significantly improving the alloy's creep resistance and rupture life. Regarding fatigue performance, the fatigue life of Example 1 was higher than that of Example 2, indicating that the microstructure obtained by a slower cooling rate has certain advantages under low-cycle fatigue conditions. Regarding microstructure stability, such as... Figure 6 and Figure 7 As shown, in Example 1, the morphology of the γ' phase remained stable after being held at 750℃ for 500 hours. In Example 2, the γ' phase remained spherical and showed no obvious coarsening after being held at 815℃ for 900 hours, indicating that the alloys under both process routes have good high-temperature structural stability.
[0073] The above comparison shows that, under the high-temperature alloy composition system of this invention, the precipitation characteristics of the γ' phase can be controlled by adjusting the cooling rate after solution heat treatment, according to the performance emphasis under the target service conditions, thereby optimizing the overall performance of the alloy. Slower cooling rates are beneficial to fatigue performance, while faster cooling rates can significantly improve creep resistance and rupture life.
[0074] To further illustrate the differences in composition design and performance between the nickel-based powder superalloy of the present invention and existing nickel-based powder superalloys, the alloy composition of the embodiments of the present invention is compared and analyzed with several published third-generation and fourth-generation nickel-based powder superalloys (Tables 2 and 3). The composition data of the comparative examples are from published literature (Wang Jie, Liu Zhiling, Jia Jian, et al. Research progress and development trend of powder superalloys [J], Powder Metallurgy Materials Science and Engineering, 2025, 30(6): 471-487).
[0075] Table 2. Comparison of the composition of the embodiments of the present invention and typical third-generation powder superalloys (wt.%)
[0076] As can be seen from Table 2, the embodiment of the present invention adopts a composition design scheme with low Nb, low Ta, low Mo, high W and combined with total Al+Ti control, which is fundamentally different from the key element ratios of typical third-generation powder superalloys.
[0077] Compared with Rene104 (ME3), Rene104 adopts a high Mo and low W design concept, with a Mo / W ratio of 2:1, which is completely opposite to the low Mo and high W design of this invention with a Mo / W ratio of about 1:2. At the same time, the Nb / Ta ratio of Rene104 is only 0.52:1, and the Ta content is much higher than that of this invention. The two composition systems are fundamentally different.
[0078] Compared to Alloy10, Alloy10 is the closest alloy to the concept of this invention, but their core designs differ fundamentally. In terms of elemental composition, Alloy10 uses a high Nb, low Ta ratio, with an Nb / Ta ratio of 2:1, while the Nb / Ta ratio of this invention is 0.75:1. Simultaneously, Alloy10 has a Ti content of only 1.8%, resulting in an Al / Ti ratio of 2.1:1, significantly different from the approximately 1:1 Al / Ti ratio of this invention. Regarding microstructure stability, Alloy10 has a low Co content, making it difficult to fully offset the phase transformation tendency caused by elements such as W and Mo, making it more prone to microstructure instability during long-term high-temperature service. Furthermore, its overall content of γ' phase stabilizing elements such as Ti, Nb, and Ta is low, leading to insufficient high-temperature stability of the γ' phase.
[0079] Compared to LSHR, LSHR has a Mo / W ratio of 0.63:1, with a significantly higher Mo content and a lower W content. W is the core high-temperature creep strengthening element of this invention, and the low W content of LSHR limits its high-temperature creep resistance. At the same time, the total Nb+Ta content of LSHR is only 3.1%, lower than the 3.66% of this invention, indicating insufficient total γ' phase stabilizing elements. In addition, the Co content of LSHR is as high as 21.3%, much higher than that of this invention. This is because its Mo content is high, requiring more Co to offset the ferrite stabilizing effect of Mo. In contrast, this invention achieves sufficient microstructure stability with a lower Co content through a low Mo design.
[0080] Compared with FGH4098, FGH4098 adopts a low W and high Mo design with a Mo / W ratio of 1.12:1, which is significantly different from the 0.48:1 of the present invention; the Nb / Ta ratio is only 0.38:1, which is also significantly different from the 0.75:1 of the present invention.
[0081] Compared with FGH100L, its Nb / Ta ratio is 1.03:1 and Mo / W ratio is 0.63:1, which are significantly different from the 0.75:1 and 0.48:1 of the present invention. Meanwhile, its (Al+Ti) / (Nb+Ta) ratio reaches 2.28:1, significantly higher than the 1.9:1 of the present invention. From the perspective of the high-temperature stability of the γ' phase, the lower ratio of the present invention means that the overall proportion of γ' phase-forming elements with low diffusion rates is higher, which is beneficial to improving high-temperature creep resistance.
[0082] Compared to FGH4113A, this invention increases the proportions of Al and W, decreases the proportions of Ti and Mo, and simultaneously increases the overall proportions of Nb and Ta. In terms of core proportions, the Nb / Ta ratio is adjusted from 1.2:1 in FGH4113A to 0.75:1 in this invention, and the Mo / W ratio is adjusted from 1:1 to 0.48:1 in this invention. These adjustments comprehensively improve the high-temperature microstructure stability of the alloy from three dimensions: γ' phase stability, element diffusion rate, and TCP phase formation tendency.
[0083] Table 3. Comparison of the composition of the embodiments of the present invention and typical fourth-generation powder superalloys (wt.%)
[0084] As can be seen from Table 3, the embodiment of the present invention adopts a composition design scheme with low Nb, low Ta, low Mo, high W and combined with total Al+Ti control, which is significantly different from the key element ratios of typical fourth-generation powder superalloys.
[0085] Compared to ME501, the core formulation of ME501 differs significantly from that of this invention. Its Nb / Ta ratio is only 0.31:1, with a much higher Ta content than in this invention; its Mo / W ratio reaches 0.97:1, with a higher Mo content and a lower W content, significantly different from the 0.48:1 of this invention; its Al content is only 3.0 wt%, while its Ta content reaches 4.8 wt%. Its core design concept is to suppress the diffusion of elements in the γ' phase through high Ta addition, which is fundamentally different from the low-Ta, precise formulation approach of this invention.
[0086] Compared to GNPM01, the two differ fundamentally in several dimensions. Regarding grain boundary strengthening, the GNPM01 reported in this literature does not contain B or Zr, and the alloy contains no boride phases, allowing for higher solution treatment temperatures without initial melting. This invention, however, adds B and Zr, utilizing borides to effectively suppress grain boundary slip in a fine-grained state; the two have completely different grain boundary strengthening design approaches. In terms of solid solution strengthening, this invention has a higher W content and a lower Mo content than GNPM01, with W dominating solid solution strengthening and focusing more on improving creep performance; while GNPM01 is dominated by Mo. Regarding the γ' phase design, GNPM01 has a higher overall proportion of Ti, Nb, and Ta than this invention, with a (Al+Ti) / (Nb+Ta) ratio of 1.3:1, resulting in a higher γ' phase solution temperature and proportion. This invention adopts a relatively conservative strategy from the perspective of special process implementation, avoiding excessively high solution temperatures and γ' phase proportions, thus balancing process feasibility and performance.
[0087] Compared with TSNA-1, the Nb / Ta ratio of this alloy is only 0.3:1, and the Ta content is much higher than that of this invention. At the same time, the total Nb+Ta content reaches 6.5%, which is much higher than the 3.66% of this invention. This is different from the precise low Nb and low Ta ratio approach of this invention.
[0088] Compared to Alloy2, Alloy2 has an Nb / Ta ratio of only 0.3:1, with a significantly higher Ta content; its Mo / W ratio is 0.7:1, with a higher Mo content and a lower W content, showing significant differences from the two core ratios of this invention. Furthermore, Alloy2 has a Co content of only 15.5%, while this invention has a Co content of 18.67%, thus balancing the mismatch control of the γ matrix and γ' precipitates, as well as the low-level stacking fault energy effect.
[0089] Compared with RRHT5, the composition of RRHT5 is fundamentally different from that of the present invention, and the composition system is completely different.
[0090] Compared to FGH4102, FGH4102 has higher Mo, Nb, and Ta contents than this invention, with both its Mo / W mass ratio and Nb / Ta mass ratio being 1:1, resulting in an atomic ratio of 2:1. In the solid solution strengthening and low diffusion rate contributions provided by Mo and W, FGH4102 is dominated by Mo, while this invention achieves a co-dominant relationship between Mo and W through precise component ratios. In the precipitation strengthening provided by Nb and Ta, FGH4102 is dominated by Nb, while this invention is co-dominant with Nb and Ta. The strengthening mechanism design of this alloy differs significantly from that of this invention.
[0091] The performance of the embodiments of the present invention was compared with that of the typical fourth-generation powder superalloy ME501, and the results are shown in Table 4.
[0092] Table 4. Performance Comparison of the Embodiments of the Invention with Typical Fourth-Generation Powder Superalloy ME501
[0093] The test data for ME501 in Table 4 are from publicly published literature (A. Powell, K. Bain, A. Wessman, et al. Advanced supersolvus nickel powder disk alloy DOE: chemistry, properties, phase formations and thermal stability[C]. Superalloys 2016: 189-197). Its heat treatment regime was 1191℃ / 1h + 843℃ / 2h + 760℃ / 8h, with an average cooling rate of 111℃ / min for each heat treatment stage. This cooling rate is very close to that of Example 1 of this invention and has important comparative reference value. The cooling rate of Example 2 is significantly higher than that of Example 1.
[0094] As shown in Table 4, under similar heat treatment cooling rates, the two embodiments of this invention are at the same level as ME501 in terms of high-temperature tensile properties, and some indicators are even better. The tensile strength and yield strength of this invention at 750℃ are comparable to the tensile properties of ME501 at 760℃. At 815℃, the tensile strength of this invention can reach 1096MPa, which is higher than that of ME501 (993MPa), and the yield strength is also at the same level as ME501, proving that the high-temperature strength of this invention fully meets the fourth-generation alloy standard.
[0095] Regarding high-temperature creep resistance, this invention surpasses that of ME501. Under the core operating condition of 815℃ / 345MPa, the 0.2% creep time of Example 1 is 133h, which is 1.91 times that of ME501 (69.5h). In Example 2, by increasing the cooling rate of heat treatment, the 0.2% creep time is further increased to 472h, reaching 6.8 times that of ME501. Under the condition of 750℃ / 520MPa, the 0.2% creep time of this invention is 1.72 to 2.18 times that of ME501 under the condition of 760℃ / 500MPa.
[0096] In terms of durability, this invention also surpasses the previous one. Under conditions of 815℃ / 345MPa, the durability of Example 2 reaches 913h, which is better than the 532h of ME501; the durability of Example 1 is 544h, which is at the same level as ME501. Under conditions of 750℃, the durability performance of this invention is also comparable to that of ME501 at 760℃.
[0097] The above comparison fully demonstrates that the high-temperature alloy of the present invention, using a design technology route of low Nb, low Ta, low Mo, and high W, can fully achieve excellent high-temperature strength, high-temperature creep resistance, and long-term microstructure stability, providing a differentiated technical approach for the composition ratio design of fourth-generation powder high-temperature alloys.
[0098] In the above embodiments, the descriptions of each embodiment have different focuses. For parts that are not described in detail in a certain embodiment, please refer to the relevant descriptions in other embodiments.
[0099] Obviously, those skilled in the art can make various modifications and variations to this invention without departing from its spirit and scope. Therefore, this invention is also intended to include these modifications and variations as long as they fall within the scope of the claims and their equivalents.
[0100] The above description is merely a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any person skilled in the art can easily conceive of various equivalent modifications or substitutions within the technical scope disclosed in the present invention, and these modifications or substitutions should all be covered within the scope of protection of the present invention. Therefore, the scope of protection of the present invention should be determined by the scope of the claims.
Claims
1. A nickel-based powder superalloy, characterized in that, Included by weight percentage: Co: 16.0%–22.0%, Cr: 10.0%–14.0%, Mo: 2.0%–3.0%, W: 4.0%–6.0%, Al: 2.8%–4.0%, Ti: 2.8%–4.0%, Nb: 0.8%–1.8%, Ta: 1.0%–2.5%, Hf: 0.1%–0.3%, Zr: 0.01%–0.1%, C: 0.03%–0.08%, B: 0.02%–0.04%, with the balance being Ni and unavoidable impurities.
2. The nickel-based powder superalloy according to claim 1, characterized in that, The total content of Al and Ti in the high-temperature alloy is 6.5% to 7.3%, the total content of Nb and Ta is 3.3% to 3.7%, and the total content of Mo and W is 6.7% to 7.7%.
3. The nickel-based powder superalloy according to claim 2, characterized in that, The mass ratio of Nb to Ta is 3:4, the mass ratio of Mo to W is 1:2, and the mass ratio of Al to Ti is 1:
1.
4. The nickel-based powder superalloy according to claim 1, characterized in that, The high-temperature alloy has a γ' phase mass fraction of 50% to 60% at 800℃, and the complete dissolution temperature of the γ' phase is 1170℃ to 1190℃.
5. The nickel-based powder superalloy according to any one of claims 1-4, characterized in that, Included by weight percentage: Co: 17.0%–20.0%, Cr: 11.0%–13.0%, Mo: 2.0%–2.8%, W: 4.4%–5.4%, Al: 3.1%–3.9%, Ti: 3.0%–3.8%, Nb: 1.2%–1.8%, Ta: 1.7%–2.3%, Hf: 0.15%–0.25%, Zr: 0.02%–0.08%, C: 0.03%–0.08%, B: 0.02%–0.04%, with the balance being Ni and unavoidable impurities.
6. The nickel-based powder superalloy according to any one of claims 1-4, characterized in that, Included by weight percentage: Co: 18.0%–19.0%, Cr: 11.5%–12.5%, Mo: 2.05%–2.55%, W: 4.65%–5.15%, Al: 3.3%–3.7%, Ti: 3.2%–3.6%, Nb: 1.4%–1.6%, Ta: 1.9%–2.1%, Hf: 0.17%–0.23%, Zr: 0.03%–0.07%, C: 0.04%–0.06%, B: 0.025%–0.035%, with the balance being Ni and unavoidable impurities.
7. A method for preparing a nickel-based powder superalloy as described in any one of claims 1-6, characterized in that, Includes the following steps: (1) Prepare raw materials according to the composition of the high-temperature alloy, and after vacuum induction melting, prepare nickel-based high-temperature alloy powder by argon atomization; (2) After vacuum sealing the high-temperature alloy powder obtained in step (1), hot isostatic pressing is performed to obtain a dense billet; (3) The dense billet obtained in step (2) is hot-extruded to obtain an extruded bar; then the extruded bar is isothermally forged to obtain a forging. (4) The forgings obtained in step (3) are subjected to solution heat treatment and aging heat treatment in sequence to obtain the nickel-based powder high-temperature alloy.
8. The preparation method according to claim 7, characterized in that, In step (2), the temperature of hot isostatic pressing is 1130-1190℃, the pressure is 130-170MPa, and the holding time is 2-6 hours.
9. The preparation method according to claim 7, characterized in that, In step (4), the solution heat treatment temperature is 1180±30℃ and the holding time is 2 to 8 hours; the aging heat treatment is: holding at 750 to 850℃ for 4 to 10 hours; or graded aging is adopted: holding at 820 to 860℃ for 2 hours, and then holding at 740 to 780℃ for 8 hours.
10. A hot-end component of an aero-engine or gas turbine, characterized in that, The component is made of a nickel-based powder superalloy as described in any one of claims 1 to 6.