A heat-resistant, high-strength aluminum alloy wire that requires no heat treatment and its preparation method

By optimizing the aluminum alloy composition and process flow, and adopting a heat-free method for preparing high-strength, heat-resistant aluminum alloy wire, the problems of high energy consumption and unstable yield in existing technologies have been solved. This method achieves high efficiency, stable high strength and heat resistance, making it suitable for the power transmission field.

CN123108359APending Publication Date: 2026-11-17TBEA XINJIANG CABLE CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611172234.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-04
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing production lines for 150℃-grade high-strength heat-resistant aluminum alloys suffer from high heat treatment energy consumption, increased production costs, unstable yield, and high equipment requirements. Furthermore, 6-series aluminum-magnesium-silicon alloys are highly temperature-sensitive, making them difficult to widely apply in general enterprises.

Method used

A method for preparing high-strength, heat-resistant aluminum alloy wire without heat treatment is adopted. By optimizing the chemical composition and process flow, including aluminum alloy composition design, alloying, refining, degassing and impurity removal, grain refinement, rolling and cold rolling, Al3Zr and AlSb phases are formed, the recrystallization temperature is increased, the heat treatment process is eliminated, and the strength is improved by dynamic recrystallization and work hardening during the cold rolling process.

Benefits of technology

It achieves reduced energy consumption without compromising performance, improves production efficiency and yield, meets the requirements of high strength, heat resistance and conductivity, and adapts to the needs of long-span power transmission.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108359A_ABST
    Figure CN123108359A_ABST
Patent Text Reader

Abstract

This invention discloses a heat-treatable high-strength heat-resistant aluminum alloy wire without heat treatment and its preparation method, relating to the field of aluminum alloy cable technology. The aluminum alloy wire is made of aluminum alloy, which, by mass percentage, comprises the following components: Si < 0.1%; Fe: 0.15-0.45%; Cu: 0.1-0.2%; Zr: 0.03-0.13%; Sb: 0.02-0.2%; rare earth elements: 0.005-0.05%, and the rare earth elements include Ce and La; the balance is Al and impurities; the balance is Al. Compared with similar heat-treatable heat-resistant aluminum alloy wires, this invention optimizes the chemical composition, eliminates the heat treatment process of the rod while ensuring the wire performance meets the requirements, optimizes the production process, and reduces energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of aluminum alloy cable technology, specifically to a heat-resistant, high-strength aluminum alloy wire that requires no heat treatment and its preparation method. Background Technology

[0002] Aluminum alloy cables are used for power transmission. Power transmission projects spanning rivers, lakes, and mountains place higher demands on the current carrying capacity, operating temperature, and mechanical strength of the cables. Existing technology involves adding Zr to a 6-series aluminum-magnesium-silicon (Al-Mg-Si) alloy to form Al3Zr and Mg2Si phases, which respectively contribute to heat resistance and strength. This process achieves a combination of strength and heat resistance and is mainly used in heat-resistant aluminum alloy conductors for long-span applications.

[0003] The existing production scheme for 150℃-grade high-strength heat-resistant aluminum alloy wire follows the process of "continuous casting and rolling (F-state alloy rod) - wire drawing - single-wire aging (performance optimization)". Heat treatment, by controlling the dispersed precipitation of Mg2Si phase and Al3Zr phase, increases the material's recrystallization temperature. However, this method has significant limitations: First, heat treatment consumes a lot of energy, increasing production costs and carbon emissions; second, the process involves many key points, making aluminum alloy rod production difficult (in terms of composition design, process parameter control, and high equipment requirements), resulting in inconsistent yield rates and affecting the consistency of the wire products. Furthermore, because 6-series alloys are solid solution strengthened alloys, they are highly sensitive to temperature, requiring high-level process control and sophisticated equipment, making production difficult for most companies. Summary of the Invention

[0004] To address the problems existing in the prior art, this invention provides a heat-treatable high-strength heat-resistant aluminum alloy wire and its preparation method. Compared with similar heat-treatable heat-resistant aluminum alloy wires, this invention optimizes the chemical composition, eliminates the heat treatment process while ensuring the wire performance meets the requirements, optimizes the production process, and reduces energy consumption.

[0005] The technical solution of the present invention is as follows: In a first aspect of the invention, a heat-treatable, high-strength, heat-resistant aluminum alloy wire is provided, made of an aluminum alloy comprising, by weight percentage, the following components: Si < 0.1%; Fe: 0.15-0.45%; Cu: 0.1-0.2%; Zr: 0.03-0.13%; Sb: 0.02-0.2%; rare earth elements: 0.005-0.05%, wherein the rare earth elements include Ce and La; the balance is Al and impurities.

[0006] In some embodiments of the present invention, the impurities include Cr, Mn, V, and Ti, and the total impurity content is ≤0.01%.

[0007] In some embodiments of the present invention, the aluminum alloy has a tensile strength ≥250MPa, elongation ≥2.0%, conductivity ≥57%IACS, and heat resistance ≥90%. In a second aspect of the present invention, a method for preparing a heat-resistant, high-strength aluminum alloy wire without heat treatment is provided, comprising the following steps: Aluminum raw materials are smelted and boronized to obtain molten aluminum; The first alloying process is carried out to ensure that the contents of Fe, Cu and rare earth elements meet the standards. A second alloying process is performed to ensure that the Zr and Sb contents meet the standards. Then, the process involves refining, degassing and impurity removal, grain refinement, casting, rolling, and cold rolling to obtain a heat-free high-strength heat-resistant aluminum alloy wire.

[0008] In some embodiments of the present invention, during the first alloying process, AlFe20 master alloy, copper plate, and AlRE10 master alloy are added; during the second alloying process, AlZr10 master alloy and AlSb5 master alloy are added.

[0009] In some embodiments of the present invention, during refining, granular refining agent is blown into the molten aluminum using 99.99% pure nitrogen gas, and uniform degassing and stirring are performed for 20-30 minutes; after stirring and standing for 5-10 minutes, the molten aluminum is fully stabilized and slag is removed, and the entire refining time is controlled within 20-40 minutes.

[0010] In some embodiments of the present invention, an aluminum-titanium-carbon-platinum feeder is used to add aluminum during the grain refinement process at a rate of 0.1-5 m / min.

[0011] In some embodiments of the present invention, the casting temperature during casting is 700-720℃, and the casting speed is 6-7t / h.

[0012] In some embodiments of the present invention, during rolling, the entry temperature is 500-550°C, the temperature of the emulsion used is controlled at 50-70°C, the concentration is controlled at 15-25%, and the take-off temperature after continuous rolling is 300-400°C.

[0013] In some embodiments of the present invention, during cold rolling, a cold rolling mill is used to roll the rod into a single filament with a diameter greater than 3 mm. The rolling temperature is controlled at 50-60°C and the emulsion concentration is 15-25%. The take-up temperature is controlled at 150-200°C.

[0014] One or more technical solutions of the present invention have the following beneficial effects: (1) Based on 1120 aluminum alloy, this invention controls Zr to 0.03-0.13% to form dispersed Al3Zr particles with the aluminum matrix, pinning subgrain boundaries and dislocations, raising the alloy recrystallization temperature to above 200℃, and ensuring that the strength loss during long-term operation at 150℃ is <10%; 0.02-0.2% Sb is introduced to form a dispersed AlSb phase, which plays a strengthening role and can improve the work hardening rate. Sb agglomerates at the grain boundaries and works with Al3Zr to pin them; RE is selected as Ce+La and the total amount is controlled at 0.005-0.05%, which purifies the grain boundaries and plays a role in refining the grains, resulting in better billet quality; the whole structure does not contain Be, avoiding toxicity and cost issues.

[0015] (2) This invention changes the traditional "solution treatment of rod material + aging of single wire" scheme. Based on the strengthening theory, it comprehensively analyzes the relevant factors affecting recrystallization and conductivity, and designs a composition formula that can improve strength through work hardening and increase recrystallization temperature through Al3Zr dispersion. Combined with the key points of process control, a set of process control schemes is formed for the key control points of continuous casting, rolling and heat treatment of aluminum alloys. The winding temperature is 300-400℃, eliminating the need for heat treatment; the large deformation in the cold rolling process introduces high dislocation density to improve strength; the high temperature in the cold rolling process simultaneously forms recrystallization structure, refines grains to maintain strength and improve elongation, and also reduces the resistivity increase caused by work hardening.

[0016] (3) The AlSb pinning system in the composition of this invention ensures strength, and the temperature control in the process can obtain aluminum rods with good mechanical and electrical properties. The prepared monofilaments can meet the requirements of conductivity, strength and heat resistance. Attached Figure Description

[0017] Figure 1 This is a flowchart of the method for preparing heat-free high-strength heat-resistant aluminum alloy wire according to the present invention. Detailed Implementation

[0018] It should be noted that the following detailed descriptions are exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0019] It should be noted that the terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of exemplary embodiments according to the invention. As used herein, unless otherwise expressly indicated by the invention, the singular form is intended to include the plural form as well. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this specification, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.

[0020] One embodiment of the present invention provides a heat-resistant, high-strength aluminum alloy wire that requires no heat treatment. The wire is made of aluminum alloy, and the aluminum alloy comprises the following components by weight percentage: Si < 0.1%; Fe: 0.15-0.45%; Cu: 0.1-0.2%; Zr: 0.03-0.13%; Sb: 0.02-0.2%; rare earth elements: 0.005-0.05%, wherein the rare earth elements include Ce and La; the balance is Al and impurities.

[0021] Furthermore, the impurities include Cr, Mn, V, and Ti, with a total impurity content of ≤0.01%.

[0022] Furthermore, the aluminum alloy has a tensile strength ≥250MPa, elongation ≥2.0%, electrical conductivity ≥57%IACS, and heat resistance ≥90%.

[0023] The heat-resistant, high-strength aluminum alloy wire provided in this embodiment improves the composition of the aluminum alloy. The addition of sulfur (Sb) forms a solid solution, which increases the work hardening rate of the single wire during processing, ultimately ensuring the strength of the single wire; while Sb has very little effect on its electrical resistance. The addition of zinc (Zr) also forms the Al3Zr phase, increasing the recrystallization temperature; the addition of iron (Fe) has the dual effect of increasing both work hardening and recrystallization temperature. Resin (RE) refines the grain size.

[0024] ‌ In another embodiment of the present invention, a method for preparing a heat-resistant, high-strength aluminum alloy wire without heat treatment is provided, such as... Figure 1 As shown, it includes the following steps: 1. Smelt aluminum raw materials and perform boronizing treatment to obtain molten aluminum; Specifically, 99.85% pure aluminum ingots are selected as the raw material, with a chemical composition content of Si < 0.1% and Fe < 0.12%. The aluminum ingots are placed in a tilting furnace for melting, and AlB8 is added simultaneously for boronizing treatment. After all the aluminum ingots in the furnace have melted, a slag rake is used to remove the slag. The rake head is kept flat against the surface of the molten aluminum and slowly and steadily pulled towards the furnace door to avoid rolling up the bottom oxides or carrying out too much molten aluminum. After the aluminum ingots are melted, the temperature needs to be controlled at 720-760℃. Before the converter, the ingots need to be left to stand for 30 minutes for sampling and analysis, and the total content of impurity elements (Cr+Mn+V+Ti) needs to be controlled to be ≤0.01%. The converter operation can only proceed after the standard is met. During the converter operation, the electromagnetic stirrer in the holding furnace should be turned on. When the weight of the molten aluminum in the holding furnace reaches the required weight, the aluminum feeding should be stopped. One sample of the cast billet is taken from each side of the furnace opening using a sampling spoon for pre-analysis of chemical composition.

[0025] 2. Perform the first alloying to ensure that the contents of Fe, Cu and rare earth elements meet the standards; Specifically, AlRE10 master alloy, AlFe20 master alloy, and copper plate (99.9% pure copper) are added respectively. The master alloy must comply with the national standard GB / T 27677 "Aluminum Master Alloys", and the copper plate must comply with the national standard GB / T 2040 "Copper and Copper Alloy Plates". After the first alloying batching, maintain electromagnetic uniform stirring for 20-40 minutes. Take samples using the same sampling method as in step 1 for chemical composition analysis to ensure that each chemical component reaches the target value, namely: Si: <0.1%; Fe: 0.15-0.45%; Cu: 0.1-0.2%; RE (Ce+La): 0.005-0.05%; Cr+Mn+V+Ti ≤0.01%. 3. Perform a second alloying process to ensure that the Zr and Sb contents meet the standards; Specifically, add AlZr10 master alloy and AlSb5 master alloy; let stand for 20-40 minutes. Take samples for chemical composition analysis to ensure that each chemical component reaches the target value, namely Si: <0.1%; Fe: 0.15-0.45%; Cu: 0.1-0.2%; Zr: 0.03-0.13%; Sb: 0.02-0.2%; RE (Ce+La): 0.005-0.05%; Cr+Mn+V+Ti ≤0.01%.

[0026] 4. Then, the process involves refining, degassing and impurity removal, grain refinement, casting, rolling, and cold rolling to obtain a heat-free high-strength heat-resistant aluminum alloy wire.

[0027] Furthermore, after confirming that the composition met the target range, a high-efficiency refining agent was blown into the molten aluminum using 99.99% pure nitrogen at a rate of 2 kg / ton. The refining agent met the requirements of YS / T 491 "Fluorides for Aluminum and Aluminum Alloys" standard. The refining process was then carried out with stirring for 20-40 minutes. This refining time range was set to ensure that gases and inclusions in the melt were fully removed. Using high-purity nitrogen as a carrier to blow in the refining agent effectively prevented primary oxidation, significantly improved the refining effect and melt purity, and laid a good foundation for subsequent processing.

[0028] After refining, let it stand for 5-10 minutes, then skim off the slag to remove surface scum and allow the gas to escape completely.

[0029] Then, a dual-rotor degassing box and a two-stage filter box (40 / 60ppi) are used for degassing and impurity removal.

[0030] Then, a grain refinement process is performed. During the process, aluminum-titanium-carbon-platinum is added using a wire feeder at a rate of 0.1-5 m / min.

[0031] During casting, the pouring temperature is 700-720℃, and the pouring speed is 6-7 t / h. Continuous and uniform addition of aluminum-titanium-carbon-platinum through the wire feeder can achieve a long-lasting grain refinement effect; controlling the pouring temperature between 700-720℃ is beneficial for obtaining good melt fluidity and solidification structure; while the pouring speed of 6-7 t / h ensures a balance between production efficiency and billet quality.

[0032] Furthermore, the rolling process involves rough rolling followed by finish rolling. The entry temperature is 500-550℃, and the emulsion temperature during rolling is 50-70℃ with a concentration of 15-25%. Continuous rolling is employed, with a take-off temperature of 300-400℃. A two-roll mill is used. Rough rolling first controls a larger deformation amount to improve rolling efficiency and strength. Then, finish rolling achieves uniform and rounded microstructure, which is beneficial for achieving uniform plastic deformation and grain evolution. Finally, a round aluminum rod is obtained after finish rolling. Controlling the entry temperature, emulsion parameters, and take-off temperature is crucial for regulating the deformation resistance, lubrication and cooling effects during the rolling process, as well as the final internal microstructure and mechanical properties of the wire.

[0033] Furthermore, the outer diameter of the rod is controlled at 9.5±0.45mm, and its performance needs to meet the following requirements: the out-of-roundness of the aluminum rod is ≤0.8mm, the strength is between 160-200MPa, the conductivity of the aluminum rod at 20℃ is ≥58%IACS, and the elongation at break is ≥8%.

[0034] Finally, cold rolling is performed to obtain a high-strength, heat-resistant monofilament that does not require heat treatment. Specifically, the rod is rolled into a single filament with a diameter greater than 3mm using a cold rolling mill. The rolling temperature is controlled at 50-60℃ and the emulsion concentration is 15-25%. The take-up temperature is controlled at 150-200℃.

[0035] In this embodiment, thorough stirring is performed after each addition of an alloying element. The purpose of this is to promote the rapid and uniform dissolution and diffusion of the newly added alloying element or intermediate alloy in the aluminum melt, prevent component segregation, ensure the uniformity of the chemical composition of the entire melt, and thus guarantee the stability of the final product performance.

[0036] It should be noted that if any component fails to meet the standard during each chemical composition test, the corresponding alloying process is repeated. Intermediate alloys refer to special alloys made by alloying certain elements to facilitate their addition to other alloys, solving problems such as burn-off and the difficulty of incorporating high-melting-point alloys, while having minimal impact on the raw materials. For example, AlFe20 refers to an aluminum matrix with a nominal iron content of 20% by mass.

[0037] The preparation method provided in this embodiment optimizes the traditional drawing technique into a cold rolling technique. The core function is that during the cold rolling deformation process, the material generates significant heat, allowing the wire to reach 200°C. This process enables dynamic recrystallization, which partially refines the grain size and optimizes mechanical properties (achieving the best overall combination of strength and elongation). Since the added elements have a negligible impact on resistivity but a significant contribution to strength, the combination of cold rolling and dynamic recrystallization achieves optimal performance.

[0038] Example 1 A heat-resistant, high-strength aluminum alloy wire that requires no heat treatment is made of aluminum alloy, wherein the aluminum alloy comprises the following components by weight percentage: Si: 0.035%; Fe: 0.42%; Cu: 0.12%; Zr: 0.06%; Sb: 0.04%; RE (Ce+La): 0.012%; Cr+Mn+V+Ti: 0.0012%.

[0039] Its preparation process is as follows: 1. Melt aluminum ingots at a temperature controlled at 720℃ and perform a preliminary chemical composition analysis, including the following components: Si: 0.03%; Cr+Mn+V+Ti: 0.03%; Fe: 0.08%; Cu: 0.00%; RE: 0.000%; Al: 99.85%. Based on the preliminary chemical composition analysis, an aluminum-boron (AlB8) master alloy was added for boronizing treatment. Samples were then taken for chemical composition analysis. Once the Cr+Mn+V+Ti content was ≤0.005%, a first alloying batching was performed. 2. Add AlFe20 master alloy, copper plate and AlRE10 master alloy for primary alloying. After primary alloying, keep the mixture under electromagnetic stirring for 30 minutes. Take samples using the same sampling method as in step 1 for chemical composition analysis. The composition includes: Si: 0.035%; Fe: 0.42%; Cu: 0.12%; RE (Ce+La): 0.008%; Cr+Mn+V+Ti: 0.0012%.

[0040] 3. Add AlZr10 master alloy and AlSb5 master alloy for secondary alloying, stir for 30 min, and let stand for 30 min. Perform a first refining and chemical composition analysis as in step 1. The composition includes: Si: 0.035%; Fe: 0.42%; Cu: 0.12%; Zr: 0.06%; Sb: 0.04%; RE (Ce+La): 0.012%; Cr+Mn+V+Ti: 0.0012%.

[0041] 4. Stir and use 99.99% pure nitrogen to blow granular refining agent into the aluminum liquid at a rate of 2 kg / t, and continue stirring and refining for 30 minutes. Then let it stand for 30 minutes.

[0042] Further, the same process as in step 1 was performed to remove the slag from the insulating aluminum and to sample and analyze its chemical composition. The composition included: Si: 0.035%; Fe: 0.42%; Cu: 0.12%; Zr: 0.06%; Sb: 0.04%; RE (Ce+La): 0.012%; Cr+Mn+V+Ti: 0.0012%.

[0043] Casting begins once the composition is deemed satisfactory; aluminum-titanium-carbon-platinum alloy is added to the runner using a wire feeder at a rate of 0.5 m / min. The casting temperature is 700℃, and the casting speed is 6 t / h. Further, during rolling, rough rolling is performed followed by fine rolling. The entry temperature is 500℃, and the emulsion temperature during rolling is 60℃ with a concentration of 15%. Continuous rolling is performed, and the take-off temperature is 380℃.

[0044] Cold rolling into wire; the aluminum rod is cold rolled into a single wire with a diameter of 3.0 mm using a cold rolling mill. The rolling temperature is controlled at 50°C and the emulsion concentration is 15%. The take-up temperature is controlled at 200°C.

[0045] Example 2 The difference from Example 1 is that the aluminum alloy includes the following components: Si: 0.05%; Fe: 0.38%; Cu: 0.15%; Zr: 0.08%; Sb: 0.08%; RE (Ce+La): 0.008%; Cr+Mn+V+Ti: 0.003%.

[0046] The difference between the preparation method and Example 1 is that the rolling temperature is 520°C; the emulsion temperature is 65°C; and the take-up temperature is 360°C.

[0047] The rod was rolled into a 3.2mm monofilament using a cold rolling mill; the take-up temperature was controlled at 180℃. The remaining steps and parameters were the same as in Example 1.

[0048] Example 3 The difference from Example 1 is that the aluminum alloy includes the following components: Si: 0.05%; Fe: 0.15%; Cu: 0.1%; Zr: 0.13%; Sb: 0.2%; RE (Ce+La): 0.005%; Cr+Mn+V+Ti: 0.006%.

[0049] The difference between the preparation method and Example 1 is that the rod finishing temperature is 340°C, the rolling temperature is 535°C, the emulsion temperature is 65°C, and the concentration is 15%.

[0050] The rod was rolled into a 3.4mm monofilament using a cold rolling mill; the take-up temperature was controlled at 150℃. The remaining steps and parameters were the same as in Example 1.

[0051] Example 4 The difference from Example 1 is that the aluminum alloy includes the following components: Si: 0.038%; Fe: 0.45%; Cu: 0.1%; Zr: 0.03%; Sb: 0.02%; RE (Ce+La): 0.05%; Cr+Mn+V+Ti: 0.008%.

[0052] The preparation method differs from Example 1 in that: the rolling temperature is 500°C, the emulsion temperature is 65°C, and the concentration is 20%; the take-up temperature is 320°C. Cold rolling is performed on 4.0mm diameter wire; the take-up temperature is controlled at 150°C. The remaining steps are the same as in Example 1.

[0053] Comparative Example 1 The difference from Example 1 is that the alloy composition for preparing the alloy wire is different: it belongs to the aluminum-magnesium-silicon series, with Si: 0.5%; Fe: 0.2%; Cu: 0.1%; Mg: 0.6%; and Zr: 0.1%.

[0054] The aluminum rod is in T4 condition, and then drawn using a large drawing machine to a diameter of 3.2mm. Different heat treatment methods are then applied to adjust the wire quality and achieve the desired monofilament properties. The wire is then held at 200-230℃ for 6-10 hours.

[0055] Comparative Example 2 The difference from Example 1 is that the alloy composition for preparing the alloy wire is different: it belongs to the aluminum-magnesium-silicon series, with Si: 0.5%; Fe: 0.2%; Cu: 0.1%; Mg: 0.6%; and Zr: 0.1%.

[0056] The aluminum rod is in T4 condition, and then drawn using a large drawing machine to a diameter of 3.6mm. Different heat treatment methods are then applied to adjust the wire quality and achieve the desired monofilament properties. The wire is then held at 200-230℃ for 6-10 hours.

[0057] Comparative Example 3 The difference from Example 1 is that the alloy composition for preparing the alloy wire is different: it belongs to the aluminum-magnesium-silicon series, with Si: 0.5%; Fe: 0.2%; Cu: 0.1%; Mg: 0.6%; and Zr: 0.1%.

[0058] The aluminum rod is in T4 condition, and then drawn using a large drawing machine to a diameter of 3.9mm. Different heat treatment methods are then applied to adjust the wire quality and achieve the desired monofilament properties. The wire is then held at 200-230℃ for 6-10 hours.

[0059] The monofilaments prepared in the above examples and comparative examples were tested for tensile strength, elongation, electrical conductivity, and heat resistance. The test results are shown in Table 1. Table 1 Performance Test Results

[0060] As can be clearly seen from the test results in Table 1, the heat-resistant aluminum alloy wire disclosed in this invention, which eliminates the need for post-drawing aging heat treatment, achieves a complete performance reconstruction of traditional aluminum-magnesium-silicon conductors in all core indicators: In terms of strength, the tensile strength of the cold-rolled wires in Examples 1-4 reaches 252-268 MPa, which is significantly improved compared to the traditional comparative examples of the same specifications (235-254 MPa), and fully covers and is significantly better than ≥225 MPa. The MPa is an industry benchmark. Regarding conductivity, thanks to the magnesium removal design and the extremely low resistivity coupling effect of Sb and RE elements, the conductivity of the single filament in this invention remains stably maintained at 57.5%~57.9% IACS, nearly 2 percentage points higher than the comparative level of 55.6%~56.2%, reducing active power loss in line operation from the source. As for the high-temperature residual rate, the most critical indicator for the reliability of heat-resistant conductors, this invention maintains a strength retention rate of 92%~93% after treatment at 230℃ / 1h, essentially on par with the comparative level after 6~10 hours of artificial aging, truly achieving "performance without heat treatment." Furthermore, as the cold-rolled specification expands from 3.0mm to 4.0mm, while the strength naturally gradients with the amount of deformation, the elongation and conductivity steadily increase, confirming that this formulation has extremely high process tolerance under cold rolling conditions, effectively resolving the industry pain points of traditional 6-series alloys being extremely sensitive to temperature and having large fluctuations in yield.

[0061] While the specific embodiments of the present invention have been described above in conjunction with the accompanying drawings, this is not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art without creative effort based on the technical solutions of the present invention are still within the scope of protection of the present invention.

Claims

1. A heat-resistant, high-strength aluminum alloy wire that requires no heat treatment, characterized in that, Made of aluminum alloy, which comprises, by weight percentage, the following components: Si < 0.1%; Fe: 0.15-0.45%; Cu: 0.1-0.2%; Zr: 0.03-0.13%; Sb: 0.02-0.2%; rare earth elements: 0.005-0.05%, wherein the rare earth elements include Ce and La; the balance is Al and impurities.

2. The heat-resistant, heat-resistant aluminum alloy wire without heat treatment as described in claim 1, characterized in that, The impurities include Cr, Mn, V, and Ti, with a total impurity content of ≤0.01%.

3. The heat-resistant, heat-resistant aluminum alloy wire without heat treatment as described in claim 1, characterized in that, The aluminum alloy has a tensile strength ≥250MPa, elongation ≥2.0%, electrical conductivity ≥57%IACS, and heat resistance ≥90%.

4. A method for preparing a heat-resistant, high-strength aluminum alloy wire without heat treatment as described in any one of claims 1-3, characterized in that, Includes the following steps: Aluminum raw materials are smelted and boronized to obtain molten aluminum; The first alloying process is carried out to ensure that the contents of Fe, Cu and rare earth elements meet the standards. A second alloying process is performed to ensure that the Zr and Sb contents meet the standards. Then, the process involves refining, degassing and impurity removal, grain refinement, casting, rolling, and cold rolling to obtain a heat-free high-strength heat-resistant aluminum alloy wire.

5. The method for preparing heat-resistant, high-strength aluminum alloy wire without heat treatment as described in claim 4, characterized in that, During the first alloying process, AlFe20 master alloy, copper plate, and AlRE10 master alloy are added; during the second alloying process, AlZr10 master alloy and AlSb5 master alloy are added.

6. The method for preparing heat-free high-strength heat-resistant aluminum alloy wire as described in claim 4, characterized in that, During refining, granular refining agent is blown into the molten aluminum using 99.99% pure nitrogen gas for 20-30 minutes of uniform degassing and stirring. After stirring and standing for 5-10 minutes, the molten aluminum is fully stabilized before slag removal. The entire refining time is controlled within 20-40 minutes.

7. The method for preparing heat-free high-strength heat-resistant aluminum alloy wire as described in claim 4, characterized in that, During the grain refinement process, aluminum-titanium-carbon-platinum is added using a wire feeder at a rate of 0.1-5 m / min.

8. The method for preparing heat-resistant, high-strength aluminum alloy wire without heat treatment as described in claim 4, characterized in that, The casting temperature during casting is 700-720℃, and the casting speed is 6-7t / h.

9. The method for preparing heat-resistant, high-strength aluminum alloy wire without heat treatment as described in claim 4, characterized in that, During rolling, the entry temperature is 500-550℃, the temperature of the emulsion is controlled at 50-70℃, the concentration is controlled at 15-25%, and the take-off temperature after continuous rolling is 300-400℃.

10. The method for preparing heat-resistant, high-strength aluminum alloy wire without heat treatment as described in claim 4, characterized in that, During cold rolling, a cold rolling mill is used to roll the rod into a single wire with a diameter greater than 3mm. The rolling temperature is controlled at 50-60℃ and the emulsion concentration is 15-25%. The take-up temperature is controlled at 150-200℃.