A low-alloy high-strength magnesium alloy and its preparation method
By using a low-alloy system and conventional hot extrusion process, a microstructure with alternating fine and coarse grains is formed, which solves the problem of high cost in improving the strength of magnesium alloys in existing technologies, and realizes efficient and low-cost industrial production, obtaining high-strength magnesium alloys with a yield strength ≥300 MPa.
Patent Information
- Application Number
- CN202611507140.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-28
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies for improving the strength of magnesium alloys typically rely on adding large amounts of rare earth elements, which increases material costs and density, and the processes are complex and energy-intensive, making it difficult to achieve low-cost and efficient industrial production.
By adopting a low-alloy system with rare earth elements ≤3.0 wt.% and combining casting and conventional hot extrusion processes, and through appropriate annealing temperature, pre-stretching deformation, aging temperature and holding time, a bimodal microstructure with alternating fine and coarse grains is formed, thereby improving the mechanical properties of magnesium alloys.
It significantly reduces the amount of rare earth elements used, simplifies the process, improves production efficiency, and produces high-strength magnesium alloys with a yield strength of ≥300 MPa, making them suitable for large-scale industrial production.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal material processing technology, and particularly relates to a low-alloy high-strength magnesium alloy and its preparation method. Background Technology
[0002] Magnesium, with a density approximately two-thirds that of aluminum alloys and one-quarter that of steel, is one of the lightest metallic structural materials available. It boasts advantages such as lightweight, abundant resources, environmental friendliness, high specific strength and stiffness, good vibration damping, strong radiation resistance, and ease of machining, earning it the reputation of a green engineering material for the 21st century. However, compared to aluminum and steel, most existing magnesium alloys have lower absolute strength, making them less suitable for widespread application as critical load-bearing components in fields such as defense and the automotive industry.
[0003] Current technologies for improving the strength of magnesium alloys mainly rely on increasing the content of alloying elements, especially rare earth elements, and employing complex multi-stage deformation and heat treatment processes. While these methods can improve the mechanical properties of magnesium alloys to some extent, they lead to a significant increase in raw material costs, and the processes are complex, energy-intensive, and time-consuming, making it difficult to simultaneously achieve low cost, low energy consumption, and industrial-scale production. Therefore, how to achieve the industrial-scale production of high-strength magnesium alloys while reducing the amount of alloying raw materials, simplifying the process, and reducing energy consumption has become a pressing technical challenge for the development of magnesium alloy materials. Summary of the Invention
[0004] The purpose of this invention is to provide a low-alloy high-strength magnesium alloy and its preparation method, thereby addressing the problems mentioned in the background art.
[0005] The present invention is implemented as follows: a low-alloy high-strength magnesium alloy, by mass percentage, is composed of the following components:
[0006] Sm: 1.6-1.9 wt.%, Ca: 0.01-0.4 wt.%, Mn: 0.01-0.6 wt.%, Zn: 0.01-0.7 wt.%, Al: 0.2-0.3 wt.%, Gd: 0.01-0.3 wt.%, Tb: 0.01-0.3 wt.%, Dy: 0.01-0.5 wt.%, with the remainder being Mg and unavoidable impurities, the content of unavoidable impurities being ≤0.05 wt.%.
[0007] The further technical solution, by weight percentage, consists of the following components:
[0008] Sm: 1.80 wt.%, Ca: 0.35 wt.%, Mn: 0.08 wt.%, Zn: 0.03 wt.%, Al: 0.29 wt.%, Gd: 0.17 wt.%, Tb: 0.13 wt.%, Dy: 0.30 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%.
[0009] The further technical solution, by weight percentage, consists of the following components:
[0010] Sm: 1.67 wt.%, Ca: 0.37 wt.%, Mn: 0.51 wt.%, Zn: 0.06 wt.%, Al: 0.27 wt.%, Gd: 0.13 wt.%, Tb: 0.20 wt.%, Dy: 0.43 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%.
[0011] The further technical solution, by weight percentage, consists of the following components:
[0012] Sm: 1.90 wt.%, Ca: 0.02 wt.%, Mn: 0.31 wt.%, Zn: 0.63 wt.%, Al: 0.25 wt.%, Gd: 0.21 wt.%, Tb: 0.24 wt.%, Dy: 0.06 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%.
[0013] The further technical solution, by weight percentage, consists of the following components:
[0014] Sm: 1.77 wt.%, Ca: 0.24 wt.%, Mn: 0.29 wt.%, Zn: 0.46 wt.%, Al: 0.29 wt.%, Gd: 0.06 wt.%, Tb: 0.04 wt.%, Dy: 0.14 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%.
[0015] Another objective of this invention is to provide a method for preparing a low-alloy high-strength magnesium alloy, comprising the following steps:
[0016] Step 1: Batching and Melting / Casting;
[0017] Under the protection of a mixed gas with a CO2 and SF6 volume ratio of (97-99):(3-1), pure Mg is held at 480-510℃ for 40-60 min, and then the temperature is raised to 700-730℃ to completely melt the pure Mg. Mg-Sm, Mg-Ca, Mg-Mn, Mg-Gd, Mg-Tb, Mg-Dy master alloys, pure Zn, and pure Al are added. The mixture is allowed to stand at 700-730℃ for 10-20 min until the alloy raw materials are completely melted. After stirring, argon gas is blown in for refining and slag removal to obtain the alloy melt. The alloy melt is then injected into a preheated mold using gravity casting to obtain a magnesium alloy ingot.
[0018] Step 2: Solution treatment, quenching, and extrusion;
[0019] The magnesium alloy ingot obtained in step 1 is solution treated and quenched in hot water. Then, the oxide scale is removed by turning to obtain a magnesium alloy billet. The billet and the extrusion die are preheated at 300-320℃ for 40-60 min and then extruded to obtain an extruded magnesium alloy. The solution treatment is carried out at 510-520℃ for 3.5-4.5 h. The extrusion is carried out at an extrusion temperature of 300-320℃ and an extrusion ratio of (6-8):1.
[0020] Step 3: Annealing, pre-stretching, and aging;
[0021] The extruded magnesium alloy obtained in step 2 is annealed, pre-stretched along the extrusion direction, and aged to obtain a low-alloy high-strength magnesium alloy. The annealing treatment is performed at 375-385℃ for 6-7 min. The pre-stretching treatment is performed with a deformation of 2-4% and a stretching speed of 0.5-0.7 mm / min. The aging treatment is performed at 160-180℃ for 9-11 h.
[0022] In a further technical solution, in step 1, the volume ratio of CO2 to SF6 is 99:1, 98:2, or 97:3.
[0023] Pure Mg is first held at 490–500℃ for 50–60 min, then heated to 720–725℃; after adding intermediate alloy, pure Zn, and pure Al, it is allowed to stand at 720℃ for 15–20 min.
[0024] In a further technical solution, in step 2, the solution treatment is carried out at 520℃ for 4 hours; the billet and extrusion die are preheated at 300-310℃ for 50-60 minutes; the extrusion temperature is 300-310℃ and the extrusion ratio is 7:1.
[0025] In a further technical solution, in step 3, the annealing treatment is performed by holding at 380℃ for 6-7 min; the pre-stretch deformation is 3% and the stretching speed is 0.6 mm / min; the aging treatment is performed by holding at 175℃ for 10 h.
[0026] The present invention provides a low-alloy high-strength magnesium alloy and its preparation method, which have the following beneficial effects:
[0027] (1) Existing technologies typically rely on adding large amounts of rare earth elements to improve the strength of magnesium alloys, which leads to increased material costs and density, as well as increased processing difficulty. The total rare earth element content in the alloy system of this invention is ≤3.0 wt.%, which reduces the amount of rare earth elements used while improving strength, thus significantly reducing raw material costs.
[0028] (2) This invention improves the mechanical properties of extruded magnesium alloys by combining casting and conventional hot extrusion processes with appropriate annealing temperature, pre-stretching deformation, aging temperature and holding time. The process of this invention is simple, easy to operate and control, and the equipment used, such as melting furnace and hot extrusion press, are all conventional and general-purpose equipment. By streamlining the process, production efficiency is significantly improved, making it suitable for large-scale industrial production.
[0029] (3) The alloy of the present invention forms a bimodal microstructure with alternating fine and coarse grains. The fine-grained region consists of equiaxed grains with a volume fraction of 60-80% and an average grain size ≤4μm, providing fine-grain strengthening. The coarse-grained region consists of elongated deformed grains with a strong basal texture. The coarse-grained region contains high-density residual dislocations and small-angle grain boundaries, with small-angle grain boundaries accounting for ≥20% of the total grain boundaries, providing dislocation strengthening and texture strengthening effects. The synergistic effect of fine, uniform recrystallized grains and deformed grains enhances the alloy's strength.
[0030] (4) The pre-stretching deformation of the present invention can promote the formation of small-angle grain boundaries and the accumulation of residual dislocations, providing channels for the diffusion of solute atoms. High-density dislocations can serve as nucleation sites for precipitated phases during subsequent aging processes, promoting the generation of more dense precipitated phases and generating a strong pinning effect on grain boundaries, thereby achieving precipitation hardening, precipitation strengthening and grain boundary strengthening effects, and thus obtaining a magnesium alloy with excellent yield strength, which is ≥300 MPa. Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0032] The specific implementation of the present invention will be described in detail below with reference to specific embodiments.
[0033] An embodiment of the present invention provides a low-alloy high-strength magnesium alloy, which, by mass percentage, is composed of the following components:
[0034] Sm: 1.6-1.9 wt.%, Ca: 0.01-0.4 wt.%, Mn: 0.01-0.6 wt.%, Zn: 0.01-0.7 wt.%, Al: 0.2-0.3 wt.%, Gd: 0.01-0.3 wt.%, Tb: 0.01-0.3 wt.%, Dy: 0.01-0.5 wt.%, with the remainder being Mg and unavoidable impurities, the content of unavoidable impurities being ≤0.05 wt.%.
[0035] Another embodiment of the present invention provides a method for preparing a low-alloy high-strength magnesium alloy, comprising the following steps:
[0036] Step 1: Batching and Melting / Casting;
[0037] Under the protection of a mixed gas with a CO2 and SF6 volume ratio of (97-99):(3-1), pure Mg is held at 480-510℃ for 40-60 min, and then the temperature is raised to 700-730℃ to completely melt the pure Mg. Mg-Sm, Mg-Ca, Mg-Mn, Mg-Gd, Mg-Tb, Mg-Dy master alloys, pure Zn, and pure Al are added. The mixture is allowed to stand at 700-730℃ for 10-20 min until the alloy raw materials are completely melted. After stirring, argon gas is blown in for refining and slag removal to obtain the alloy melt. The alloy melt is then injected into a preheated mold using gravity casting to obtain a magnesium alloy ingot.
[0038] Step 2: Solution treatment, quenching, and extrusion;
[0039] The magnesium alloy ingot obtained in step 1 is solution treated and quenched in hot water. Then, the oxide scale is removed by turning to obtain a magnesium alloy billet. The billet and the extrusion die are preheated at 300-320℃ for 40-60 min and then extruded to obtain an extruded magnesium alloy. The solution treatment is carried out at 510-520℃ for 3.5-4.5 h. The extrusion is carried out at an extrusion temperature of 300-320℃ and an extrusion ratio of (6-8):1.
[0040] Step 3: Annealing, pre-stretching, and aging;
[0041] The extruded magnesium alloy obtained in step 2 is annealed, pre-stretched along the extrusion direction, and aged to obtain a low-alloy high-strength magnesium alloy. The annealing treatment is performed at 375-385℃ for 6-7 min. The pre-stretching treatment is performed with a deformation of 2-4% and a stretching speed of 0.5-0.7 mm / min. The aging treatment is performed at 160-180℃ for 9-11 h.
[0042] The following analysis is based on specific embodiments and comparative examples.
[0043] Example 1:
[0044] In this embodiment, a low-alloy high-strength magnesium alloy is composed of the following components by mass percentage:
[0045] Sm: 1.80 wt.%, Ca: 0.35 wt.%, Mn: 0.08 wt.%, Zn: 0.03 wt.%, Al: 0.29 wt.%, Gd: 0.17 wt.%, Tb: 0.13 wt.%, Dy: 0.30 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%. The preparation method includes the following steps:
[0046] Step 1: According to the alloy composition ratio, under the protection of a mixed gas of CO2 and SF6 with a volume ratio of 99:1, pure Mg is held at 500℃ for 60 minutes, and then the temperature is raised to 725℃ to completely melt the pure Mg. Then, Mg-Sm, Mg-Ca, Mg-Mn, Mg-Gd, Mg-Tb, Mg-Dy master alloys, pure Zn, and pure Al are added. After standing at 720℃ for 15 minutes to allow the alloy raw materials to completely melt, the mixture is stirred, argon gas is blown in for refining and slag removal to obtain the alloy melt. The alloy melt is then poured into a preheated mold using gravity casting to obtain a magnesium alloy ingot.
[0047] Step 2: The magnesium alloy ingot obtained in Step 1 is solution treated and quenched in hot water. Then, the oxide scale is removed by turning to obtain a magnesium alloy billet. The billet and the extrusion die are preheated at 310℃ for 60 min and then extruded to obtain an extruded magnesium alloy. The solution treatment is: holding at 520℃ for 4 h. The extrusion treatment is: extrusion temperature 310℃, extrusion ratio 7:1.
[0048] Step 3: The extruded magnesium alloy obtained in Step 2 is annealed, pre-stretched along the extrusion direction, and aged to obtain a low-alloy high-strength magnesium alloy; the annealing treatment is performed at 380℃ for 6 min; the pre-stretching treatment along the extrusion direction is performed with a deformation of 3% and a stretching speed of 0.6 mm / min; the aging treatment is performed at 175℃ for 10 h; the yield strength of the obtained low-alloy high-strength magnesium alloy is 313 MPa.
[0049] Example 2:
[0050] In this embodiment, a low-alloy high-strength magnesium alloy is composed of the following components by mass percentage:
[0051] Sm: 1.67 wt.%, Ca: 0.37 wt.%, Mn: 0.51 wt.%, Zn: 0.06 wt.%, Al: 0.27 wt.%, Gd: 0.13 wt.%, Tb: 0.20 wt.%, Dy: 0.43 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%. The preparation method includes the following steps:
[0052] Step 1: According to the alloy composition ratio, under the protection of a mixed gas of CO2 and SF6 with a volume ratio of 98:2, pure Mg is held at 500℃ for 50 min, and then the temperature is raised to 725℃ to completely melt the pure Mg. Then, Mg-Sm, Mg-Ca, Mg-Mn, Mg-Gd, Mg-Tb, Mg-Dy master alloys, pure Zn, and pure Al are added. After standing at 720℃ for 20 min until the alloy raw materials are completely melted, the mixture is stirred, argon gas is blown in for refining and slag removal to obtain the alloy melt. The alloy melt is then injected into a preheated mold using gravity casting to obtain a magnesium alloy ingot.
[0053] Step 2: The magnesium alloy ingot obtained in Step 1 is solution treated and quenched in hot water. Then, the oxide scale is removed by turning to obtain a magnesium alloy billet. The billet and the extrusion die are preheated at 310℃ for 50 min and then extruded to obtain an extruded magnesium alloy. The solution treatment is: holding at 520℃ for 4 h. The extrusion treatment is: extrusion temperature 310℃, extrusion ratio 7:1.
[0054] Step 3: The extruded magnesium alloy obtained in Step 2 is annealed, pre-stretched along the extrusion direction, and aged to obtain a low-alloy high-strength magnesium alloy; the annealing treatment is carried out at 380℃ for 6 min; the pre-stretching treatment along the extrusion direction is carried out at a deformation amount of 3% and a stretching speed of 0.6 mm / min; the aging treatment is carried out at 175℃ for 10 h; the yield strength of the obtained low-alloy high-strength magnesium alloy is 318 MPa.
[0055] Example 3:
[0056] In this embodiment, a low-alloy high-strength magnesium alloy is composed of the following components by mass percentage:
[0057] Sm: 1.90 wt.%, Ca: 0.02 wt.%, Mn: 0.31 wt.%, Zn: 0.63 wt.%, Al: 0.25 wt.%, Gd: 0.21 wt.%, Tb: 0.24 wt.%, Dy: 0.06 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%. The preparation method includes the following steps:
[0058] Step 1: According to the alloy composition ratio, under the protection of a mixed gas of CO2 and SF6 with a volume ratio of 98:2, pure Mg is held at 490℃ for 60 min, and then the temperature is raised to 720℃ to completely melt the pure Mg. Then, Mg-Sm, Mg-Ca, Mg-Mn, Mg-Gd, Mg-Tb, Mg-Dy master alloys, pure Zn, and pure Al are added. After standing at 720℃ for 15 min to allow the alloy raw materials to completely melt, the mixture is stirred, argon gas is blown in for refining and slag removal to obtain the alloy melt. The alloy melt is then injected into a preheated mold using gravity casting to obtain a magnesium alloy ingot.
[0059] Step 2: The magnesium alloy ingot obtained in Step 1 is solution treated and quenched in hot water. Then, the oxide scale is removed by turning to obtain a magnesium alloy billet. The billet and the extrusion die are preheated at 300℃ for 60 min and then extruded to obtain an extruded magnesium alloy. The solution treatment is: holding at 520℃ for 4 h. The extrusion treatment is: extrusion temperature 300℃, extrusion ratio 7:1.
[0060] Step 3: The extruded magnesium alloy obtained in Step 2 is annealed, pre-stretched along the extrusion direction, and aged to obtain a low-alloy high-strength magnesium alloy; the annealing treatment is performed at 380℃ for 7 min; the pre-stretching treatment along the extrusion direction is performed with a deformation of 3% and a stretching speed of 0.6 mm / min; the aging treatment is performed at 175℃ for 10 h; the yield strength of the obtained low-alloy high-strength magnesium alloy is 302 MPa.
[0061] Example 4:
[0062] In this embodiment, a low-alloy high-strength magnesium alloy is composed of the following components by mass percentage:
[0063] Sm: 1.77 wt.%, Ca: 0.24 wt.%, Mn: 0.29 wt.%, Zn: 0.46 wt.%, Al: 0.29 wt.%, Gd: 0.06 wt.%, Tb: 0.04 wt.%, Dy: 0.14 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%. The preparation method includes the following steps:
[0064] Step 1: According to the alloy composition ratio, under the protection of a mixed gas of CO2 and SF6 with a volume ratio of 97:3, pure Mg is held at 490℃ for 50 min, and then the temperature is raised to 720℃ to completely melt the pure Mg. Then, Mg-Sm, Mg-Ca, Mg-Mn, Mg-Gd, Mg-Tb, Mg-Dy master alloys, pure Zn, and pure Al are added. After standing at 720℃ for 20 min to allow the alloy raw materials to completely melt, the mixture is stirred, argon gas is blown in for refining and slag removal to obtain the alloy melt. The alloy melt is then injected into a preheated mold using gravity casting to obtain a magnesium alloy ingot.
[0065] Step 2: The magnesium alloy ingot obtained in Step 1 is solution treated and quenched in hot water. Then, the oxide scale is removed by turning to obtain a magnesium alloy billet. The billet and the extrusion die are preheated at 300℃ for 50 min and then extruded to obtain an extruded magnesium alloy. The solution treatment is: holding at 520℃ for 4 h. The extrusion treatment is: extrusion temperature 300℃, extrusion ratio 7:1.
[0066] Step 3: The extruded magnesium alloy obtained in Step 2 is annealed, pre-stretched along the extrusion direction, and aged to obtain a low-alloy high-strength magnesium alloy; the annealing treatment is carried out at 380℃ for 7 min; the pre-stretching treatment along the extrusion direction is carried out at a deformation amount of 3% and a stretching speed of 0.6 mm / min; the aging treatment is carried out at 175℃ for 10 h; the yield strength of the obtained low-alloy high-strength magnesium alloy is 310 MPa.
[0067] Comparative Example 1:
[0068] The WE43 alloy reported in the paper "Optimizing the torsional properties and corrosion resistance of biodegradable WE43 Mg alloy by ECAP and subsequent aging," published in Volume 35, pp. 402-410, 2020, consists of the following mass percentages: Y: 3.97 wt.%, Nd: 2.40 wt.%, Zr: 0.55 wt.%, with the balance being Mg. Its preparation method includes the following steps: Before extrusion, the WE43 ingot is homogenized by holding at 500℃ for 18 h, then preheated at 460℃ for 2 h, and extruded at an extrusion temperature of 460℃ and an extrusion ratio of 64. The extruded bar is preheated at 250℃ for 15 min, and then ECAP treated at 250℃. The single-pass ECAP-treated sample is aged at 200℃ for 24 h, yielding a WE43 alloy with a yield strength of 255 MPa. Compared to the present invention, this comparative example has a higher rare earth element content of 6.37 wt.%, undergoes high-temperature and long-term homogenization treatment, and employs a complex ECAP deformation process. Therefore, the alloy raw materials and production costs in this comparative example are higher than those in the present invention, but its yield strength is significantly lower than that of the alloy obtained in the present invention.
[0069] Comparative Example 2:
[0070] The paper titled "Improving age hardening response and mechanical properties of a new Mg-RE alloy via simple pre-cold rolling," published in the Journal of Alloys and Compounds, Volume 777, pages 1375-1385 in 2019, reports a Mg-2.1Gd-1.7Ho-1.4Y-1.3Nd-0.9Er-0.5Zn-0.5Zr alloy, with the following mass percentages: Gd: 2.1 wt.%, Ho: 1.7 wt.%, Y: 1.4 wt.%, Nd: 1.3 wt.%, Er: 0.9 wt.%, Zn: 0.5 wt.%, Zr: 0.5 wt.%, with the balance being Mg. Its preparation method includes the following steps: the alloy sheet is solution-treated at 520℃ for 5 hours, followed by four passes of rolling, with each pass reducing the thickness by approximately 3%, resulting in a total thickness reduction of approximately 12%. The rolled sample was aged at 200℃ for 9 h, and the resulting alloy yield strength was 251 MPa. Compared with the present invention, the comparative example added a higher content and more types of rare earth elements and adopted a complex multi-pass rolling process. The present invention reduces the amount of rare earth elements added, and obtains a magnesium alloy with a yield strength superior to that of the comparative example while saving costs, reducing energy consumption, and simplifying the process.
[0071] In summary, existing technologies for improving the strength of magnesium alloys mainly involve increasing the content of alloying elements and rare earth elements, as well as complex heat treatment or large deformation processes, such as multi-stage high-temperature homogenization or multi-pass rolling. This leads to a significant increase in raw material costs, and the complex processes are energy-intensive and time-consuming, further increasing time, process costs, and energy consumption, making it difficult to achieve simultaneous improvement in alloy strength and industrial production. This invention reduces the amount of rare earth elements added to the alloy, with a rare earth element content ≤3.0 wt.%, and employs casting and conventional hot extrusion processes. By selecting appropriate annealing temperatures, pre-deformation amounts, aging temperatures, and holding times, it achieves superior results compared to existing technologies while saving costs, reducing energy consumption, and simplifying the process, obtaining magnesium alloys with a yield strength ≥300 MPa. Furthermore, different component ratios and process parameters in the embodiments of this invention result in different yield strengths, demonstrating that the advantages of this invention are not determined by a specific process or composition. This invention improves the strength of alloys and enables the industrial production of high-strength magnesium alloys by synergistically controlling the interaction between alloy components, their proportions, extrusion process parameters, and heat treatment processes, thus meeting the application needs of aerospace, 3C, and new energy vehicle industries.
[0072] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A low-alloy high-strength magnesium alloy, characterized in that, It consists of the following components by mass percentage: Sm: 1.6-1.9 wt.%, Ca: 0.01-0.4 wt.%, Mn: 0.01-0.6 wt.%, Zn: 0.01-0.7 wt.%, Al: 0.2-0.3 wt.%, Gd: 0.01-0.3 wt.%, Tb: 0.01-0.3 wt.%, Dy: 0.01-0.5 wt.%, with the remainder being Mg and unavoidable impurities, the content of unavoidable impurities being ≤0.05 wt.%.
2. The low-alloy high-strength magnesium alloy according to claim 1, characterized in that, By weight percentage, it consists of the following components composition: Sm: 1.80 wt.%, Ca: 0.35 wt.%, Mn: 0.08 wt.%, Zn: 0.03 wt.%, Al: 0.29 wt.%, Gd: 0.17 wt.%, Tb: 0.13 wt.%, Dy: 0.30 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%.
3. The low-alloy high-strength magnesium alloy according to claim 1, characterized in that, It consists of the following components by weight percentage: Sm: 1.67 wt.%, Ca: 0.37 wt.%, Mn: 0.51 wt.%, Zn: 0.06 wt.%, Al: 0.27 wt.%, Gd: 0.13 wt.%, Tb: 0.20 wt.%, Dy: 0.43 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%.
4. The low-alloy high-strength magnesium alloy according to claim 1, characterized in that, By weight percentage, it consists of the following components composition: Sm: 1.90 wt.%, Ca: 0.02 wt.%, Mn: 0.31 wt.%, Zn: 0.63 wt.%, Al: 0.25 wt.%, Gd: 0.21 wt.%, Tb: 0.24 wt.%, Dy: 0.06 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%.
5. The low-alloy high-strength magnesium alloy according to claim 1, characterized in that, It consists of the following components by weight percentage: Sm: 1.77 wt.%, Ca: 0.24 wt.%, Mn: 0.29 wt.%, Zn: 0.46 wt.%, Al: 0.29 wt.%, Gd: 0.06 wt.%, Tb: 0.04 wt.%, Dy: 0.14 wt.%, with the remainder being Mg and unavoidable impurities, the content of which is ≤0.05 wt.%.
6. A method for preparing a low-alloy high-strength magnesium alloy as described in any one of claims 1-5, characterized in that, Includes the following steps: Step 1: Under the protection of a mixed gas with a CO2 and SF6 volume ratio of (97-99):(3-1), pure Mg is held at 480-510℃ for 40-60 min, and then the temperature is raised to 700-730℃ to completely melt the pure Mg. Mg-Sm, Mg-Ca, Mg-Mn, Mg-Gd, Mg-Tb, Mg-Dy master alloys, pure Zn, and pure Al are added. The mixture is allowed to stand at 700-730℃ for 10-20 min until the alloy raw materials are completely melted. After stirring, argon gas is blown in for refining and slag removal to obtain the alloy melt. The alloy melt is then injected into a preheated mold using gravity casting to obtain a magnesium alloy ingot. Step 2: The magnesium alloy ingot obtained in Step 1 is solution treated and quenched in hot water, then the oxide scale is removed by turning to obtain a magnesium alloy billet; the billet and extrusion die are preheated at 300-320℃ for 40-60 min and then extruded to obtain an extruded magnesium alloy; the solution treatment is: holding at 510-520℃ for 3.5-4.5 h; the extrusion is: extrusion temperature 300-320℃, extrusion ratio (6-8):1; Step 3: The extruded magnesium alloy obtained in Step 2 is annealed, pre-stretched along the extrusion direction, and then aged to obtain a low-alloy high-strength magnesium alloy. The annealing treatment is performed at 375-385℃ for 6-7 min. The pre-stretching treatment is performed with a deformation of 2-4% and a stretching speed of 0.5-0.7 mm / min. The aging treatment is performed at 160-180℃ for 9-11 h.
7. The method for preparing low-alloy high-strength magnesium alloy according to claim 6, characterized in that, In step 1, the volume ratio of CO2 to SF6 is 99:1, 98:2, or 97:3; Pure Mg is first held at 490–500℃ for 50–60 min, then heated to 720–725℃; after adding intermediate alloy, pure Zn, and pure Al, it is allowed to stand at 720℃ for 15–20 min.
8. The method for preparing low-alloy high-strength magnesium alloy according to claim 6, characterized in that, In step 2, the solution treatment is performed by holding at 520°C for 4 hours; the billet and extrusion die are preheated at 300-310°C for 50-60 minutes; the extrusion temperature is 300-310°C and the extrusion ratio is 7:
1.
9. The method for preparing low-alloy high-strength magnesium alloy according to claim 6, characterized in that, In step 3, the annealing treatment is performed at 380℃ for 6-7 min; the pre-stretch deformation is 3% and the stretching speed is 0.6 mm / min; the aging treatment is performed at 175℃ for 10 h.