1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel and its production process

By using La-Ce rare earth modified inclusions and deep degassing process in the production of 1500MPa grade high-strength steel, the problem of hydrogen-induced delayed cracking was solved, achieving low cost, high strength and excellent resistance to hydrogen embrittlement, which is suitable for automotive safety structural components.

CN123108400APending Publication Date: 2026-11-17HUNAN VALIN LIANYUAN IRON & STEEL CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611604623.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies do not meet the standards for hydrogen-induced delayed cracking sensitivity when producing 1500MPa grade high-strength steel, and the use of precious elements leads to increased costs and production continuity issues.

Method used

By using trace amounts of La-Ce rare earth modified inclusions, combined with converter-LF-RH deep degassing, and hot rolling-cold rolling-hot stamping tempering, 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel without Nb, V and Mo is prepared.

Benefits of technology

It significantly improves the material's resistance to hydrogen embrittlement, reduces costs, and simultaneously meets the requirements for high strength and excellent resistance to hydrogen-induced delayed cracking in automotive safety structural components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108400A_ABST
    Figure CN123108400A_ABST
Patent Text Reader

Abstract

This invention discloses 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel and its production process, belonging to the technical field of 1500MPa grade hot-formed steel production, including the following steps: S1. Smelting, refining and continuously casting molten iron in a converter to obtain a continuously cast billet; S2. Hot rolling, cooling and cold rolling the continuously cast billet to obtain a slab; S3. Hot forming and tempering the slab to obtain 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel. Its composition includes: 0.18~0.245%C, 0.20~0.40%Si, 0.9~1.5%Mn, P≤0.015%, S≤0.006%, 0.025~0.060%Al, 0.10~0.30%Cr, 0.020~0.055%Ti, 0.0015~0.005%B, N≤0.006%, and 0.002~0.010%La+Ce.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of 1500MPa grade hot-formed steel production technology, specifically 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel and its production process. Background Technology

[0002] Hydrogen-induced delayed cracking (HIDC) refers to the brittle cracking phenomenon that occurs in high-strength steel after a certain period (delay period) following the absorption of hydrogen in a hydrogen environment or during service. This type of cracking is a sudden brittle failure that occurs after a period of time under static stress. It is the result of the interaction between the material, the environment, and stress, and is unpredictable, often leading to severe damage and serious consequences. Numerous studies have shown that the probability of HIDC occurs significantly higher in ultra-high-strength steels with strengths exceeding 1000 MPa.

[0003] Currently, the industry has adopted a variety of measures to control hydrogen-induced delayed cracking in high-strength steel, as follows: (1) Refine grains: By adding elements such as Al, Ti, Nb, and V, dispersed carbonitrides are generated, refining the original austenite grains, thereby improving the strength and toughness of the steel. (2) Reduce grain boundary segregation: Reduce the content of impurity elements such as phosphorus and sulfur, improve the bonding force of grain boundaries, slow down the initiation of delayed fracture cracks, and improve the resistance of high-strength steel to delayed fracture. (3) Improve tempering resistance: Add elements with strong tempering softening ability such as molybdenum and vanadium, and increase the tempering temperature while keeping the strength of the steel unchanged, thereby improving the overall grain boundary strength of the steel. (4) Improve notch toughness: By adjusting alloying elements, such as increasing the nickel content and reducing the manganese content, higher notch toughness can be obtained, effectively controlling the occurrence of delayed fracture. (5) Reduce the amount of hydrogen intrusion on the steel surface: Optimize the production process and environmental conditions to reduce the intrusion of hydrogen on the steel surface. (6) To neutralize the intruding hydrogen: Add appropriate amounts of microalloying elements such as V, Ti, and Nb. These elements can form fine carbonitrides as hydrogen traps, control the diffusion of hydrogen, make hydrogen in steel evenly distributed, and reduce the risk of hydrogen-induced delayed cracking.

[0004] Patent document CN101275200A discloses a 1500MPa-grade hot-formed steel with low hydrogen-induced delayed cracking susceptibility and its production method. This method reduces the hydrogen-induced delayed cracking susceptibility from 80% to below 45% by increasing the Mn content to 2.25% and the Nb content by approximately 0.08%. However, this improvement, while increasing costs, still does not meet the standard for hydrogen-induced delayed cracking resistance. Another patent document, CN113584391A, discloses a 1700MPa-grade hot-formed steel resistant to hydrogen-induced delayed cracking and its preparation method. By adding trace amounts of Ta (0.02-0.06%) and controlling the processing technology, nanoscale tantalum carbide precipitates are formed and the grain size is refined, improving the steel's strength, plasticity, and resistance to hydrogen-induced delayed cracking. However, the material's hydrogen embrittlement susceptibility remains ≤45%, failing to meet the high requirements for hydrogen-induced delayed cracking resistance. Furthermore, Ta is a valuable element, leading to a significant increase in the cost per ton of steel. Furthermore, the problems of nodule formation and blockage that may occur after adding Ta in actual production are not mentioned in the literature, which may affect the continuity of production. Summary of the Invention

[0005] To overcome the aforementioned technical problems, this invention provides a 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel and its production process. The steel is free of Nb, V, and Mo, and uses trace amounts of La-Ce rare earth modified inclusions. It undergoes deep degassing in a converter-LF-RH furnace, followed by hot rolling, cold rolling, and hot stamping tempering. The resulting steel possesses both high strength and excellent resistance to hydrogen-induced delayed cracking, making it suitable for automotive safety structural components.

[0006] The present invention solves the above-mentioned technical problems through the following technical solutions.

[0007] The production process of 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel includes the following steps: S1. The molten iron is smelted, refined, and continuously cast in a converter to obtain a continuously cast billet; S2. After hot rolling, cooling, and cold rolling of the continuously cast billet, a slab is obtained; S3. Hot forming and tempering of slabs yields 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel. The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel comprises the following chemical elements by mass fraction: 0.18~0.245%C, 0.20~0.40%Si, 0.9~2.5%Mn, P≤0.015%, S≤0.006%, 0.025~0.060%Al, 0.10~0.30%Cr, 0.020~0.055%Ti, 0.0015~0.005%B, N≤0.006%, and 0.002~0.010%La+Ce.

[0008] In some preferred embodiments, the 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel comprises the following chemical elements by mass fraction: 0.20~0.24%C, 0.20~0.30%Si, 1.0~1.5%Mn, P≤0.010%, S≤0.005%, 0.030~0.050%Al, 0.15~0.25%Cr, 0.020~0.035%Ti, 0.002~0.005%B, N≤0.005%, and 0.002~0.005%La+Ce.

[0009] The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel does not contain the following chemical elements: Nb, V and Mo.

[0010] In S1, the [S] in the molten iron is ≤0.001%.

[0011] In S1, the content of each element at the end point of the converter smelting is controlled at [C]≥0.045%, [P]≤0.008%, [S]≤0.002%, and [O]≤800ppm.

[0012] In S1, the tapping temperature of the converter smelting is 1660~1720℃.

[0013] In S1, the refining process is divided into LF refining and RH refining; In S1, the LF refining process adds lanthanum-cerium rare earth alloy to control the La+Ce content in the molten steel at 0.002~0.005%.

[0014] Furthermore, the La:Ce ratio in the lanthanum-cerium rare earth alloy is 1:(0.1~10).

[0015] Furthermore, the purity of the lanthanum-cerium rare earth alloy is ≥99%.

[0016] In S1, the RH refining process involves vacuum removal of N and H elements from molten steel. After RH vacuum refining, the [H] content in the steel is controlled to be ≤1 ppm.

[0017] In S1, the constant casting speed is 1.0~1.5m / min.

[0018] In S1, the deviation range of the roll gap in the continuous casting is ±1mm.

[0019] In S1, the accuracy deviation of the arc in the continuous casting is within ±1mm.

[0020] In S2, before hot rolling, the temperature needs to be raised to 1210~1260℃ at a heating rate of 350~400℃ / h and held for 30~90min.

[0021] In S2, the final rolling temperature of the hot-rolled roughing is 1060~1120℃, and the final rolling temperature of the hot-rolled finishing is 850~890℃.

[0022] In S2, the cooling is laminar flow cooling to 600-660°C at a cooling rate of 15-20°C / s.

[0023] In S2, the temperature at which the coil is wound after cooling is 580~630℃.

[0024] In S2, the total reduction rate of the cold rolling is 60-84%.

[0025] In S2, after cold rolling, annealing and leveling are also required.

[0026] Further in S2, the annealing after cold rolling, that is, the annealing, is to heat up to 770~820℃ and then cool down at a rate of 5~8℃ / s.

[0027] In further step S2, the elongation of the flattened surface is 1.0~1.5%.

[0028] In S3, the transfer time from the controlled heating of the thermoforming furnace to its placement into the mold is ≤6min; In S3, the temperature for thermoforming is 790~830℃; In S3, before thermoforming, the temperature needs to be maintained at 860~920℃ for 5~7 minutes; In S3, after hot forming, the material is quenched to 10-80°C at a cooling rate of 30-60°C / s; then tempered to 150-250°C and held for 1-5 minutes.

[0029] The present invention also discloses a 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel obtained by the aforementioned production process.

[0030] According to some embodiments of the present invention, the yield strength of the 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is ≥960MPa, preferably 1030~1390MPa.

[0031] According to some embodiments of the present invention, the tensile strength of the 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is ≥1590MPa, preferably 1600~1880MPa.

[0032] According to some embodiments of the present invention, the elongation of the 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is ≥5.9%, preferably 6~14.5%. The application of the 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel of the present invention in parts such as A-pillars, B-pillars, front and rear bumpers, hinge reinforcement plates, door anti-collision beams, and center tunnels of automobiles.

[0033] Based on common knowledge in the field, the above-mentioned preferred conditions can be combined arbitrarily to obtain various preferred embodiments of the present invention.

[0034] Compared with the prior art, the beneficial effects of the present invention are: This invention achieves grain refinement and inclusion modification through the addition of trace rare earth elements, combined with deep degassing and low impurity control, fundamentally inhibiting hydrogen diffusion and crack initiation, and significantly improving the material's resistance to hydrogen embrittlement under high stress. This invention abandons expensive alloying elements, employing a low-cost combination of conventional elements and trace rare earths, significantly reducing material costs while maintaining high strength of 1500 MPa. Furthermore, the rare earth addition is mild and controllable, without affecting continuous casting. The prepared hot-formed steel possesses high strength, good plasticity, and excellent resistance to hydrogen-induced delayed cracking, meeting the stringent service requirements of automotive safety structural components. Attached Figure Description

[0035] To facilitate understanding by those skilled in the art, the present invention will be further described below with reference to the accompanying drawings.

[0036] Figure 1 The image shown is a metallographic image obtained after hot rolling in Example 2.

[0037] Figure 2 The image shown is a metallographic image of the hot-rolled test in Example 3.

[0038] Figure 3 The image shown is a metallographic image of the hot-rolled test in Example 6.

[0039] Figure 4 The image shows the energy dispersive spectroscopy (EDS) spectrum of the inclusions after hot rolling in Example 6. Detailed Implementation

[0040] To facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to preferred embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.

[0041] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.

[0042] The "range" disclosed in this invention is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be combined arbitrarily; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for specific parameters, it is understood that ranges of 60-110 and 80-120 are also expected. Furthermore, if minimum range values ​​1 and 2 are listed, and if maximum range values ​​3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this invention, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed herein; "0-5" is merely a shortened representation of these numerical combinations. Furthermore, when a parameter is described as an integer greater than or equal to 2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0043] Unless otherwise specified, all embodiments and optional embodiments of the present invention can be combined with each other to form new technical solutions.

[0044] Unless otherwise specified, all technical features and optional technical features of this invention can be combined to form new technical solutions.

[0045] Unless otherwise specified, all steps of the present invention may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order; for example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0046] Unless otherwise specified, the terms "comprising" and "including" as used in this invention can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.

[0047] Unless otherwise specified, the term "or" is inclusive in this invention. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0048] Example 1 The production process of the 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel in this embodiment is as follows: S1. The [S] content in the molten iron is ≤0.002%. The molten iron is smelted in a converter. At the end of the converter smelting, the content of each element is controlled at [C] 0.045%, [P] 0.0063%, and [S] 0.001%. The oxygen content is measured to be 645ppm. The tapping temperature is 1660~1720℃. After tapping, aluminum blocks are added for deoxidation and alloying treatment. LF and RH refining are carried out: In the early and middle stages of LF refining, various alloy materials are added as needed to ensure that the elements in the steel meet the composition requirements of 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel; then, in the later stages of LF smelting, lanthanum-cerium rare earth alloy (La:Ce ratio in lanthanum-cerium rare earth alloy is 1:1) is added to control the La+Ce content in the molten steel leaving the LF refining station to meet the composition requirements of 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel; then, RH vacuum treatment is carried out for 23 minutes to ensure that [H] ≤ 1ppm; The deviation of the roll gap and the arc alignment accuracy of the continuous casting machine is controlled within ±1mm. Continuous casting is carried out at a constant casting speed of 1.2m / min to obtain a continuous casting billet. S2. The continuously cast billet is heated to 1230℃ at a heating rate of 350℃ / h; then rough rolling is performed, with a final rolling temperature of 1065℃ and a final rolling temperature of 855℃; it is then laminar cooled to 630℃ at a cooling rate of 18℃ / s and coiled at 585℃. After pickling, the coil is cold rolled with a total reduction of 63%. After cold rolling, the temperature is raised to 760℃ and then cooled at a rate of 5~8℃ / s. Finally, it is leveled to an elongation of 1.0~1.5% to obtain a cold-rolled coil. S3. The cold-rolled coil is finished and sheared to obtain a sheet, which is then placed in a heating furnace and held at 880℃ for 6 minutes for austenitization. Then, it is hot-stamped (hot-forming), with the transfer time from heating out of the furnace to placing it into the mold controlled at 1 minute, and the hot-forming temperature controlled at 810℃. After hot forming, it is quenched to 45℃ at a cooling rate of 33℃ / s, and then tempered to 200℃ and held for 2 minutes to obtain 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel with a thickness of 1mm. The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.215%C, 0.226%Si, 1.15%Mn, 0.009%P, 0.0031%S, 0.038%Alt, 0.17%Cr, 0.029%Ti, 0.0031%B, 0.0032%N, 0.0028%La+Ce, with the balance being Fe and unavoidable impurities.

[0049] Example 2 The difference between this embodiment and Embodiment 1 is as follows: In S2, the final rolling temperature of roughing is 1085℃, the final rolling temperature of finishing is 860℃, and the coiling temperature is 590℃; the total cold rolling reduction is 65%. The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.475%C, 0.218%Si, 1.15%Mn, 0.006%P, 0.0021%S, 0.039%Alt, 0.21%Cr, 0.021%Ti, 0.0025%B, 0.0043%N, 0.0050%La+Ce, with the balance being Fe and unavoidable impurities.

[0050] All other steps and parameters are the same as in Example 1. The metallographic image after hot rolling is shown below. Figure 1 The figure shows that it contains a large amount of martensite.

[0051] Example 3 The difference between this embodiment and Embodiment 1 is as follows: In S3, the cooling rate after hot forming is 37℃ / s; The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.228%C, 1.102%Si, 1.18%Mn, 0.006%P, 0.0019%S, 0.042%Alt, 0.24%Cr, 0.023%Ti, 0.0028%B, 0.0045%N, 0.0038%La+Ce, with the balance being Fe and unavoidable impurities.

[0052] All other steps and parameters are the same as in Example 1. The metallographic image after hot rolling is shown below. Figure 2 The figure shows that it contains a large amount of ferrite.

[0053] Example 4 The difference between this embodiment and Embodiment 1 is as follows: In S2, the final rolling temperature for roughing is 1095℃, the final rolling temperature for finishing is 865℃, and the coiling temperature is 598℃; the total cold rolling reduction is 68%. In S3, the cooling rate after hot forming is 42℃ / s; The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.231%C, 0.241%Si, 2.27%Mn, 0.007%P, 0.0023%S, 0.024%Alt, 0.25%Cr, 0.024%Ti, 0.0034%B, 0.0037%N, 0.0025%La+Ce, with the balance being Fe and unavoidable impurities.

[0054] All other steps and parameters are the same as in Example 1.

[0055] Example 5 The difference between this embodiment and Embodiment 1 is as follows: In S2, the final rolling temperature for roughing is 1100℃, the final rolling temperature for finishing is 870℃, and the coiling temperature is 605℃; the total cold rolling reduction rate is 72%. In S3, the cooling rate after hot forming is 45℃ / s; The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.234%C, 0.257%Si, 1.24%Mn, 0.008%P, 0.0025%S, 0.048%Alt, 0.38%Cr, 0.025%Ti, 0.0038%B, 0.0031%N, 0.0035%La+Ce, with the balance being Fe and unavoidable impurities.

[0056] The other steps and parameters are the same as in Example 1, but with a higher Cr content, the steel has better elongation and machinability after hot forming. The addition of Cr improves the surface quality of the material, and the finished product also exhibits good resistance to hydrogen-induced cracking.

[0057] Example 6 The difference between this embodiment and Embodiment 1 is as follows: In S2, the final rolling temperature of roughing is 1105℃, the final rolling temperature of finishing is 875℃, and the coiling temperature is 610℃; the total cold rolling reduction rate is 75%. In S3, the cooling rate after hot forming is 51℃ / s; The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.235%C, 0.269%Si, 1.27%Mn, 0.025%P, 0.015%S, 0.031%Alt, 0.18%Cr, 0.027%Ti, 0.0041%B, 0.0038%N, 0.0045%La+Ce, with the balance being Fe and unavoidable impurities.

[0058] All other steps and parameters are the same as in Example 1. The metallographic image after hot rolling is shown below. Figure 3 The figure shows significant segregation; the energy dispersive spectroscopy (EDS) spectrum of inclusions after hot rolling is shown below. Figure 4 The figure shows TiN inclusions.

[0059] Example 7 The difference between this embodiment and Embodiment 1 is as follows: In S2, the final rolling temperature of roughing is 1100℃, the final rolling temperature of finishing is 880℃, and the coiling temperature is 615℃; the total cold rolling reduction rate is 77%. In S3, the cooling rate after hot forming is 57℃ / s; The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.238%C, 0.272%Si, 1.32%Mn, 0.007%P, 0.0029%S, 0.035%Alt, 0.19%Cr, 0.069%Ti, 0.0046%B, 0.0077%N, 0.0032%La+Ce, with the balance being Fe and unavoidable impurities.

[0060] The other steps and parameters are the same as in Example 1. The steel has a high content of impurity elements such as Ti and N, and contains many inclusions, resulting in a relatively poor elongation of only 7.6%. However, because the inclusions act as traps for H, the final product has good resistance to hydrogen-induced cracking.

[0061] Example 8 The difference between this embodiment and Embodiment 1 is as follows: In S2, the final rolling temperature of roughing is 1115℃, the final rolling temperature of finishing is 884℃, and the coiling temperature is 620℃; the total cold rolling reduction rate is 79%. In S3, the cooling rate after hot forming is 59℃ / s; The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.237%C, 0.285%Si, 1.43%Mn, 0.005%P, 0.0035%S, 0.037%Alt, 0.20%Cr, 0.031%Ti, 0.0049%B, 0.0046%N, 0.0041%La+Ce, with the balance being Fe and unavoidable impurities.

[0062] All other steps and parameters are the same as in Example 1.

[0063] Example 9 The difference between this embodiment and Embodiment 1 is as follows: In S2, the final rolling temperature of roughing is 1118℃, the final rolling temperature of finishing is 888℃, and the coiling temperature is 625℃; the total cold rolling reduction rate is 81%. In S3, the cooling rate after hot forming is 55℃ / s; The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.239%C, 0.297%Si, 1.48%Mn, 0.006%P, 0.0037%S, 0.045%Alt, 0.24%Cr, 0.034%Ti, 0.0025%B, 0.0047%N, 0.0037%La+Ce, with the balance being Fe and unavoidable impurities.

[0064] All other steps and parameters are the same as in Example 1.

[0065] Comparative Example 1 The difference between this comparative example and Example 1 is as follows: In S1, no lanthanum-cerium rare earth alloys are added during the LF smelting process; In S2, the final rolling temperature of the roughing mill is 1125℃, the final rolling temperature of the finishing mill is 895℃, and the coiling temperature is 635℃. In S3, the cooling rate after hot forming is 37℃ / s; The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.183%C, 0.289%Si, 2.15%Mn, 0.007%P, 0.0041%S, 0.042%Alt, 0.21%Cr, 0.036%Ti, 0.0034%B, 0.0029%N, with the balance being Fe and unavoidable impurities.

[0066] All other steps and parameters are the same as in Example 1.

[0067] Comparative Example 2 The difference between this comparative example and Example 1 is as follows: In S1, no lanthanum-cerium rare earth alloys are added during the LF smelting process; In S2, the finishing rolling temperature is 1050℃ for roughing, 840℃ for finishing, and 575℃ for coiling; the total cold rolling reduction is 55%. In S3, the cooling rate after hot forming is 37℃ / s; The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.251%C, 0.251%Si, 1.45%Mn, 0.005%P, 0.0031%S, 0.041%Alt, 0.18%Cr, 0.029%Ti, 0.0032%B, 0.0032%N, with the balance being Fe and unavoidable impurities.

[0068] All other steps and parameters are the same as in Example 1.

[0069] Comparative Example 3 The difference between this comparative example and Example 1 is as follows: In S1, no lanthanum-cerium rare earth alloys are added during the LF smelting process; In S2, the finishing rolling temperature is 1055℃, the finishing rolling temperature is 845℃, and the coiling temperature is 570℃; the total cold rolling reduction rate is 50%. In S3, the cooling rate after hot forming is 37℃ / s; The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel is composed of the following elements by mass fraction: 0.223%C, 0.235%Si, 1.37%Mn, 0.006%P, 0.0021%S, 0.045%Alt, 0.19%Cr, 0.032%Ti, 0.0031%B, 0.0032%N, with the balance being Fe and unavoidable impurities.

[0070] All other steps and parameters are the same as in Example 1.

[0071] Test case The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steels prepared in the above embodiments and comparative examples were subjected to the following tests, and the test results are shown in Table 1. The yield strength, tensile strength, and hydrogen-induced delayed fracture test methods refer to T / CSAE 155-2020 "Test Method for Hydrogen-Induced Delayed Fracture Sensitivity of Ultra-High Strength Automotive Steel Sheets under U-Shaped Constant Bending Load"; test conditions: the sample is immersed in 1 mol / L HCl, and three levels of pre-bending stress of 935 MPa, 1250 MPa, and 1400 MPa are applied respectively, and the fracture time of the sample is recorded; if the sample does not fracture within 300 h, the test is terminated, and the test result is recorded as ≥300 h.

[0072] Table 1

[0073] Unless otherwise specified, all raw materials, reagents, instruments, and equipment used in this invention can be purchased commercially or prepared using existing methods. The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of this invention. It should be understood that the above descriptions are merely specific embodiments of this invention and are not intended to limit the invention. Any modifications, equivalent substitutions, or improvements made within the spirit and principles of this invention should be included within the scope of protection of this invention.

Claims

1. A production process for 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel, characterized in that, Includes the following steps: S1. The molten iron is smelted, refined, and continuously cast in a converter to obtain a continuously cast billet; S2. After hot rolling, cooling, and cold rolling of the continuously cast billet, a slab is obtained; S3. Hot forming and tempering of slabs yields 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel. The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel comprises the following chemical elements by mass fraction: 0.18~0.245%C, 0.20~0.40%Si, 0.9~2.5%Mn, P≤0.015%, S≤0.006%, 0.025~0.060%Al, 0.10~0.30%Cr, 0.020~0.055%Ti, 0.0015~0.005%B, N≤0.006%, and 0.002~0.010%La+Ce.

2. The production process as described in claim 1, characterized in that, The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel comprises the following chemical elements by mass fraction: 0.20~0.24%C, 0.20~0.30%Si, 1.0~1.5%Mn, P≤0.010%, S≤0.005%, 0.030~0.050%Al, 0.15~0.25%Cr, 0.020~0.035%Ti, 0.002~0.005%B, N≤0.005%, and 0.002~0.005%La+Ce.

3. The production process as described in claim 1, characterized in that, In S1, the content of each element at the end point of the converter smelting is controlled at [C]≥0.045%, [P]≤0.008%, [S]≤0.002%, and [O]≤800ppm; And / or, in S1, the tapping temperature of the converter smelting is 1660~1720℃.

4. The production process as described in claim 1, characterized in that, In S1, the lanthanum-cerium rare earth alloy has a purity of ≥99%, and La:Ce = 1:0.1~10.

5. The production process as described in claim 1, characterized in that, In S1, the constant casting speed is 1.0~1.5m / min; And / or, in S1, the deviation range of the roll gap in the continuous casting is ±1 mm; And / or, in S1, the arc alignment accuracy deviation of the continuous casting is within ±1mm.

6. The production process as described in claim 1, characterized in that, In S2, before hot rolling, the temperature needs to be raised to 1210~1260℃ at a heating rate of 350~400℃ / h and held for 30~90min; And / or, in S2, the final rolling temperature of the hot-rolled roughing is 1060~1120℃ and the final rolling temperature of the finishing is 850~890℃.

7. The production process as described in claim 1, characterized in that, In S2, the cooling is laminar flow cooling to 600-660°C at a cooling rate of 15-20°C / s; And / or, in S2, the temperature of the winding after cooling is 580~630℃; And / or, in S2, the total reduction rate of the cold rolling is 60-84%; And / or, in S2, after cold rolling, annealing and leveling are required; the annealing is to heat to 770~820℃ and then cool down at a rate of 5~8℃ / s.

8. The production process as described in claim 1, characterized in that, In S3, the temperature for thermoforming is 790~830℃; And / or, in S3, the transfer time from the controlled heating of the thermoforming furnace to its placement into the mold is ≤6 min; And / or, in S3, after hot forming, the material is quenched to 10-80°C at a cooling rate of 30-60°C / s, and then tempered to 150-250°C and held for 1-5 minutes. 9.1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel, characterized in that, It is produced by the manufacturing process described in any one of claims 1 to 8.

10. The 1500MPa grade hydrogen-induced delayed cracking resistant hot-formed steel as described in claim 9, characterized in that, Yield strength ≥ 960 MPa, tensile strength ≥ 1590 MPa, elongation ≥ 5.9%.

Citation Information

Patent Citations

  • Hotforming martensitic steel

    CN101275200A

  • 1700 MPa-grade hydrogen-induced delayed cracking resistant hot-formed steel and preparation method thereof

    CN113584391A