A low-expansion, high-specific-strength, and high-specific-stiffness iron-nickel alloy and its preparation method.

By optimizing the proportions of C, Mn, Si, Ni, Cr, and V, a stable austenitic microstructure and a composite reinforced structure of dispersed carbides are formed, solving the problem that existing low-expansion iron-nickel alloys cannot simultaneously achieve high specific strength and high specific stiffness. This achieves synergistic optimization of low thermal expansion, high specific stiffness, and low density over a wide temperature range, making it suitable for high-precision service environments such as aerospace.

CN123108416APending Publication Date: 2026-11-17XIAN GANGYAN SPECIAL ALLOY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610972548.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-01
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing low-expansion iron-nickel alloys cannot simultaneously achieve high specific strength and high specific stiffness, and have a high coefficient of thermal expansion over a wide temperature range, which cannot meet the requirements of high-precision service environments such as aerospace.

Method used

By optimizing the proportions of C, Mn, Si, Ni, Cr, and V, a stable austenitic microstructure and a composite reinforced structure of dispersed carbides are formed. Ni ensures low expansion characteristics, while C, Cr, and V form precipitation strengthening and fine grain strengthening. Mn and Si improve the uniformity and plasticity of the microstructure. By controlling the matching relationship of Cr, V, and C, low thermal expansion, high specific strength, high specific stiffness, and good comprehensive mechanical properties are achieved.

Benefits of technology

It achieves synergistic optimization of low thermal expansion, high specific strength, high specific stiffness, and low density over a wide temperature range, resulting in more stable and consistent material properties, making it suitable for aerospace structural components, precision instrument support components, and high-precision mechanical parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108416A_ABST
    Figure CN123108416A_ABST
Patent Text Reader

Abstract

This invention relates to the field of iron-nickel alloy technology, specifically to an iron-nickel alloy with low expansion, high specific strength, and high specific stiffness, and its preparation method. The alloy comprises, by mass percentage, 0.05%~0.18% C, 0.2%~0.5% Mn, 0.15%~0.25% Si, 33%~35% Ni, 0.4%~0.8% Cr, 0.4%~0.8% V, (V+Cr)≤1.6%, 5.0≤(V+Cr) / C≤15.0, Mn / Si≥2.0, with the balance being Fe and unavoidable impurities. This invention optimizes the proportions of C, Mn, Si, Ni, Cr, and V. Ni ensures low expansion characteristics, C forms dispersed carbides with Cr and V to achieve precipitation strengthening and grain refinement, Mn and Si improve microstructure uniformity and plasticity, and by controlling the matching relationship of Cr, V, and C, the alloy density is reduced while maintaining low thermal expansion, high specific strength, high specific stiffness, and good comprehensive mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of iron-nickel alloy technology, specifically to an iron-nickel alloy with low expansion, high specific strength and high specific stiffness and its preparation method. Background Technology

[0002] Low-expansion, high-performance iron-nickel alloys are widely used in aerospace precision structural components, optical instrument support components, electronic packaging, and high-precision mechanical parts due to their excellent dimensional stability, high specific strength, and high specific stiffness. During service, these materials typically need to maintain an extremely low coefficient of thermal expansion over a wide temperature range while also possessing high mechanical properties to meet the structural stability requirements of high-precision service environments.

[0003] Existing low-expansion iron-nickel alloy systems are mostly based on Fe-Ni binary or Fe-Ni-based multi-element alloys, with performance controlled by adding small amounts of alloying elements. However, while achieving low thermal expansion characteristics, it is difficult to simultaneously achieve high specific strength and high specific stiffness. Summary of the Invention

[0004] (a) Purpose of the invention The purpose of this invention is to provide a low-expansion, high-specific-strength, and high-specific-stiffness iron-nickel alloy and its preparation method. By optimizing the ratio of C, Mn, Si, Ni, Cr, and V, Ni ensures low expansion characteristics, C forms dispersed carbides with Cr and V to achieve precipitation strengthening and grain refinement, Mn and Si improve microstructure uniformity and plasticity, and by controlling the matching relationship of Cr, V, and C, the alloy density is reduced while taking into account low thermal expansion, high specific strength, high specific stiffness, and good comprehensive mechanical properties.

[0005] (II) Technical Solution To address the aforementioned problems, this invention provides a low-expansion, high-specific-strength, and high-specific-stiffness iron-nickel alloy. The alloy comprises: C, Mn, Si, Ni, Cr, V, Fe, and unavoidable impurities. By mass percentage, C is 0.05%~0.18%, Mn is 0.2%~0.5%, Si is 0.15%~0.25%, Ni is 33%~35%, Cr is 0.4%~0.8%, V is 0.4%~0.8%, (V+Cr)≤1.6%, 5.0≤(V+Cr) / C≤15.0, Mn / Si≥2.0, and the balance is Fe and unavoidable impurities.

[0006] In another aspect of the present invention, preferably, Mn / Si ≥ 1.5.

[0007] In another aspect of the invention, preferably, (V+Cr) ≤ 1.4%, 7.0 ≤ (V+Cr) / C ≤ 12.0.

[0008] In another aspect of the present invention, preferably, a method for preparing a low-expansion, high-specific-strength, and high-specific-stiffness iron-nickel alloy includes: weighing a first raw material, a second raw material, and a third raw material according to the composition ratio of the alloy, wherein the first raw material includes Fe-Ni recycled material, pure iron, and electrolytic nickel plate, the second raw material includes manganese and silicon, and the third raw material includes vanadium, chromium, and carbon; The first raw material is smelted, deoxidized, and refined to obtain a first alloy; Under preset environmental parameters, the second raw material is added to the first alloy, and the third raw material is added at preset time intervals to obtain the second alloy; The second alloy is forged, hot-rolled, and solution-treated to obtain the alloy.

[0009] In another aspect of the present invention, preferably, the step of smelting, deoxidizing, and refining the first raw material to obtain the first alloy includes: The first raw material is vacuum melted, the vacuum is drawn to less than 10Pa, preheated with 20Kw~30Kw power for 20min~30min, heated with 40Kw~60Kw power until the material melts, and heated with 60Kw~65Kw power for 10min~15min. During deoxidation, the deoxidized graphite carbon is added in three portions, with each addition being 0.02% to 0.03% of the furnace charge. The refining process is carried out using 60kW of power, and the refining time is 40-50 minutes.

[0010] In another aspect of the present invention, preferably, the step of adding the second raw material to the first alloy under preset environmental parameters, and adding the third raw material at preset time intervals to obtain the second alloy includes: The second raw material is added to the first alloy under preset environmental parameters, including a protective atmosphere and a vacuum of -0.50 MPa. The third raw material is added at a preset time interval, which is 5 minutes. After a 5-minute interval, the mixture is poured and cooled for more than 12 hours before demolding to obtain the second alloy.

[0011] In another aspect of the invention, preferably, the forging includes: The second alloy is loaded into the furnace at a temperature of less than or equal to 450°C, and heated to 850±10°C at a rate of 60°C / h~80°C / h and held for 3h~5h. The furnace temperature is raised to 1100±10℃ and held for 1 to 2 hours before forging. The forging was carried out using a 750Kg free forging hammer, with a forging size of 50×200mm, an initial forging temperature of ≥1050℃, and a final forging temperature of ≥900℃.

[0012] In another aspect of the invention, preferably, the hot rolling comprises: After removing the oxide scale from the surface of the second alloy after forging, the furnace is loaded at a temperature of less than or equal to 450°C, and the temperature is increased to 850±10°C at a rate of 60°C / h~80°C / h and held for 3h~4h. Heat the furnace to 1080±10℃ and hold for 1~2 hours; Hot rolling is carried out using a four-roll hot rolling mill. The hot rolling size is 15×200mm, the initial rolling temperature is greater than or equal to 1050℃, and the final rolling temperature is greater than or equal to 900℃.

[0013] In another aspect of the present invention, preferably, the solution treatment includes: The hot-rolled second alloy is loaded into the furnace at a temperature of less than or equal to 300°C, and spacers are placed between adjacent hot-rolled second alloys, the thickness of which is greater than or equal to the thickness of the hot-rolled second alloy. Heat to 850℃ at a rate of 60℃ / h~80℃ / h, and hold for 6h~8h; After being removed from the furnace and cooled by water, the temperature at which the furnace glows red is less than or equal to 80℃.

[0014] In another aspect of the present invention, preferably, the Fe-Ni recycled material and pure iron are baked at 600°C to 850°C for at least 24 hours, the electrolytic nickel plate is baked at 800°C to 900°C for 4 to 5 hours, and the manganese, silicon, vanadium, chromium and carbon are baked at 100°C to 200°C for at least 24 hours.

[0015] (III) Beneficial Effects The above-described technical solution of the present invention has the following beneficial technical effects: This invention utilizes the proportions of multiple alloying elements—C, Mn, Si, Ni, Cr, and V—and limits the total amount of (V+Cr) and the (V+Cr) / C ratio to achieve a stable austenitic structure and a dispersed carbide composite strengthening structure within a Fe-Ni matrix. This results in a synergistic optimization of low thermal expansion, high specific strength, high specific stiffness, and low density. Ni ensures the thermal stability and low expansion characteristics of the matrix. C, Cr, and V work together to form fine and uniform carbide precipitates, achieving precipitation strengthening and grain boundary pinning. Mn and Si, while ensuring microstructure uniformity and processing performance, synergistically regulate solid solution strengthening and thermal expansion properties. Attached Figure Description

[0016] Figure 1 This is a schematic diagram of the overall process of one embodiment of the present invention. Detailed Implementation

[0017] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments and the accompanying drawings. It should be understood that these descriptions are merely exemplary and not intended to limit the scope of the invention. Furthermore, descriptions of well-known structures and techniques are omitted in the following description to avoid unnecessarily obscuring the concept of the invention.

[0018] Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without inventive effort are within the scope of protection of the present invention.

[0019] In the description of this invention, it should be noted that the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0020] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0021] Example A low-expansion, high-specific-strength, and high-specific-stiffness iron-nickel alloy, comprising: C, Mn, Si, Ni, Cr, V, Fe, and unavoidable impurities, wherein, by mass percentage, C is 0.05%~0.18%, specifically 0.05%, 0.07%, 0.09%, 0.11%, 0.13%, 0.15%, or 0.18%, etc.; Mn is 0.2%~0.5%, specifically 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, or 0.5%, etc.; Si is 0.15%~0.25%, specifically 0.15%, 0.16%, 0.18%, 0.2%, 0.22%, 0.23%, or 0.25%, etc.; and Ni is 33%~35%, specifically 33%. The content of Cr is 0.4%~0.8%, specifically 0.4%, 0.5%, 0.6%, 0.7% or 0.8%, and V is 0.4%~0.8%, specifically 0.4%, 0.5%, 0.6%, 0.7% or 0.8%, etc., and (V+Cr)≤1.6%, specifically 1.6%, 1.5%, 1.4%, 1.3% or 1.2%, etc., and 5.0≤(V+Cr) / C≤15.0, specifically 5, 6, 7, 8, 9, 10, 11, 12, 13, 14 or 15, etc., and Mn / Si≥2.0, specifically 2, 2.1 or 2.2, etc., with the balance being Fe and unavoidable impurities. C can form carbides with elements such as Cr and V, making it a beneficial solid solution strengthening element that can improve the strength and hardness of materials. Excessive C content can impair the plasticity and toughness of alloys, while insufficient C content will prevent the formation of enough carbides. The density of Mn is 7.2 g / cm³. 3 A suitable amount of manganese (Mn) can improve the plasticity of an alloy, but excessive Mn content will increase the alloy's coefficient of thermal expansion. The density of silicon (Si) is 2.3 g / cm³. Similarly, a suitable amount of silicon (Si) can improve the plasticity of an alloy, but excessive Si content will increase the alloy's coefficient of thermal expansion. The density of nickel (Ni) is 8.9 g / cm³. 3 Appropriately reducing the Ni content can decrease the material density, but it will increase the coefficient of thermal expansion. The density of V is 6.1 g / cm³. 3V can form VC compounds with C, which can act as pinning agents during heat treatment, refining grains and improving the strength and plasticity of the material. However, excessive V will increase the coefficient of thermal expansion of the material. The density of Cr is 7.19 g / cm3. Cr can partially replace V to form CrC compounds with C, which can also act as pinning agents during heat treatment, refining grains and improving the strength and plasticity of the material. However, excessive Cr will increase the coefficient of thermal expansion of the material. In this embodiment, the interaction between C, Cr, and V determines the nucleation mode, precipitation kinetics, and spatial distribution characteristics of carbides. Carbon participates in interstitial solid solution strengthening and is also an essential element for carbide formation, participating in the formation of precipitated phases together with Cr and V. However, excessively high or low carbon content will change the quantity balance and distribution continuity of precipitated phases, thus affecting the integrity of the microstructure. Mn and Si mainly exist in the matrix in solid solution form, which plays a regulatory role in lattice distortion and atomic size differences, thus affecting the uniformity of the microstructure and the subsequent deformation coordination during solidification. Simultaneously, changes in their content alter the overall thermophysical response characteristics of the alloy, requiring the system to maintain a balanced distribution within the composition range. Ni, as a matrix stabilizing element, plays a decisive role in the stable existence of the austenite phase. Changes in its content affect the structural stability of the matrix and the overall thermal expansion response characteristics, thus constraining the overall microstructure stability. Furthermore, Cr and V exhibit a competitive tendency to bind with C under different thermodynamic conditions, causing the precipitated phases to exhibit different evolution paths in morphology and size. The proportional relationships between Cr and V, and between Cr and C, including (V+Cr) and (V+Cr) / C, constrain the formation intensity and spatial distribution continuity of the carbide phase, thereby avoiding microstructure inhomogeneity caused by local enrichment or coarsening precipitation. This creates a dynamic balance between precipitation strengthening and matrix stability, with fine, dispersed carbides strengthening grain boundaries while maintaining extremely high ductility and toughness.

[0022] Furthermore, in this embodiment, the Mn / Si ratio is ≥1.5, specifically 1.5, 2, 2.5, or 3. While ensuring the deoxidation effect during smelting, the negative impacts of Mn and Si on the coefficient of thermal expansion and plasticity are reduced, allowing Mn and Si to be in a synergistic equilibrium state of solid solution regulation within the alloy system. This enables the control of oxygen activity, inclusion formation behavior, and the degree of solid solution strengthening of the matrix during smelting and solidification. During smelting, both Mn and Si possess certain deoxidation capabilities. Mn primarily participates in the primary deoxidation reaction by forming MnO-like oxides with dissolved oxygen, while Si tends to form SiO2 or composite silicate inclusions, deeply removing residual oxygen from the melt. By constraining the Mn / Si ratio, the deoxidation reaction can be transformed from a single oxide formation path to a multi-phase synergistic deoxidation path, thereby reducing the tendency for single inclusions to aggregate and grow, improving the refinement and dispersion of inclusions, and resulting in a cleaner metal matrix during smelting. Meanwhile, both Mn and Si exist in solid solution form in the Fe-Ni matrix. Their atomic size difference introduces lattice distortion effects, thus affecting lattice vibrations and thermal expansion behavior. When the Mn content is relatively dominant over Si, i.e., Mn / Si ≥ 1.5, the strong bonding effect and local structural rigidity enhancement caused by Si are somewhat suppressed, thereby avoiding the problems of increased thermal expansion coefficient and decreased plasticity caused by excessive Si. In addition, during solidification, the coexistence of Mn and Si affects the solute redistribution behavior during dendrite growth and the degree of compositional enrichment in the grain boundary region. Through the above ratio constraints, the segregation degree of Mn and Si in the grain boundary and interdendritic regions can be reduced, thereby improving the uniformity of the microstructure, reducing the sources of local stress concentration, and further reducing the thermal expansion inhomogeneity caused by compositional fluctuations. Therefore, by controlling the Mn / Si ratio and limiting the total amount, a balance is achieved between the deoxidation reaction path, inclusion morphology, solid solution strengthening strength and lattice distortion. This ensures the purity of smelting while reducing the adverse effects of Mn and Si on the thermal expansion properties and plasticity of the alloy, making the overall properties of the alloy more stable and consistent.

[0023] Furthermore, in this embodiment, (V+Cr) ≤ 1.4%, 7.0 ≤ (V+Cr) / C ≤ 12.0, and Mn / Si ≥ 1.9. V+Cr, as the total amount of carbide-forming elements, determines the carbide nucleation density and precipitation driving force during melt solidification and subsequent heat treatment. When its total amount is controlled at ≤ 1.4%, excessive carbide formation tendency can be avoided, leading to the formation of continuous network carbides or coarse blocky carbides, thereby suppressing the risk of continuous strengthening phase formation at grain boundaries and preventing grain boundary embrittlement and continuous crack initiation paths. Simultaneously, it allows the precipitated phases to be distributed more in the form of dispersed particles within the grains and near the grain boundaries, which is beneficial for forming a uniform dislocation pinning lattice structure. Furthermore, by limiting 7.0 ≤ (V+Cr) / C ≤ 12.0, the carbon element and carbide-forming elements are kept within a relatively stable stoichiometric matching range. Within this ratio range, insufficient C will not limit the number of carbide precipitates, nor will excessive C lead to a dominant state of interstitial solid solution strengthening. This allows carbon to primarily participate in microstructure construction as stable carbides, achieving a balanced control over the number, size, and distribution density of precipitates. During heat treatment, this ratio also influences the diffusion rate and segregation behavior of carbon in the austenitic matrix, transforming the precipitation process from rapid coarsening to controlled dispersion precipitation, thereby improving precipitation strengthening efficiency. By setting Mn / Si ≥ 2, the proportion of Mn in the solid solution system is significantly higher than that of Si, thus forming a dominant regulatory pathway in terms of lattice distortion contribution and thermophysical property influence. A higher relative Mn content helps reduce the influence of Si on the strengthening of the crystal structure's rigidity, reduces the local bonding enhancement and thermal vibration restriction effects caused by Si, and thus reduces the adverse effects on the coefficient of thermal expansion. Meanwhile, Mn dominance allows it to preferentially participate in oxide formation reactions during solidification, causing some oxygen to preferentially precipitate and float to the surface as MnO-type inclusions. This helps reduce the probability of Si participating in the formation of high-viscosity silicate inclusions, thereby improving the morphology and distribution uniformity of inclusions. The combined effect of these three constraints creates a stable transition path between the solidified and heat-treated structures, preventing local enrichment, coarsening precipitation, and continuous grain boundary embrittlement, thus achieving a synergistic match between low expansion and high specific strength and high specific stiffness.

[0024] This embodiment also provides a method for preparing a low-expansion, high-specific-strength, and high-specific-stiffness iron-nickel alloy. Figure 1 A schematic diagram of the overall process of an embodiment of the present invention is shown, as follows: Figure 1 As shown, it includes: According to the composition ratio of the alloy, the first raw material, the second raw material, and the third raw material are weighed. The first raw material includes Fe-Ni recycled material, pure iron, and electrolytic nickel plate. The second raw material includes manganese and silicon. The third raw material includes vanadium, chromium, and carbon. This provides the main Fe-Ni solid solution matrix, and the recycled material introduces a certain process genetic structure to reduce smelting energy consumption and promote uniform composition transition. Manganese and silicon are introduced as the second raw material in subsequent stages for deoxidation strengthening and grain boundary energy regulation. Vanadium, chromium, and carbon are added as the third raw material in stages to form a dispersed strengthening phase and regulate grain size, thereby improving the alloy's specific strength and high-temperature stability. The Fe-Ni recycled material and pure iron are baked at 600~850℃ for at least 24 hours, the electrolytic nickel plate is baked at 800~900℃ for 4~5 hours, and the manganese, silicon, vanadium, chromium, and carbon are baked at 100~200℃ for at least 24 hours.

[0025] The first raw material is smelted, deoxidized, and refined to obtain a first alloy, including: vacuum smelting the first raw material in a vacuum induction furnace, evacuating the furnace to less than 10 Pa, and performing low-pressure pretreatment to significantly reduce the oxygen and nitrogen partial pressures in the furnace, avoiding the adverse effects of oxide inclusions and nitride formation on subsequent properties. Preheating is performed at 20-30 kW for 20-30 minutes to gradually raise the temperature of the charge and remove adsorbed gases and moisture, avoiding rapid heating that could lead to splashing or localized overheating. Heating is then performed at 40-60 kW until the material melts completely, forming a stable molten pool. During this stage, the surface of the molten pool must be kept stable and tumbling to promote uniform diffusion of components. Heating is then performed at 60-65 kW for 10-15 minutes to achieve a uniformly overheated state in the molten pool, thereby improving the conditions for subsequent deoxidation and dissolution of alloying elements.

[0026] During deoxidation, the deoxidized graphite carbon is added in three stages, with each addition being 0.02% to 0.03% of the furnace charge. The purpose of adding it in three stages is to avoid local carbon oversaturation or violent reaction caused by adding it all at once, and to achieve purification by gradually consuming oxygen elements and removing them from the system.

[0027] After deoxygenation, once the liquid surface is calm, refining is carried out using 60kW of power for 40-50 minutes. By maintaining a stable vacuum environment and power, inclusions are floated, gases are released, and the composition is homogenized, resulting in a high degree of cleanliness and stable chemical homogeneity in the melt.

[0028] Under preset environmental parameters, the second raw material is added to the first alloy, and the third raw material is added at preset time intervals to obtain the second alloy, comprising: The second raw material is added to the first alloy under preset environmental parameters, including a protective atmosphere and a vacuum of -0.50 MPa. The protective atmosphere is argon, and the negative pressure environment can further reduce the risk of oxidation, while ensuring that manganese and silicon dissolve quickly and are evenly distributed in the high-temperature melt.

[0029] The third raw material is added at a preset time interval of 5 minutes to avoid excessively high local concentration peaks that could lead to the formation of coarse carbides or segregated structures, while also helping to control the size and uniformity of the precipitated phase.

[0030] After a 5-minute interval, the mixture is poured and cooled for more than 12 hours before demolding to obtain the second alloy.

[0031] The second alloy is forged, hot-rolled, and solution-treated to obtain the alloy. The forging process employs a staged heating method, and the forging includes: The second alloy is charged into the furnace at a temperature of 450°C or less to avoid excessive temperature difference between the inside and outside of the ingot, which could lead to thermal stress concentration and reduce the risk of cracking during heating. The temperature is then increased to 850±10°C at a rate of 60°C / h to 80°C / h and held for 3 to 5 hours. The furnace temperature is then increased to 1100±10°C and held for 1 to 2 hours before forging. This ensures a sufficiently uniform internal temperature for the ingot and promotes the initial diffusion of alloying elements in the dendritic segregation region, reducing the inhomogeneity of the as-cast structure. The furnace temperature is then further increased to 1100±10°C and held for 1 to 2 hours to allow for complete solid solution of the second phase, ensuring a uniform hot-worked microstructure throughout the ingot.

[0032] Forging was performed using a 750kg free forging hammer, with a forging size of 50×200mm. The initial forging temperature was greater than or equal to 1050℃, and the final forging temperature was greater than or equal to 900℃. The initial forging temperature was controlled above 1050℃ to ensure good plasticity and sufficiently low deformation resistance of the material. The final forging temperature was controlled above 900℃ to avoid cracking due to decreased plasticity caused by excessively low temperatures, while also ensuring sufficient dynamic recrystallization, refining the grains, and improving the uniformity of the microstructure. During the forging process, large-sized as-cast grains were fully broken up, the dendritic structure was significantly improved, and casting defects such as internal shrinkage cavities and porosity were compacted and welded together, providing a uniform and stable microstructure foundation for subsequent hot rolling.

[0033] The hot rolling includes: After removing the oxide scale from the surface of the second alloy after forging, the oxide scale on the surface of the forging is removed to prevent it from being pressed into the matrix and forming inclusion defects, thereby improving the surface quality of the subsequent hot-rolled sheet. A staged heating regime is adopted, with the furnace charged at a temperature of less than or equal to 450℃, and the temperature increased at 60℃ / h~80℃ / h to 850±10℃ and held for 3h~4h; this ensures uniform heating of the forging and reduces residual stress caused by temperature differences during hot rolling. The furnace temperature is raised to 1080±10℃ and held for 1~2 hours to further homogenize the microstructure and ensure good plasticity during hot rolling.

[0034] Hot rolling is performed using a four-roll hot rolling mill with a rolled size of 15×200mm. The initial rolling temperature is greater than or equal to 1050℃, and the final rolling temperature is greater than or equal to 900℃. This facilitates continuous dynamic recovery and recrystallization, avoids microstructure coarsening, and simultaneously forms uniform and fine deformed grains. During the hot rolling process, a large number of dislocations are continuously formed and rearranged, further refining the coarse grains in the cast state and further improving the microstructure density.

[0035] The solution treatment includes: By loading the hot-rolled second alloy into the furnace at a temperature of 300°C or less, excessive thermal stress caused by rapid localized temperature rise in the sheet material can be avoided. Spacers with a thickness equal to or greater than the thickness of the hot-rolled second alloy are placed between adjacent sheets to maintain sufficient spacing, ensuring air circulation and uniform heat transfer within the furnace. This allows each sheet to receive consistent heating conditions, thereby improving the consistency of product performance during mass production.

[0036] The temperature is increased to 850℃ at a rate of 60℃ / h to 80℃ / h and held for 6h to 8h; this allows alloying elements such as Cr and V to diffuse fully and achieve a homogenized microstructure, while eliminating work hardening and residual stress formed during hot working, thus stabilizing the microstructure.

[0037] After being removed from the furnace and water-cooled, the re-heating temperature is less than or equal to 80℃. Immediately after the holding period, the material is removed from the furnace and water-cooled rapidly. This rapid cooling suppresses the precipitation of the second phase, maintains the solid solution state, ensures the stability of the low-expansion microstructure, and reduces the impact of grain boundary precipitation on plasticity. Maintaining the re-heating temperature below 80℃ indicates that the entire plate has undergone rapid cooling, which helps ensure consistent microstructure across the entire plate cross-section, improving the stability and repeatability of the final product's performance. Through the synergistic effect of the forging, hot rolling, and solution treatment processes described above, the coarse grains in the as-cast state of the second alloy are fully broken up and refined, elemental segregation is effectively eliminated, microstructure uniformity is significantly improved, residual stress is fully released, and a stable low-expansion microstructure is formed, giving the material high strength, high plasticity, and low thermal expansion characteristics.

[0038] In this embodiment, the prepared δ15×200mm solution-treated plate has a tensile strength ≥500MPa, a yield strength ≥300MPa, an elongation ≥38%, and a coefficient of thermal expansion ≤1.7×10⁻⁶. -6 / ℃ (20~100℃), elastic modulus ≥145GPa, specific strength ≥62MPa / (g / cm) 3 ), specific stiffness ≥17.8GPa / (g / cm) 3 The iron-nickel alloy of this embodiment has higher strength, ductility, and better specific strength and specific stiffness than conventional Invar alloys, and has lower density, making it promising for applications in aerospace structural components, precision instrument supports, and lightweight molds.

[0039] Example 1 The alloy comprises: C, Mn, Si, Ni, Cr, V, Fe and unavoidable impurities, with C accounting for 0.12% by mass, Mn 0.38%, Si 0.20%, Ni 35%, Cr 0.51%, V 0.54%, (V+Cr) = 1.05%, (V+Cr) / C = 8.75, Mn / Si = 1.9, and the balance being Fe and unavoidable impurities.

[0040] Preparation methods include: According to the composition ratio of the alloy, the first raw material, the second raw material and the third raw material are weighed. The first raw material includes Fe-Ni recycled material, pure iron and electrolytic nickel plate. The second raw material includes manganese and silicon. The third raw material includes vanadium, chromium and carbon. The first raw material is smelted, deoxidized, and refined to obtain a first alloy; the vacuum is drawn to less than 10 Pa, preheated with 25 kW power for 25 min, heated with 50 kW power until the material melts, and heated with 63 kW power for 12 min; during deoxidation, deoxidized graphite carbon is added in three portions, with each addition being 0.025% of the furnace charge; refining is performed with 60 kW power for 45 min; Under preset environmental parameters, the second raw material is added to the first alloy, and the third raw material is added at preset time intervals to obtain the second alloy; under preset environmental parameters, the second raw material is added to the first alloy, including a protective atmosphere and a vacuum degree of -0.50 MPa; the third raw material is added at preset time intervals, the preset time interval being 5 minutes; after 5 minutes, casting is performed, and after cooling for more than 12 hours, the alloy is demolded to obtain the second alloy. The second alloy is forged, hot-rolled, and solution-treated to obtain the alloy. The forging process includes: loading the second alloy into a furnace at a temperature of ≤450°C, heating it at 70°C / h to 850±10°C and holding it for 4 hours; heating it in the furnace to 1100±10°C and holding it for 1.5 hours before forging; forging is performed using a 750kg free forging hammer, with a forging size of 50×200mm, an initial forging temperature ≥1050°C, and a final forging temperature ≥900°C.

[0041] The hot rolling process includes: removing the oxide scale from the surface of the second alloy after forging, loading it into the furnace at a temperature of less than or equal to 450°C, raising the temperature to 850±10°C at a rate of 70°C / h and holding it at that temperature for 3.5h; raising the temperature in the furnace to 1080±10°C and holding it at that temperature for 1.5h; hot rolling is performed using a four-roll hot rolling mill, with a hot-rolled size of 15×200mm, an initial rolling temperature of greater than or equal to 1050°C, and a final rolling temperature of greater than or equal to 900°C.

[0042] The solution treatment includes: loading the hot-rolled second alloy into the furnace at a temperature of less than or equal to 300°C, placing a spacer between adjacent hot-rolled second alloys, the thickness of the spacer being greater than or equal to the thickness of the hot-rolled second alloy; heating to 850°C at a rate of 70°C / h and holding at that temperature for 7h; water cooling after exiting the furnace, with the reddening temperature being less than or equal to 80°C.

[0043] Example 2 The alloy comprises: C, Mn, Si, Ni, Cr, V, Fe, and unavoidable impurities, with C accounting for 0.053%, Mn 0.23%, Si 0.15%, Ni 33%, Cr 0.4%, and V 0.4% by mass percentage. (V+Cr) = 0.8%, (V+Cr) / C = 15, Mn / Si = 1.53, with the balance being Fe and unavoidable impurities.

[0044] Preparation methods include: According to the composition ratio of the alloy, the first raw material, the second raw material and the third raw material are weighed. The first raw material includes Fe-Ni recycled material, pure iron and electrolytic nickel plate. The second raw material includes manganese and silicon. The third raw material includes vanadium, chromium and carbon. The first raw material is smelted, deoxidized, and refined to obtain a first alloy; the vacuum is evacuated to less than 10 Pa, preheated with 20 kW power for 20 min, heated with 40 kW power until the material melts, and heated with 60 kW power for 10 min; during deoxidation, deoxidized graphite carbon is added in three portions, with each addition being 0.02% of the furnace charge; refining is performed with 60 kW power for 40 min. Under preset environmental parameters, the second raw material is added to the first alloy, and the third raw material is added at preset time intervals to obtain the second alloy; under preset environmental parameters, the second raw material is added to the first alloy, including a protective atmosphere and a vacuum degree of -0.50 MPa; the third raw material is added at preset time intervals, the preset time interval being 5 minutes; after 5 minutes, casting is performed, and after cooling for more than 12 hours, the alloy is demolded to obtain the second alloy. The second alloy is forged, hot-rolled, and solution-treated to obtain the alloy. The forging process includes: loading the second alloy into a furnace at a temperature of ≤450°C, heating it at 60°C / h to 850±10°C and holding it for 3 hours; heating it in the furnace to 1100±10°C and holding it for 1 hour before forging; forging is performed using a 750kg free forging hammer, with a forging size of 50×200mm, an initial forging temperature ≥1050°C, and a final forging temperature ≥900°C.

[0045] The hot rolling process includes: removing the oxide scale from the surface of the second alloy after forging, loading it into the furnace at a temperature of less than or equal to 450°C, raising the temperature to 850±10°C at a rate of 60°C / h and holding it for 3 hours; raising the temperature in the furnace to 1080±10°C and holding it for 1 hour; using a four-roll hot rolling mill for hot rolling, with a hot-rolled size of 15×200mm, an initial rolling temperature of greater than or equal to 1050°C, and a final rolling temperature of greater than or equal to 900°C.

[0046] The solution treatment includes: loading the hot-rolled second alloy into the furnace at a temperature of less than or equal to 300°C, placing a spacer between adjacent hot-rolled second alloys, the thickness of which is greater than or equal to the thickness of the hot-rolled second alloy; heating to 850°C at a rate of 60°C / h and holding for 6 hours; water cooling after exiting the furnace, with a reddening temperature of less than or equal to 80°C.

[0047] Example 3 The alloy comprises: C, Mn, Si, Ni, Cr, V, Fe, and unavoidable impurities, with C accounting for 0.18%, Mn 0.5%, Si 0.2%, Ni 34%, Cr 0.8%, and V 0.8% by mass percentage. (V+Cr) = 1.6%, (V+Cr) / C = 8.89, Mn / Si = 2.5, with the balance being Fe and unavoidable impurities.

[0048] Preparation methods include: According to the composition ratio of the alloy, the first raw material, the second raw material and the third raw material are weighed. The first raw material includes Fe-Ni recycled material, pure iron and electrolytic nickel plate. The second raw material includes manganese and silicon. The third raw material includes vanadium, chromium and carbon. The first raw material is smelted, deoxidized, and refined to obtain a first alloy; the vacuum is drawn to less than 10 Pa, preheated with 30 kW power for 30 min, heated with 60 kW power until the material melts, and heated with 65 kW power for 15 min; during deoxidation, deoxidized graphite carbon is added in three portions, with each addition being 0.03% of the furnace charge; refining is performed with 60 kW power for 50 min; Under preset environmental parameters, the second raw material is added to the first alloy, and the third raw material is added at preset time intervals to obtain the second alloy; under preset environmental parameters, the second raw material is added to the first alloy, including a protective atmosphere and a vacuum degree of -0.50 MPa; the third raw material is added at preset time intervals, the preset time interval being 5 minutes; after 5 minutes, casting is performed, and after cooling for more than 12 hours, the alloy is demolded to obtain the second alloy. The second alloy is forged, hot-rolled, and solution-treated to obtain the alloy. The forging process includes: loading the second alloy into a furnace at a temperature of ≤450°C, heating it at 80°C / h to 850±10°C and holding it for 5 hours; heating it in the furnace to 1100±10°C and holding it for 2 hours before forging; forging is performed using a 750kg free forging hammer, with a forging size of 50×200mm, an initial forging temperature ≥1050°C, and a final forging temperature ≥900°C.

[0049] The hot rolling process includes: removing the oxide scale from the surface of the second alloy after forging, loading it into the furnace at a temperature of less than or equal to 450°C, raising the temperature to 850±10°C at a rate of 80°C / h and holding it at that temperature for 4 hours; raising the temperature in the furnace to 1080±10°C and holding it at that temperature for 2 hours; using a four-roll hot rolling mill for hot rolling, with a hot-rolled size of 15×200mm, an initial rolling temperature of greater than or equal to 1050°C, and a final rolling temperature of greater than or equal to 900°C.

[0050] The solution treatment includes: loading the hot-rolled second alloy into the furnace at a temperature of less than or equal to 300°C, placing a spacer between adjacent hot-rolled second alloys, the thickness of which is greater than or equal to the thickness of the hot-rolled second alloy; heating to 850°C at a rate of 80°C / h and holding for 8 hours; water cooling after exiting the furnace, with the reddening temperature being less than or equal to 80°C.

[0051] Example 4 The alloy comprises: C, Mn, Si, Ni, Cr, V, Fe, and unavoidable impurities, with C accounting for 0.1%, Mn 0.4%, Si 0.2%, Ni 33%, Cr 0.6%, and V 0.6% by mass percentage. (V+Cr) = 1.2%, (V+Cr) / C = 12, Mn / Si = 2, with the balance being Fe and unavoidable impurities.

[0052] The preparation method is the same as in Example 1.

[0053] Example 5 The alloy comprises: C, Mn, Si, Ni, Cr, V, Fe, and unavoidable impurities, with C accounting for 0.15%, Mn 0.3%, Si 0.18%, Ni 34%, Cr 0.7%, and V 0.7% by mass percentage. (V+Cr) = 1.4%, (V+Cr) / C = 9.3, Mn / Si = 1.67, with the balance being Fe and unavoidable impurities.

[0054] The preparation method is the same as in Example 1.

[0055] Table 1 shows the alloy composition of Comparative Examples 1-4; Table 2 shows the composition ratio of Examples 1-5 and Comparative Examples 1-4; Table 3 shows the gas content and inclusion content of Examples 1-5 and Comparative Examples 1-4; Table 4 shows the coefficient of thermal expansion of Examples 1-5 and Comparative Examples 1-4; Table 5 shows the physical properties of Examples 1-5 and Comparative Examples 1-4; Table 6 shows the density, specific strength, and specific stiffness of Examples 1-5 and Comparative Examples 1-4. The gas content detection methods include: oxygen content determination according to GB / T11261-2006, nitrogen content determination according to GB / T20124-2006, and hydrogen content determination according to GB / T20124-2006. The content determination method is GB / T223.82-2018; the method for detecting impurity content is GB / T10561-2023-A; the method for detecting the coefficient of thermal expansion is GB / T4339-2008; the methods for detecting physical properties include: room temperature tensile strength GB / T228.1-2021, Vickers hardness GB / T4340.1-2024; the density detection method is GB / T1423-1996; the grain size detection method is GB / T6394-2017; specific strength is the ratio of alloy strength to alloy density; specific stiffness is the ratio of the elastic modulus of the material to its density.

[0056] Table 1 Alloy composition of Comparative Examples 1-4 Table 2. Component proportions of Examples 1-5 and Comparative Examples 1-4 Table 3. Gas content and inclusion content of Examples 1-5 and Comparative Examples 1-4 Table 4. Coefficients of thermal expansion of Examples 1-5 and Comparative Examples 1-4 Table 5 Physical properties of Examples 1-5 and Comparative Examples 1-4 Note: Comparative Example 3 showed cracking during forging.

[0057] Table 6. Density, specific strength, and specific stiffness of Examples 1-5 and Comparative Examples 1-4 As shown in Table 1, the C content of Comparative Example 1 (0.0084%) is lower than that of Example 1 (0.12%), while other components are similar; the C content of Comparative Example 2 (0.018%) is lower than that of this Example by 0.05%~0.18%; and the Cr content of Comparative Example 3 (1.96%) is lower than that of this Example by 0.4%~0.8%. The Ni content in Example 1 and Comparative Examples 1-3 is lower than that of the conventional Invar alloy in Comparative Example 4.

[0058] As shown in Tables 2-6, this embodiment exhibits significant comprehensive performance advantages compared to the comparative example. The δ15mm solution-treated sheet of Example 1 achieves a tensile strength of 563 MPa, a yield strength of 332 MPa, an elongation of 39.5%, and a density of only 8.10 g / cm³. 3 Its elastic modulus reaches 147 GPa, and its specific strength reaches 69.51 MPa / (g / cm). 3 Its specific stiffness reaches 18.15 GPa / (g / cm). 3 The performance of this model is superior to that of the comparative model, with the coefficient of thermal expansion controlled at 1.7 × 10^2℃ from 20 to 100℃. 6 The temperature below / ℃ indicates that this embodiment achieves a synergistic improvement in strength, plasticity, lightweight and stiffness while maintaining ultra-low expansion characteristics. It has excellent comprehensive performance and can meet the application requirements of low expansion, high specific strength and high specific stiffness materials in aerospace structural components, precision instrument brackets, lightweight molds and other fields.

[0059] It should be understood that the specific embodiments described above are merely illustrative or explanatory of the principles of the invention and do not constitute a limitation thereof. Therefore, any modifications, equivalent substitutions, improvements, etc., made without departing from the spirit and scope of the invention should be included within the protection scope of the invention. Furthermore, the appended claims are intended to cover all variations and modifications falling within the scope and boundaries of the appended claims, or equivalent forms of such scope and boundaries.

[0060] The present invention has been described above with reference to embodiments thereof. However, these embodiments are merely illustrative and not intended to limit the scope of the invention. The scope of the invention is defined by the appended claims and their equivalents. Various substitutions and modifications can be made by those skilled in the art without departing from the scope of the invention, and all such substitutions and modifications should fall within the scope of the invention.

[0061] Although embodiments of the present invention have been described in detail, it should be understood that various changes, substitutions, and modifications can be made to the embodiments of the present invention without departing from the spirit and scope of the invention.

[0062] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A low-expansion, high-specific-strength, and high-specific-stiffness iron-nickel alloy, characterized in that, The alloy comprises: C, Mn, Si, Ni, Cr, V, Fe and unavoidable impurities, in the following mass percentages: C 0.05%~0.18%, Mn 0.2%~0.5%, Si 0.15%~0.25%, Ni 33%~35%, Cr 0.4%~0.8%, V 0.4%~0.8%, (V+Cr) ≤1.6%, 5.0 ≤ (V+Cr) / C ≤15.0, Mn / Si ≥2.0, with the balance being Fe and unavoidable impurities.

2. The low-expansion, high-specific-strength, and high-specific-stiffness iron-nickel alloy according to claim 1, characterized in that, Mn / Si≥1.

5.

3. The low-expansion, high-specific-strength, and high-specific-stiffness iron-nickel alloy according to claim 1, characterized in that, (V+Cr)≤1.4%, 7.0≤(V+Cr) / C≤12.

0.

4. A method for preparing a low-expansion, high-specific-strength, and high-specific-stiffness iron-nickel alloy, characterized in that, include: According to the composition ratio of the alloy, the first raw material, the second raw material and the third raw material are weighed. The first raw material includes Fe-Ni recycled material, pure iron and electrolytic nickel plate. The second raw material includes manganese and silicon. The third raw material includes vanadium, chromium and carbon. The first raw material is smelted, deoxidized, and refined to obtain a first alloy; Under preset environmental parameters, the second raw material is added to the first alloy, and the third raw material is added at preset time intervals to obtain the second alloy; The second alloy is forged, hot-rolled, and solution-treated to obtain the alloy.

5. The preparation method according to claim 4, characterized in that, The process of smelting, deoxidizing, and refining the first raw material to obtain the first alloy includes: The first raw material is vacuum melted, the vacuum is drawn to less than 10Pa, preheated with 20Kw~30Kw power for 20min~30min, heated with 40Kw~60Kw power until the material melts, and heated with 60Kw~65Kw power for 10min~15min. During deoxidation, the deoxidized graphite carbon is added in three portions, with each addition being 0.02% to 0.03% of the furnace charge. The refining process is carried out using 60kW of power, and the refining time is 40-50 minutes.

6. The preparation method according to claim 4, characterized in that, The step of adding the second raw material to the first alloy under preset environmental parameters, and adding the third raw material at preset time intervals to obtain the second alloy includes: The second raw material is added to the first alloy under preset environmental parameters, including a protective atmosphere and a vacuum of -0.50 MPa. The third raw material is added at a preset time interval, which is 5 minutes. After a 5-minute interval, the mixture is poured and cooled for more than 12 hours before demolding to obtain the second alloy.

7. The preparation method according to claim 4, characterized in that, The forging process includes: The second alloy is loaded into the furnace at a temperature of less than or equal to 450°C, and heated to 850±10°C at a rate of 60°C / h~80°C / h and held for 3h~5h. The furnace temperature is raised to 1100±10℃ and held for 1 to 2 hours before forging. The forging was carried out using a 750Kg free forging hammer, with a forging size of 50×200mm, an initial forging temperature of ≥1050℃, and a final forging temperature of ≥900℃.

8. The preparation method according to claim 4, characterized in that, The hot rolling includes: After removing the oxide scale from the surface of the second alloy after forging, the furnace is loaded at a temperature of less than or equal to 450°C, and the temperature is increased to 850±10°C at a rate of 60°C / h~80°C / h and held for 3h~4h. Heat the furnace to 1080±10℃ and hold for 1~2 hours; Hot rolling is carried out using a four-roll hot rolling mill. The hot rolling size is 15×200mm, the initial rolling temperature is greater than or equal to 1050℃, and the final rolling temperature is greater than or equal to 900℃.

9. The preparation method according to claim 4, characterized in that, The solution treatment includes: The hot-rolled second alloy is loaded into the furnace at a temperature of less than or equal to 300°C, and spacers are placed between adjacent hot-rolled second alloys, the thickness of which is greater than or equal to the thickness of the hot-rolled second alloy. Heat to 850℃ at a rate of 60℃ / h~80℃ / h, and hold for 6h~8h; After being removed from the furnace and cooled by water, the temperature at which the furnace glows red is less than or equal to 80℃.

10. The preparation method according to claim 4, characterized in that, The Fe-Ni recycled material and pure iron are baked at 600℃~850℃ for at least 24 hours, the electrolytic nickel plate is baked at 800℃~900℃ for 4~5 hours, and the manganese, silicon, vanadium, chromium and carbon are baked at 100℃~200℃ for at least 24 hours.