A strip of elastic element and its manufacturing method
By designing the high-carbon C-Mn-Si composition and using the isothermal quenching and cold rolling process, we prepared elastic element strips with an ultrafine sorbitic structure, which solved the contradiction between strength and toughness and the high cost problem of martensitic spring steel, and realized high-performance elastic elements with high strength, low cost and green mass production.
Patent Information
- Application Number
- CN202611461151.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing martensitic spring steels suffer from a contradiction between strength and toughness, high alloy costs, lengthy production processes, and unstable performance of thick-gauge products, making it difficult to meet the high strength, high fatigue, and lightweight requirements of new energy vehicles and high-end precision instruments.
By employing a high-carbon C-Mn-Si composition design and using isothermal quenching and high-reduction cold rolling processes, elastic element strips with ultrafine sorbite structure are prepared, simplifying the process flow, avoiding the addition of precious metal alloys, and achieving high strength and high fatigue performance.
It has achieved low-cost, high-performance elastic element strips with high strength and fatigue resistance, making them suitable for applications in new energy vehicles and high-end precision instruments, and meeting the requirements for green mass production.
Smart Images

Figure CN123108432A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-elasticity steel material processing technology, specifically relating to an elastic element strip and its manufacturing method, which can be widely used in the preparation of elastic structural parts in the fields of automobiles, precision instruments, and intelligent equipment. Background Technology
[0002] Elastic elements are core components in industrial equipment, transportation, and precision instruments, primarily relying on the controllable elastic deformation of materials to achieve functions such as energy storage, buffering, shock absorption, resetting, and sensing. Currently, the mainstream materials for elastic elements are quenched and tempered spring steels, including grades such as 65Mn, 60Si2MnA, 51CrV4, 55SiCr, and SUP6, which are widely used in the manufacture of various springs, clockwork, diaphragms, and elastic gaskets. This invention addresses the performance shortcomings and processing difficulties of thick-gauge elastic strips by developing a novel spring steel strip based on cold-rolled strengthening of a sorbitic structure, suitable for the mass production needs of medium-thickness elastic elements with a thickness of 1.5mm or more.
[0003] The existing manufacturing process for commercial spring steel strip includes: hot rolling and pickling, multiple cold rolling and annealing, quenching, and medium-temperature tempering. The core process involves heating the spring steel to above the austenitizing temperature, followed by rapid cooling through oil quenching to obtain a high-hardness martensitic structure, and then tempering at a medium temperature of 350℃ to 600℃ to achieve a balance between strength and toughness, ultimately obtaining martensitic spring steel that meets the requirements of conventional elastic components.
[0004] With the rapid development of emerging fields such as new energy vehicles, humanoid robots, and high-precision instruments, elastic components are gradually moving towards higher strength, higher fatigue resistance, and lighter weight. The technical shortcomings of traditional martensitic spring steel are becoming increasingly prominent, mainly due to the following problems: First, there is a significant contradiction between strength and toughness. Traditional quenched and tempered martensitic spring steel has an inherent strength-toughness limit relationship. When the material is strengthened by increasing hardness, plasticity, toughness and fatigue resistance are significantly sacrificed. Under high-frequency alternating loads and impact loads, it is prone to failure problems such as elastic decay and fatigue fracture, which cannot meet the long service life requirements of high-end equipment.
[0005] Second, the alloy cost is high and the production process is lengthy. High-end spring steel generally adds precious metal alloying elements such as Cr, Mo, and V to improve its overall performance, resulting in high raw material costs. At the same time, the production process requires quenching and tempering heat treatment, which is lengthy, energy-intensive, and inefficient, leading to high carbon emissions and production costs, which does not conform to the trend of green mass production.
[0006] Currently, existing technologies only involve sporadic research on the modification of sorbite in spring steel. A complete technical solution based on the preparation of fine lamellar sorbite by isothermal quenching of high carbon steel and strengthening by cold rolling with a large reduction rate has not yet been formed. In particular, there is a lack of mature process systems suitable for low-cost, high-fatigue elastic strips with a thickness of 1.5 mm or more, resulting in a significant technological gap. Summary of the Invention
[0007] The present invention aims to overcome the technical defects of existing martensitic spring steel, such as the contradiction between strength and toughness, high cost, complex process, and poor performance stability of thick-gauge products, and provides an elastic element strip with simple composition, low cost, short process, and high fatigue stability and its manufacturing method.
[0008] To achieve the above objectives, the present invention provides the following technical solution: an elastic element strip, comprising, by weight percentage: C: 0.85–1.00%, Si: 0.10–0.40%, Mn: 0.20–0.80%, Cr: 0.05–0.40%, N: 0.002–0.008%, Al: 0.005–0.060%, P: 0–0.025%, S: 0–0.025%, with the balance being Fe and unavoidable impurities.
[0009] The composition of this invention by mass percentage is as follows: C: 0.85%, Si: 0.20%, Mn: 0.30%, Cr: 0.15%, N: 0.006%, Al: 0.040%, P: 0.015%, S: 0.010%, with the balance being Fe and unavoidable impurities.
[0010] The composition of this invention by mass percentage is as follows: C: 0.88%, Si: 0.25%, Mn: 0.45%, Cr: 0.05~0.40%, N: 0.005%, Al: 0.028%, P: 0.012%, S: 0.003%, with the balance being Fe and unavoidable impurities.
[0011] The composition of this invention by mass percentage is as follows: C: 0.90%, Si: 0.25%, Mn: 0.75%, Cr: 0.10%, N: 0.005%, Al: 0.035%, P: 0.012%, S: 0.005%, with the balance being Fe and unavoidable impurities.
[0012] The composition of this invention by mass percentage is as follows: C: 0.85-1.00%, Si: 0.95%, Mn: 0.60%, Cr: 0.10%, N: 0.004%, Al: 0.030%, P: 0.011%, S: 0.003%, with the balance being Fe and unavoidable impurities.
[0013] The composition of this invention by mass percentage is as follows: C: 0.99%, Si: 0.30%, Mn: 0.50%, Cr: 0.35%, N: 0.003%, Al: 0.040%, P: 0.010%, S: 0.002%, with the balance being Fe and unavoidable impurities.
[0014] A method for manufacturing an elastic element strip includes the following steps: (1) Raw material pretreatment and austenitization: Select hot-rolled or cold-rolled base strip steel, remove surface iron oxide scale, oil stains and impurities, and cut to the target width; continuously feed the strip steel into the heating furnace and austenitize it in the range of 780℃~980℃; (2) Isothermal quenching: Cool the austenitized strip to 450℃~550℃ and perform isothermal quenching, and keep it at the temperature until the austenite completes the isothermal transformation to obtain an ultrafine uniform sorbite structure. (3) Cold rolling: The sorbitic steel strip is cold rolled, and the cumulative cold rolling reduction rate is controlled at 50% to 80%. During the cold rolling process, the fine sorbitic cementite lamellae bend and deform, and gradually tend to be oriented parallel to the rolling direction. At the same time, the matrix dislocation density increases sharply, resulting in a strong work hardening effect. As the reduction rate increases, the material strength continues to increase. When the reduction rate is increased to more than 70%, a strip with a strength of 1800MPa can be stably obtained.
[0015] The austenitizing temperature described in this invention is 850℃~920℃.
[0016] Compared to existing traditional martensitic spring steels and their preparation processes, this invention abandons the traditional Cr-Mo-V high-alloy spring steel system and adopts a simplified high-carbon C-Mn-Si composition design, eliminating the need for precious metal alloying elements. A uniform, fine-laminated sorbite structure is obtained through a precise isothermal quenching process, followed by secondary strengthening and toughening through high-reduction cold rolling. It has the following advantages and effects: (1) Simple composition and extremely low production cost: This invention adopts a pure C-Mn-Si high carbon system, which gives full play to the strengthening effect of carbon elements. No precious metal alloying elements are added. Compared with traditional alloy spring steels such as 51CrV4 and 60Si2MnA, the raw material cost is greatly reduced, there is no waste of precious metal resources, and the material has a significant cost-performance advantage. The composition comparison is shown in Table 1.
[0017] Table 1. Comparison of components (mass fraction, %).
[0018] .
[0019] (2) Short process, low energy consumption, green and environmentally friendly mass production: abandoning the long process of traditional spring steel “multiple cold rolling + annealing + quenching + tempering”, the preparation can be completed through only two core processes of isothermal quenching and cold rolling, which greatly shortens the production cycle, reduces equipment energy consumption, labor costs and production losses, reduces carbon emissions from heat treatment, and is suitable for large-scale and green industrial production.
[0020] The process steps are compared below, with the number of process steps reduced by 57%.
[0021] The production process of 51CrV4 and 60Si2MnA is as follows: hot-rolled coil --- pickling --- annealing --- cold rolling --- annealing --- cold rolling --- quenching --- tempering (a total of 7 processes). This invention involves: hot-rolled coil --- pickling --- isothermal quenching --- cold rolling (a total of 3 processes).
[0022] (3) High elasticity, high fatigue resistance, and excellent comprehensive performance: This invention completely solves the contradiction between strength and toughness in traditional martensitic spring steel through a composite strengthening mechanism of ultrafine sorbite structure and cold rolling dislocation strengthening. The tensile strength of the finished product is stable at ≥1600MPa; the material has extremely high elastic limit, resistance to elastic relaxation and notch toughness. Under high-frequency alternating load and reciprocating deformation conditions, its fatigue life and elastic stability are far superior to those of traditional quenched and tempered martensitic spring steel, which can effectively avoid elastic relaxation and fatigue fracture failure. As the design basis for selecting materials for spiral springs, the performance comparison between this invention and traditional spring steel is shown in Table 2.
[0023] Table 2. Comparison of the properties of traditional spring steel and the material of this invention.
[0024] .
[0025] (4) The product of this invention is specially adapted to elastic element strips with a thickness of 1.5mm to 2.5mm. The tensile strength of the finished product can reach more than 1600MPa, and can exceed 2000MPa under extreme strengthening state. The elastic limit, anti-elastic reduction performance and alternating fatigue life are significantly better than traditional quenched and tempered martensitic spring steel, taking into account the multiple advantages of low cost, low energy consumption and high performance. Attached Figure Description
[0026] Figure 1 This is a micrograph of the original sorbite microstructure of the steel strip after isothermal quenching in an embodiment of the present invention. Figure 2 This is a microstructure diagram of the structure after cold rolling and reduction by 50% in an embodiment of the present invention. Figure 3 This is a microstructure diagram of the structure after 80% reduction during cold rolling, according to an embodiment of the present invention. Detailed Implementation
[0027] The technical solution of the present invention will be described in detail below with reference to specific embodiments. The following embodiments are only used to explain the present invention and are not intended to limit the scope of protection of the present invention.
[0028] I. This embodiment provides an elastic element strip, which is a high-carbon low-alloy cold-rolled spring steel strip, using a high-purity C-Mn-Si composition system, without the addition of Ni, Mo, and V precious metal alloys, and its composition by mass percentage is as follows: C: 0.85–1.00%, Si: 0.10–0.40%, Mn: 0.20–0.80%, Cr: 0.05–0.40%, N: 0.002–0.008%, Al: 0.005–0.060%, P: 0–0.025%, S: 0–0.025%, with the balance being Fe and unavoidable impurities.
[0029] The composition system of this invention corresponds to national standards T9A and T10A, and Japanese standards SK85 and SK95, among other high-carbon tool steel standards. The composition system is mature, the raw materials are readily available, and the cost-effectiveness is extremely high. The roles of each element and the reasons for the content limits are as follows: Carbon (C: 0.85~1.00%): As the most economical strengthening element, it is the core strengthening element of this invention, directly determining the hardness, strength, and structural stability of the sorbite structure after isothermal quenching. When the carbon content is below 0.85%, the cementite content in the matrix is insufficient, resulting in low strength, which cannot meet the high strength requirements of over 1600MPa. When the carbon content is above 1.00%, the carbon content in the matrix is too high, the plasticity and cold working properties of the steel decrease significantly, and cracking and band breakage defects are prone to occur during high reduction rate cold rolling, resulting in extremely poor production stability.
[0030] Silicon (Si: 0.10–0.40%): It has a dual function of deoxidation and purification as well as microstructure regulation. It can effectively remove oxygen impurities from molten steel and reduce inclusion defects in the matrix; at the same time, it can inhibit the precipitation of coarse lamellar cementite during isothermal transformation, refine the lamellar structure of sorbite, and improve the uniformity and toughness of the microstructure. A silicon content below 0.10% results in insufficient deoxidation and poor steel purity; a content above 0.40% will exacerbate the cold brittleness of the steel and reduce its elasticity and fatigue performance.
[0031] Manganese (Mn: 0.20~0.80%): Its core function is to improve the hardenability of steel, ensuring that 1.5mm~2.5mm thick strip achieves a uniform sorbitic transformation across the entire cross-section during isothermal quenching, preventing the formation of abnormal soft structures such as ferrite and coarse pearlite, and guaranteeing uniform hardness and strength of the strip cross-section. Too low a manganese content results in insufficient hardenability and substandard core microstructure in thick strips; too high a content easily leads to central segregation during continuous casting and rolling, forming banded structures, disrupting matrix continuity, and significantly reducing fatigue life under alternating loads.
[0032] Chromium (Cr: 0.05~0.40%): In this invention, chromium is controlled as a limited element. Trace amounts of chromium can help improve the hardenability of thick strip and optimize the uniformity of the microstructure. If the chromium content exceeds the limit, it will significantly increase the resistance to cold rolling deformation, increase the equipment load and production costs, and cannot improve the elasticity and fatigue properties of the sorbite structure, thus providing no technical benefit. Therefore, the upper limit is strictly limited.
[0033] Nitrogen (0.002~0.008%) and aluminum (0.005~0.060%): Trace amounts of Al and N can combine to form fine and dispersed AlN nanoprecipitates, effectively refining austenite grains and sorbite lamellae, achieving fine-grain strengthening, and simultaneously improving the material's toughness and microstructure stability. Excessive N and Al will aggregate to form coarse inclusions, creating stress concentration points and impairing the steel's plasticity, toughness, and fatigue properties; therefore, strict control of their amounts is necessary.
[0034] Phosphorus (0-0.025%) and sulfur (0-0.025%) are typical harmful impurities in steel. Phosphorus easily causes brittleness in the matrix, while sulfur easily forms sulfide inclusions that disrupt the continuity of the microstructure. This invention strictly limits the content of both to maximize the purity of the steel, eliminate internal defects, and ensure the long-term stability of the elastic element.
[0035] The specific weight percentages of the seven embodiments of the present invention are shown in Table 3 below: Table 3.
[0036] .
[0037] II. This embodiment provides a method for manufacturing elastic element strip, the overall process route of which is: strip raw material pretreatment → continuous austenitizing heating → isothermal quenching → cold rolling. The core simplified process is: austenitizing + isothermal quenching + cold rolling strengthening, eliminating the need for the traditional multiple cold rolling + annealing, quenching, and high-temperature tempering processes of spring steel. Specifically, it includes the following steps: (1) Raw material pretreatment and austenitization: Select hot-rolled or cold-rolled base strip steel, thoroughly remove surface iron oxide scale, oil stains and impurities, and cut to the target width; continuously feed the strip steel into the heating furnace, and perform austenitization in the range of 780℃~980℃ (preferably austenitization temperature of 850℃~920℃), accurately control the holding time, realize complete homogenization of austenitic structure, refine grains, eliminate rolling residual stress, and provide a stable microstructure basis for subsequent isothermal transformation.
[0038] (2) Isothermal quenching: The austenitized strip is rapidly cooled to 450℃~550℃ and isothermally quenched until the austenite completes the isothermal transformation, resulting in an ultrafine and uniform sorbite structure with a lamellar spacing of about 100 nanometers. This structure has both high strength and excellent plasticity, and is free from martensitic brittle defects, which is the core basis for the material's high elasticity and high fatigue performance.
[0039] (3) Cold rolling: The sorbitic steel strip is cold rolled, with the cumulative cold rolling reduction rate controlled between 50% and 80%. During the cold rolling process, the fine sorbitic cementite lamellae bend and deform, and gradually tend to align parallel to the rolling direction; at the same time, the dislocation density of the matrix increases sharply, resulting in a strong work hardening effect. As the reduction rate increases, the material strength continues to increase, and a strength of 1800 MPa can be stably obtained when the reduction rate is increased to over 70%. The finished product thickness covers the specification range of 1.5 mm to 2.5 mm.
[0040] III. Experiment.
[0041] In this embodiment, room temperature tensile properties of finished strips of various specifications were tested, and the tensile strength data of the finished products are shown in Table 4 below: Table 4.
[0042] .
[0043] The tensile strength of the finished products of this invention, ranging from 1.5mm to 2.5mm, is consistently ≥1600MPa, which is far superior to that of traditional quenched and tempered spring steel strips of the same specifications. Furthermore, the performance degradation is controllable and the overall stability is excellent as the thickness increases, making it perfectly suited for the use of thick elastic components.
[0044] See Figures 1-3 Microstructural observation results show that the initial isothermal quenched state is a uniformly dispersed fine lamellar sorbite structure; as the cold rolling reduction rate gradually increases, the sorbite lamellae gradually deform and deflect, eventually aligning in parallel along the rolling direction, the lamellar spacing is further refined, the matrix dislocation density continues to increase, and the strength increases step by step.
[0045] Industrial Application Prospects: This invention breaks through the technical bottlenecks of traditional spring steel, which suffers from high alloy content, high energy consumption, imbalance between strength and toughness, and unstable performance in thick specifications. Using low-cost high-carbon steel as the base material, and through an innovative process of isothermal martensitization combined with large-strain cold rolling strengthening, it achieves low-cost mass production substitution for high-end elastic strips. The elastic element strips prepared by this invention require no subsequent quenching and tempering treatment, resulting in a short process flow, low energy consumption, and significant cost advantages. The products possess ultra-high strength, high elastic stability, and high fatigue resistance, and can be widely used in various fields such as automotive precision instrument springs, mechanical elastic components, and elastic sensing elements for intelligent equipment. They are particularly suitable for high-end emerging industries such as new energy vehicles and humanoid robots. With high technical barriers and strong market competitiveness, this invention possesses significant industrialization promotion value and economic benefits.
[0046] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above descriptions are merely specific embodiments of the present invention and are not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A type of elastic element strip, characterized in that: Composition by weight percentage: C: 0.85–1.00%, Si: 0.10–0.40%, Mn: 0.20–0.80%, Cr: 0.05–0.40%, N: 0.002–0.008%, Al: 0.005–0.060%, P: 0–0.025%, S: 0–0.025%, with the balance being Fe and unavoidable impurities.
2. The elastic element strip according to claim 1, characterized in that: The composition by mass percentage is: C: 0.85%, Si: 0.20%, Mn: 0.30%, Cr: 0.15%, N: 0.006%, Al: 0.040%, P: 0.015%, S: 0.010%, with the balance being Fe and unavoidable impurities.
3. The elastic element strip according to claim 1, characterized in that: The composition by mass percentage is: C: 0.88%, Si: 0.25%, Mn: 0.45%, Cr: 0.05~0.40%, N: 0.005%, Al: 0.028%, P: 0.012%, S: 0.003%, with the balance being Fe and unavoidable impurities.
4. The elastic element strip according to claim 1, characterized in that: The composition by mass percentage is: C: 0.90%, Si: 0.25%, Mn: 0.75%, Cr: 0.10%, N: 0.005%, Al: 0.035%, P: 0.012%, S: 0.005%, with the balance being Fe and unavoidable impurities.
5. The elastic element strip according to claim 1, characterized in that: The composition by mass percentage is: C: 0.85–1.00%, Si: 0.95%, Mn: 0.60%, Cr: 0.10%, N: 0.004%, Al: 0.030%, P: 0.011, S: 0.003%, balance is Fe and unavoidable impurities.
6. The elastic element strip according to claim 1, characterized in that: The composition by mass percentage is: C: 0.99%, Si: 0.30%, Mn: 0.50%, Cr: 0.35%, N: 0.003%, Al: 0.040%, P: 0.010%, S: 0.002%, with the balance being Fe and unavoidable impurities.
7. A method for manufacturing an elastic element strip according to any one of claims 1-6, characterized in that: Includes the following steps: (1) Raw material pretreatment and austenitization: Select hot-rolled or cold-rolled base strip steel, remove surface iron oxide scale, oil stains and impurities, and cut to the target width; continuously feed the strip steel into the heating furnace and austenitize it in the range of 780℃~980℃; (2) Isothermal quenching: Cool the austenitized strip to 450℃~550℃ and perform isothermal quenching, and keep it at the temperature until the austenite completes the isothermal transformation to obtain an ultrafine and uniform sorbite structure. (3) Cold rolling: The sorbitic steel strip is cold rolled, and the cumulative cold rolling reduction rate is controlled at 50% to 80%. During the cold rolling process, the fine sorbitic cementite lamellae bend and deform, and gradually tend to be oriented parallel to the rolling direction. At the same time, the matrix dislocation density increases sharply, resulting in a strong work hardening effect. As the reduction rate increases, the material strength continues to increase. When the reduction rate is increased to over 70%, strips with a strength of 1800MPa can be stably obtained.
8. The method for manufacturing the elastic element strip according to claim 7, characterized in that: The austenitizing temperature is 850℃~920℃.