A fiber-reinforced magnesium alloy composite material and its preparation method

By setting an amorphous SiOC diffusion barrier layer and a porous MgAl2O4 wetting anchoring layer on the surface of continuous silicon carbide fibers, and combining low-pressure pre-impregnation and high-pressure deep impregnation methods, the problems of interfacial reaction and insufficient wetting in magnesium alloy composites were solved, and high strength and high durability of high fiber content composites were achieved.

CN123108442APending Publication Date: 2026-11-17HANGZHOU TAOFEILUN NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611151542.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Insufficient interfacial reaction and wetting between continuous silicon carbide fibers and magnesium alloy melt makes it difficult for the fiber bundle to be fully impregnated. Direct high-pressure impregnation leads to fiber bundle deformation and coating erosion, resulting in insufficient transverse crack resistance and surface finish of high fiber content composite materials.

Method used

An amorphous SiOC diffusion barrier layer and a porous MgAl2O4 wetting anchoring layer are set on the surface of continuous silicon carbide fibers. A gradient mechanical anchoring zone is formed by combining low-pressure pre-impregnation and high-pressure deep impregnation to ensure melt flowability and matrix continuity. Longitudinal fiber bundles and cross-constrained fiber bundles are set in the composite material to improve crack resistance.

Benefits of technology

It effectively suppressed interfacial reactions, improved melt wettability and load transfer capacity, reduced porosity, enhanced longitudinal load-bearing capacity and transverse crack resistance of composite materials, and improved surface finish.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108442A_ABST
    Figure CN123108442A_ABST
Patent Text Reader

Abstract

This invention discloses a fiber-reinforced magnesium alloy composite material and its preparation method, relating to the field of metal matrix composite technology. The material includes a magnesium alloy matrix and a continuous silicon carbide fiber preform embedded in the magnesium alloy matrix. The continuous silicon carbide fiber preform has a volume fraction of 25%–45% in the composite material, which improves specific stiffness and load-bearing capacity while reserving necessary space for melt flow and matrix continuity. An amorphous SiOC diffusion barrier layer and a porous MgAl2O4 wetting and anchoring layer are sequentially disposed on the surface of the continuous silicon carbide fibers from the inside out. The amorphous SiOC diffusion barrier layer directly covers the surface of the silicon carbide fibers, with a thickness of 80 nm–250 nm. Through direct contact between the amorphous SiOC diffusion barrier layer and the silicon carbide fibers, the diffusion path of magnesium and silicon at the interface can be extended, reducing the tendency for the formation of a continuous Mg2Si reaction layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of metal matrix composites, specifically to a fiber-reinforced magnesium alloy composite material and its preparation method. Background Technology

[0002] Magnesium alloys possess low density and high specific strength and specific stiffness, making them suitable for lightweight structures in aerospace, rail transportation, low-altitude aircraft, and high-speed moving components. However, conventional magnesium alloys have limited absolute elastic modulus and high-temperature load-bearing capacity, making them prone to fatigue crack initiation under repeated loading, thus failing to directly meet the requirements for long-life, high-specific-stiffness components. Introducing continuous silicon carbide fibers into magnesium alloys can leverage the high modulus and heat resistance of the fibers to improve the longitudinal load-bearing capacity of the composite material, representing a feasible direction for enhancing the efficiency of magnesium alloy structures.

[0003] The practical preparation of continuous silicon carbide fiber-reinforced magnesium matrix composites still faces two mutually restrictive problems. First, the magnesium alloy melt may undergo an interfacial reaction with the silicon carbide fibers at the infiltration temperature, forming brittle reactive phases such as Mg2Si. This continuous reactive layer weakens the fibers and becomes a crack initiation point during thermal cycling. Second, the dense inert layer set to suppress the interfacial reaction easily reduces the wettability of the melt, resulting in unimpregnated areas and residual porosity within the fiber bundle, preventing the load from being effectively transferred from the magnesium alloy matrix to the fibers.

[0004] Existing pressure impregnation methods typically apply high pressure directly to force the melt into the fiber bundle. While direct and rapid pressure increases can improve the macroscopic filling speed, they can also cause localized compaction of the fiber preform, premature closure of channels, or fiber bundle misalignment. When a coating is present on the fiber surface, the high-pressure front may also erode the coating and trap gas within the bundle. Simply increasing the impregnation pressure cannot simultaneously solve the problems of fiber protection, interfacial bonding, and internal densification.

[0005] Furthermore, while unidirectional high-volume-fraction fiber structures possess high longitudinal modulus, they suffer from insufficient transverse crack resistance and edge processing integrity. At high fiber contents, the surface layer is prone to fiber exposure, notch sensitivity, and processing chipping. Therefore, a systematic technical solution is needed that balances interfacial chemical stability, melt wetting and mechanical interlocking, preform impregnation, transverse crack restraint, and surface processing performance. Summary of the Invention

[0006] The purpose of this invention is to provide a fiber-reinforced magnesium alloy composite material and its preparation method, in order to solve the problems of contradictory interfacial reactions and insufficient wetting between continuous silicon carbide fibers and magnesium alloy melt, difficulty in sufficient infiltration into the fiber bundle, fiber bundle deformation and coating erosion caused by direct high-pressure infiltration, and insufficient transverse crack resistance and surface processing integrity of high fiber content composite materials.

[0007] To achieve the above objectives, the present invention provides the following technical solution: a fiber-reinforced magnesium alloy composite material, comprising a magnesium alloy matrix and a continuous silicon carbide fiber preform embedded in the magnesium alloy matrix. The continuous silicon carbide fiber preform has a volume fraction of 25% to 45% in the composite material, so as to improve the specific stiffness and load-bearing capacity while reserving the necessary space for melt flow and matrix continuity.

[0008] An amorphous SiOC diffusion barrier layer and a porous MgAl2O4 wetting and anchoring layer are sequentially disposed on the surface of continuous silicon carbide fibers from the inside out. The amorphous SiOC diffusion barrier layer directly covers the surface of the silicon carbide fibers, with a thickness of 80 nm to 250 nm; the porous MgAl2O4 wetting and anchoring layer covers the amorphous SiOC diffusion barrier layer, with a thickness of 0.3 μm to 1.5 μm, an open porosity of 15% to 35%, and a pore size of 0.1 μm to 0.6 μm.

[0009] During pressure infiltration, the magnesium alloy matrix penetrates inward along the open pores of the porous MgAl2O4 wetting anchoring layer to a depth of 30%–80% of the layer's thickness. This creates a gradient mechanical anchoring zone between the magnesium alloy matrix and the amorphous SiOC diffusion barrier layer, formed by the interlocking of magnesium alloy matrix and MgAl2O4 particles. This gradient mechanical anchoring zone is not a continuous brittle reaction layer, but rather a load transfer zone formed by the interlacing of the ceramic skeleton and the infiltrated metallic phase.

[0010] The magnesium alloy matrix preferably comprises, by mass percentage, 5.0%–9.0% aluminum, 0.2%–1.5% zinc, 0.10%–0.60% manganese, 0.05%–0.50% calcium, and 0.10%–1.00% yttrium, with the balance being magnesium and unavoidable impurities; wherein the iron content is not higher than 0.010%, the nickel content is not higher than 0.005%, and the copper content is not higher than 0.030%. Aluminum and zinc are used to improve the matrix strength and casting fluidity, manganese is used to reduce the adverse effects of iron impurities, and calcium and yttrium are used to improve the high-temperature structural stability and reduce the tendency of the melt to oxidize.

[0011] The diameter of the continuous silicon carbide fibers is preferably 8 μm to 16 μm. The continuous silicon carbide fiber preform includes longitudinal fiber bundles arranged along the main load-bearing direction and cross-constrained fiber bundles arranged at an angle of ±30° to ±60° to the longitudinal fiber bundles. The longitudinal fiber bundles account for 60% to 85% of the total fiber volume. Interconnected impregnation channels are provided between adjacent fiber bundles. The equivalent width of the impregnation channels is 80 μm to 300 μm, and the impregnation channels account for 4% to 12% of the total volume of the continuous silicon carbide fiber preform.

[0012] The preferred ratio of oxygen to carbon atoms in the amorphous SiOC diffusion barrier layer is 0.3–1.2. The porous MgAl₂O₄ wetting anchoring layer is formed by connecting MgAl₂O₄ grains with a particle size of 30 nm–150 nm. In the interfacial region within 2 μm of the continuous silicon carbide fiber surface, the Mg₂Si reactive phase is distributed in a discontinuous granular form, with an area fraction of no more than 3%, and no continuous Mg₂Si reactive layer with a thickness greater than 150 nm exists.

[0013] Preferably, to improve the surface processing integrity of the component, the composite material may be provided with a surface transition zone and an internal load-bearing zone sequentially along the thickness direction. The thickness of the surface transition zone is 0.5 mm to 3.0 mm, and the volume fraction of continuous silicon carbide fibers in the surface transition zone is 15% to 28%; the volume fraction of continuous silicon carbide fibers in the internal load-bearing zone is 32% to 50%, and the fiber volume fraction between the surface transition zone and the internal load-bearing zone changes continuously along the thickness direction.

[0014] Another aspect of the present invention provides a method for preparing the above-mentioned fiber-reinforced magnesium alloy composite material, comprising: degumming and surface activation of continuous silicon carbide fibers to prepare an amorphous SiOC diffusion barrier layer on its surface; depositing MgAl2O4 particles on the surface of the amorphous SiOC diffusion barrier layer and solidifying and sintering them to form a porous MgAl2O4 wetting and anchoring layer with interconnected open pores; forming a preform with interconnected impregnation channels from a double-layer interface modified fiber; melting a magnesium alloy and preheating the preform; performing low-pressure pre-impregnation under vacuum conditions, followed by high-pressure deep impregnation; and finally, directional solidification under the condition of maintaining the impregnation pressure, followed by solution treatment and aging treatment.

[0015] To prepare the amorphous SiOC diffusion barrier layer, continuous silicon carbide fibers after degumming are immersed in a polysiloxane precursor solution with a solid content of 3%–12%, and pulled at a speed of 1 mm / s–10 mm / s. The fibers are then crosslinked and cured at 150℃–250℃ for 30 min–120 min. Subsequently, the temperature is increased to 750℃–900℃ in an inert atmosphere at a heating rate of 2℃ / min–10℃ / min and held for 1 h–3 h, transforming the polysiloxane into an amorphous SiOC layer. The impregnation, crosslinking, curing, and pyrolysis processes can be repeated 1 to 3 times.

[0016] To prepare a porous MgAl2O4 wetting anchoring layer, MgAl2O4 powder with an average particle size of 30nm to 100nm can be dispersed in an alumina sol, with a mass ratio of MgAl2O4 powder to the solid components in the alumina sol of 70:30 to 90:10. Fibers with an amorphous SiOC layer are immersed in the resulting slurry, dried, and then sintered in nitrogen or argon at 700℃ to 850℃ for 30 to 120 minutes. By controlling the solid content of the slurry, the pore-forming components, the pulling speed, and the number of coatings, the resulting anchoring layer can have an open porosity of 15% to 35%.

[0017] The preheating temperature of the continuous fiber preform is 520℃~620℃, and the infiltration temperature of the magnesium alloy melt is 680℃~730℃. After reducing the absolute pressure in the infiltration mold to below 100Pa, the magnesium alloy melt is brought into contact with the preform. Pre-infiltration is first performed at 0.3MPa~1.0MPa for 10s~60s, allowing the melt to spread evenly along the macroscopic infiltration channels and expel inter-bundle gas. Then, the pressure is increased to 8MPa~18MPa at a rate of 0.5MPa / s~3MPa / s and held for 60s~240s, allowing the melt to further penetrate into the fiber bundle interior and the open pores of the porous MgAl2O4 layer. Argon gas is preferably used as the pressurizing medium for both low-pressure pre-infiltration and high-pressure deep infiltration.

[0018] During the solidification stage, a pressure of 8 MPa to 18 MPa is maintained until the temperature of the magnesium alloy matrix drops to 80°C to 150°C below the solidus. After demolding, solution treatment is carried out at 390°C to 420°C for 4 to 12 hours, followed by water quenching at 60°C to 90°C and artificial aging at 170°C to 210°C for 6 to 16 hours. After the above treatment, the overall porosity of the composite material is preferably no higher than 1.5%, and the open porosity of the unfilled magnesium alloy in the porous MgAl2O4 layer is 3% to 12%.

[0019] Compared with existing technologies, this invention provides a fiber-reinforced magnesium alloy composite material and its preparation method, which has the following beneficial effects: By directly contacting the amorphous SiOC diffusion barrier layer with the silicon carbide fibers, the diffusion path of magnesium and silicon at the interface can be extended, reducing the tendency for continuous Mg2Si reaction layers to form. Maintaining the amorphous state of this layer and controlling its size between 80nm and 250nm can reduce penetrating grain boundaries and local defects, while avoiding excessively thick, brittle layers that could lead to delamination.

[0020] The porous MgAl2O4 wetting anchoring layer is located outside the SiOC layer. Its interconnected open pores allow the magnesium alloy melt to partially penetrate during the high-pressure stage, forming a gradient mechanical anchoring zone with metal-ceramic interlacing, so that the load is not dependent on a single flat interface for transmission. The incompletely filled micropores can also provide local buffering for thermal expansion mismatch.

[0021] By first achieving uniform filling of macroscopic channels and fiber bundle gaps through low-pressure pre-impregnation, and then driving the melt into the micropores through high-pressure deep impregnation, the venting and deep impregnation processes are separated. This sequence reduces gas congestion, sudden fiber bundle compaction, and coating erosion, thereby improving the integrity of the bilayer interface.

[0022] The longitudinal fiber bundles bear the main axial load, while the cross-constrained fiber bundles limit the propagation of transverse cracks; the interconnected infiltration channels also prevent the cross structures from blocking the melt. The surface transition zone reduces fiber exposure and notch sensitivity at the processed surface, while the internal load-bearing zone maintains a high fiber volume fraction.

[0023] The dual-layer interface, connecting channels, and graded pressure are not simply independent combinations. If there is only a reaction barrier layer without a porous anchoring layer, melt wetting and load transfer will be insufficient; if there is only a porous anchoring layer without a reaction barrier layer, the interfacial reaction will be intensified at high temperatures; if there is a dual-layer interface but the graded pressure or connecting channels are removed, high porosity will still occur due to gas closure or coating erosion. Attached Figure Description

[0024] Figure 1 This is a high-resolution transmission electron microscope image of the cross-section of the SiOC diffusion barrier layer and the porous MgAl2O4 wetting anchoring layer on the surface of the continuous silicon carbide fiber in Example 4 of the present invention. Figure 2 This is a cross-sectional SEM image of the fiber / matrix interface region in Embodiment 4 of the present invention; Figure 3 This is a cross-sectional SEM image of the fiber / matrix interface region in Comparative Example 3 of the present invention. Detailed Implementation

[0025] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0026] Please see Figures 1-3 This invention provides a technical solution for fiber-reinforced magnesium alloy composite materials and their preparation method: Terminology and Parameter Determination The "amorphous SiOC diffusion barrier layer" refers to a continuous layer composed primarily of silicon, oxygen, and carbon, in which selected area electron diffraction does not produce resolvable crystalline diffraction spots or bands, and is situated between silicon carbide fibers and a porous MgAl2O4 layer. Its thickness is determined by the average value of measurements taken at no fewer than 20 equally spaced locations in a cross-sectional TEM image.

[0027] "Porous MgAl2O4 wetting anchoring layer" refers to a ceramic layer formed by the connection of MgAl2O4 grains, having pores that communicate with the outer surface and allow partial entry of molten magnesium alloy. The open porosity of the coating was cross-checked using cross-sectional image analysis and nitrogen adsorption results; the pore size was the statistical median value of the equivalent circle diameter of no less than 200 open pores.

[0028] "Penetration depth" refers to the percentage obtained by dividing the average distance from the outer surface of the porous MgAl2O4 layer inward to the continuous metal penetration front by the total thickness of the MgAl2O4 layer at that point. Measurements are taken every 30° along the fiber circumference, with 12 locations per fiber and no fewer than 10 fibers per group.

[0029] "Connecting infiltration channels" are continuous voids intentionally retained during preform formation and connected to the infiltration inlet. Their equivalent width is calculated by dividing the channel's cross-sectional area by the channel's projected length on the cross-section; the channel's volume fraction is determined by three-dimensional X-ray microscopy or the preform mass-geometric volume method.

[0030] The "total porosity" is calculated as the difference between the measured density of the composite material and the theoretical density calculated based on the true density and volume fraction of each component phase, i.e., total porosity P = [1 − ρ_measured / ρ_theoretical] × 100%. At least 5 samples should be taken for each test group and the average value should be reported.

[0031] Raw materials and general equipment The continuous silicon carbide fiber uses near-stoichiometric SiC fibers with a bundle size of 500 fibers / bundle, and the original monofilament strength is not less than 2.6 GPa. The polysiloxane precursor is a liquid polymer that can be converted into SiOC ceramic in an inert atmosphere, and the solid content is adjusted with a mixed solvent of anhydrous ethanol and xylene. The purity of MgAl2O4 powder is not less than 99.5%, and the Al2O3 solid content in the alumina sol is 20%. The purity of magnesium, aluminum, zinc, manganese, calcium, and magnesium-yttrium master alloys meets the smelting requirements.

[0032] The main equipment includes a continuous fiber degumming furnace, an impregnation and lifting device, an inert atmosphere tube furnace, a fiber weaving / layout device, graphite or heat-resistant steel impregnation molds, a vacuum pressure impregnation furnace, a directional solidification device with a bottom water-cooled plate, and a protective atmosphere heat treatment furnace. All parts in contact with the molten magnesium are dried and coated with a boron nitride release layer before use.

[0033] General preparation method of bilayer interface Continuous silicon carbide fibers are heated in air at 400℃~480℃ for 20min~60min to remove the original sizing agent, and then treated in an ethanol aqueous solution containing 1%~3% silane coupling agent for 5min~15min. After drying, surface-activated fibers are obtained. For oxygen-sensitive fibers, air desizing can be replaced with segmented pyrolysis under a nitrogen atmosphere, and surface activation can be performed with low-power oxygen plasma for 30s~120s.

[0034] Activated fibers are immersed in a polysiloxane precursor solution and pulled at a specified speed. They are first dried at 80°C, then crosslinked and cured at a specified temperature and time. The cured fibers are placed in an argon tube furnace, heated to the pyrolysis temperature at a specified rate, and held at that temperature. After cooling, an amorphous SiOC layer is obtained. The layer thickness is adjusted by the precursor solid content and the number of cycles.

[0035] A coating slurry was prepared by mixing MgAl2O4 nanoparticles, alumina sol, polyethylene glycol pore-forming agent, and ethanol, and ball milling for 2-6 hours. SiOC-modified fibers were immersed in the slurry and pulled, dried, and then sintered under an inert atmosphere. This process allowed MgAl2O4 particles to form necks through a small amount of alumina sol, while simultaneously decomposing and removing the polyethylene glycol, creating interconnected open pores. The layer thickness and porosity were adjusted by combining the slurry solids content, pore-forming agent content, pulling speed, coating cycles, and sintering temperature.

[0036] General methods for prefabrication and impregnation The bilayer interface-modified fibers are laid out or three-dimensionally shallowly woven according to a predetermined ratio of longitudinal fiber bundles to cross-constrained fiber bundles. Connecting impregnation channels are formed between adjacent fiber bundles using pyrolytic spacer filaments or extractable core strips. The surface transition zone is formed by progressively reducing the number of fiber bundles, while the internal load-bearing zone maintains a high fiber volume fraction, with at least two gradient layers between them.

[0037] The preform is placed into a preheated mold and a slight positioning pressure is applied to prevent it from moving during vacuuming. When smelting the magnesium alloy, magnesium, aluminum, and zinc are added first. After melting, manganese, calcium, and magnesium-yttrium master alloy are added. The mixture is then refined under an SF6 alternative protective gas or argon atmosphere. After slag removal, the temperature is adjusted to the infiltration temperature.

[0038] The impregnation mold is evacuated to an absolute pressure below 100 Pa and maintained for 5 to 20 minutes to expel the gas inside the preform. The melt channel is opened to allow the magnesium alloy melt to cover the preform inlet, and argon gas is introduced to perform low-pressure pre-impregnation. Subsequently, the pressure is increased to high pressure at a specified rate and maintained. After impregnation, cooling begins from the bottom of the mold, allowing the solidification front to advance in the opposite direction to the main impregnation direction until the matrix temperature is below the specified solidus temperature, at which point the pressure is released.

[0039] Example 1: After degumming and activating continuous silicon carbide fibers with a diameter of 8 μm, a polysiloxane precursor solution with a solid content of 3% was used for one pull at 1 mm / s and crosslinked at 150 °C for 30 min; then the temperature was raised to 750 °C at 2 °C / min in argon and held for 1 h to obtain an amorphous SiOC diffusion barrier layer with an average thickness of 80 nm and an O / C atomic ratio of 0.30.

[0040] MgAl2O4 powder with an average particle size of 30 nm was mixed with alumina sol solid at a ratio of 70:30, and an appropriate amount of polyethylene glycol pore-forming agent was added. After coating, the mixture was sintered at 700 °C for 30 min to obtain a porous MgAl2O4 wetting and anchoring layer with a thickness of 0.30 μm, an open porosity of 15%, and a median pore size of 0.10 μm.

[0041] The modified fibers were used to make a preform with a total fiber volume fraction of 25%, of which longitudinal fibers accounted for 60%, and the cross fibers were at ±30° to the longitudinal fibers. The equivalent width of the connecting impregnation channels was 80 μm and the volume fraction was 4%. A 0.5 mm thick transition zone was set on the surface of the preform, with a fiber volume fraction of 15% in the transition zone and a fiber volume fraction of 32% in the internal load-bearing zone.

[0042] The magnesium alloy was prepared with the following composition: Al 5.0%, Zn 0.2%, Mn 0.10%, Ca 0.05%, Y 0.10%, and the balance Mg. The preform was preheated to 520℃, and the melt temperature was controlled at 680℃. After the mold was evacuated to 80Pa, it was pre-impregnated under argon pressure at 0.3MPa for 10s, then increased to 8MPa at 0.5MPa / s and held for 60s. The pressure was maintained at 8MPa for directional solidification until the temperature was 80℃ below the solidus. After demolding, it was solution-treated at 390℃ for 4h, water-quenched at 60℃, and then aged at 170℃ for 6h.

[0043] Cross-sectional statistics show that the average penetration depth of the magnesium alloy in the porous MgAl2O4 layer is 30% of the layer thickness, with an overall porosity of 1.18% and a residual unfilled open porosity of 11.8%. This example demonstrates that a complete bilayer interface can still be formed and acceptable infiltration density can be obtained under the combination of endpoints in each major range.

[0044] Example 2: An amorphous SiOC layer with an average thickness of 160 nm and an O / C atomic ratio of 0.75 was obtained by two cycles of polysiloxane dip coating-crosslinking-pyrolysis; then, a slurry with a MgAl2O4 to sol solid mass ratio of 80:20 was sintered at 775 °C for 75 min to obtain a porous anchoring layer with a thickness of 0.90 μm, an open porosity of 25%, and a median pore size of 0.35 μm.

[0045] The preform has an overall fiber volume fraction of 35%, with longitudinal fibers accounting for 72%, cross-fiber angles of ±45°, channel width of 180μm, and channel volume fraction of 8%. The surface transition zone is 1.5mm thick with a fiber volume fraction of 22%, and the internal load-bearing zone has a fiber volume fraction of 41%. The magnesium alloy contains Al 7.0%, Zn 0.8%, Mn 0.35%, Ca 0.25%, Y 0.50%, with the balance being Mg.

[0046] The preform was preheated at 570℃, and the melt was infiltrated at 705℃. After the mold was evacuated to 60Pa, it was pre-infiltrated at 0.65MPa for 35s, then increased to 13MPa at 1.5MPa / s and held for 150s. It was then solidified under pressure to 115℃ below the solidus, solution-treated at 405℃ for 8h, water-quenched at 75℃, and aged at 190℃ for 11h.

[0047] The average penetration depth of the magnesium alloy in the obtained material was 55% of the anchoring layer thickness, with an overall porosity of 0.74% and a residual open porosity of 7.6%. No continuous Mg2Si layer with a thickness greater than 150 nm was observed by interfacial TEM.

[0048] Example 3: A SiOC layer with an average thickness of 250 nm and an O / C atomic ratio of 1.20 was obtained by three cycles of dip coating-crosslinking-pyrolysis; an anchoring layer with a thickness of 1.50 μm, an open porosity of 35%, and a median pore size of 0.60 μm was obtained by using a slurry with a MgAl2O4 to sol solid mass ratio of 90:10 and sintering at 850 °C for 120 min.

[0049] The preform has an overall fiber volume fraction of 45%, with longitudinal fibers accounting for 85%, an intersection angle of ±60°, a channel width of 300μm, and a channel volume fraction of 12%. The surface transition zone is 3.0mm thick with a fiber volume fraction of 28%, while the internal load-bearing zone has a fiber volume fraction of 50%. The magnesium alloy contains Al 9.0%, Zn 1.5%, Mn 0.60%, Ca 0.50%, Y 1.00%, with the balance being Mg.

[0050] The preform was preheated to 620℃, with a melt temperature of 730℃. The mold was evacuated to 40Pa, pre-impregnated at 1.0MPa for 60s, then increased to 18MPa at 3.0MPa / s and held for 240s. Solidification was carried out at 18MPa until 150℃ below the solidus, followed by solution treatment at 420℃ for 12h, water quenching at 90℃, and aging at 210℃ for 16h.

[0051] The magnesium alloy penetration depth in the obtained material reached 80% of the anchoring layer thickness, with an overall porosity of 1.28% and a residual open porosity of 3.2%. This example demonstrates that it can still be implemented when the main parameters are at the upper end; however, due to the increased tortuosity of the local penetration path caused by the fiber volume fraction and coating porosity at the upper end, its fatigue stability is slightly lower than that of Example 4, but its longitudinal strength and modulus are higher.

[0052] Example 4: A uniform amorphous SiOC layer with an average thickness of 180 nm and an O / C atomic ratio of 0.65 was formed on the fiber surface through two cycles of polysiloxane impregnation-crosslinking-pyrolysis with a solid content of 8%. A slurry with a solid mass ratio of MgAl2O4 to alumina sol of 82:18 was sintered at 800℃ for 90 min to form a MgAl2O4 layer with an average thickness of 1.00 μm, an open porosity of 28%, and a median pore size of 0.30 μm.

[0053] The precast structure has an overall fiber volume fraction of 38%, with longitudinal fibers accounting for 75% and cross fibers at ±45°. The impregnation channel has an equivalent width of 160μm and occupies 7% of the precast structure volume. A 1.2mm thick surface transition zone with a fiber volume fraction of 20% is provided; the internal load-bearing zone has a fiber volume fraction of 43%, and three transition layers with progressively varying fiber volume fractions are provided between the two.

[0054] The magnesium alloy contains 7.5% Al, 0.9% Zn, 0.35% Mn, 0.20% Ca, and 0.60% Y, with the balance being Mg. The preform is preheated to 580℃, and the melt is infiltrated at 710℃. The mold is evacuated to 50 Pa and held for 10 min, then pre-infiltrated under 0.6 MPa argon pressure for 40 s, then increased to 14 MPa at 1.2 MPa / s and held for 180 s. It is then directionally solidified at 14 MPa to 120℃ below the solidus, followed by solution treatment at 405℃ for 8 h, water quenching at 75℃, and aging at 190℃ for 12 h.

[0055] The magnesium alloy penetration depth of the resulting composite material is 65% of the MgAl2O4 layer thickness, with an overall porosity of 0.62% and a residual open porosity of 6.1%. Mg2Si in the interfacial region exists as discrete particles with an area fraction of 1.1%, and no continuous reaction layer is formed.

[0056] Comparative Example 1: Except for not preparing an amorphous SiOC diffusion barrier layer and directly coating a porous MgAl2O4 wetting anchor layer onto the surface of silicon carbide fibers, the raw material composition, preform structure, impregnation parameters, and heat treatment conditions were the same as in Example 4. This comparative example only changed the presence or absence of a SiOC diffusion barrier layer.

[0057] Comparative Example 2: Except for retaining only the amorphous SiOC diffusion barrier layer with an average thickness of 180 nm and not setting a porous MgAl2O4 wetting anchor layer on its outer side, all other conditions were the same as in Example 4. This comparative example only changed the presence or absence of a porous MgAl2O4 wetting anchor layer.

[0058] Comparative Example 3: Except for removing the pore-forming agent in the MgAl2O4 slurry and increasing the proportion of sol-sol solids, which reduced the open porosity of the resulting MgAl2O4 layer from 28% to 3.0%, and keeping other layer thicknesses and compositions the same, all other conditions were the same as in Example 4. This comparative example only changed the open pore structure of the MgAl2O4 layer.

[0059] Comparative Example 4: Except for the absence of low-pressure pre-impregnation at 0.6 MPa during the impregnation stage, the pressure was directly increased from 3.0 MPa / s to 14 MPa after the melt contacted the preform and held for 180 s, all other conditions were the same as in Example 4. This comparative example only changed the pressurization path.

[0060] Comparative Example 5: Except that no pyrolytic spacer fibers were used during preform forming, reducing the volume fraction of the impregnation channels from 7% to below 0.5%, and keeping the total fiber volume fraction and fiber orientation ratio unchanged, all other conditions were the same as in Example 4. This comparative example only changed whether there were intentionally formed interconnected impregnation channels in the preform.

[0061] Performance testing methods To avoid deviations caused by different sample processing and testing conditions, both the example and comparative examples were prepared in three batches, with samples taken from the same location in each batch. Except for the microstructure, the performance results were the average of no fewer than five valid samples; each fatigue test group consisted of no fewer than eight samples.

[0062] (1) Density and total porosity of composite materials: The measured density was determined by Archimedes method according to GB / T 3850—2015 "Method for Determination of Density of Dense Sintered Metal Materials and Hard Alloys". The theoretical density was calculated based on the volume fraction of each constituent phase and the actual density. The total porosity was then calculated by P=[1−ρmeasured / ρtheoretical]×100%.

[0063] (2) Strength retention rate of continuous silicon carbide fiber: The strength of the original fiber and the recovered fiber after double coating, preheating and equivalent impregnation heat exposure were determined according to GB / T 43307—2023 "Determination of room temperature tensile properties of fine ceramic fiber monofilaments". The strength retention rate is equal to the ratio of the average monofilament strength after treatment to the original average monofilament strength.

[0064] (3) Room temperature tensile properties: Specimens were prepared along the main load-bearing direction according to GB / T 32498—2016 "Metal Matrix Composites - Tensile Testing at Room Temperature" and the tensile strength and elastic modulus were determined. Aluminum alloy reinforcing plates were used at both ends of the specimens and fixed with low-temperature adhesive to reduce clamping damage.

[0065] (4) High-temperature tensile properties: Tensile test was performed at 350℃ for 20 min according to GB / T 228.2—2015 "Metallic materials - Tensile testing - Part 2: High temperature test method", and the high-temperature tensile strength was recorded. The loading axis was consistent with the longitudinal fiber bundle direction.

[0066] (5) Axial fatigue performance: Axial fatigue tests were conducted at room temperature with a stress ratio R=0.1 and a frequency of 20Hz, according to GB / T 3075—2021 "Methods for Controlling Axial Force in Fatigue Testing of Metallic Materials". A maximum stress of 320MPa was used, and the number of cycles until fracture was recorded; the required number of cycles was 1.0×10⁻⁶. 7 Those that do not break are recorded as "running out".

[0067] (6) Microstructure and interfacial reaction layer: Prepare cross-sectional specimens according to GB / T 13298—2015 "Methods for Testing the Microstructure of Metals" and observe the porosity, fiber distribution and interfacial continuity; confirm the amorphous characteristics and interfacial reaction phases of the SiOC layer according to GB / T 18907—2013 "Microbeam Analysis, Electron Microscopy, Transmission Electron Microscopy, Selected Area Electron Diffraction Analysis". Perform image statistics on no less than 20 fields of view.

[0068] (7) Thermal expansion performance as an auxiliary indicator: The average linear expansion coefficient along the main load-bearing direction at 25℃~300℃ was determined in accordance with GB / T 4339—2008 "Determination of thermal expansion characteristic parameters of metallic materials" to evaluate the influence of fiber structure and interface integrity on thermal dimensional stability.

[0069] Table 1 Group Total porosity / % Fiber strength retention rate / % <![CDATA[Maximum thickness of continuous Mg2Si layer / nm]]> <![CDATA[Mg₂Si area fraction / %]]> Interface / Porosity Features Example 1 1.18 92.5 128 2.6 Double-layered and intact, with shallow penetration. Example 2 0.74 94.8 86 1.5 Uniform anchoring with few pores Example 3 1.28 91.7 112 2.2 High fiber content, localized bends Example 4 0.62 95.6 68 1.1 Double-layer integrity, gradient interlocking continuity Comparative Example 1 0.70 76.3 438 6.8 Formation of a continuous brittle reaction layer Comparative Example 2 2.35 96.0 72 1.2 Insufficient wetting, flat interface debonding Comparative Example 3 1.88 95.2 75 1.3 The dense layer prevents metal from penetrating. Comparative Example 4 1.72 95.1 73 1.2 Internal sealing of pores and localized coating erosion Comparative Example 5 2.68 95.4 71 1.2 The fiber bundle core was not impregnated Table 2 Group Room temperature tensile strength / MPa Longitudinal elastic modulus / GPa Tensile strength at 350℃ / MPa Maximum stress 320MPa, fatigue life / cycle <![CDATA[Linear expansion coefficient at 25 to 300℃ / (10⁻ 6 K⁻¹)]]> Example 1 548 101 342 <![CDATA[2.6×10 6 ]]> 17.1 Example 2 692 121 456 <![CDATA[7.8×10 6 ]]> 14.9 Example 3 808 145 526 <![CDATA[6.4×10 6 ]]> 12.7 Example 4 762 133 508 <![CDATA[>1.0×10 7 ]]> 13.8 Comparative Example 1 603 128 356 <![CDATA[1.9×10 6 ]]> 14.2 Comparative Example 2 578 118 401 <![CDATA[1.4×10 6 ]]> 14.0 Comparative Example 3 629 125 432 <![CDATA[3.2×10 6 ]]> 13.9 Comparative Example 4 641 127 438 <![CDATA[3.8×10 6 ]]> 14.0 Comparative Example 5 586 120 394 <![CDATA[1.6×10 6 ]]> 14.1 In Examples 1, 2, and 3, all three groups of materials formed identifiable SiOC layers, porous MgAl2O4 layers, and magnesium alloy infiltrating regions, with overall porosity below 1.5%. Their room temperature tensile strength was significantly higher than that of the control group without optimized interfaces. Example 4 exhibited the lowest overall porosity and a fatigue strength of 1.0 × 10⁻⁶. 7 The fact that the fracture did not occur indicates that a good overall balance can be achieved when the parameters are appropriately selected.

[0070] Example 4 and Comparative Example 1 were identical except for the presence or absence of the SiOC layer. After removing the SiOC layer, the fiber strength retention rate decreased from 95.6% to 76.3%, the maximum thickness of the continuous Mg2Si reaction layer at the interface increased from 68 nm to 438 nm, the tensile strength at 350℃ decreased from 508 MPa to 356 MPa, and the fatigue life increased from over 1.0 × 10⁻⁶ MPa. 7 The next drop was to 1.9 × 10 6 This result demonstrates that the SiOC layer not only reduces fiber thermochemical damage but also suppresses the adverse effects of the continuous brittle reaction layer on high-temperature strength and fatigue performance.

[0071] Example 4 differs from Comparative Example 2 only in the presence or absence of a porous MgAl2O4 layer. With only the SiOC layer retained, although the fiber strength retention and Mg2Si inhibition effect are similar to Example 4, the overall porosity increases from 0.62% to 2.35%, the room temperature tensile strength decreases from 762 MPa to 578 MPa, and the fatigue life decreases to 1.4 × 10⁻⁶. 6 The fracture surface shows a debonding zone extending along the straight SiOC interface, indicating that a single barrier layer cannot provide sufficient melt wetting and mechanical load transfer.

[0072] Example 4 differs from Comparative Example 3 only in the open porosity of the MgAl2O4 layer. Replacing the 28% porous layer with a 3% dense layer increased the overall porosity to 1.88%, while both tensile strength and fatigue life decreased. This result demonstrates that the open porosity required by this invention is not a common coating defect, but rather a functional structure that allows the magnesium alloy to form gradient mechanical anchoring zones.

[0073] Example 4 differs from Comparative Example 4 only in the pressurization path. A direct and rapid increase to 14 MPa increased the overall porosity from 0.62% to 1.72%, and closed pores and localized coating erosion were observed in the fiber bundle core, reducing fatigue life to 3.8 × 10⁻⁶. 6 Therefore, it can be seen that the low-pressure pre-impregnation stage is responsible for uniform spreading and venting, while the high-pressure stage is responsible for deep penetration into micropores; the two stages have different functions.

[0074] Example 4 differs from Comparative Example 5 only in the presence or absence of a connecting infiltration channel. After removing the channel, the overall porosity increased to 2.68%, the tensile strength decreased to 586 MPa, and the fatigue life decreased to 1.6 × 10⁻⁶ MPa. 6 Even with the same double-layer interface and graded pressure, the lack of macroscopic connectivity can still result in incomplete impregnation of the fiber bundle core. Therefore, prefabricated channels and graded pressure impregnation work in tandem.

[0075] Comparative Example 1 shows that a low macroscopic porosity can be obtained with only a porous MgAl2O4 layer, but interfacial reactions lead to fiber damage and decreased high-temperature and fatigue performance. Comparative Example 2 shows that only a SiOC layer can protect the fibers, but wetting and mechanical bonding are insufficient. Comparative Example 3 shows that after changing the porous layer to a dense layer, even if both material layers are present, a metal-ceramic interlocking anchor cannot be formed. Example 4 simultaneously satisfies SiOC blocking, porous MgAl2O4 infiltration, interconnected channels, and staged pressurization; its strength, porosity, fiber retention rate, and fatigue life cannot be achieved by any single characteristic.

[0076] Taking room temperature tensile strength as an example, Comparative Example 1 and Comparative Example 2 were 603 MPa and 578 MPa, respectively, while Example 4 reached 762 MPa; taking fatigue life as an example, Comparative Example 1 and Comparative Example 2 were 1.9 × 10⁻⁶ MPa, respectively. 6 The sum is 1.4 × 10⁻⁶. 6 In Example 4, the result was 1.0 × 10⁻⁶. 7 More than once. Combined with the lower Mg2Si area fraction and overall porosity of Example 4, it can be confirmed that the bilayer interface both inhibits chemical reactions and forms mechanical interlocking, and produces a synergistic effect with staged infiltration.

[0077] The above embodiments demonstrate that by sequentially constructing an amorphous SiOC diffusion barrier layer and a porous MgAl2O4 wetting anchoring layer on the surface of continuous silicon carbide fibers, and combining a directional preform with interconnected impregnation channels with a low-pressure pre-impregnation-high-pressure deep impregnation process, the present invention can simultaneously suppress the continuous reaction layer at the interface, improve the fiber strength retention rate, reduce the porosity of the composite material, and improve room temperature, high temperature, and fatigue performance.

[0078] Figure 2 In Example 4, the porous MgAl2O4 layer allows the magnesium alloy matrix to penetrate and form a mechanical interlock; Figure 3 In Comparative Example 3, the dense MgAl2O4 layer hindered the entry of the matrix, and the interface was mainly characterized by relatively flat direct contact.

[0079] Any conventional substitutions made by those skilled in the art based on the description herein, without requiring inventive effort, for material grades, specific equipment forms, precursor solvents, and preform fixing methods, that still utilize the combination of SiOC blocking, porous MgAl2O4 anchoring, and graded impregnation, should fall within the scope of the inventive concept of this invention.

Claims

1. A fiber-reinforced magnesium alloy composite material, characterized in that, The composite material includes a magnesium alloy matrix and a continuous silicon carbide fiber preform embedded in the magnesium alloy matrix, wherein the volume fraction of the continuous silicon carbide fiber preform in the composite material is 25% to 45%. The surface of the continuous silicon carbide fiber is provided with an amorphous SiOC diffusion barrier layer and a porous MgAl2O4 wetting and anchoring layer from the inside to the outside. The thickness of the amorphous SiOC diffusion barrier layer is 80nm to 250nm, and the thickness of the porous MgAl2O4 wetting anchoring layer is 0.3μm to 1.5μm, with an open porosity of 15% to 35% and a pore size of 0.1μm to 0.6μm. The magnesium alloy matrix penetrates inward along the opening pores of the porous MgAl2O4 wetting anchoring layer to a depth of 30% to 80% of the thickness of the porous MgAl2O4 wetting anchoring layer, so as to form a gradient mechanical anchoring zone between the magnesium alloy matrix and the amorphous SiOC diffusion barrier layer, which is composed of the interlocking of the magnesium alloy matrix and MgAl2O4 particles.

2. The fiber-reinforced magnesium alloy composite material according to claim 1, characterized in that, The magnesium alloy matrix comprises, by weight percentage: Aluminum 5.0%–9.0%, Zinc 0.2%–1.5%, Manganese 0.10%–0.60%, Calcium 0.05%–0.50%, Yttrium 0.10%–1.00%, with the balance being magnesium and unavoidable impurities; The iron content is no higher than 0.010%, the nickel content is no higher than 0.005%, and the copper content is no higher than 0.030%.

3. The fiber-reinforced magnesium alloy composite material according to claim 1, characterized in that, The diameter of the continuous silicon carbide fiber is 8μm to 16μm; The continuous silicon carbide fiber preform includes longitudinal fiber bundles arranged along the main load-bearing direction and cross-constraining fiber bundles arranged at an angle of ±30° to ±60° with the longitudinal fiber bundles, wherein the longitudinal fiber bundles account for 60% to 85% of the total fiber volume; Interconnected impregnation channels are provided between adjacent fiber bundles. The equivalent width of the impregnation channels is 80μm to 300μm, and the impregnation channels account for 4% to 12% of the total volume of the continuous silicon carbide fiber preform.

4. The fiber-reinforced magnesium alloy composite material according to claim 1, characterized in that, The ratio of oxygen atoms to carbon atoms in the amorphous SiOC diffusion barrier layer is 0.3 to 1.

2. The porous MgAl2O4 wetting anchoring layer is formed by connecting MgAl2O4 grains with a particle size of 30nm to 150nm. In the interface region within 2 μm of the continuous silicon carbide fiber surface, the Mg2Si reaction phase is distributed in a discontinuous particulate form, the area fraction of the Mg2Si reaction phase is not higher than 3%, and there is no continuous Mg2Si reaction layer with a thickness greater than 150 nm.

5. The fiber-reinforced magnesium alloy composite material according to claim 1, characterized in that, The composite material includes, along its thickness direction, a surface transition zone and an internal load-bearing zone. The thickness of the surface transition zone is 0.5 mm to 3.0 mm, and the volume fraction of continuous silicon carbide fibers in the surface transition zone is 15% to 28%. The volume fraction of continuous silicon carbide fibers in the internal bearing area is 32% to 50%, and the fiber volume fraction between the surface transition area and the internal bearing area changes continuously along the thickness direction.

6. A method for preparing the fiber-reinforced magnesium alloy composite material according to any one of claims 1 to 5, characterized in that, Includes the following steps: S1. The continuous silicon carbide fiber is subjected to degumming and surface activation treatment to prepare an amorphous SiOC diffusion barrier layer on the surface of the continuous silicon carbide fiber; S2. MgAl2O4 particles are deposited on the surface of the amorphous SiOC diffusion barrier layer and then solidified and sintered to form a porous MgAl2O4 wetting and anchoring layer with interconnected open pores, thus obtaining a double-layer interface modified silicon carbide fiber. S3. The double-layer interface modified silicon carbide fiber is made into a continuous fiber preform with interconnected impregnation channels, and the continuous fiber preform is placed in an impregnation mold; S4. Melt and refine the magnesium alloy matrix according to its composition to obtain a magnesium alloy melt, while preheating the continuous fiber preform. S5. Vacuum the impregnation mold to bring the magnesium alloy melt into contact with the continuous fiber preform, and perform low-pressure pre-impregnation and high-pressure deep impregnation in sequence, so that the magnesium alloy melt first fills the impregnation channel and then penetrates into the open pores of the porous MgAl2O4 wetting anchor layer. S6. Under the condition of maintaining the infiltration pressure, the magnesium alloy melt is directionally solidified, and after demolding, it is subjected to solution treatment and aging treatment to obtain the fiber-reinforced magnesium alloy composite material.

7. The preparation method according to claim 6, characterized in that, Step S1 includes: The degummed continuous silicon carbide fiber was immersed in a polysiloxane precursor solution with a solid content of 3% to 12% and pulled at a speed of 1 mm / s to 10 mm / s, and then crosslinked and cured at 150℃ to 250℃ for 30 min to 120 min. The cross-linked and cured continuous silicon carbide fiber is placed in an inert gas atmosphere and heated to 750℃~900℃ at a heating rate of 2℃ / min~10℃ / min and held for 1h~3h to transform the polysiloxane precursor into an amorphous SiOC diffusion barrier layer. The impregnation, cross-linking curing and pyrolysis processes are performed 1 to 3 times.

8. The preparation method according to claim 6, characterized in that, Step S2 includes: MgAl2O4 powder with an average particle size of 30nm to 100nm is dispersed in alumina sol, wherein the mass ratio of MgAl2O4 powder to the solid component in alumina sol is 70:30 to 90:10, to obtain MgAl2O4 coating slurry. Continuous silicon carbide fibers with an amorphous SiOC diffusion barrier layer are immersed in the MgAl2O4 coating slurry, dried, and then sintered at 700℃~850℃ for 30min~120min in a nitrogen or argon atmosphere. By controlling the solid content, pulling speed, and coating times of the MgAl2O4 coating slurry, the resulting porous MgAl2O4 wetting anchoring layer can have an open porosity of 15% to 35%.

9. The preparation method according to claim 6, characterized in that, In step S4, the preheating temperature of the continuous fiber preform is 520℃~620℃, and the infiltration temperature of the magnesium alloy melt is 680℃~730℃. In step S5, after reducing the absolute pressure in the impregnation mold to below 100 Pa, the magnesium alloy melt is brought into contact with the continuous fiber preform. The pressure of the low-pressure pre-impregnation is 0.3MPa to 1.0MPa, and the pressure holding time is 10s to 60s; The pressure of the high-pressure deep infiltration is 8MPa to 18MPa, the pressure increase rate is 0.5MPa / s to 3MPa / s, and the pressure holding time is 60s to 240s; Both the low-pressure pre-impregnation and high-pressure deep impregnation use argon gas as the pressurizing medium.

10. The preparation method according to claim 6, characterized in that, In step S6, solidification is maintained under a pressure of 8MPa to 18MPa until the temperature of the magnesium alloy matrix drops to 80°C to 150°C below its solidus temperature. After demolding, the resulting composite material is subjected to solution treatment at 390℃~420℃ for 4h~12h, followed by quenching with water at 60℃~90℃, and then artificial aging treatment at 170℃~210℃ for 6h~16h. After the solution and aging treatment, the overall porosity of the composite material is not higher than 1.5%, and the open porosity of the porous MgAl2O4 wetting anchor layer that is not filled by the magnesium alloy matrix is ​​3% to 12%.