A method for preparing high-strength rare-earth magnesium alloy plates
By using high-frequency pulsed direct current treatment, the problem of traditional heat treatment being unable to balance the strength and plasticity of magnesium alloys was solved, and the comprehensive performance improvement of high strength and high plasticity of magnesium alloy sheets was achieved.
Patent Information
- Application Number
- CN202611473487.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional heat treatment methods struggle to balance the strength and plasticity of wrought magnesium alloys, limiting their application in the processing.
The rolled magnesium alloy sheet is annealed using high-frequency pulsed DC current treatment. Specific parameters include a frequency of 10kHz-20kHz, a current density of 20A/mm2-35A/mm2, a duty cycle of 80%-97%, and a treatment time of 10min-30min. The current flows along the rolling direction of the sheet.
It significantly improves the strength and plasticity of magnesium alloy sheets, forms a uniform solid solution structure, eliminates dislocations and internal stress, inhibits grain growth, promotes element precipitation, and meets the requirements for use under complex working conditions.
Smart Images

Figure CN123108447A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of alloy preparation, specifically to a method for preparing high-strength rare-earth magnesium alloy plates. Background Technology Magnesium alloys, as the lightest structural engineering metal material currently available (with a density of only about 1.74 g / cm³), possess excellent properties such as high specific strength, electromagnetic shielding, and good damping. They have been widely used in fields such as automotive lightweighting, aerospace, and portable electronic devices. Especially against the backdrop of the current global transformation towards low-carbon and green manufacturing, magnesium alloys have shown great market potential in high-end equipment manufacturing fields such as new energy vehicles, low-altitude aircraft, and 3C consumer electronics.
[0002] However, the hexagonal close-packed (HCP) crystal structure of magnesium alloys limits the number of slip systems available at room temperature, resulting in poor intrinsic plasticity. In particular, it is prone to cracking and instability during processing, which has become the core bottleneck restricting the further expansion of its structural applications.
[0003] WE43 (Mg-4Y-3RE-Zr), a high-strength, heat-resistant rare-earth magnesium alloy sheet, has significant application value in aerospace and transportation fields due to its low density, high specific strength, and excellent creep resistance. Currently, WE43 is mostly available in casting form. Further optimizing its microstructure and phase distribution through large plastic deformation processes such as rolling is a key research direction for developing high-strength, high-plasticity deformable magnesium alloy sheets to replace traditional aluminum-titanium alloys. However, after rolling, traditional heat treatment cannot simultaneously maintain the strength and plasticity of the deformed magnesium alloy, which has certain limitations. Summary of the Invention
[0004] To address the aforementioned shortcomings of existing technologies, this invention provides a method for preparing high-strength rare-earth magnesium alloy plates, aiming to solve the technical problem that traditional heat treatment methods struggle to balance the strength and plasticity of deformed magnesium alloys.
[0005] This invention provides a method for preparing high-strength rare-earth magnesium alloy plates, comprising the following steps: (1) The magnesium alloy plate prepared according to the formula ratio is cut into rectangular samples. (2) Roll the magnesium alloy plate of the rectangular sample obtained in step (1) to obtain a magnesium alloy rolled plate. (3) The magnesium alloy rolled plate obtained in step (2) is subjected to high-frequency pulsed DC current treatment.
[0006] Furthermore, in step (1), the thickness of the magnesium alloy plate is 5 mm.
[0007] Furthermore, in step (2), the rolling is carried out in a single-pass rolling method, with a rolling temperature of 25°C, a rolling speed of 10m / min, and a rolling reduction of 25%.
[0008] Furthermore, in step (3), the frequency of the pulsed DC current is 10kHz-20kHz, the duty cycle is 80%-97%, and the current density is 20A / mm². 2 -35A / mm 2 The processing time is 10-30 minutes.
[0009] Furthermore, in step (3), the pulsed DC current flows through the magnesium alloy plate along the rolling direction of the plate.
[0010] Furthermore, in step (1), the rare earth magnesium alloy plate contains the following elements by mass percentage: Y 4.04%, Zr 0.46%, Gd 0.7%, Nd 2.17%, with the remainder being Mg and unavoidable impurities, totaling 100%.
[0011] The beneficial effects of this invention are as follows: (1) In this invention, high-frequency pulsed DC current annealing significantly improves the fracture elongation of the material while basically maintaining the high strength of the rolled state, overcoming the disadvantage of strength reduction after traditional annealing of magnesium alloys. It allows the alloying elements to be fully dissolved, resulting in a uniform solid solution structure; the non-thermal effect generated by the pulsed DC current can eliminate dislocations and release internal stress, while preventing rare earth elements from growing into coarse particles, maintaining the matrix in a micron-level strengthening state, and generating favorable element segregation / precipitation inside the alloy, so that the strength, hardness, plasticity and other mechanical properties of the rare earth magnesium alloy plate are comprehensively and significantly improved, meeting the requirements for use under complex working conditions.
[0012] (2) The key to this invention lies in the use of high-frequency, low-current-density pulsed direct current treatment, which can precisely control the annealing temperature of the rolled plate and precipitate a large number of precipitates at the grain boundaries, forming a pinning effect and inhibiting grain growth. The pulsed direct current promotes dislocation recovery and rearrangement, forming a stable, low-distortion dislocation substructure. This is the reason why the strength and plasticity of rare earth magnesium alloy plates are improved simultaneously. Attached Figure Description
[0013] Figure 1 These are the engineering stress-strain curves of WE43 magnesium alloy in the rolled state in step (2) and the current annealed state in step (3) of Examples 1, 2, and 3; Figure 2 a is the IPF diagram and pole figure of the WE43 magnesium alloy rolled plate obtained in step (2) of Example 1; Figure 2b is the KAM diagram of the WE43 magnesium alloy rolled plate obtained in step (2) of Example 1; Figure 2 c is a grain size statistical diagram of the WE43 magnesium alloy rolled plate obtained in step (2) of Example 1; Figure 2 d is the IPF diagram and pole diagram of the pulsed DC current treated WE43 magnesium alloy rolled plate obtained in step (3) of Example 1; Figure 2 e is the KAM diagram of the pulsed DC current processed WE43 magnesium alloy rolled plate obtained in step (3) of Example 1; Figure 2 f is a statistical chart of grain size of WE43 magnesium alloy rolled plate obtained by pulsed DC current treatment in step (3) of Example 1; Figure 3 a is the TEM image of the WE43 magnesium alloy rolled plate obtained in step (2) of Example 1. Figure 1 ; Figure 3 b is the TEM image of the WE43 magnesium alloy rolled plate obtained in step (2) of Example 1. Figure 2 ; Figure 3 c is the TEM image of the WE43 magnesium alloy rolled plate obtained by pulsed DC current treatment in step (3) of Example 1. Figure 1 ; Figure 3 d is the TEM image of the WE43 magnesium alloy rolled plate obtained by pulsed DC current treatment in step (3) of Example 1. Figure 2 ; Figure 4 The diagram shows the engineering stress-strain curves of the current-annealed WE43 magnesium alloys of Examples 3 and Comparative Examples 1-6. Detailed Implementation
[0014] The specific embodiments of the present invention are described below to enable those skilled in the art to understand the present invention. However, it should be understood that the present invention is not limited to the scope of the specific embodiments. For those skilled in the art, various changes are obvious as long as they are within the spirit and scope of the present invention as defined and determined by the appended claims. All inventions utilizing the concept of the present invention are protected.
[0015] Example 1 The preparation method of high-strength rare-earth magnesium alloy sheet includes the following steps: Step (1): Prepare WE43 magnesium alloy sheet: Cut WE43 magnesium alloy into 60mm×35mm×5mm sheets, polish the sheets with 400# and 600# sandpaper in turn, clean with anhydrous ethanol, and then air dry to obtain a clean WE43 magnesium alloy sheet.
[0016] The rare earth magnesium alloy contains the following elements by mass percentage: Y 4.04%, Zr 0.46%, Gd 0.7%, Nd 2.17%, with the remainder being Mg and unavoidable impurities, totaling 100%.
[0017] Step (2), rolling: The clean WE43 magnesium alloy plate obtained in step (1) is rolled at room temperature of 25°C. The rolling speed is 10m / min and the reduction is 25% for a single pass to obtain a WE43 magnesium alloy plate with a thickness of 3.75mm.
[0018] Step (3) High-frequency pulsed DC current treatment: The two end faces of the WE43 magnesium alloy rolled plate obtained in step (2) are clamped on the copper electrode fixture of the pulsed DC power supply along the rolling direction. The high-frequency pulsed DC current treatment is carried out with a frequency of 10kHz, a current density of 25A / mm2, and a duty cycle of 95%. The pulsed DC current flows through the magnesium alloy rolled plate along the rolling direction of the rolled plate. The treatment time is 30min. The plate is cooled under natural air cooling to obtain the WE43 magnesium alloy rolled plate treated with high-frequency pulsed DC current.
[0019] Figure 1 The figures show the engineering stress-strain curves of WE43 magnesium alloy in the initial state (1), the rolled state (2), and the current-annealed state (3) of this embodiment. Example 1 is named A1. Figure 1 As can be seen, the initial rolled strength of WE43 magnesium alloy is about 265 MPa and the plasticity is about 5%. After high-frequency pulsed DC current treatment, the strength of WE43 magnesium alloy increases significantly, and the plasticity is slightly improved, reaching 320 MPa and about 6%.
[0020] Figure 2 The WE43 magnesium alloy rolled plate obtained in step (2) of this embodiment ( Figure 2 a) The pulsed DC current processed WE43 magnesium alloy rolled plate obtained in step (3) Figure 2(b) IPF plot, pole figure, KAM plot, and grain size statistics. The grain size statistics show that the average grain size of the magnesium alloy after rolling is 6.73 μm, and the average grain size after high-frequency pulsed DC current treatment is 8.53 μm. The slight increase in grain size indicates that static recrystallization and moderate grain growth occurred during the current treatment process. Although the grains grew slightly, the microstructure after current treatment was more uniform and equiaxed, improving deformation compatibility and introducing a small amount of twinned structure. The KAM plot shows that the average KAM value of the magnesium alloy after rolling is 1.12, and the average KAM value after high-frequency pulsed DC current treatment is 0.84. The electroplastic effect generated by the pulsed DC current significantly promoted dislocation recovery and annihilation, effectively eliminating the brittleness caused by work hardening, resulting in a significant improvement in plasticity. As can be seen from the pole figures, the maximum texture strength (MAX) of the magnesium alloy after rolling is 4.29, and the maximum texture strength (MAX) after high-frequency pulsed DC current treatment is 5.03. This indicates that while the pulsed DC current treatment eliminates stress, it does not destroy the basal strengthening texture formed by rolling; on the contrary, it further stabilizes it. This stable strong texture ensures that the material maintains a high level of strength.
[0021] Figure 3 The WE43 magnesium alloy rolled plate obtained in step (2) of this embodiment ( Figure 3 a) The pulsed DC current processed WE43 magnesium alloy rolled plate obtained in step (3) Figure 3 b) TEM image. Pulsed DC current induces dislocation proliferation and rearrangement at the atomic scale through "non-thermal effects," forming a more dense and uniform dislocation substructure than the rolled state. This high-energy-density lattice activation state, combined with current-triggered nanophase grain boundary pinning, not only suppresses grain coarsening under Joule heating but also achieves micro-level strengthening and compensation while releasing macroscopic internal stress, maintaining extremely high yield strength and excellent plasticity matching.
[0022] Example 2 The preparation method of high-strength rare-earth magnesium alloy sheet includes the following steps: Step (1): Prepare WE43 magnesium alloy sheet: Cut WE43 magnesium alloy into 60mm×35mm×5mm sheets, polish the sheets with 400# and 600# sandpaper in turn, clean with anhydrous ethanol, and then air dry to obtain a clean WE43 magnesium alloy sheet.
[0023] The rare earth magnesium alloy contains the following elements by mass percentage: Y 4.04%, Zr 0.46%, Gd 0.7%, Nd 2.17%, with the remainder being Mg and unavoidable impurities, totaling 100%.
[0024] Step (2), rolling: The clean WE43 magnesium alloy plate obtained in step (1) is rolled at room temperature of 25°C. The rolling speed is 10m / min and the reduction is 25%. A single pass rolling is performed to obtain a flat WE43 magnesium alloy plate with a thickness of 3.75mm.
[0025] Step (3) High-frequency pulsed DC current treatment: The two end faces of the WE43 magnesium alloy rolled plate obtained in step (2) along the rolling direction are clamped on the copper electrode fixture of the pulsed DC power supply. High-frequency pulsed DC current treatment is performed with a frequency of 10kHz, a current density of 20A / mm2, and a duty cycle of 97%. The pulsed DC current flows through the magnesium alloy rolled plate along the rolling direction of the rolled plate. The treatment time is 20min. The plate is cooled under natural air cooling to obtain the WE43 magnesium alloy rolled plate treated with high-frequency pulsed DC current.
[0026] Figure 1 The images show the engineering stress-strain curves of WE43 magnesium alloy in the initial state (1), the rolled state (2), and the current-annealed state (3) of this embodiment. The sample in this embodiment is named A2. Figure 1 As can be seen, after high-frequency pulsed DC current treatment, the strength of WE43 magnesium alloy increased significantly and its plasticity improved.
[0027] Example 3 The preparation method of high-strength rare-earth magnesium alloy sheet includes the following steps: Step (1): Prepare WE43 magnesium alloy sheet: Cut WE43 magnesium alloy into 60mm×35mm×5mm sheets, polish the sheets with 400# and 600# sandpaper in turn, clean with anhydrous ethanol, and then air dry to obtain a clean WE43 magnesium alloy sheet.
[0028] The rare earth magnesium alloy contains the following elements by mass percentage: Y 4.04%, Zr 0.46%, Gd 0.7%, Nd 2.17%, with the remainder being Mg and unavoidable impurities, totaling 100%.
[0029] Step (2), rolling: The clean WE43 magnesium alloy plate obtained in step (1) is rolled at room temperature of 25°C. The rolling speed is 10m / min and the reduction is 25%. A single pass rolling is performed to obtain a flat WE43 magnesium alloy plate with a thickness of 3.75mm.
[0030] Step (3), High-frequency pulsed DC current treatment: The two end faces of the WE43 magnesium alloy rolled plate obtained in step (2) along the rolling direction are clamped on the copper electrode fixture of the pulsed DC power supply, with a frequency of 20kHz and a current density of 30A / mm. 2The high-frequency pulsed DC current was applied at a duty cycle of 80%, and the pulsed DC current flowed through the magnesium alloy plate along the rolling direction for 10 minutes. The plate was then cooled under natural air cooling to obtain the WE43 magnesium alloy plate treated with high-frequency pulsed DC current.
[0031] Figure 1 The images show the engineering stress-strain curves of WE43 magnesium alloy in the initial state (1), the rolled state (2), and the current-annealed state (3) of this embodiment. The sample in this embodiment is named A3. Figure 1 As can be seen, the strength and plasticity of WE43 magnesium alloy are increased after high-frequency pulsed DC current treatment.
[0032] Comparative Example 1 The preparation method of rare earth magnesium alloy plates includes the following steps: Step (1): Prepare WE43 magnesium alloy sheet: Cut WE43 magnesium alloy into 60mm×35mm×5mm sheets, polish the sheets with 400# and 600# sandpaper in turn, clean with anhydrous ethanol, and then air dry to obtain a clean WE43 magnesium alloy sheet.
[0033] The rare earth magnesium alloy contains the following elements by mass percentage: Y 4.04%, Zr 0.46%, Gd 0.7%, Nd 2.17%, with the remainder being Mg and unavoidable impurities, totaling 100%.
[0034] Step (2), rolling: The clean WE43 magnesium alloy plate obtained in step (1) is rolled at room temperature of 25°C. The rolling speed is 10m / min and the reduction is 25%. A single pass rolling is performed to obtain a flat WE43 magnesium alloy plate with a thickness of 3.75mm.
[0035] Step (3) High-frequency pulsed DC current treatment: The two end faces of the WE43 magnesium alloy rolled plate obtained in step (2) along the rolling direction are clamped on the copper electrode fixture of the pulsed DC power supply. The high-frequency pulsed DC current treatment is performed with a frequency of 20kHz, a current density of 15A / mm2, and a duty cycle of 80%. The pulsed DC current flows through the magnesium alloy rolled plate along the rolling direction of the rolled plate. The treatment time is 10min. The plate is then cooled under natural air cooling to obtain the WE43 magnesium alloy rolled plate.
[0036] Figure 4 This is the engineering stress-strain curve of the current-annealed WE43 magnesium alloy in this comparative example, which is named B1. From... Figure 4 As can be seen, the strength and plasticity of Example 3 (A3) are higher than those of the comparative example (B1).
[0037] Comparative Example 2 The preparation method of rare earth magnesium alloy plates includes the following steps: Step (1): Prepare WE43 magnesium alloy sheet: Cut WE43 magnesium alloy into 60mm×35mm×5mm sheets, polish the sheets with 400# and 600# sandpaper in turn, clean with anhydrous ethanol, and then air dry to obtain a clean WE43 magnesium alloy sheet.
[0038] The rare earth magnesium alloy contains the following elements by mass percentage: Y 4.04%, Zr 0.46%, Gd 0.7%, Nd 2.17%, with the remainder being Mg and unavoidable impurities, totaling 100%.
[0039] Step (2), rolling: The clean WE43 magnesium alloy plate obtained in step (1) is rolled at room temperature of 25°C. The rolling speed is 10m / min and the reduction is 25%. A single pass rolling is performed to obtain a flat WE43 magnesium alloy plate with a thickness of 3.75mm.
[0040] Step (3) High-frequency pulsed DC current treatment: The two end faces of the WE43 magnesium alloy rolled plate obtained in step (2) along the rolling direction are clamped on the copper electrode fixture of the pulsed DC power supply. The high-frequency pulsed DC current treatment is performed with a frequency of 20kHz, a current density of 45A / mm2, and a duty cycle of 80%. The pulsed DC current flows through the magnesium alloy rolled plate along the rolling direction of the rolled plate. The treatment time is 10min. The plate is then cooled under natural air cooling to obtain the WE43 magnesium alloy rolled plate.
[0041] Figure 4 This is the engineering stress-strain curve of the current-annealed WE43 magnesium alloy in this comparative example, which is named B2. From... Figure 4 As can be seen, the strength and plasticity of Example 3 (A3) are higher than those of the comparative example (B2).
[0042] Comparative Example 3 The preparation method of rare earth magnesium alloy plates includes the following steps: Step (1): Prepare WE43 magnesium alloy sheet: Cut WE43 magnesium alloy into 60mm×35mm×5mm sheets, polish the sheets with 400# and 600# sandpaper in turn, clean with anhydrous ethanol, and then air dry to obtain a clean WE43 magnesium alloy sheet.
[0043] The rare earth magnesium alloy contains the following elements by mass percentage: Y 4.04%, Zr 0.46%, Gd 0.7%, Nd 2.17%, with the remainder being Mg and unavoidable impurities, totaling 100%.
[0044] Step (2), rolling: The clean WE43 magnesium alloy plate obtained in step (1) is rolled at room temperature of 25°C. The rolling speed is 10m / min and the reduction is 25%. A single pass rolling is performed to obtain a flat WE43 magnesium alloy plate with a thickness of 3.75mm.
[0045] Step (3) High-frequency pulsed DC current treatment: The two end faces of the WE43 magnesium alloy rolled plate obtained in step (2) are clamped on the copper electrode fixture of the pulsed DC power supply along the rolling direction. The high-frequency pulsed DC current treatment is performed with a frequency of 20kHz, a current density of 30A / mm2, and a duty cycle of 70%. The pulsed DC current flows through the magnesium alloy rolled plate along the rolling direction of the rolled plate. The treatment time is 10min. The plate is then cooled under natural air cooling to obtain the WE43 magnesium alloy rolled plate.
[0046] Figure 4 This is the engineering stress-strain curve of the current-annealed WE43 magnesium alloy in this comparative example, which is named B3. From... Figure 4 As can be seen, the strength of Example 3 (A3) is higher than that of the comparative example (B3), and the plasticity of Example 3 (A3) is slightly lower than that of the comparative example (B3). However, the overall performance of Example 3 (A3) is significantly better than that of the comparative example (B3).
[0047] Comparative Example 4 The preparation method of rare earth magnesium alloy plates includes the following steps: Step (1): Prepare WE43 magnesium alloy sheet: Cut WE43 magnesium alloy into 60mm×35mm×5mm sheets, polish the sheets with 400# and 600# sandpaper in turn, clean with anhydrous ethanol, and then air dry to obtain a clean WE43 magnesium alloy sheet.
[0048] The rare earth magnesium alloy contains the following elements by mass percentage: Y 4.04%, Zr 0.46%, Gd 0.7%, Nd 2.17%, with the remainder being Mg and unavoidable impurities, totaling 100%.
[0049] Step (2), rolling: The clean WE43 magnesium alloy plate obtained in step (1) is rolled at room temperature of 25°C. The rolling speed is 10m / min and the reduction is 25%. A single pass rolling is performed to obtain a flat WE43 magnesium alloy plate with a thickness of 3.75mm.
[0050] Step (3) High-frequency pulsed DC current treatment: The two end faces of the WE43 magnesium alloy rolled plate obtained in step (2) are clamped on the copper electrode fixture of the pulsed DC power supply along the rolling direction. The high-frequency pulsed DC current treatment is performed with a frequency of 20kHz, a current density of 30A / mm2, and a duty cycle of 98%. The pulsed DC current flows through the magnesium alloy rolled plate along the rolling direction of the rolled plate. The treatment time is 10min. The plate is then cooled under natural air cooling to obtain the WE43 magnesium alloy rolled plate.
[0051] Figure 4 This is the engineering stress-strain curve of the current-annealed WE43 magnesium alloy in this comparative example, which is named B4. From... Figure 4 As can be seen, the strength and plasticity of Example 3 (A3) are higher than those of the comparative example (B4).
[0052] Comparative Example 5 The preparation method of rare earth magnesium alloy plates includes the following steps: Step (1): Prepare WE43 magnesium alloy sheet: Cut WE43 magnesium alloy into 60mm×35mm×5mm sheets, polish the sheets with 400# and 600# sandpaper in turn, clean with anhydrous ethanol, and then air dry to obtain a clean WE43 magnesium alloy sheet.
[0053] The rare earth magnesium alloy contains the following elements by mass percentage: Y 4.04%, Zr 0.46%, Gd 0.7%, Nd 2.17%, with the remainder being Mg and unavoidable impurities, totaling 100%.
[0054] Step (2), rolling: The clean WE43 magnesium alloy plate obtained in step (1) is rolled at room temperature of 25°C. The rolling speed is 10m / min and the reduction is 25%. A single pass rolling is performed to obtain a flat WE43 magnesium alloy plate with a thickness of 3.75mm.
[0055] Step (3) High-frequency pulsed DC current treatment: The two end faces of the WE43 magnesium alloy rolled plate obtained in step (2) along the rolling direction are clamped on the copper electrode fixture of the pulsed DC power supply. High-frequency pulsed DC current treatment is performed with a frequency of 5kHz, a current density of 30A / mm2, and a duty cycle of 80%. The pulsed DC current flows through the magnesium alloy rolled plate along the rolling direction. The treatment time is 10min. After cooling under natural air cooling, the WE43 magnesium alloy rolled plate is obtained. Figure 4 This is the engineering stress-strain curve of the current-annealed WE43 magnesium alloy in this comparative example, which is named B5. From... Figure 4As can be seen, the strength of Example 3 (A3) is higher than that of the comparative example (B5), and the plasticity of Example 3 (A3) is slightly lower than that of the comparative example (B5). However, the overall performance of Example 3 (A3) is significantly better than that of the comparative example (B5).
[0056] Comparative Example 6 The preparation method of rare earth magnesium alloy plates includes the following steps: Step (1): Prepare WE43 magnesium alloy sheet: Cut WE43 magnesium alloy into 60mm×35mm×5mm sheets, polish the sheets with 400# and 600# sandpaper in turn, clean with anhydrous ethanol, and then air dry to obtain a clean WE43 magnesium alloy sheet.
[0057] The rare earth magnesium alloy contains the following elements by mass percentage: Y 4.04%, Zr 0.46%, Gd 0.7%, Nd 2.17%, with the remainder being Mg and unavoidable impurities, totaling 100%.
[0058] Step (2), rolling: The clean WE43 magnesium alloy plate obtained in step (1) is rolled at room temperature of 25°C. The rolling speed is 10m / min and the reduction is 25%. A single pass rolling is performed to obtain a flat WE43 magnesium alloy plate with a thickness of 3.75mm.
[0059] Step (3) High-frequency pulsed DC current treatment: The two end faces of the WE43 magnesium alloy rolled plate obtained in step (2) along the rolling direction are clamped on the copper electrode fixture of the pulsed DC power supply. The high-frequency pulsed DC current treatment is performed with a frequency of 30kHz, a current density of 30A / mm2, and a duty cycle of 80%. The direction of the applied current is the rolling direction. The treatment time is 10min. The plate is cooled under natural air cooling to obtain the WE43 magnesium alloy rolled plate.
[0060] Figure 4 This is the engineering stress-strain curve of the current-annealed WE43 magnesium alloy in this comparative example, which is named B6. From... Figure 4 As can be seen, the strength and plasticity of Example 3 (A3) are higher than those of the comparative example (B6).
[0061] Table 1. Mechanical properties of samples A1-A3 and B1-B6
Claims
1. A method for preparing a high-strength rare-earth magnesium alloy sheet, characterized in that, Includes the following steps: (1) The magnesium alloy plate prepared according to the formula ratio is cut into rectangular samples. (2) Roll the magnesium alloy plate of the rectangular sample obtained in step (1) to obtain a magnesium alloy rolled plate. (3) The magnesium alloy rolled plate obtained in step (2) is subjected to high-frequency pulsed DC current treatment.
2. The preparation method according to claim 1, characterized in that, In step (1), the thickness of the magnesium alloy plate is 5 mm.
3. The preparation method according to claim 1, characterized in that, In step (2), the rolling is carried out in a single-pass rolling method, with a rolling temperature of 25°C, a rolling speed of 10m / min, and a rolling reduction of 25%.
4. The preparation method according to claim 1, characterized in that, In step (3), the frequency of the pulsed DC current is 10kHz-20kHz, the duty cycle is 80%-97%, and the current density is 20A / mm². 2 -35A / mm 2 The processing time is 10-30 minutes.
5. The preparation method according to claim 1, characterized in that, In step (3), the pulsed DC current flows through the magnesium alloy plate along the rolling direction of the plate.
6. The preparation method according to claim 1, characterized in that, In step (1), the rare earth magnesium alloy plate contains the following elements by mass percentage: Y 4.04%, Zr 0.46%, Gd 0.7%, Nd 2.17%, with the remainder being Mg and unavoidable impurities, totaling 100%.