A reflective film for ultraviolet light and a coating method thereof.

By depositing a multilayer structure of AL2O3, aluminum film, MgF2 and AL2O3 layers on the substrate, and combining room temperature and high temperature coating processes, the problem of insufficient aluminum film reflectivity was solved, and high reflectivity and durability were improved.

CN123108481APending Publication Date: 2026-11-17MLOPTIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611233836.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, aluminum films have insufficient reflectivity in the ultraviolet band, which cannot meet the requirements of high reflectivity optical systems, and the reflectivity caused by conventional aluminum plating processes is only about 88%.

Method used

A multilayer structure is adopted, in which a dielectric film AL2O3, an aluminum film, a MgF2 layer and an AL2O3 layer are sequentially deposited on a substrate. The thickness and evaporation rate of each layer are controlled by room temperature and high temperature deposition processes. Combined with ion source cleaning and ultrasonic cleaning, the adhesion and density of the film layers are improved.

Benefits of technology

It significantly improves the reflectivity in the ultraviolet band, enhances the abrasion resistance and durability of the film, and achieves a reflectivity level higher than that of conventional processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108481A_ABST
    Figure CN123108481A_ABST
Patent Text Reader

Abstract

This invention discloses a reflective film for ultraviolet (UV) radiation and a coating method thereof. The reflective film comprises a dielectric film Al₂O₃, an aluminum film, a MgF₂ layer, and an Al₂O₃ layer sequentially deposited on a substrate. The MgF₂ layer is coated in two stages: a first stage at room temperature and a second stage at high temperature (150-200°C). This invention uses the Al₂O₃ dielectric film as the underlayer, which effectively improves the adhesion between the aluminum film and the substrate. Using the MgF₂ and Al₂O₃ layers as protective layers improves the reflectivity in the UV band, while magnesium fluoride prevents oxidation of the aluminum film caused by the temperature rise during the coating process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of coating technology, and in particular to a reflective film for ultraviolet light and a coating method thereof. Background Technology

[0002] Aluminum films are materials with high reflectivity from the ultraviolet to the infrared region. Therefore, the method of adding a protective layer to aluminum films is commonly used to prepare high-reflectivity films in the ultraviolet band. Other metals, such as silver and gold films, have high absorption in the ultraviolet, resulting in relatively low reflectivity. However, high-reflectivity films prepared by conventional aluminum plating processes (using an aluminum film with magnesium fluoride protection and cold plating at a specific temperature) only have an average ultraviolet reflectivity of about 88%, which cannot meet the requirements of optical systems that require high reflectivity. Summary of the Invention

[0003] Purpose of the invention: The first objective of this invention is to provide a reflective film for ultraviolet light to improve the reflectivity of aluminum films in the ultraviolet band.

[0004] A second objective of this invention is to provide a coating method for a reflective film used in ultraviolet radiation.

[0005] Technical solution: To achieve the above objective, the present invention provides a reflective film for ultraviolet radiation, wherein the reflective film comprises a dielectric film Al2O3, an aluminum film, a MgF2 layer and an Al2O3 layer sequentially deposited on a substrate, wherein the MgF2 layer is deposited in two stages, the first stage being a room temperature deposition and the second stage being a high temperature deposition, wherein the high temperature is 150-200℃.

[0006] Preferably, the substrate is glass, crystal, single-crystal silicon, or aluminum substrate.

[0007] Preferably, the thickness of the dielectric film AL2O3 is 15-30 nm, and the evaporation rate is 2 A / S.

[0008] Preferably, the aluminum film has a thickness of 80-100 nm and an evaporation rate of 30-50 A / s.

[0009] Preferably, the MgF2 layer has a thickness of 15-30 nm, the first-stage coating thickness is 5-10 nm, and the evaporation rate is 4-6 A / S.

[0010] Preferably, the AL2O3 film thickness is 15-30 nm, and the evaporation rate is 2 A / S.

[0011] The present invention provides a coating method for a reflective film as described above, comprising:

[0012] (1) The substrate and the substrate are ultrasonically cleaned and then placed into the vacuum coating machine.

[0013] (2) Set the temperature inside the vacuum coating machine to room temperature and the vacuum degree to 2.0E-4, and use an ion source to further clean the substrate;

[0014] (3) At room temperature, in a vacuum of 2.0E-4 and in an oxygen environment, the first stage of coating is carried out on the substrate in sequence: dielectric film AL2O3, aluminum film and MgF2 layer.

[0015] (4) Stop the oxygen supply, set the temperature to 150-200℃, and then keep it at a constant temperature for 40-60 minutes before proceeding with the second stage of MgF2 layer and AL2O3 layer coating.

[0016] Preferably, the further cleaning of the substrate using an ion source includes: using a hollow cathode ion source, voltage 200V, current 5A, and bombarding the substrate with oxygen for 3-5 minutes.

[0017] Preferably, the ultrasonic cleaning includes: using 1 / 2 tank of alkaline cleaning agent, 3-9 tanks of pure water cleaning, and slow drying.

[0018] Beneficial effects: The present invention has the following advantages: Aluminum oxide as the base layer can effectively improve the film-layer adhesion between the aluminum film and the substrate; using magnesium fluoride and aluminum oxide as protective layers can improve the reflectivity in the ultraviolet band, while magnesium fluoride can prevent the aluminum film from being oxidized due to the temperature rise during the coating process. Attached Figure Description

[0019] Figure 1 This is a schematic diagram of the film system structure of the reflective film in Example 1;

[0020] Figure 2 The graph shows a comparison of the reflectivity of the reflective film prepared in Example 2 and the reflective film prepared by a conventional coating process. Detailed Implementation

[0021] The technical solution of the present invention will be described in detail below with reference to the embodiments and accompanying drawings.

[0022] Example 1

[0023] This embodiment provides a reflective film for ultraviolet light, the film structure of which is as follows: Figure 1 As shown, specifically, an underlayer, an aluminum film, a first dielectric protective layer, and a second dielectric protective layer are sequentially deposited on the substrate, which can achieve the high reflectivity requirement of deep ultraviolet light.

[0024] The substrate includes glass, crystal, monocrystalline silicon, or aluminum substrate.

[0025] Underlying layer: dielectric film AL2O3, thickness 15-30nm, evaporation rate 2A / S;

[0026] Aluminum film: thickness 80-100nm, evaporation rate 30-50A / s;

[0027] First dielectric protective layer: magnesium fluoride MgF2, film thickness 15-30nm, evaporation rate 4-6A / S;

[0028] Second protective dielectric layer: aluminum oxide (AL2O3), film thickness 15-30nm, evaporation rate 2A / S.

[0029] In this film structure, the dielectric film AL2O3 is used as the substrate as the bottom layer, which can prevent the risk of film delamination caused by weak bonding between the aluminum film and the substrate. The dielectric film AL2O3 can form strong Si-O-AL chemical bonds with the glass substrate.

[0030] In an ultra-high vacuum environment, an aluminum film is rapidly evaporated and then coated with magnesium fluoride as the first dielectric protective layer in the ultraviolet band to prevent the aluminum film from being oxidized by air. The temperature is then slowly increased to 150-200℃ to provide kinetic energy for the aluminum film molecules to rearrange on the substrate, thereby improving the density and reflectivity of the metal film layer. Finally, a second dielectric protective layer is deposited. Because aluminum oxide has higher hardness and density than magnesium fluoride, it can improve the overall abrasion resistance and environmental resistance of the reflective film.

[0031] Example 2

[0032] Based on the film structure of the reflective film described in Example 1, this embodiment provides a coating method, specifically including the following:

[0033] 1. Coating process: Vacuum coating is used, which includes room temperature coating technology and high temperature coating technology, and is carried out in two different stages.

[0034] 2. Coating steps:

[0035] 2.1 Taking H-K9L glass substrate as an example, after ultrasonic cleaning, the H-K9L glass substrate and H-K9L glass coating sheet are put into the vacuum coating machine OTFC-1300.

[0036] The ultrasonic cleaning process includes: 1 / 2 tank of alkaline cleaning agent, 3-9 tanks of pure water cleaning, and slow drying.

[0037] 2.2. Set the parameters of the OTFC-1300 vacuum coating machine: temperature is room temperature (20-30℃), vacuum degree is 2.0E-4.

[0038] Before plating, the substrate is cleaned using an ion source. Cleaning parameters: hollow cathode ion source, voltage 200V, current 5A, oxygen bombardment for 3-5 minutes. Cleaning removes particulate matter adsorbed on the substrate surface and simultaneously activates the substrate surface to improve the adhesion between the substrate and the film layer.

[0039] 2.3. Depositing the base layer: Under the conditions of room temperature and vacuum degree of 2.0E-4, the thickness of the dielectric film AL2O3 is 15-30nm, and the evaporation rate is 2A / S;

[0040] 2.4. Aluminum film is deposited on the substrate: Under the conditions of room temperature and vacuum degree of 2.0E-4, the thickness of the aluminum film is 80-100nm and the evaporation rate is 30-50A / s.

[0041] 2.5. Deposit the first dielectric protective layer on the aluminum film: Under the conditions of room temperature and vacuum degree of 2.0E-4, deposit magnesium fluoride MgF2 with a film thickness of 5-10nm and an evaporation rate of 4-6A / S.

[0042] Stop the oxygen supply, keep the vacuum level constant, set the temperature to 150-200℃, and hold the temperature for 40-60 minutes. Then continue to deposit magnesium fluoride (MgF2) until the thickness of the first dielectric protective layer reaches 15-30 nm. In this step, the temperature increase can increase the kinetic energy of the aluminum film and MgF2, making them more densely arranged, thereby improving the overall reflectivity.

[0043] 2.6. Deposit a second dielectric protective layer on the first dielectric protective layer: Under the conditions of temperature of 150-200℃ and porosity of 2.0E-4, deposit aluminum oxide (AL2O3) with a film thickness of 15-30nm and an evaporation rate of 2A / S.

[0044] like Figure 2 The figure shows a comparison of reflectivity in the 190-990nm wavelength range between the reflective film prepared in Example 2 and the reflective film prepared by a conventional coating process (using an AL coating with magnesium fluoride protection, cold coating temperature, resulting in significantly lower overall reflectivity and poor abrasion resistance). As can be seen from the figure, the reflective film prepared in Example 2 has a significantly improved reflectivity, especially in the 190-400nm range.

Claims

1. A reflective film for ultraviolet light, characterized by, The reflective film includes a dielectric film AL2O3, an aluminum film, a MgF2 layer and an AL2O3 layer sequentially deposited on a substrate. The MgF2 layer is obtained by two-stage deposition: the first stage is room temperature deposition and the second stage is high temperature deposition, wherein the high temperature is 150-200℃.

2. The reflective film of claim 1, wherein The substrate is glass, crystal, monocrystalline silicon, or aluminum substrate.

3. The reflective film of claim 1, wherein The dielectric film AL2O3 has a thickness of 15-30 nm and an evaporation rate of 2 A / S.

4. The reflective film of claim 1, wherein The aluminum film has a thickness of 80-100 nm and an evaporation rate of 30-50 A / s.

5. The reflective film according to claim 1, characterized in that, The MgF2 layer has a thickness of 15-30 nm, the first stage coating thickness is 5-10 nm, and the evaporation rate is 4-6 A / S.

6. The reflective film according to claim 1, characterized in that, The AL2O3 film is 15-30 nm thick and has an evaporation rate of 2 A / S.

7. A method for coating a reflective film as described in claim 1, characterized in that, include: (1) The substrate and the substrate are ultrasonically cleaned and then placed into the vacuum coating machine. (2) Set the temperature inside the vacuum coating machine to room temperature and the vacuum degree to 2.0E-4, and use an ion source to further clean the substrate; (3) At room temperature, in a vacuum of 2.0E-4 and in an oxygen environment, the first stage of coating is carried out on the substrate in sequence: dielectric film AL2O3, aluminum film and MgF2 layer. (4) Stop the oxygen supply, set the temperature to 150-200℃, and then keep it at a constant temperature for 40-60 minutes before proceeding with the second stage of MgF2 layer and AL2O3 layer coating.

8. The coating method according to claim 7, characterized in that, The method of further cleaning the substrate using an ion source includes: using a hollow cathode ion source, voltage 200V, current 5A, and filling it with oxygen to bombard the substrate for 3-5 minutes.

9. The coating method according to claim 7, characterized in that, The ultrasonic cleaning process includes: using 1 / 2 tank of alkaline cleaning agent, 3-9 tanks of pure water cleaning, and slow drying.