A wear-resistant thin film on a metal surface and its preparation method
By forming a composite wear-resistant layer through pulsed cavitation-micro-etching, Ar ion activation, and co-sputtering, and modifying the surface with octadecylphosphonic acid, the problems of low surface hardness and easy corrosion of aluminum alloys are solved, achieving high bonding strength and wear resistance, and enhancing the wear resistance and sweat resistance of aluminum alloy surfaces.
Patent Information
- Application Number
- CN202611622454.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-20
- Publication Date
- 2026-11-17
AI Technical Summary
Aluminum alloys have low surface hardness, are easily worn, and are prone to corrosion when in contact with human skin. Existing multi-layer hard films have the risk of interfacial stress concentration and cracking, and the problem of sweat corrosion has not been effectively solved.
The aluminum alloy substrate was pretreated by pulsed cavitation-micro-etching combined with nitric acid treatment, followed by Ar ion activation treatment under alternating bias voltage, and a ZrB2, NbC, graphite and CrN composite wear-resistant layer was formed by co-sputtering. Finally, the surface was modified with octadecylphosphonic acid to improve the bonding strength and hydrophobicity.
It improves the bonding performance between the film layer and the substrate, enhances the wear resistance and sweat resistance of the aluminum alloy surface, reduces the risk of corrosion, and extends the service life.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to the field of thin film technology, and specifically to a wear-resistant thin film for metal surfaces and its preparation method. Background Technology
[0002] Aluminum alloys are lightweight, high-strength, easy to process, and have a good appearance, making them commonly used in watch cases, electronic product housings, and other metal structural components. However, aluminum alloys have relatively low surface hardness. For high-frequency contact components such as watch cases, their surfaces are continuously subjected to friction during wear and tear. Surface wear not only affects the product's appearance but can also damage the protective layer and gradually expose the aluminum alloy substrate. Therefore, improving the wear resistance of aluminum alloy surfaces is crucial for extending their service life and maintaining their appearance quality.
[0003] Currently, methods for improving the wear resistance of aluminum alloy surfaces mainly include anodizing, chemical conversion, thermal spraying, and physical vapor deposition. Patent application CN119685746A discloses a coating method for aluminum alloy surfaces, including: ultrasonic cleaning of the aluminum alloy substrate; ion sputtering cleaning of the ultrasonically cleaned aluminum alloy substrate; depositing a nickel layer on the surface of the ion-cleaned aluminum alloy substrate; depositing a nickel nitride layer on the surface of the nickel layer; and depositing a chromium nitride layer on the surface of the nickel nitride layer, thereby improving the hardness, wear resistance, and corrosion resistance of the aluminum alloy surface to a certain extent. However, this multi-layer hard film mainly relies on the nitride layer to improve surface hardness, and there are relatively obvious material interfaces between the layers. Furthermore, the aluminum alloy substrate is relatively soft, while the hardness and elastic modulus of the hard wear-resistant film layer are usually significantly higher than those of the aluminum alloy, resulting in a large difference in mechanical properties. Under long-term friction and localized loads, interfacial stress concentration is easily generated, and there is a risk of cracking or peeling.
[0004] In addition, the watch case is in long-term contact with human skin and sweat during wear. The moisture, chloride ions and acidic components in sweat can easily wet and remain on the surface of the watch case, and may penetrate into the aluminum alloy substrate along the defects in the protective layer, causing surface discoloration and corrosion.
[0005] Therefore, there is a need to provide a wear-resistant thin film on a metal surface and a method for preparing the same, in order to solve the above-mentioned technical problems. Summary of the Invention
[0006] In view of this, the present invention provides a wear-resistant thin film on a metal surface and a method for preparing the same, which can improve wear resistance while also having a certain degree of sweat resistance.
[0007] To achieve the above objectives, the present invention provides a method for preparing a wear-resistant thin film on a metal surface, comprising the following steps: S1. The aluminum alloy substrate is ultrasonically cleaned with acetone and anhydrous ethanol in sequence, then placed in sodium hydroxide aqueous solution for pulse cavitation-micro etching treatment, washed with water and then placed in nitric acid aqueous solution. After washing with water, washing with anhydrous ethanol, blowing with nitrogen and vacuum drying, the pretreated aluminum alloy substrate is obtained. S2. The pretreated aluminum alloy substrate is placed in a magnetron sputtering chamber, vacuumed, and argon gas is introduced. Ar ion activation treatment is carried out under alternating high and low bias conditions. Then, the substrate temperature and bias are adjusted. First, co-sputtering is performed with ZrB2 target 60~70W, NbC target 40~50W, graphite target 20~30W and CrN target 15~20W. Then, the target power is gradually increased to ZrB2 target 90~110W, NbC target 70~90W, graphite target 50~70W and CrN target 25~40W for continued co-sputtering. After cooling, a composite wear-resistant layer is obtained. S3. After the composite wear-resistant layer is treated with a mixed plasma of argon and oxygen, it is immersed in an octadecylphosphonic acid-ethanol solution, left to stand, and then washed and dried to obtain a wear-resistant film on the metal surface.
[0008] This invention employs pulsed cavitation-micro-etching to pretreat the aluminum alloy substrate, which facilitates the removal of the surface oxide layer and promotes the formation of microscopic pits and undulating structures on the aluminum alloy surface. Subsequent nitric acid treatment removes impurities remaining on the surface after alkaline etching. Combined with alternating bias Ar ion activation and low-power initial co-sputtering, the substrate surface is further cleaned and activated, promoting uniform nucleation and deposition of the deposition components on the substrate surface. This increases the actual contact area between the film and the substrate, generating a mechanical anchoring effect, which improves the bonding performance between the composite wear-resistant layer and the aluminum alloy substrate, and reduces cracking and peeling of the film during friction and scratching.
[0009] This invention employs co-sputtering with ZrB2, NbC, graphite, and CrN targets, which facilitates the formation of a composite system containing Zr-B, Nb-C, and Cr-N related hard components and amorphous carbon-related structures within the film. The introduction of Zr-B, Nb-C, and Cr-N related hard components improves the film's hardness and load-bearing capacity, helps disperse frictional loads, and reduces plastic deformation and localized wear during friction. The Cr-N related components improve the stress distribution of the film under localized loads and enhance its wear resistance. Simultaneously, the carbon component provided by the graphite target facilitates the formation of a carbon phase with low shear resistance within the film, thereby reducing adhesion and shearing at the friction interface. The synergistic load-bearing capacity of the various hard components combined with the friction-reducing effect of the carbon phase results in a composite wear-resistant film that possesses excellent hardness, load-bearing capacity, and friction-reducing properties.
[0010] This invention further employs argon and oxygen mixed plasma treatment of the composite wear-resistant layer, which facilitates cleaning the film surface and introducing oxygen-containing active sites, thus providing favorable conditions for the adsorption and binding of octadecylphosphonic acid on the film surface. Subsequently, octadecylphosphonic acid is used for surface modification; its phosphonic acid groups facilitate adsorption or binding with the activated film surface, while the long-chain alkyl groups tend to align towards the outer side of the film, thereby reducing the surface free energy and weakening the wetting, spreading, and retention of moisture and sweat on the film surface. Simultaneously, the composite wear-resistant layer exhibits good density and wear resistance, which helps to prevent the penetration of moisture and corrosive ions into the aluminum alloy substrate and reduces film defects caused by friction and scratches. The combination of the hydrophobic and anti-wetting effects of octadecylphosphonic acid and the wear-resistant and barrier effects of the composite wear-resistant layer effectively improves the sweat resistance and corrosion resistance of the aluminum alloy surface.
[0011] Optionally, the aluminum alloy substrate is a pre-polished 6061-T6 aluminum alloy; the concentration of the sodium hydroxide aqueous solution is 2~4wt%; and the concentration of the nitric acid aqueous solution is 20~30wt%.
[0012] Optionally, in step S1, after ultrasonic cleaning, the substrate is immersed and fixed in an ultrasonic bath containing sodium hydroxide aqueous solution, with the temperature controlled at 25~28℃. The surface to be treated faces the ultrasonic radiation surface, and the vertical distance between the surface to be treated and the ultrasonic radiation surface is 30~50mm. Pulsed cavitation-micro-etching is performed under ultrasonic conditions of 28~40kHz and 25~40W / L. After each ultrasonic treatment, the substrate is paused for 10~20s after each 10~20s of ultrasonic treatment, and this cycle is repeated 5~7 times. The substrate is then immediately cleaned with deionized water, then immersed in nitric acid aqueous solution, and treated at 23~27℃ for 30~60s. After removal, the substrate is washed sequentially with deionized water and anhydrous ethanol, dried with nitrogen, and then vacuum dried at 70~80℃ to obtain the pretreated aluminum alloy substrate.
[0013] Pulsed cavitation-micro-etching involves alternating on and off ultrasonic treatment in a sodium hydroxide aqueous solution, causing cavitation bubbles to be generated and collapse periodically. During the ultrasonic on-phase phase, the microjets and localized impacts generated by cavitation help disturb the liquid boundary layer on the aluminum alloy surface, promoting the removal of the surface oxide layer and the slight etching of the aluminum alloy surface by sodium hydroxide. The pause phase allows fresh etching solution to re-enter the surface micro-area and reduces the possibility of over-erosion caused by continuous cavitation. After multiple cycles, it is beneficial to form certain shallow micro-pits and micro-undulation structures on the aluminum alloy surface, thereby increasing the actual contact area between the subsequent film layer and the substrate and improving the film-substrate bonding stability.
[0014] Preferably, the ultrasonic cleaning time is 10-15 min; the vacuum drying time is 20-30 min.
[0015] Optionally, in step S2, the flow rate of argon gas used is 35~45 sccm; when performing Ar ion activation treatment under alternating high and low bias conditions, the high bias is -600~-500V and the low bias is -250~-200V, and the high bias is maintained for 5~10s and the low bias is maintained for 15~20s, and the cycle is repeated 8~12 times.
[0016] By alternating between high and low bias voltages multiple times, the risk of excessive bombardment can be reduced while thoroughly cleaning and activating the substrate surface, which is beneficial to improving the bonding stability of subsequent film layers.
[0017] Optionally, in step S2, after Ar ion activation treatment under alternating high and low bias conditions, the substrate temperature is adjusted to 80~100℃, the bias voltage is adjusted to -60~-40V, and the rotation speed is adjusted to 6~10r / min. First, co-sputtering is performed with ZrB2 target 60~70W, NbC target 40~50W, graphite target 20~30W, and CrN target 15~20W for 5~8min. Then, the target power is gradually increased to ZrB2 target 90~110W, NbC target 70~90W, graphite target 50~70W, and CrN target 25~40W within 3~5min. Co-sputtering continues for 100~120min. After cooling to below 50℃ under argon protection, the composite wear-resistant layer is obtained.
[0018] Using a lower target power for initial co-sputtering can reduce the impact of high-energy particles on the aluminum alloy substrate and interfacial stress, and promote uniform nucleation of the deposited components in the micro-pits. Subsequently, the target power is gradually increased, which can gradually increase the content of hard components and the density of the film, reduce abrupt changes in interfacial properties, and thus improve the film-substrate bonding stability and wear resistance.
[0019] Optionally, the thickness of the composite wear-resistant layer is 2.8~3.2μm.
[0020] Controlling the thickness of the composite wear-resistant layer to 2.8~3.2μm can ensure that the film layer has good coverage, load-bearing capacity and wear resistance, while avoiding the risk of residual stress accumulation, cracking or peeling caused by excessive film thickness.
[0021] Optionally, the octadecylphosphonic acid-ethanol solution is obtained by adding 0.14-0.16 parts of octadecylphosphonic acid to 98-99 parts of anhydrous ethanol, stirring at 35-40°C, and cooling to room temperature.
[0022] Preferably, the stirring time is 20-30 minutes.
[0023] Optionally, in step S3, the composite wear-resistant layer is subjected to plasma treatment with a mixture of argon and oxygen at a power of 20-30W for 30-60s; then it is immersed in an octadecylphosphonic acid-ethanol solution and left to stand at 30-35℃ for 10-14h. After removal, it is washed with anhydrous ethanol 3-5 times, dried with nitrogen, and then vacuum dried at 70-80℃ to obtain a wear-resistant film on the metal surface.
[0024] Preferably, the vacuum drying time is 1 to 2 hours.
[0025] Optionally, the total flow rate of the argon and oxygen mixture is 20-25 sccm, and the volume flow rate ratio of argon to oxygen is 9:1.
[0026] The present invention also provides a wear-resistant thin film for metal surfaces, which is prepared by the above preparation method. The wear-resistant thin film for metal surfaces includes a composite wear-resistant layer and an octadecylphosphonic acid modified layer located on the surface of the composite wear-resistant layer.
[0027] In wear-resistant films on metal surfaces, a composite wear-resistant layer is used to improve the film's load-bearing capacity and wear resistance, while an octadecylphosphonic acid modified layer is used to reduce surface wettability. The synergistic effect of the two is beneficial to improving the film's wear resistance, sweat resistance, and corrosion resistance.
[0028] The above-described technical solution of the present invention has at least the following beneficial effects: 1. This invention employs pulsed cavitation-micro-etching combined with nitric acid treatment to pretreat the aluminum alloy substrate, which is beneficial for removing surface oxides and residual impurities and for forming certain micro-pits and undulating structures. Combined with alternating bias Ar ion activation and low-power initial co-sputtering, the actual contact area between the film and the substrate and the mechanical anchoring effect can be increased, thereby improving the film-substrate bonding performance and reducing film cracking and peeling.
[0029] 2. This invention employs co-sputtering with ZrB2, NbC, graphite, and CrN targets, which facilitates the formation of a composite system containing multiple hard components and amorphous carbon-related structures. The Zr-B, Nb-C, and Cr-N hard components enhance the film's hardness, load-bearing capacity, and scratch resistance, while also improving stress distribution under frictional loads. The carbon phase helps reduce shear and adhesion at the friction interface. The combined effect of the synergistic load-bearing capacity of the hard components and the friction-reducing effect of the carbon phase improves the film's wear resistance.
[0030] 3. This invention employs a mixed plasma of argon and oxygen to activate the surface of the composite wear-resistant layer. This facilitates the formation of oxygen-containing active sites on the film surface and promotes the adsorption and bonding of octadecylphosphonic acid on the film surface. Its long-chain alkyl groups are more likely to align towards the outer side of the film, thereby reducing surface free energy and weakening the wetting and retention of moisture and sweat. Simultaneously, the composite wear-resistant layer exhibits good density and wear resistance, reducing film defects and hindering the penetration of corrosive media into the substrate. The combination of hydrophobic anti-wetting properties with wear resistance and dense barrier effects effectively improves the sweat resistance and corrosion resistance of the aluminum alloy surface. Detailed Implementation
[0031] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. The described embodiments are some embodiments of the present invention, and all other embodiments obtained by those skilled in the art based on the described embodiments of the present invention are within the scope of protection of the present invention.
[0032] Example 1 The aluminum alloy substrate was a pre-polished 6061-T6 aluminum alloy. It was ultrasonically cleaned with acetone and anhydrous ethanol for 12 min in sequence, then immersed and fixed in an ultrasonic bath containing 3 wt% sodium hydroxide aqueous solution. The temperature was controlled at 26℃, with the surface to be treated facing the ultrasonic radiation surface and the vertical distance between the surface to be treated and the ultrasonic radiation surface being 40 mm. Pulsed cavitation-micro-etching was performed under ultrasonic conditions of 35 kHz and 32 W / L. Each ultrasonic treatment was performed for 15 s and then paused for 15 s. After 6 cycles, it was immediately cleaned with deionized water 3 times, then immersed in 25 wt% nitric acid aqueous solution and treated at 25℃ for 45 s. After removal, it was cleaned with deionized water 3 times, then washed with anhydrous ethanol 3 times, dried with nitrogen, and then vacuum dried at 75℃ for 25 min to obtain the pre-treated aluminum alloy substrate.
[0033] The pretreated aluminum alloy substrate was placed in the magnetron sputtering chamber, and a vacuum of 5 × 10⁻⁶ was applied. -4 Below Pa, argon gas with a flow rate of 40 sccm was introduced, and Ar ion activation treatment was performed alternately between a high bias voltage of -550V and a low bias voltage of -225V, maintaining the high bias voltage for 8s and the low bias voltage for 18s, for 10 cycles. Then, the substrate temperature was adjusted to 90℃, the bias voltage to -50V, and the rotation speed to 8r / min. First, ZrB2 target 65W, NbC target 45W, graphite target 25W and CrN target 18W were co-sputtered for 6min. Then, the target power was gradually increased to ZrB2 target 100W, NbC target 80W, graphite target 60W and CrN target 32W within 4min, and co-sputtering continued for 110min. After cooling to below 50℃ under argon protection, it was removed to obtain a composite wear-resistant layer with a thickness of 3.0μm.
[0034] 0.15 parts of octadecylphosphonic acid were added to 98.5 parts of anhydrous ethanol and stirred at 38°C for 25 min. The mixture was then cooled to room temperature to obtain an octadecylphosphonic acid-ethanol solution. The composite wear-resistant layer was subjected to plasma treatment with a mixture of argon and oxygen at a total flow rate of 23 sccm, where the volume flow rate ratio of argon to oxygen was 9:1, the plasma treatment power was 25 W, and the treatment time was 45 s. Subsequently, the layer was immersed in the octadecylphosphonic acid-ethanol solution and allowed to stand at 32°C for 12 h. After removal, the layer was washed four times with anhydrous ethanol, dried with nitrogen, and then vacuum dried at 75°C for 1.5 h to obtain a wear-resistant film on the metal surface.
[0035] Example 2 The aluminum alloy substrate was a pre-polished 6061-T6 aluminum alloy. It was ultrasonically cleaned with acetone and anhydrous ethanol for 15 min in sequence, then immersed and fixed in an ultrasonic bath containing 4 wt% sodium hydroxide aqueous solution. The temperature was controlled at 28℃, with the surface to be treated facing the ultrasonic radiation surface and the vertical distance between the surface to be treated and the ultrasonic radiation surface being 50 mm. Pulsed cavitation-micro-etching was performed under ultrasonic conditions of 40 kHz and 40 W / L. The ultrasonic treatment was repeated 7 times, with each ultrasonic treatment lasting 20 s and then pausing for 20 s. After that, it was immediately cleaned with deionized water 4 times, then immersed in 30 wt% nitric acid aqueous solution and treated at 27℃ for 60 s. After that, it was removed, cleaned with deionized water 4 times, washed with anhydrous ethanol 3 times, dried with nitrogen, and then vacuum dried at 80℃ for 30 min to obtain the pre-treated aluminum alloy substrate.
[0036] The pretreated aluminum alloy substrate was placed in the magnetron sputtering chamber, and a vacuum of 5 × 10⁻⁶ was applied. -4 Below Pa, argon gas with a flow rate of 45 sccm was introduced, and Ar ion activation treatment was performed alternately between a high bias voltage of -600V and a low bias voltage of -250V, maintaining the high bias voltage for 10s and the low bias voltage for 20s, for 12 cycles. Subsequently, the substrate temperature was adjusted to 100℃, the bias voltage to -60V, and the rotation speed to 10r / min. First, co-sputtering was performed with ZrB2 target 70W, NbC target 50W, graphite target 30W, and CrN target 20W for 8min. Then, the target power was gradually increased to ZrB2 target 110W, NbC target 90W, graphite target 70W, and CrN target 40W within 5min, and co-sputtering was continued for 120min. After cooling to below 50℃ under argon protection, the composite wear-resistant layer with a thickness of 3.2μm was obtained.
[0037] 0.16 parts of octadecylphosphonic acid were added to 99 parts of anhydrous ethanol and stirred at 40°C for 30 min. The mixture was then cooled to room temperature to obtain an octadecylphosphonic acid-ethanol solution. The composite wear-resistant layer was subjected to plasma treatment with a mixture of argon and oxygen at a total flow rate of 25 sccm, wherein the volume flow rate ratio of argon to oxygen was 9:1, the plasma treatment power was 30 W, and the treatment time was 60 s. Subsequently, the layer was immersed in the octadecylphosphonic acid-ethanol solution and allowed to stand at 35°C for 14 h. After removal, the layer was washed 5 times with anhydrous ethanol, dried with nitrogen, and then vacuum dried at 80°C for 2 h to obtain a wear-resistant film on the metal surface.
[0038] Example 3 The aluminum alloy substrate was a pre-polished 6061-T6 aluminum alloy. It was ultrasonically cleaned with acetone and anhydrous ethanol for 10 min in sequence, then immersed and fixed in an ultrasonic bath containing 2 wt% sodium hydroxide aqueous solution. The temperature was controlled at 25℃, with the surface to be treated facing the ultrasonic radiation surface and the vertical distance between the surface to be treated and the ultrasonic radiation surface being 30 mm. Pulsed cavitation-micro-etching was performed under ultrasonic conditions of 28 kHz and 25 W / L. The ultrasonic treatment was repeated 5 times, with each ultrasonic treatment lasting 10 s and then paused for 10 s. After that, it was immediately cleaned twice with deionized water, then immersed in 20 wt% nitric acid aqueous solution, treated at 23℃ for 30 s, removed, cleaned twice with deionized water, washed twice with anhydrous ethanol, dried with nitrogen, and then vacuum dried at 70℃ for 20 min to obtain the pre-treated aluminum alloy substrate.
[0039] The pretreated aluminum alloy substrate was placed in the magnetron sputtering chamber, and a vacuum of 5 × 10⁻⁶ was applied. -4 Below Pa, argon gas with a flow rate of 35 sccm was introduced, and Ar ion activation treatment was performed alternately between a high bias voltage of -500V and a low bias voltage of -200V, maintaining the high bias voltage for 5s and the low bias voltage for 15s, for 8 cycles. Then, the substrate temperature was adjusted to 80℃, the bias voltage to -40V, and the rotation speed to 6r / min. First, ZrB2 target 60W, NbC target 40W, graphite target 20W and CrN target 15W were co-sputtered for 5min. Then, the target power was gradually increased to ZrB2 target 90W, NbC target 70W, graphite target 50W and CrN target 25W within 3min, and co-sputtering was continued for 100min. After cooling to below 50℃ under argon protection, it was removed to obtain a composite wear-resistant layer with a thickness of 2.8μm.
[0040] 0.14 parts of octadecylphosphonic acid were added to 98 parts of anhydrous ethanol and stirred at 35°C for 20 min. The mixture was then cooled to room temperature to obtain an octadecylphosphonic acid-ethanol solution. The composite wear-resistant layer was subjected to plasma treatment with a mixture of argon and oxygen at a total flow rate of 20 sccm, where the volume flow rate ratio of argon to oxygen was 9:1, the plasma treatment power was 20 W, and the treatment time was 30 s. Subsequently, the layer was immersed in the octadecylphosphonic acid-ethanol solution and allowed to stand at 30°C for 10 h. After removal, the layer was washed three times with anhydrous ethanol, dried with nitrogen, and then vacuum dried at 70°C for 1 h to obtain a wear-resistant film on the metal surface.
[0041] Example 4 The aluminum alloy substrate was a pre-polished 6061-T6 aluminum alloy. It was ultrasonically cleaned with acetone and anhydrous ethanol for 11 min in sequence, then immersed and fixed in an ultrasonic bath containing 2.5 wt% sodium hydroxide aqueous solution, with the temperature controlled at 26℃. The surface to be treated was oriented towards the ultrasonic radiation surface, and the vertical distance between the surface to be treated and the ultrasonic radiation surface was 35 mm. Pulsed cavitation-micro-etching was performed under ultrasonic conditions of 30 kHz and 28 W / L. The ultrasonic treatment was repeated 6 times, with each ultrasonic treatment lasting 12 s and then paused for 14 s. Immediately after each treatment, the substrate was cleaned 3 times with deionized water, then immersed in 22 wt% nitric acid aqueous solution, treated at 24℃ for 40 s, removed, cleaned 3 times with deionized water, washed 2 times with anhydrous ethanol, dried with nitrogen, and then vacuum dried at 72℃ for 22 min to obtain the pre-treated aluminum alloy substrate.
[0042] The pretreated aluminum alloy substrate was placed in the magnetron sputtering chamber, and a vacuum of 5 × 10⁻⁶ was applied. -4 Below Pa, argon gas with a flow rate of 37 sccm was introduced, and Ar ion activation treatment was performed alternately between a high bias voltage of -520V and a low bias voltage of -210V, maintaining the high bias voltage for 6s and the low bias voltage for 16s, for 9 cycles. Subsequently, the substrate temperature was adjusted to 85℃, the bias voltage to -45V, and the rotation speed to 7r / min. First, co-sputtering was performed with ZrB2 target 62W, NbC target 42W, graphite target 22W, and CrN target 16W for 6min. Then, the target power was gradually increased to ZrB2 target 95W, NbC target 75W, graphite target 55W, and CrN target 28W within 3.5min, and co-sputtering was continued for 105min. After cooling to below 50℃ under argon protection, the composite wear-resistant layer with a thickness of 2.9μm was obtained.
[0043] 0.145 parts of octadecylphosphonic acid were added to 98.2 parts of anhydrous ethanol and stirred at 36°C for 22 min. The mixture was then cooled to room temperature to obtain an octadecylphosphonic acid-ethanol solution. The composite wear-resistant layer was subjected to plasma treatment with a mixture of argon and oxygen at a total flow rate of 21 sccm, wherein the volume flow ratio of argon to oxygen was 9:1, the plasma treatment power was 22 W, and the treatment time was 35 s. Subsequently, the layer was immersed in the octadecylphosphonic acid-ethanol solution and allowed to stand at 31°C for 11 h. After removal, the layer was washed three times with anhydrous ethanol, dried with nitrogen, and then vacuum dried at 72°C for 1.2 h to obtain a wear-resistant film on the metal surface.
[0044] Example 5 The aluminum alloy substrate was a pre-polished 6061-T6 aluminum alloy. It was ultrasonically cleaned with acetone and anhydrous ethanol for 13 min in sequence, then immersed and fixed in an ultrasonic bath containing 3.5 wt% sodium hydroxide aqueous solution, with the temperature controlled at 27℃. The surface to be treated was oriented towards the ultrasonic radiation surface, and the vertical distance between the surface to be treated and the ultrasonic radiation surface was 45 mm. Pulsed cavitation-micro-etching was performed under ultrasonic conditions of 38 kHz and 36 W / L. The ultrasonic treatment was repeated 7 times, with each ultrasonic treatment lasting 18 s and then paused for 16 s. After each cycle, the substrate was immediately cleaned with deionized water 4 times, then immersed in 28 wt% nitric acid aqueous solution, treated at 26℃ for 50 s, removed, cleaned with deionized water 4 times, washed with anhydrous ethanol 3 times, dried with nitrogen, and then vacuum dried at 78℃ for 28 min to obtain the pre-treated aluminum alloy substrate.
[0045] The pretreated aluminum alloy substrate was placed in the magnetron sputtering chamber, and a vacuum of 5 × 10⁻⁶ was applied. -4 Below Pa, argon gas with a flow rate of 43 sccm was introduced, and Ar ion activation treatment was performed alternately between a high bias voltage of -580V and a low bias voltage of -240V, maintaining the high bias voltage for 9s and the low bias voltage for 19s, for 11 cycles. Subsequently, the substrate temperature was adjusted to 95℃, the bias voltage to -55V, and the rotation speed to 9r / min. First, co-sputtering was performed with ZrB2 target 68W, NbC target 48W, graphite target 28W, and CrN target 19W for 7min. Then, the target power was gradually increased to ZrB2 target 105W, NbC target 85W, graphite target 65W, and CrN target 36W within 4.5min, and co-sputtering was continued for 115min. After cooling to below 50℃ under argon protection, the composite wear-resistant layer with a thickness of 3.1μm was obtained.
[0046] 0.155 parts of octadecylphosphonic acid were added to 98.8 parts of anhydrous ethanol and stirred at 39°C for 28 min. The mixture was then cooled to room temperature to obtain an octadecylphosphonic acid-ethanol solution. The composite wear-resistant layer was subjected to plasma treatment with a mixture of argon and oxygen at a total flow rate of 24 sccm, where the volume flow ratio of argon to oxygen was 9:1, the plasma treatment power was 28 W, and the treatment time was 55 s. Subsequently, the layer was immersed in the octadecylphosphonic acid-ethanol solution and allowed to stand at 34°C for 13 h. After removal, the layer was washed 5 times with anhydrous ethanol, dried with nitrogen, and then vacuum dried at 78°C for 1.8 h to obtain a wear-resistant film on the metal surface.
[0047] Example 6 The aluminum alloy substrate was a pre-polished 6061-T6 aluminum alloy. It was ultrasonically cleaned with acetone and anhydrous ethanol for 14 min in sequence, then immersed and fixed in an ultrasonic bath containing 3.2 wt% sodium hydroxide aqueous solution, with the temperature controlled at 27℃. The surface to be treated was oriented towards the ultrasonic radiation surface, and the vertical distance between the surface to be treated and the ultrasonic radiation surface was 42 mm. Pulsed cavitation-micro-etching was performed under ultrasonic conditions of 32 kHz and 34 W / L. The ultrasonic treatment was repeated 6 times, with each ultrasonic treatment lasting 16 s and then paused for 18 s. After each cycle, the substrate was immediately cleaned with deionized water 3 times, then immersed in 26 wt% nitric acid aqueous solution, treated at 26℃ for 48 s, removed, cleaned with deionized water 3 times, washed with anhydrous ethanol 3 times, dried with nitrogen, and then vacuum dried at 76℃ for 26 min to obtain the pre-treated aluminum alloy substrate.
[0048] The pretreated aluminum alloy substrate was placed in the magnetron sputtering chamber, and a vacuum of 5 × 10⁻⁶ was applied. -4 Below Pa, argon gas with a flow rate of 41 sccm was introduced, and Ar ion activation treatment was performed alternately between a high bias voltage of -560V and a low bias voltage of -230V, maintaining the high bias voltage for 7s and the low bias voltage for 17s, for 10 cycles. Subsequently, the substrate temperature was adjusted to 92℃, the bias voltage to -52V, and the rotation speed to 8r / min. First, co-sputtering was performed with ZrB2 target 66W, NbC target 46W, graphite target 26W, and CrN target 17W for 7min. Then, the target power was gradually increased to ZrB2 target 102W, NbC target 82W, graphite target 62W, and CrN target 34W within 4min, and co-sputtering was continued for 112min. After cooling to below 50℃ under argon protection, the composite wear-resistant layer with a thickness of 3.05μm was obtained.
[0049] 0.152 parts of octadecylphosphonic acid were added to 98.6 parts of anhydrous ethanol and stirred at 37°C for 26 min. The mixture was then cooled to room temperature to obtain an octadecylphosphonic acid-ethanol solution. The composite wear-resistant layer was subjected to plasma treatment with a mixture of argon and oxygen at a total flow rate of 22 sccm, where the volume flow rate ratio of argon to oxygen was 9:1, the plasma treatment power was 26 W, and the treatment time was 50 s. Subsequently, the layer was immersed in the octadecylphosphonic acid-ethanol solution and allowed to stand at 33°C for 12.5 h. After removal, the layer was washed four times with anhydrous ethanol, dried with nitrogen, and then vacuum dried at 76°C for 1.6 h to obtain a wear-resistant film on the metal surface.
[0050] The present invention also includes comparative examples and related experiments.
[0051] Comparative Example 1 Compared with Example 1, the only difference is that static alkaline etching is used instead of pulsed cavitation-micro-etching. Specifically, the aluminum alloy substrate is a pre-polished 6061-T6 aluminum alloy, which is ultrasonically cleaned with acetone and anhydrous ethanol for 12 min in sequence, then immersed in an aqueous solution containing 3 wt% sodium hydroxide, and statically treated at 26°C for 180 s without ultrasonic treatment. After treatment, it is immediately cleaned three times with deionized water, then immersed in an aqueous solution of 25 wt% nitric acid, and treated at 25°C for 45 s. After removal, it is cleaned three times with deionized water, then washed three times with anhydrous ethanol, dried with nitrogen, and then vacuum dried at 75°C for 25 min to obtain the pretreated aluminum alloy substrate. The subsequent preparation method is completely consistent with the composition, and finally a wear-resistant film on the metal surface is obtained.
[0052] Comparative Example 2 Compared with Example 1, the only difference is that a graphite target was not used in the preparation of the composite wear-resistant layer, and the subsequent preparation method and composition were completely consistent, finally obtaining a wear-resistant film on the metal surface.
[0053] Comparative Example 3 Compared with Example 1, the only difference is that the CrN target was not used in the preparation of the composite wear-resistant layer, and the subsequent preparation method and composition were completely consistent, finally obtaining a wear-resistant film on the metal surface.
[0054] Comparative Example 4 Compared with Example 1, the only difference is that after the composite wear-resistant layer was prepared, no further octadecylphosphonic acid surface modification was performed, and it was directly used as the final wear-resistant film on the metal surface.
[0055] Performance testing Performance tests were conducted on the wear-resistant films on the metal surfaces prepared in Examples 1-6 and Comparative Examples 1-4. Hardness tests were performed according to GB / T21838.1-2019 "Instrumented Indentation Tests of Hardness and Material Parameters of Metallic Materials - Part 1: Test Methods". The critical load corresponding to the occurrence of continuous cracking or peeling of the film layer was recorded as the critical load to evaluate the surface adhesion, according to GB / T30707-2014 "Test Method for Adhesion of Fine Ceramic Coatings - Scratch Method". Additionally, a ball-disc friction and wear tester was used for wear resistance testing. Al2O3 ceramic balls with a diameter of 6 mm were used as the grinding balls. The normal load was 2 N, the sliding speed was 0.1 m / s, the wear mark radius was 3 mm, the total sliding distance was 100 m, and the test environment temperature was 23±2℃ and the relative humidity was 50±5%. The average friction coefficient during the stable wear stage was recorded. After the test, a three-dimensional profilometer was used to measure the cross-sectional area of the wear mark and the wear volume, and the specific wear rate was calculated using the following formula: Specific wear rate = V / (F×L); Where V represents the wear volume, in mm. 3 F represents the normal load in N; L represents the total sliding distance in m.
[0056] The test results are shown in Table 1.
[0057] Table 1
[0058] In addition, the static water contact angle of the thin film surface was tested using an optical contact angle meter; artificial sweat was prepared according to QB / T4775-2023 "Test Method for Corrosion Resistance of Housings and Accessories by Artificial Sweat and Salt Spray" and tested for 168 hours. After the test, the sample was removed, cleaned with deionized water, dried with nitrogen, and the discoloration, corrosion spots, and blistering on the sample surface were observed using an optical microscope; a 240-hour neutral salt spray test was conducted according to GB / T10125-2021 "Civilized Atmosphere Corrosion Test - Salt Spray Test". After the test, the sample was removed, cleaned with deionized water and dried, and the corrosion, blistering, cracking, and peeling on the film surface were observed; the specific test results are shown in Table 2.
[0059] Table 2
[0060] As shown in Tables 1 and 2, the nanohardness of the wear-resistant films on the metal surfaces obtained in Examples 1-6 is 21.9-23.8 GPa, the critical load is 34.7-38.6 N, the average coefficient of friction is 0.16-0.20, and the specific wear rate is 1.8 × 10⁻⁶. -6 ~2.8×10 -6 mm 3The N·m value indicates that the obtained film has good hardness, film-substrate adhesion, friction reduction, and wear resistance. Meanwhile, the water contact angles of the films obtained in Examples 1-6 were 109.2-112.8°. After 168 hours of artificial sweat testing and 240 hours of neutral salt spray testing, no obvious discoloration, corrosion spots, blistering, cracking, or peeling appeared on the film surface, indicating that the obtained films have good hydrophobic properties, sweat resistance, and corrosion resistance.
[0061] Compared to Example 1, Comparative Example 1 used static alkaline etching instead of pulsed cavitation-micro-etching, resulting in a significant reduction in the critical load to 24.3 N, and a significant increase in the average friction coefficient and specific wear rate. Comparative Example 2 did not use a graphite target during the preparation of the composite wear-resistant layer, and its average friction coefficient and specific wear rate increased most significantly. Comparative Example 3 did not use a CrN target during the preparation of the composite wear-resistant layer, resulting in the most significant decrease in nano-hardness, and an increase in both the average friction coefficient and specific wear rate. After artificial sweat and neutral salt spray tests, the film surface showed slight discoloration, pitting corrosion, and localized blistering. Comparative Example 4 did not undergo octadecylphosphonic acid surface modification, resulting in a significant reduction in its water contact angle. After artificial sweat and neutral salt spray tests, the film surface showed significant discoloration, numerous corrosion spots, localized blistering, cracking, and peeling.
[0062] The above are preferred embodiments of the present invention. Those skilled in the art can make several improvements and modifications without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a wear-resistant thin film on a metal surface, characterized in that, Includes the following steps: S1. The aluminum alloy substrate is ultrasonically cleaned with acetone and anhydrous ethanol in sequence, then placed in sodium hydroxide aqueous solution for pulse cavitation-micro etching treatment, washed with water and then placed in nitric acid aqueous solution. After washing with water, washing with anhydrous ethanol, blowing with nitrogen and vacuum drying, the pretreated aluminum alloy substrate is obtained. S2. The pretreated aluminum alloy substrate is placed in a magnetron sputtering chamber, vacuumed, and argon gas is introduced. Ar ion activation treatment is carried out under alternating high and low bias conditions. Then, the substrate temperature and bias are adjusted. First, co-sputtering is performed with ZrB2 target 60~70W, NbC target 40~50W, graphite target 20~30W and CrN target 15~20W. Then, the target power is gradually increased to ZrB2 target 90~110W, NbC target 70~90W, graphite target 50~70W and CrN target 25~40W for continued co-sputtering. After cooling, a composite wear-resistant layer is obtained. S3. After the composite wear-resistant layer is treated with a mixed plasma of argon and oxygen, it is immersed in an octadecylphosphonic acid-ethanol solution, left to stand, and then washed and dried to obtain a wear-resistant film on the metal surface.
2. The method for preparing a wear-resistant thin film on a metal surface according to claim 1, characterized in that, The aluminum alloy substrate is a pre-polished 6061-T6 aluminum alloy; the concentration of the sodium hydroxide aqueous solution is 2~4wt%; and the concentration of the nitric acid aqueous solution is 20~30wt%.
3. The method for preparing a wear-resistant thin film on a metal surface according to claim 1, characterized in that, In step S1, after ultrasonic cleaning, the substrate is immersed and fixed in an ultrasonic bath containing sodium hydroxide aqueous solution, with the temperature controlled at 25~28℃. The surface to be treated faces the ultrasonic radiation surface, and the vertical distance between the surface to be treated and the ultrasonic radiation surface is 30~50mm. Pulsed cavitation-micro-etching treatment is performed under ultrasonic conditions of 28~40kHz and 25~40W / L. Each time the ultrasonic treatment is started for 10~20s and then paused for 10~20s, the process is repeated 5~7 times. The substrate is then immediately cleaned with deionized water, then immersed in nitric acid aqueous solution, and treated at 23~27℃ for 30~60s. After removal, the substrate is washed with deionized water and anhydrous ethanol in sequence, dried with nitrogen, and then vacuum dried at 70~80℃ to obtain the pretreated aluminum alloy substrate.
4. The method for preparing a wear-resistant thin film on a metal surface according to claim 1, characterized in that, In step S2, the flow rate of argon gas used is 35~45 sccm; when performing Ar ion activation treatment under alternating high and low bias conditions, the high bias is -600~-500V and the low bias is -250~-200V, and the high bias is maintained for 5~10s and the low bias is maintained for 15~20s, and the cycle is repeated 8~12 times.
5. The method for preparing a wear-resistant thin film on a metal surface according to claim 1, characterized in that, In step S2, after Ar ion activation treatment under alternating high and low bias conditions, the substrate temperature is adjusted to 80~100℃, the bias voltage is adjusted to -60~-40V, and the rotation speed is adjusted to 6~10r / min. First, co-sputtering is performed with ZrB2 target 60~70W, NbC target 40~50W, graphite target 20~30W, and CrN target 15~20W for 5~8min. Then, the target power is gradually increased to ZrB2 target 90~110W, NbC target 70~90W, graphite target 50~70W, and CrN target 25~40W within 3~5min. Co-sputtering continues for 100~120min. After cooling to below 50℃ under argon protection, the composite wear-resistant layer is obtained.
6. The method for preparing a wear-resistant thin film on a metal surface according to claim 1, characterized in that, The thickness of the composite wear-resistant layer is 2.8~3.2μm.
7. The method for preparing a wear-resistant thin film on a metal surface according to claim 1, characterized in that, The octadecylphosphonic acid-ethanol solution is obtained by adding 0.14-0.16 parts of octadecylphosphonic acid to 98-99 parts of anhydrous ethanol, stirring at 35-40°C, and cooling to room temperature.
8. The method for preparing a wear-resistant thin film on a metal surface according to claim 1, characterized in that, In step S3, the composite wear-resistant layer is subjected to plasma treatment with a mixture of argon and oxygen at a power of 20-30W for 30-60s; then it is immersed in an octadecylphosphonic acid-ethanol solution and left to stand at 30-35℃ for 10-14h. After removal, it is washed with anhydrous ethanol 3-5 times, dried with nitrogen, and then vacuum dried at 70-80℃ to obtain a wear-resistant film on the metal surface.
9. The method for preparing a wear-resistant thin film on a metal surface according to claim 8, characterized in that, The total flow rate of the argon and oxygen mixture is 20-25 sccm, and the volumetric flow rate ratio of argon to oxygen is 9:
1.
10. A wear-resistant thin film on a metal surface, characterized in that, The wear-resistant film on a metal surface is prepared by the method described in any one of claims 1 to 9, wherein the wear-resistant film comprises a composite wear-resistant layer and an octadecylphosphonic acid modified layer located on the surface of the composite wear-resistant layer.