A chemical copper plating solution and its preparation method, and a method for preparing a high aspect ratio glass through-hole seed layer.

By combining magnetron sputtering and electroless copper plating on a glass substrate, the problems of insufficient coverage and adhesion in high aspect ratio through holes are solved, achieving full hole wall coverage and strong adhesion, simplifying the process and reducing the void defect rate of electroplated through holes.

CN123108542APending Publication Date: 2026-11-17TIANJIN MUHUA QINGYAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611522740.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve high coverage and strong adhesion in seed layer preparation within high aspect ratio vias on glass substrates. Physical vapor deposition methods result in uneven coverage, while chemical plating methods require complex pretreatment and exhibit weak adhesion.

Method used

A first seed layer is deposited on the surface of a glass substrate using magnetron sputtering, and a second seed layer is deposited in the via using an electroless copper plating solution. The electroless copper plating solution is composed of copper sulfate pentahydrate, disodium ethylenediaminetetraacetate, potassium sodium tartrate, etc., which provides catalytic activity and high adhesion. Polyethylene glycol reduces surface tension and achieves full coverage of the via wall.

Benefits of technology

It achieves high coverage and strong adhesion of the entire inner wall of high aspect ratio through holes, simplifies the process, reduces electroplating filling defects, and significantly improves the filling effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention belongs to the field of glass substrate through-hole metallization technology, specifically relating to a chemical copper plating solution and its preparation method, and a method for preparing a high aspect ratio glass through-hole seed layer. Based on 1L, the chemical copper plating solution comprises the following chemical components by weight: 6-10g copper sulfate pentahydrate; 20-30g disodium ethylenediaminetetraacetate; 12-18g potassium sodium tartrate; 4-8g reducing agent; 8-14g pH adjuster; 0.006-0.025g stabilizer; 0.003-0.01g surfactant; the remainder being deionized water. This invention combines magnetron sputtering and chemical plating processes to achieve high adhesion and high coverage of the entire inner wall of high aspect ratio through-holes, simplifying the process and overcoming the shortcomings of existing methods that rely solely on sputtering or chemical plating. It provides a qualified composite conductive seed layer for subsequent glass through-hole electroplating and significantly reduces the rate of voids in the filled holes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of glass substrate through-hole metallization technology, specifically relating to a chemical copper plating solution and its preparation method, and a method for preparing a high aspect ratio glass through-hole seed layer. Background Technology

[0002] Through-Glass Vias (TGV) are the core carrier for realizing three-dimensional vertical interconnection of glass substrates. The process includes hole formation, seed layer preparation, and electroplating filling steps. Among them, the quality of seed layer preparation directly determines the success or failure of subsequent electroplating filling. There are two main methods for preparing TGV seed layers: (1) Physical vapor deposition (PVD) method, represented by magnetron sputtering, deposits titanium / copper or chromium / copper composite layers on the glass surface and the inner wall of the through-hole. The film layer of this process is dense and has good adhesion. However, due to the linear motion characteristics of sputtered particles, in through-holes with high aspect ratios (usually ≥5:1), the energy of particles reaching the lower part of the hole wall is severely attenuated, and the uniformity of sidewall coverage deteriorates sharply. When the aspect ratio exceeds 5:1, the coverage of the hole bottom is usually less than 30% of the surface coverage, which cannot provide a complete and continuous conductive path for the entire inner wall of the through-hole, resulting in voids in the hole during subsequent electroplating. (2) The electroless plating method utilizes chemical solutions to undergo autocatalytic deposition on the inner wall of the through-hole. The chemical solution can enter the deep hole through liquid convection, theoretically achieving full coverage of the hole wall. However, the catalytic activity of the glass surface is extremely low, requiring complex pretreatment such as sensitization and activation. Furthermore, the adhesion between the electroless plating layer and the glass substrate is generally weaker than that of the sputtered film, making it prone to peeling in subsequent processes. Therefore, it is of great significance to prepare a seed layer with both high coverage and strong adhesion in a three-dimensional deep hole structure with a high aspect ratio on glass, a non-conductive substrate with low surface energy. Summary of the Invention

[0003] To overcome the above-mentioned defects, the present invention aims to provide a chemical copper plating solution and its preparation method, as well as a method for preparing a high aspect ratio glass through-hole seed layer.

[0004] To achieve the above objectives, the present invention adopts the following technical solution: A chemical copper plating solution, per liter, comprises the following chemical components by weight: Copper sulfate pentahydrate 6-10g; 20-30g of disodium ethylenediaminetetraacetate; 12-18g of potassium sodium tartrate; 4-8g of reducing agent; pH adjuster 8-14g; Stabilizer 0.006-0.025g; Surfactant 0.003-0.01g; The rest is deionized water.

[0005] Preferably, the reducing agent is formaldehyde, and the formaldehyde mass concentration is 30-45%.

[0006] Preferably, the pH adjuster is sodium hydroxide.

[0007] Preferably, the pH value of the chemical copper plating solution is 12-13.

[0008] Preferably, the stabilizer is 2,2'-bipyridine and potassium ferrocyanide, wherein the mass ratio of potassium ferrocyanide to 2,2'-bipyridine is 0.5-3:1.

[0009] Preferably, the surfactant is polyethylene glycol, and the polyethylene glycol has a molecular weight of 1000-4000.

[0010] A method for preparing a chemical copper plating solution includes the following steps: Copper sulfate pentahydrate is dissolved in deionized water to obtain a copper salt solution; Disodium ethylenediaminetetraacetate and sodium potassium tartrate were dissolved in deionized water to obtain a complexing agent solution; Slowly add the copper salt solution to the complexing agent solution, then add the stabilizer and surfactant, stir well, then add the pH adjuster to adjust the pH value to 12-13, and then add deionized water to make up the volume of the solution to 1L. Finally, add the reducing agent, stir well, filter, and the product is ready.

[0011] A method for preparing a high aspect ratio glass through-hole seed layer includes the following steps: A first seed layer is magnetron sputtered onto the surface of the glass substrate and inside the via; The glass substrate after magnetron sputtering is immersed in the electroless copper plating solution to deposit a second seed layer, thus obtaining the desired product.

[0012] Preferably, the first seed layer is made of titanium and copper, and the thickness of the first seed layer is 40-160 nm, wherein the titanium layer is 10-60 nm and the copper layer is 30-100 nm; the magnetron sputtering adopts DC magnetron sputtering, the sputtering target is a titanium target and a copper target, the sputtering power is 2-5 kW, and the working gas pressure is 0.3-0.6 Pa.

[0013] Preferably, the material of the second seed layer is copper, and the thickness of the second seed layer is 100-500 nm.

[0014] The positive and beneficial effects of this invention are as follows: The first seed layer of the glass through-hole in this invention is deposited on the surface of the glass substrate and the inner wall of the through-hole by magnetron sputtering. It is the base layer of the entire composite seed layer. Its core functions are: (1) to provide a high bonding interface with the glass substrate: glass is a non-conductive, low surface energy inorganic substrate, while titanium and copper are highly active metals. After sputtering, they can form chemical bonds with oxygen elements on the glass surface to build a metal transition interface, which significantly improves the adhesion of the subsequent second seed layer copper layer on the glass and solves the problem that the metal coating is easy to peel off from the glass substrate; (2) to provide a catalytically active substrate for the chemical plating reaction, eliminating the glass sensitization and activation process: glass itself does not have the self-catalytic activity of chemical plating. Directly electroless copper plating on glass requires sensitization and activation treatment (palladium salt activation, etc.), which is complex, costly, and prone to causing residual impurities in the via. The first seed layer sputtered in this invention is a metal layer, which is itself a catalytic substrate for electroless copper plating. There is no need to sensitize or activate the glass substrate before treatment, simplifying the process. (3) Provide basic conductivity as the bottom conductive framework: Due to the linear motion characteristics of magnetron sputtering particles, the sputtered film layer in the lower part of the hole wall and the bottom of the hole in the high aspect ratio via is very thin or even locally discontinuous. However, a continuous metal film can be formed on the substrate surface and the upper part of the via, providing initial conductive / catalytic sites for subsequent electroless copper plating.

[0015] This invention involves immersing a glass substrate after magnetron sputtering into a chemical copper plating solution to deposit a second seed layer, thus growing a thickened coating layer. The chemical copper plating solution contains copper sulfate pentahydrate, which provides a copper ion source; formaldehyde, as a reducing agent, reduces copper ions to metallic copper; EDTA and sodium potassium tartrate form a dual complexing agent system to complex copper ions and prevent the precipitation of copper hydroxide under alkaline conditions; sodium hydroxide is used to adjust the alkalinity of the plating solution; 2,2'-bipyridine and potassium ferrocyanide act as stabilizers to inhibit spontaneous decomposition of the plating solution; and polyethylene glycol acts as a surfactant to reduce the surface tension of the plating solution and improve the wetting effect on the inner walls of the through-holes. The chemical components of the electroless copper plating solution of this invention work synergistically, resulting in a uniform and stable solution. Relying on the fluidity of the liquid, it can penetrate deep into the high aspect ratio through holes, fully depositing copper layers and compensating for the physical shortcomings of the sputtering process. Its core functions are as follows: (1) Filling in the discontinuous areas of the inner wall of the through hole to achieve high coverage of the entire hole wall: The electroless copper plating solution is liquid and is not restricted by the linear motion of particles. It can enter the lower part of the through hole and the bottom of the hole, and continue to deposit copper on the thin and discontinuous metal sites of the first seed layer, filling the weak and discontinuous positions of the sputtered layer into a continuous and complete metal conductive film, so that the side wall and bottom of the through hole form a continuous conductive path; (2) Thickening the seed layer and reducing the surface resistance: The overall seed layer thickness is increased, the overall resistance of the seed layer is reduced, and the current distribution at each position of the through hole is uniform during subsequent electroplating of copper, avoiding electroplating defects caused by excessive local resistance; (3) Enhancing the interface bonding: The second seed layer and the first seed layer are both metals, and the two are metal-to-metal bonded, with a strong interface bonding and no interlayer peeling.

[0016] In summary, the first seed layer addresses the issues of "adhesion at the glass-metal interface" and "chemical plating catalytic substrate," but it fails to resolve the problem of insufficient coverage deep within high aspect ratio vias. The second seed layer addresses the issues of "internal coverage and film continuity within deep vias," but it cannot be directly applied to glass substrates and must rely on the metal catalytic substrate provided by the first seed layer. This invention combines magnetron sputtering and chemical plating processes to achieve high adhesion and high coverage of the entire inner wall of high aspect ratio vias, simplifying the process and overcoming the shortcomings of either sputtering or chemical plating alone in existing technologies. It provides a qualified composite conductive seed layer for subsequent electroplating and filling of glass vias, significantly reducing the void filling defect rate. Detailed Implementation

[0017] The present invention will be further described below with reference to some specific embodiments.

[0018] Example 1

[0019] A chemical copper plating solution, comprising the following components, per 1L: 10g of copper sulfate pentahydrate; 25g of disodium ethylenediaminetetraacetate; 15g of potassium sodium tartrate; 6g of formaldehyde (37% by mass) as a reducing agent; 10g of sodium hydroxide; 0.005 g of 2,2'-bipyridine; Potassium ferrocyanide 0.01g; Surfactant polyethylene glycol (molecular weight 2000) 0.005g; The rest is deionized water.

[0020] The preparation method of the above-mentioned electroless copper plating solution is as follows: (1) Dissolve copper sulfate pentahydrate in 300 mL of deionized water to obtain a copper salt solution; (2) Dissolve disodium ethylenediaminetetraacetate and sodium potassium tartrate in 500 mL of deionized water to obtain a complexing agent solution; (3) Dissolve sodium hydroxide in 50 mL of deionized water beforehand, dissolve 2,2'-bipyridine and potassium ferrocyanide in 50 mL of deionized water beforehand, and dissolve polyethylene glycol in 50 mL of deionized water beforehand; (4) At a temperature of 50°C, the copper salt solution is slowly added to the complexing agent solution, followed by the pre-dissolved 2,2'-bipyridine, potassium ferrocyanide and polyethylene glycol, and stirred evenly. Then, the pre-dissolved sodium hydroxide is added to adjust the pH value to 12-13. Finally, deionized water is added to bring the solution to a final volume of 1L. (5) Add formaldehyde 10 minutes before use, stir well, filter and you will get the product.

[0021] Example 2

[0022] A chemical copper plating solution, comprising the following components, per 1L: 8g of copper sulfate pentahydrate; 20g of disodium ethylenediaminetetraacetate; 18g of potassium sodium tartrate; 8g of formaldehyde (37% by mass) as a reducing agent; 12g of sodium hydroxide; 0.005 g of 2,2'-bipyridine; Potassium ferrocyanide 0.01g; Surfactant polyethylene glycol (molecular weight 2000) 0.01g; The rest is deionized water.

[0023] The preparation method of the above-mentioned chemical copper plating solution is the same as that in Example 1.

[0024] Example 3

[0025] A chemical copper plating solution, comprising the following components, per 1L: 10g of copper sulfate pentahydrate; 30g of disodium ethylenediaminetetraacetate; 12g of potassium sodium tartrate; 5g of formaldehyde (37% by mass) as a reducing agent; 8g of sodium hydroxide; 0.01 g of 2,2'-bipyridine; Potassium ferrocyanide 0.005g; Surfactant polyethylene glycol (molecular weight 2000) 0.01g; The rest is deionized water.

[0026] The preparation method of the above-mentioned chemical copper plating solution is the same as that in Example 1.

[0027] Example 4

[0028] A chemical copper plating solution, comprising the following components, per 1L: 6g of copper sulfate pentahydrate; 25g of disodium ethylenediaminetetraacetate; 14g of potassium sodium tartrate; Reducing agent formaldehyde (mass concentration 37%) 4g; 14g of sodium hydroxide; 0.005 g of 2,2'-bipyridine; Potassium ferrocyanide 0.015g; Surfactant polyethylene glycol (molecular weight 2000) 0.008g; The rest is deionized water.

[0029] The preparation method of the above-mentioned chemical copper plating solution is the same as that in Example 1.

[0030] Example 5

[0031] A method for preparing a high aspect ratio glass through-hole seed layer includes the following steps: (1) Select a borosilicate glass substrate with a thickness of 0.5 mm and a through-hole depth-to-width ratio of 10:1, and magnetron sputter the first seed layer on the surface of the glass substrate and inside the through-hole. The first seed layer is made of titanium and copper, and the thickness of the first seed layer is 80 nm. The magnetron sputtering uses DC magnetron sputtering with titanium and copper targets. The sputtering power is 2-5kW, the working pressure is 0.3-0.6Pa, the titanium layer sputtering time is 5min, the copper layer sputtering time is 10min, the titanium layer is 20nm, and the copper layer is 60nm.

[0032] (2) Immerse the glass substrate after magnetron sputtering in step (1) into the chemical copper plating solution described in Example 1 to deposit a second seed layer. The material of the second seed layer is copper, and the thickness of the second seed layer is 240 nm.

[0033] Example 6

[0034] The preparation method of the high aspect ratio glass through-hole seed layer in this embodiment is basically the same as that in Example 5, and the similarities will not be repeated. The difference is: (2) Immerse the glass substrate after magnetron sputtering in step (1) into the chemical copper plating solution described in Example 2 to deposit a second seed layer. The material of the second seed layer is copper, and the thickness of the second seed layer is 310 nm.

[0035] Example 7

[0036] The preparation method of the high aspect ratio glass through-hole seed layer in this embodiment is basically the same as that in Example 5, and the similarities will not be repeated. The difference is: (2) Immerse the glass substrate after magnetron sputtering in step (1) into the chemical copper plating solution described in Example 3 to deposit a second seed layer. The material of the second seed layer is copper, and the thickness of the second seed layer is 200 nm.

[0037] Example 8

[0038] The preparation method of the high aspect ratio glass through-hole seed layer in this embodiment is basically the same as that in Example 5, and the similarities will not be repeated. The difference is: (2) Immerse the glass substrate after magnetron sputtering in step (1) into the chemical copper plating solution described in Example 4 to deposit a second seed layer. The material of the second seed layer is copper, and the thickness of the second seed layer is 160 nm.

[0039] Comparative Example 1 The high aspect ratio glass through-hole seed layer in this embodiment is basically the same as that in Embodiment 5, and the similarities will not be repeated. The difference is that only magnetron sputtering is performed, as detailed below: A seed layer was magnetron sputtered on the surface of a glass substrate and inside a via. The seed layer was made of titanium and copper and had a thickness of 80 nm. The magnetron sputtering was performed using DC magnetron sputtering with titanium and copper targets. The sputtering power was 2-5 kW and the working pressure was 0.3-0.6 Pa. The sputtering time for the titanium layer was 5 min and the sputtering time for the copper layer was 10 min. The titanium layer was 20 nm thick and the copper layer was 60 nm thick.

[0040] Comparative Example 2 The high aspect ratio glass through-hole seed layer in this embodiment is basically the same as that in Example 5, and the similarities will not be repeated. The difference is that only chemical plating is performed, as detailed below: The glass substrate was immersed in the electroless copper plating solution described in Example 1 to deposit a seed layer. The seed layer was made of copper and had a thickness of 240 nm.

[0041] The performance of the glass through-hole seed layer of Examples 5-8 and Comparative Examples 1-2 of the present invention was tested, and the test results are shown in Table 1.

[0042] Table 1. Performance test results of glass through-hole seed layers in Examples 5-8 and Comparative Examples 1-2 of the present invention

[0043] As shown in Table 1, the composite seed layer of the present invention achieves both high adhesion and high coverage of the entire inner wall of the through hole with a high aspect ratio, reduces surface resistivity, simplifies the process, overcomes the shortcomings of the existing technologies of separate sputtering and separate chemical plating, provides a qualified composite conductive seed layer for subsequent glass through hole electroplating and filling, and significantly reduces the defect rate of hole filling voids.

[0044] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Any other modifications or equivalent substitutions made by those skilled in the art to the technical solutions of the present invention, as long as they do not depart from the spirit and scope of the technical solutions of the present invention, should be covered within the scope of the claims of the present invention.

Claims

1. A chemical copper plating solution, characterized in that, Based on 1L, it includes the following chemical components by weight: Copper sulfate pentahydrate 6-10g; 20-30g of disodium ethylenediaminetetraacetate; 12-18g of potassium sodium tartrate; 4-8g of reducing agent; pH adjuster 8-14g; Stabilizer 0.006-0.025g; Surfactant 0.003-0.01g; The rest is deionized water.

2. The electroless copper plating solution according to claim 1, characterized in that, The reducing agent is formaldehyde, and the formaldehyde mass concentration is 30-45%.

3. The electroless copper plating solution according to claim 1, characterized in that, The pH adjuster is sodium hydroxide.

4. The electroless copper plating solution according to claim 1, characterized in that, The pH value of the chemical copper plating solution is 12-13.

5. The electroless copper plating solution according to claim 1, characterized in that, The stabilizer is 2,2'-bipyridine and potassium ferrocyanide, wherein the mass ratio of potassium ferrocyanide to 2,2'-bipyridine is 0.5-3:

1.

6. The electroless copper plating solution according to claim 1, characterized in that, The surfactant is polyethylene glycol, and the molecular weight of the polyethylene glycol is 1000-4000.

7. A method for preparing the electroless copper plating solution according to any one of claims 1-6, characterized in that, Includes the following steps: Copper sulfate pentahydrate is dissolved in deionized water to obtain a copper salt solution; Disodium ethylenediaminetetraacetate and sodium potassium tartrate were dissolved in deionized water to obtain a complexing agent solution; Slowly add the copper salt solution to the complexing agent solution, then add the stabilizer and surfactant, stir well, then add the pH adjuster to adjust the pH value to 12-13, and then add deionized water to make up the volume of the solution to 1L. Finally, add the reducing agent, stir well, filter, and the product is ready.

8. A method for preparing a high aspect ratio glass through-hole seed layer, characterized in that, Includes the following steps: A first seed layer is magnetron sputtered onto the surface of the glass substrate and inside the vias. The glass substrate after magnetron sputtering is immersed in the electroless copper plating solution described in any one of claims 1-6 to deposit a second seed layer, thus obtaining the desired product.

9. The method for preparing a high aspect ratio glass through-hole seed layer according to claim 8, characterized in that, The first seed layer is made of titanium and copper, and its thickness is 40-160 nm, of which the titanium layer is 10-60 nm and the copper layer is 30-100 nm. The magnetron sputtering is carried out by DC magnetron sputtering, the sputtering target is a titanium target and a copper target, the sputtering power is 2-5 kW, and the working gas pressure is 0.3-0.6 Pa.

10. The method for preparing a high aspect ratio glass through-hole seed layer according to claim 8, characterized in that, The second seed layer is made of copper and has a thickness of 100-500 nm.