A method for preparing an underwater superoleophobic metal film

By activating porous metal substrates and covalently linking them with low surface energy compounds, the problem of oil adhesion to porous metal materials underwater is solved, achieving improved underwater superoleophobic properties and mechanical stability, applicable to various metal materials and forms.

CN123108560APending Publication Date: 2026-11-17WESTERN BAODE TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202611193322.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve stable and widely applicable underwater superoleophobic properties on porous metal surfaces, leading to easy adhesion of oil and affecting equipment efficiency and lifespan.

Method used

After degreasing, cleaning, and drying the porous metal substrate, it is immersed in an activation solution for activation. Then, a binder is added to an acidic alcohol-water mixed solvent, which is then adjusted to an alkaline solvent and a low surface energy compound is added to form a stable covalent bond. Finally, it is dried to form an underwater superoleophobic film.

Benefits of technology

It achieves an underwater oil contact angle of more than 150° on metal surfaces, exhibits excellent oleophobic properties, ensures a strong bond between the functional layer and the substrate, and significantly improves mechanical stability and durability, making it suitable for various metal materials and shapes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108560A_ABST
    Figure CN123108560A_ABST
Patent Text Reader

Abstract

This method discloses a method for preparing an underwater superoleophobic metal film. The method includes: pretreating a porous metal substrate; immersing the pretreated metal substrate in an activation solution and reacting it at a first temperature for a first time to obtain an activated metal substrate; immersing it in an acidic alcohol-water mixed solvent and adding a binder to the mixed solvent, and reacting it at a second temperature for a second time; adjusting the mixed solvent to alkaline and adding a low surface energy compound containing active functional groups, and reacting it at a third temperature for a third time to obtain a reaction product; removing the reaction product for cleaning and drying it at a fourth temperature for a fourth time to obtain a dried product; and finally cleaning and drying the product to obtain an underwater superoleophobic metal film. This method effectively solves the problem of oil adhesion to metal materials underwater by constructing an activation layer on the metal surface and connecting low surface energy molecules to form an underwater superoleophobic functional layer; at the same time, it significantly improves the mechanical stability and durability of the film layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This solution relates to the field of membrane preparation technology, and in particular to a method for preparing an underwater superoleophobic metal membrane. Background Technology

[0002] Porous metallic materials are widely used in industrial production and daily life due to their excellent mechanical properties, thermal and electrical conductivity, and processing performance. However, metal surfaces typically have high surface energy, making them highly susceptible to wetting and adhesion of oil in underwater separation environments, leading to a series of problems such as equipment contamination and clogging, and increased resistance. In fields such as marine engineering and petrochemicals, oil buildup on the surface of filter elements can severely affect their working efficiency and service life.

[0003] To address the technical challenge of metal films being easily clogged by oil and to achieve underwater superoleophobic properties for porous metal films, researchers have developed various surface modification techniques with unique wettability. Currently, methods for constructing superoleophobic surfaces mainly include laser micromachining, chemical etching, sol-gel methods, and coating techniques. Patent 1 (CN107158754A) discloses a method for preparing a copper mesh with oil-water separation function by laser etching on a copper sheet. The copper mesh obtained by this method has surface through holes and surface micro-nano structures. However, laser processing is currently only applicable to dense metal materials and cannot be processed on porous metal materials. At the same time, laser processing is currently only in the laboratory stage and the processing cost is extremely high, making it difficult to industrialize. Patent 2 (CN109758789A) discloses a method for modifying aluminum foil with low surface energy using chemical etching, which can obtain an aluminum mesh with superhydrophilic / underwater superoleophobic properties. However, the chemical etching process weakens the mechanical strength of the film and causes environmental pollution. Patent 3 (CN115889145A) discloses a method for preparing an oil-water separation mesh by spraying perfluorinated modified silica nanoparticles onto a stainless steel mesh, which can achieve oil-water separation. However, this method is a physical coating, and the coating and the substrate are mainly bonded by van der Waals forces. The bonding force is limited, and it is very easy to peel off and fail due to mechanical wear in actual use.

[0004] Therefore, developing an underwater superoleophobic metal film with a simple process, wide applicability to metal substrates, and a stable and robust oleophobic functional layer has significant practical application value. Summary of the Invention

[0005] This solution aims to at least address the technical problems existing in the prior art. Therefore, the first aspect of this invention proposes a method for preparing an underwater superoleophobic metal film, the method comprising: The porous metal substrate is degreased, cleaned, and dried to remove surface oil and impurities, resulting in a pretreated metal substrate. The pretreated metal substrate is immersed in an activation solution and reacted at a first temperature for a first time to obtain an activated metal substrate. The activated metal substrate is immersed in an acidic alcohol-water mixed solvent, and a binder is added to the mixed solvent, and the reaction is carried out at a second temperature for a second duration. The mixed solvent was adjusted to an alkaline solvent, and a low surface energy compound containing active functional groups was added. The mixture was reacted at a third temperature for a third time to obtain the reaction product. The reaction product is removed, cleaned, and dried at a fourth temperature for a fourth time to obtain a dried product; the dried product is cleaned in an ultrasonic machine and dried in an oven to obtain an underwater superoleophobic metal film.

[0006] Optionally, the porous metal substrate may be made of any of the following materials, including but not limited to: stainless steel, titanium and titanium alloys, nickel and nickel alloys, copper and copper alloys, magnesium and magnesium alloys, refractory metals and alloys, iron-aluminum alloys, Hastelloy, iron, cobalt, zinc, tin, and lead.

[0007] Optionally, the morphology of the porous metal substrate includes, but is not limited to, any of the following: flat plate, mesh, tubular, membrane, cylindrical, honeycomb, foam, sintered metal fiber felt, gradient composite structure, wire mesh composite structure, and powder fiber composite structure.

[0008] Optionally, the first temperature is 15℃-180℃, and the first duration is 2min-240min; the second temperature is 0℃-90℃, and the second duration is 1h-12h.

[0009] Optionally, the pH of the acidic alcohol-water mixed solvent is 2-6, the pH of the alkaline solvent is 8-11, the third temperature is 60℃-200℃, and the third duration is 2h-24h.

[0010] Optionally, the low surface energy compounds containing active functional groups include, but are not limited to, organosilicon compounds with a main chain of -Si-O- structure, long-chain alkanes and their derivatives, fluorinated silanes containing CF bonds, fluorinated organics, fluorinated polymers, and fluorinated compounds.

[0011] Optionally, the reaction product may be washed with a solvent, including but not limited to pure water, ethanol, and acetone.

[0012] Optionally, the fourth temperature is 50℃-200℃, and the fourth duration is 2h-48h.

[0013] The embodiments of the present invention have the following beneficial effects: The present invention provides a method for preparing an underwater superoleophobic metal film, comprising: degreasing, cleaning, and drying a porous metal substrate to remove surface oil and impurities, obtaining a pretreated metal substrate; immersing the pretreated metal substrate in an activation solution and reacting at a first temperature for a first duration to obtain an activated metal substrate; immersing the activated metal substrate in an acidic alcohol-water mixed solvent, adding a binder to the mixed solvent, reacting at a second temperature for a second duration, adjusting the mixed solvent to an alkaline solvent, adding a low surface energy compound containing active functional groups, reacting at a third temperature for a third duration to obtain a reaction product; removing the reaction product for cleaning and drying at a fourth temperature for a fourth duration to obtain a dried product; cleaning the dried product in an ultrasonic machine and drying it in an oven to obtain an underwater superoleophobic metal film. This method forms an underwater superoleophobic functional layer by constructing an activation layer on the metal surface and connecting low surface energy molecules. The material has an underwater oil contact angle of over 150°, which can effectively solve the problem of oil adhesion to metal materials underwater; at the same time, since the functional layer is firmly bonded to the substrate through chemical bonding, it can significantly improve the mechanical stability and durability of the film. Attached Figure Description

[0014] Figure 1 A flowchart illustrating the steps of a method for preparing an underwater superoleophobic metal film according to an embodiment of the present invention; Figure 2 A scanning electron microscope image of the surface of an untreated stainless steel mesh provided in an embodiment of the present invention; Figure 3 A scanning electron microscope image of the surface of a stainless steel mesh after underwater superoleophobic modification, provided in an embodiment of the present invention; Figure 4 Photographs showing the contact angle between a stainless steel mesh and diesel fuel underwater, provided as an embodiment of the present invention; Figure 5 Photographs showing the contact angle of a stainless steel mesh and gasoline underwater, provided as an embodiment of the present invention; Figure 6 Photographs showing the contact angle of a stainless steel mesh and vegetable oil underwater, provided as an embodiment of the present invention; Figure 7 The underwater contact angle curves of the stainless steel mesh under different friction distances provided in the embodiments of the present invention; Figure 8 The underwater contact angle curves of the stainless steel mesh under different ultrasonic treatment times provided in the embodiments of the present invention are shown. Detailed Implementation

[0015] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present solution, and not all embodiments. Based on the embodiments of the present solution, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present solution.

[0016] Hereinafter, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of indicated technical features. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of embodiments of this disclosure, unless otherwise stated, "a plurality of" means two or more. Furthermore, the use of "based on" or "according to" implies openness and inclusiveness, because processes, steps, calculations, or other actions "based on" or "according to" one or more of the stated conditions or values ​​may in practice be based on additional conditions or beyond the stated values.

[0017] Figure 1 This is a flowchart illustrating the steps of a method for preparing an underwater superoleophobic metal film according to an embodiment of the present invention.

[0018] like Figure 1 As shown, the method includes the following steps: Step 101: Degrease, clean, and dry the porous metal substrate to remove surface oil and impurities, and obtain a pretreated metal substrate.

[0019] Degreasing refers to removing surface grease using cleaning agents, water, or organic solvents (such as acetone or ethanol). Deionized water is typically used for ultrasonic cleaning to remove degreasing agent residue and soluble impurities. Drying removes surface moisture to prevent it from interfering with subsequent activation reactions.

[0020] After these pretreatments, a clean pretreated metal substrate is obtained, creating conditions for subsequent oleophobic layer bonding.

[0021] Step 102: Immerse the pretreated metal substrate in the activation solution and react at a first temperature for a first duration to obtain the activated metal substrate.

[0022] Metals spontaneously form a dense oxide layer in the air. This oxide layer has a low surface activity density, making it difficult to bond directly and firmly with binders.

[0023] The purpose of immersing the pretreated metal substrate in the activation solution for activation is to introduce abundant active groups.

[0024] Step 103: Immerse the activated metal substrate in an acidic alcohol-water mixed solvent, add a binder to the mixed solvent, and react at a second temperature for a second duration.

[0025] The activated metal substrate has a specific surface area that reacts fully with the binder in the reaction solution, forming a molecular layer or sub-monolayer on the metal surface. One end of the layer is tightly connected to the substrate, while the other end has reactive functional groups, awaiting the next reaction.

[0026] The second temperature here can be 0℃-90℃, and the second duration can be 1h-12h.

[0027] Step 104: Adjust the mixed solvent to an alkaline solvent, add a low surface energy compound containing active functional groups, and react at a third temperature for a third time to obtain the reaction product.

[0028] The molecular structure of low surface energy compounds is characterized by having an active functional group at one end that can react with the reaction sites on the surface of the activated metal substrate, and a low surface energy chain segment at the other end.

[0029] An alkaline environment can catalyze the reaction between the reaction sites on the surface of a metal substrate and the active groups on a low surface energy compound, forming stable covalent bonds.

[0030] Ultimately, a multi-layered molecular structure is formed on the metal surface: metal substrate - covalent bonds - linker - covalent bonds - low surface energy compound molecules. The outermost layer consists of low surface energy segments. This structure exhibits superoleophobicity underwater. The principle is that the outermost low surface energy segments preferentially adsorb and bind water molecules in water, forming a continuous and dense hydration layer. This hydration layer acts as a physical barrier, preventing oil droplets from directly contacting the solid surface. Oil droplets must overcome an extremely high energy barrier to displace water molecules and adhere to the surface, thus achieving underwater oleophobicity.

[0031] Step 105: Take out the reaction product, clean it, and dry it at a fourth temperature for a fourth time to obtain a dried product; clean the dried product in an ultrasonic machine and dry it in an oven to obtain an underwater superoleophobic metal film.

[0032] After removing the reaction product and cleaning it, and drying it at the fourth temperature for the fourth time, a small amount of solvent still remains in the pores of the substrate. The dried product is then cleaned in an ultrasonic cleaner for 10-80 minutes and dried in an oven at 60°C. Drying completely evaporates these solvents, promotes the curing of the functional film, and yields a dried finished product.

[0033] This step induces a cross-linking reaction between the low surface energy compound molecules already bonded to the surface, forming a stable three-dimensional molecular network structure on the substrate surface. This cross-linked network is denser and stronger than a simple monolayer, ultimately resulting in a stable underwater superoleophobic metal film that can persistently repel oil droplets underwater.

[0034] As an optional embodiment, the porous metal substrate may be made of any of the following materials, including but not limited to: stainless steel, titanium and titanium alloys, nickel and nickel alloys, copper and copper alloys, magnesium and magnesium alloys, refractory metals and alloys, iron-aluminum alloys, Hastelloy, iron, cobalt, zinc, tin, and lead.

[0035] The modification method described in this solution can be effectively applied to all of the aforementioned metal materials. The process described in this solution has broad material applicability and is not limited to any specific metal.

[0036] As an optional embodiment, the morphology of the porous metal substrate includes, but is not limited to, any of the following morphologies that can form porous metal materials: flat plate, mesh, tubular, membrane, cylindrical, honeycomb, foam, sintered metal fiber felt, gradient composite structure, wire mesh composite structure, and powder fiber composite structure.

[0037] The preparation method described in this scheme employs a liquid-phase impregnation method—immersing the substrate in a reaction solution. This process enables diffusion into the internal channels, achieving uniform modification of the inner and outer surfaces of the porous material.

[0038] Therefore, the preparation process of this scheme has broad morphological applicability, and is especially suitable for complex-shaped porous materials that are difficult to process by other vapor deposition or physical coating methods.

[0039] As an optional embodiment, the first temperature is 15℃-180℃, and the first duration is 2min-240min; the second temperature is 0℃-90℃, and the second duration is 1h-12h.

[0040] The wide range of parameters described above allows operators to make flexible adjustments based on the different materials and shapes of the substrate. At higher temperatures, the activation time can be shortened (e.g., 2 minutes at 180°C), while at lower temperatures, the activation time needs to be extended (e.g., 240 minutes at 15°C). Both factors together determine the degree of activation.

[0041] As an optional embodiment, the pH of the acidic alcohol-water mixed solvent is 2-6, the pH of the alkaline solvent is 8-11, the third temperature is 60℃-200℃, and the third duration is 2h-24h.

[0042] Acidic conditions (pH 2-6) favor the activation of active sites on metal surfaces. Alkaline conditions (pH 8-11) catalyze the grafting reaction between the ends of active sites and low surface energy compounds.

[0043] In addition, higher temperatures can shorten the reaction time (e.g., 2 hours at 200°C), while lower temperatures require longer times (e.g., 24 hours at 60°C). Both factors together determine the grafting density and the integrity of the modified layer.

[0044] As an optional embodiment, the low surface energy compound containing active functional groups includes, but is not limited to, organosilicon compounds with a main chain of -Si-O- structure, long-chain alkanes and their derivatives, fluorinated silanes containing CF bonds, fluorinated organics, fluorinated polymers, and fluorinated compounds.

[0045] This invention is not limited to a specific low surface energy compound; operators can flexibly choose according to performance requirements, cost budgets, and application scenarios.

[0046] As an optional embodiment, the reaction product is cleaned using a solvent, including but not limited to pure water, ethanol, and acetone. The solvent is capable of dissolving non-polar or weakly polar organic matter. Cleaning typically employs immersion followed by ultrasonication or multiple rinsing to ensure that residues in the internal and external pores of the porous material are thoroughly removed.

[0047] As an optional embodiment, the fourth temperature is 50℃-200℃, and the fourth duration is 2h-48h.

[0048] During drying, higher temperatures can shorten the drying time (e.g., 2 hours at 200℃), while lower temperatures require longer drying times (e.g., 48 hours at 50℃). Stepped heating or vacuum drying can be used to avoid damaging the porous structure due to rapid vaporization of moisture or solvents.

[0049] Compared with the prior art, the present invention has the following beneficial effects: (1) Excellent oleophobic properties: The obtained metal film exhibits super oleophobic properties for various oils such as diesel, gasoline and vegetable oil underwater. The underwater oil contact angle is greater than 150°, oil droplets roll off easily, and the anti-oil adhesion performance is significant. It has good self-cleaning performance and is easy to regenerate.

[0050] (2) High bonding strength of the oleophobic functional layer: This invention achieves dual connection through a metal surface activation layer, which forms stable chemical bonds with oleophobic molecules. Compared with the van der Waals forces or mechanical interlocking of traditional physical coatings, this bonding method significantly improves the bonding strength, ensuring the long-term stability of the oleophobic properties. The oleophobic modified sample can still maintain its superoleophobic properties underwater under long-term ultrasound, with an underwater oil contact angle greater than 150°, while also having good wear resistance, and the oleophobicity does not decrease significantly after long-distance friction.

[0051] (3) Wide applicability of substrates: This method is applicable to a variety of metal materials such as stainless steel, aluminum, titanium, nickel and nickel alloys, copper and copper alloys, as well as different structural forms such as flat plate, mesh, tubular, membrane and cylindrical. The prepared metal membrane can be applied to fields such as oil-water separation and self-cleaning filtration.

[0052] Example 1: Underwater superoleophobic modification of stainless steel mesh S1: Take a piece of 316 stainless steel mesh (20μm), and ultrasonically clean it for 20 minutes each with acetone, ethanol and deionized water, then dry it for later use.

[0053] S2: Preparation of Activation Solution: Dilute concentrated sulfuric acid with deionized water at a volume ratio of 1:4, then add 5% hydrogen peroxide (volume fraction) and stir until homogeneous. Immerse the cleaned stainless steel mesh in the acid-washing oxidation solution and react in a 60°C water bath for 1 hour. After removal, rinse thoroughly with plenty of deionized water until neutral, and then dry.

[0054] S3: Place the activated stainless steel mesh into a beaker, add a mixed solvent of ethanol and deionized water (volume ratio 95:5), and adjust the pH to 6.0 with dilute acetic acid.

[0055] S4: Add a certain amount of γ-aminopropyltriethoxysilane to the solution and stir magnetically at room temperature for 1 hour to allow it to fully hydrolyze.

[0056] S5: Adjust the pH of the solution system to 11.

[0057] S6: Add 1H,1H,2H,2H-perfluorodecyltrimethoxysilane to the solution, heat to 70℃, and react for 6 hours.

[0058] S7: After the reaction is complete, the beaker and stainless steel mesh are transferred into a vacuum dryer. After standing for 12 hours, the stainless steel mesh is removed, ultrasonically cleaned with ethanol for 20 minutes, dried at 70°C, and then ultrasonically cleaned with ethanol for 20 minutes and dried at 60°C to obtain the modified stainless steel mesh, i.e., the underwater superoleophobic metal film.

[0059] Figure 2 A scanning electron microscope image of the surface of an untreated stainless steel mesh provided in an embodiment of the present invention; Figure 3 A scanning electron microscope image of the surface of a stainless steel mesh after underwater superoleophobic modification, provided in an embodiment of the present invention.

[0060] like Figure 2 As shown, the stainless steel substrate has a relatively flat surface with only a few small pores, a dense overall structure, and rounded, large metal particles that make up the substrate with smooth surfaces and low roughness.

[0061] like Figure 3As shown, the modification treatment creates a rich, multi-level micro-nano rough porous structure on the surface of the stainless steel mesh. The original smooth and coarse metal grains are transformed into a fine, interwoven, concave-convex skeleton, significantly improving the surface roughness and enabling the material to achieve superoleophobic properties underwater.

[0062] Figure 4 Photographs showing the contact angle between a stainless steel mesh and diesel fuel underwater, provided as an embodiment of the present invention; Figure 5 Photographs showing the contact angle of a stainless steel mesh and gasoline underwater, provided as an embodiment of the present invention; Figure 6 Photographs showing the contact angle of a stainless steel mesh and vegetable oil underwater, provided as an embodiment of the present invention; Figure 7 The underwater contact angle curves of the stainless steel mesh under different friction distances provided in the embodiments of the present invention; Figure 8 The underwater contact angle curves of the stainless steel mesh under different ultrasonic treatment times provided in the embodiments of the present invention are shown.

[0063] like Figures 4-8 As shown in the test results, the modified stainless steel mesh exhibits excellent underwater superoleophobic properties, with contact angles of 156° for diesel, 158° for gasoline, and 162° for vegetable oil. Furthermore, the modified stainless steel mesh demonstrates excellent bonding strength; even after long-distance friction and prolonged ultrasonic treatment, its underwater oil contact angle remains above 150°, showcasing promising prospects for industrial applications.

[0064] In summary, the method for preparing an underwater superoleophobic metal film provided in this embodiment of the invention includes: A pretreated metal substrate is obtained by degreasing, cleaning, and drying to remove surface oil and impurities. The pretreated metal substrate is then immersed in an activation solution and reacted at a first temperature for a first duration to obtain an activated metal substrate. The activated metal substrate is then immersed in an acidic alcohol-water mixed solvent with a binder added, and reacted at a second temperature for a second duration. The mixed solvent is then adjusted to an alkaline state, and a low surface energy compound containing active functional groups is added. The reaction is continued at a third temperature for a third duration to obtain a reaction product. The reaction product is then removed, cleaned, and dried at a fourth temperature for a fourth duration to obtain a dried product. The dried product is then cleaned in an ultrasonic cleaner and dried in an oven to obtain an underwater superoleophobic metal film. This method constructs an activation layer on the metal surface and connects low surface energy molecules to form an underwater superoleophobic functional layer. The material exhibits an underwater oil contact angle exceeding 150°, effectively solving the problem of oil adhesion to metal materials underwater. Simultaneously, the functional layer is firmly bonded to the substrate through a bonding method, significantly improving the mechanical stability and durability of the film.

[0065] It should be noted that, in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.

[0066] The various embodiments in this specification are described in a related manner. Similar or identical parts between embodiments can be referred to mutually. Each embodiment focuses on describing the differences from other embodiments. In particular, the system embodiments are basically similar to the method embodiments, so the description is relatively simple; relevant parts can be referred to the descriptions of the method embodiments.

[0067] The above description is merely a preferred embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention are included within the scope of protection of the present invention.

Claims

1. A method for preparing an underwater superoleophobic metal film, characterized in that, The method includes: The porous metal substrate is degreased, cleaned, and dried to remove surface oil and impurities, resulting in a pretreated metal substrate. The pretreated metal substrate is immersed in an activation solution and reacted at a first temperature for a first time to obtain an activated metal substrate. The activated metal substrate is immersed in an acidic alcohol-water mixed solvent, and a binder is added to the mixed solvent, and the reaction is carried out at a second temperature for a second duration. The mixed solvent was adjusted to alkaline, and a low surface energy compound containing active functional groups was added. The mixture was reacted at a third temperature for a third time to obtain the reaction product. The reaction product is removed, cleaned, and dried at a fourth temperature for a fourth time to obtain a dried product; the dried product is cleaned in an ultrasonic machine and dried in an oven to obtain an underwater superoleophobic metal film.

2. The method according to claim 1, characterized in that, The porous metal substrate may be made of any of the following materials, including but not limited to: stainless steel, titanium and titanium alloys, nickel and nickel alloys, copper and copper alloys, magnesium and magnesium alloys, refractory metals and alloys, iron-aluminum alloys, Hastelloy, iron, cobalt, zinc, tin, and lead.

3. The method according to claim 1, characterized in that, The morphology of the porous metal substrate includes, but is not limited to, any of the following: flat plate, mesh, tubular, membrane, cylindrical, honeycomb, foam, sintered metal fiber felt, gradient composite structure, wire mesh composite structure, and powder fiber composite structure.

4. The method according to claim 1, characterized in that, The first temperature is 15℃-180℃, and the first duration is 2min-240min; the second temperature is 0℃-90℃, and the second duration is 1h-12h.

5. The method according to claim 1, characterized in that, The acidic alcohol-water mixed solvent has a pH of 2-6, the alkaline solvent has a pH of 8-11, the third temperature is 60℃-200℃, and the third duration is 2h-24h.

6. The method according to claim 1, characterized in that, The low surface energy compounds containing active functional groups include, but are not limited to, organosilicon compounds with a main chain of -Si-O- structure, long-chain alkanes and their derivatives, fluorinated silanes containing CF bonds, fluorinated organics, fluorinated polymers, and fluorinated compounds.

7. The method according to claim 1, characterized in that, The reaction product is washed with a solvent, including but not limited to pure water, ethanol, and acetone.

8. The method according to claim 1, characterized in that, The fourth temperature is 50℃-200℃, and the fourth duration is 2h-48h.

Citation Information

Patent Citations

  • Method for preparing copper net with oil-water separation function

    CN107158754A

  • Method for preparing super-hydrophilic / underwater super-oleophobic aluminum net

    CN109758789A

  • High-durability oil-water separation net and preparation method thereof

    CN115889145A