Processing technology for composite wear-resistant layers adapted to high-speed chain links and pins
By using a segmented gradient deposition process and low-temperature heat treatment, a composite wear-resistant layer is formed, which solves the problems of adhesion stability and lubrication performance of high-speed chains under high-speed friction conditions, and achieves high wear resistance and long service life of chain links and pins.
Patent Information
- Application Number
- CN202611320901.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, the wear-resistant layer of high-speed chains has insufficient adhesion stability, hardness and anti-peeling ability under high-speed friction conditions, and poor lubrication performance, which makes the contact pair between the chain links and the pins prone to wear and fatigue failure.
A segmented gradient deposition process is adopted to first form a dense bonding layer, then introduce a silicon carbide support skeleton, gradually introduce a layered solid lubricating phase, and finally form a functional layer. Through low-temperature heat treatment and pre-run-in treatment, a composite wear-resistant layer is formed to ensure the stability of the interface bonding and lubrication performance.
It improves the adhesion stability and hardness of the chain links and pins, reduces friction damage, and extends the service life of high-speed chains.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-speed chain processing technology, specifically to the processing technology of a composite wear-resistant layer adapted to high-speed chain links and pins. Background Technology
[0002] Chains, as commonly used mechanical transmission components, are widely used in vehicle transmission, industrial conveying, power transmission, and high-speed operating equipment. For high-speed chains, the chain links and pins not only need to withstand periodic tensile loads, but also need to repeatedly experience relative sliding friction during high-speed meshing, bending, and rotation. Especially in the hinged contact area between the chain link hole wall and the outer circle of the pin, the contact area is small, the load is concentrated, and the lubricating oil film is easily squeezed out or destroyed. Therefore, this part is usually the key area for chain wear, increased clearance, and fatigue failure.
[0003] In existing technologies, in order to improve the wear resistance of chains, the chain links and pins are often treated by carburizing, quenching, nitriding, phosphating, blackening, nickel plating, chromium plating, or coating with lubricating grease. Among these, heat treatment can improve the hardness of the base material, phosphating and blackening can improve rust prevention and oil retention performance to a certain extent, ordinary plating can improve surface protection, and lubricating grease can reduce the coefficient of friction between the chain links and pins. However, under high-speed operation conditions, the chain links and pin contact pairs experience high friction frequency and large impact loads, and the stability of the lubricating oil film is poor. Although traditional composite coating technology has a solution to increase the coating hardness by adding hard particles such as silicon carbide and alumina, while increasing the content of hard particles and coating hardness, stress concentration is easily generated in the chain during high-speed articulation friction, leading to coating cracking or peeling. If friction is reduced by increasing the content of solid lubricating materials such as molybdenum disulfide, graphite, and boron nitride, the load-bearing capacity of the coating is easily reduced, and it is easily crushed or worn through in high-load contact areas.
[0004] Furthermore, for high-speed chains, the wear-resistant layer not only needs to have high hardness in static tests, but also needs to maintain stable interlayer bonding during actual operation and form a continuous and stable lubricating contact state on the relative moving surfaces of the chain links and pins. If the coating structure lacks a performance transition from the inside to the outside, abrupt interface changes can easily occur between the hard layer and the lubricating layer, thereby affecting the service life of the coating under high-speed friction conditions.
[0005] To address this technical deficiency, a solution is proposed. Summary of the Invention
[0006] The purpose of this invention is to provide a processing technology for a composite wear-resistant layer adapted to high-speed chain links and pins, in order to solve the technical problem that the adhesion stability, hardness, anti-peeling ability and high-speed wear-resistant and friction-reducing performance of the wear-resistant layer of high-speed chain in the prior art need to be further improved.
[0007] The objective of this invention can be achieved through the following technical solution: a processing technology for a composite wear-resistant layer adapted to high-speed chain links and pins, comprising the following steps: S1. The chain links and pins are placed in an alkaline degreasing solution for chemical degreasing, and then subjected to micro-roughening and activation treatment to obtain a pretreated matrix. S2. Place the pretreated substrate in the pre-plating nickel solution to form a nickel bonding transition layer with a thickness of 0.2-0.6 μm on the pretreated substrate to obtain a transition nickel carrier; S3. Place the transition nickel carrier in the chemical plating solution to deposit a particle-free interface locking layer, then add hard particles to the chemical plating solution to deposit a hard bearing skeleton layer, and then add a modified layered solid lubricating phase to the chemical plating solution to deposit a gradient transition layer, thus obtaining the carrier with the bearing layer plating. S4. A solid lubrication functional layer is deposited on the substrate coated with the receiving layer to obtain the coated modified substrate; S5. Heat-treat the coated modified carrier to obtain chain pieces and pins with composite wear-resistant layers. After assembling the chain pieces and pins with composite wear-resistant layers, pre-run them to obtain a high-speed chain.
[0008] Furthermore, the alkaline degreasing solution is prepared by mixing sodium hydroxide, sodium carbonate, sodium phosphate, Span-80, and deionized water in a ratio of 30-40g:20-26g:15-18g:0.3-0.5g:1L. The micro-roughening and activation treatment includes micro-spraying treatment and acid activation treatment. After micro-spraying treatment, the surface roughness of the chain links and pins reaches 0.35-0.45μm. The acid activation treatment is prepared by mixing oleic acid imidazoline and 0.5-0.7mol / L hydrochloric acid in a ratio of 0.5-0.8g:1L to prepare an acid activation solution. The chain links and pins after micro-spraying treatment are immersed in the acid activation solution, ultrasonically treated at room temperature for 30-50s, then washed with deionized water until neutral and dried.
[0009] Furthermore, the pre-plating nickel solution is prepared by mixing nickel chloride and 1.3-1.7 mol / L hydrochloric acid at a ratio of 220-260 g: 1 L. The electroplating deposition temperature for the pre-plating nickel is 25-35℃, and the current density is 5-7 A / dm³. 2 The coating thickness is 0.2-0.6μm.
[0010] Furthermore, the chemical plating solution is prepared by dissolving a mixture of nickel sulfate, sodium hypophosphite, sodium citrate, lactic acid, sodium tungstate, stabilizer, and surface wetting agent in 26-28g:24-26g:16-18g:10-12mL:2-2.5g:1mg:50mg in 1L of deionized water and adjusting the pH to 4.8-5.2.
[0011] Furthermore, the particle-free interface locking layer deposition involves placing the transition nickel support in a chemical plating solution at a temperature of 85-90℃ and performing autocatalytic chemical deposition for 10-15 minutes at a stirring speed of 280-320 r / min to form a particle-free interface locking layer with a thickness of 0.8-1.5 μm on the outside of the nickel-bonded transition layer.
[0012] Furthermore, the hard particles are nano-silicon carbide, the thickness of the hard load-bearing skeleton layer is 2-4 μm, and the thickness of the gradient transition layer is 2-3 μm.
[0013] Furthermore, the modified layered solid lubricating phase is prepared by mixing tungsten disulfide and hexagonal boron nitride to obtain a layered solid; adding the layered solid to a dopamine solution and stirring and dispersing it at room temperature for 2-3 hours; then adding nickel sulfate and stirring for 10-15 minutes, followed by adding sodium hypophosphite and stirring and dispersing it for 80-100 minutes; and finally obtaining the modified layered solid lubricating phase after filtration, washing and drying.
[0014] Furthermore, the weight ratio of tungsten disulfide to hexagonal boron nitride is 2:1, the particle size of tungsten disulfide is 1.0-1.5 μm, and the particle size of hexagonal boron nitride is 0.2-0.8 μm; the ratio of layered solids, dopamine solution, nickel sulfate, and sodium hypophosphite is 1 g:100 mL:0.15 g:0.15 g, and the dopamine solution is an aqueous solution of dopamine hydrochloride with a concentration of 2 g / L and a pH of 8.5.
[0015] Furthermore, the functionalized plating solution is a mixture composed of nickel sulfate, sodium hypophosphite, sodium citrate, lactic acid, sodium tungstate, nano-silicon carbide, layered solid lubricating phase, stabilizer, and surface wetting agent in a ratio of 26-28g:24-26g:18-20g:10-12mL:2.8-3.2g:0.6-1g:5-7g:1mg:100mg, dissolved in 1L of deionized water, and the pH is adjusted to 4.8-5.2; the thickness of the solid lubricating functional layer is 4-6μm.
[0016] Furthermore, the heat treatment temperature is 230-250℃, the heat treatment is carried out under an inert gas atmosphere, and the heat treatment time is 1.5-2h; the pre-run-in speed is 600-800r / min, and the pre-run-in time is 30-50min.
[0017] The present invention has the following beneficial effects: 1. This invention employs segmented gradient deposition, first forming a dense bonding layer to stabilize the interface, then introducing silicon carbide to form a load-bearing skeleton, followed by the gradual introduction of a layered solid lubricating phase to achieve a performance transition from the hard layer to the lubricating layer, and finally forming a functional layer on the outer side mainly for friction reduction. After low-temperature heat treatment and pre-run-in treatment, the density and stability of the coating are further improved. The pre-run-in process promotes the early completion of the break-in on the contact surface between the chain link and the pin, and forms a relatively stable lubricating transfer film, connecting the functions of interface bonding, load bearing, stress buffering and surface friction reduction. This makes it less likely for the chain link and pin to experience coating peeling, local wear and abnormal wear during high-speed operation, effectively extending the service life of high-speed chains.
[0018] 2. This invention also removes oil stains, oxide films, and weak bonding layers from the surfaces of the chain links and pins through alkaline degreasing, micro-spray roughening, and acid activation, while forming a moderately rough micro-uneven structure on the surface. Subsequently, a thin nickel bonding transition layer is formed on the substrate surface through pre-plating nickel. The nickel bonding transition layer is located between the substrate and the composite wear-resistant layer, playing an interface transition and locking role. This makes the subsequent interface locking layer, hard load-bearing skeleton layer, gradient transition synergistic layer, and solid lubrication functional layer less prone to peeling, cracking, or flaking under high-speed alternating friction and impact loads, thereby improving the adhesion stability and service reliability of the composite wear-resistant layer.
[0019] 3. This invention also modifies the surface of the layered solid lubricating phases of molybdenum disulfide and hexagonal boron nitride with dopamine to form an adhesive coating layer on their surface. Furthermore, nickel and phosphorus components are introduced to improve the dispersibility of the layered solid lubricating phases in the electroless plating solution and their compatibility with the coating. Nano-silicon carbide is introduced as a hard reinforcing phase into the hard load-bearing skeleton layer. Nano-silicon carbide mainly provides hard support, resists indentation, and resists abrasive wear. The layered solid lubricating phases of molybdenum disulfide and hexagonal boron nitride mainly provide shear resistance, reduce friction, and reduce adhesive wear. This results in a composite coating structure that combines a hard load-bearing skeleton with solid lubricating components. This avoids the problems of frictional heating and brittle spalling caused by simply increasing hardness, and insufficient load-bearing capacity caused by simply adding a lubricating phase, thus achieving a synergistic balance between increased hardness and reduced wear. Detailed Implementation
[0020] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0021] In this invention, the lubricating oil is a commercially available product, brand name Great Wall, model name SHT-600; In this invention, the nano-silicon carbide is a commercially available product with a particle size of 20-50 nm and an effective ingredient content of 99.9%. In this invention, the chain links and pins are chain link substrates and pin substrates that have undergone forming, basic heat treatment and surface activation treatment.
[0022] Example 1 This embodiment provides a processing technology for a composite wear-resistant layer adapted to high-speed chain links and pins, including the following steps: Step 1: Matrix Pretreatment Sodium hydroxide, sodium carbonate, sodium phosphate, Span-80 and deionized water were mixed evenly in a ratio of 30g:20g:15g:0.3g:1L to obtain an alkaline degreasing solution. The alkaline degreasing solution is heated to 70°C. Chain plates and pins are added to the alkaline degreasing solution at a solid-liquid ratio of 1:8. The solution is ultrasonically dispersed for 10 minutes to obtain the degreasing matrix. Alumina particles with a particle size of 10-20μm were used as abrasives. They were mixed with deionized water at a solid-liquid ratio of 1:5 and placed in a shot peening machine. The spraying pressure was set to 0.2MPa to perform micro-spraying treatment on the degreased substrate, so that the surface roughness of the degreased substrate reached 0.35μm, and a roughened substrate was obtained. Oleic acid imidazoline and 0.5 mol / L hydrochloric acid were mixed evenly at a ratio of 0.5 g: 1 L to obtain an acid-activated solution; The roughened matrix was completely immersed in the acid activation solution and ultrasonically dispersed for 30 seconds at room temperature. Then, the roughened matrix was removed from the acid activation solution, washed with deionized water until neutral, and transferred to a drying oven at 70°C to dry to constant weight, thus obtaining the pretreated matrix.
[0023] Step 2: Pre-plating nickel Nickel chloride and 1.3 mol / L hydrochloric acid were mixed evenly at a ratio of 220 g: 1 L to obtain a pre-plating nickel solution; The pretreated substrate was placed in a pre-plating nickel bath at 25°C for electroplating deposition, with a current density of 5 A / dm³. 2 A nickel-bonded transition layer with a thickness of 0.2-0.6 μm is formed on the surface of the pretreated substrate to obtain a transition nickel support.
[0024] Step 3: Preparation of layered solid lubricating phase Tungsten disulfide with a particle size of 1.0-1.5 μm and hexagonal boron nitride with a particle size of 0.2-0.8 μm were mixed evenly at a weight ratio of 2:1 to obtain a layered solid. Dopamine hydrochloride and deionized water were mixed and stirred to dissolve, resulting in a 2 g / L solution. The pH of the solution was adjusted to 8.5 to obtain the dopamine solution. Weigh out 10g of layered solid and 1L of dopamine solution, mix them, and stir and disperse at room temperature for 2h. Add 1.5g of nickel sulfate to the solution and stir for 10min. Add 1.5g of sodium hypophosphite to the solution and stir and disperse for 80min. Filter the solution, wash the filter cake three times with purified water and dry it. Transfer the filter cake to a drying oven at 65℃ and dry it to constant weight to obtain a layered solid lubricating phase.
[0025] Step 4: Gradient Transition Deposition Weigh out: 26g nickel sulfate, 24g sodium hypophosphite, 16g sodium citrate, 10mL lactic acid, 2g sodium tungstate, 1mg thiourea, and 50mg sodium dodecyl sulfate. Mix them thoroughly and dissolve them in 1L of deionized water. Adjust the pH to 4.8 to obtain the chemical plating solution. During the plating process as follows, measure the solution pH every 5 minutes to maintain the solution pH at 4.8±0.2. Nano-silicon carbide and chemical plating solution were mixed and stirred for 30 minutes at a solid-liquid ratio of 1:3 to obtain silicon carbide premix solution; The layered solid lubricating phase and the chemical plating solution were mixed and stirred for 30 minutes at a solid-liquid ratio of 1:2 to obtain a premixed layered solid lubricating phase solution. The transition nickel support was placed in a chemical plating solution and stirred. The stirring speed was set to 280 r / min, and the temperature of the chemical plating solution was raised to 85℃. After self-deposition for 10 min, an interface locking layer with a thickness of 0.8-1.5 μm was formed on the outside of the transition nickel support. Add silicon carbide premix to the solution with a silicon carbide concentration of 2 g / L, and assist in intermittent ultrasonic dispersion. Set the ultrasonic frequency to 30 kHz, sonicate for 20 seconds every 6 min, and deposit for 20 min to form a hard load-bearing skeleton layer with a thickness of 2-4 μm on the outside of the interface locking layer. A layered solid lubricating phase premix was added to the chemical plating solution at a concentration of 1 g / L. After deposition for 15 min, a gradient transition synergistic layer with a thickness of 2-3 μm was formed on the outside of the hard bearing skeleton layer, thus obtaining the substrate for the bearing layer plating.
[0026] Step 5: Functional Layer Deposition Weigh out: 26g nickel sulfate, 24g sodium hypophosphite, 18g sodium citrate, 10mL lactic acid, 2.8g sodium tungstate, 0.6g nano silicon carbide, 5g layered solid lubricating phase, 1mg stabilizer, and 100mg surface wetting agent. Mix and dissolve in 1L deionized water, adjust pH to 4.8 to obtain functionalized plating solution. During the following plating process, measure the solution pH every 5 minutes to maintain the solution pH at 4.8±0.2. The substrate for the substrate coating was placed in a functionalized plating solution and stirred with intermittent ultrasonic dispersion. The stirring speed was set to 160 r / min and the ultrasonic frequency was set to 30 kHz. Ultrasonic dispersion was performed for 20 seconds every 6 minutes. The temperature of the functionalized plating solution was raised to 85℃ and deposition was carried out for 40 minutes. A solid lubricating functional layer with a thickness of 4-6 μm was formed on the outside of the substrate for the substrate coating, thus obtaining the coated modified substrate.
[0027] Step Six: Low-Temperature Heat Treatment and Pre-Run-In The coated modified carrier was placed in a nitrogen-protected atmosphere furnace, heated to 230°C, and held for 1.5 hours. After cooling to room temperature with the furnace, chain pieces and pins with a composite wear-resistant layer were obtained. After applying lubricating oil to the outside, they were assembled into a chain. The speed was set to 600 r / min, and the chain was pre-run for 30 minutes to form a composite wear-resistant layer on the chain pieces and pins, thus obtaining a high-speed chain.
[0028] Example 2 This embodiment provides a processing technology for a composite wear-resistant layer adapted to high-speed chain links and pins, including the following steps: Step 1: Matrix Pretreatment Sodium hydroxide, sodium carbonate, sodium phosphate, Span-80 and deionized water were mixed evenly at a ratio of 35g:23g:16.5g:0.4g:1L to obtain an alkaline degreasing solution. The alkaline degreasing solution was heated to 73°C. Chain plates and pins were added to the alkaline degreasing solution at a solid-liquid ratio of 1:9. The solution was ultrasonically dispersed for 15 minutes to obtain the degreasing matrix. Alumina particles with a particle size of 10-20μm were used as abrasives. They were mixed with deionized water at a solid-liquid ratio of 1:5.5 and placed in a shot peening machine. The blasting pressure was set to 0.25MPa to perform micro-blasting treatment on the degreased substrate, so that the surface roughness of the degreased substrate reached 0.40μm, thus obtaining a roughened substrate. Oleic acid imidazoline and 0.6 mol / L hydrochloric acid were mixed evenly at a ratio of 0.65 g: 1 L to obtain an acid-activated solution; The roughened matrix was completely immersed in the acid activation solution and ultrasonically dispersed for 40 seconds at room temperature. Then, the roughened matrix was removed from the acid activation solution, washed with deionized water until neutral, and transferred to a drying oven at 75°C to dry to constant weight, thus obtaining the pretreated matrix.
[0029] Step 2: Pre-plating nickel Nickel chloride and 1.5 mol / L hydrochloric acid were mixed evenly at a ratio of 240 g: 1 L to obtain a pre-plating nickel solution; The pretreated substrate was placed in a pre-plating nickel bath at 30°C for electroplating deposition, with a current density of 6 A / dm³. 2 A nickel-bonded transition layer with a thickness of 0.2-0.6 μm is formed on the surface of the pretreated substrate to obtain a transition nickel support.
[0030] Step 3: Preparation of layered solid lubricating phase Tungsten disulfide with a particle size of 1.0-1.5 μm and hexagonal boron nitride with a particle size of 0.2-0.8 μm were mixed evenly at a weight ratio of 2:1 to obtain a layered solid. Dopamine hydrochloride and deionized water were mixed and stirred to dissolve, resulting in a 2 g / L solution. The pH of the solution was adjusted to 8.5 to obtain the dopamine solution. Weigh out 10g of layered solid and 1L of dopamine solution, mix them, and stir and disperse at room temperature for 2.5h. Add 1.5g of nickel sulfate to the solution and stir for 13min. Add 1.5g of sodium hypophosphite to the solution and stir and disperse for 90min. Filter the solution, wash the filter cake three times with purified water and dry it. Transfer the filter cake to a drying oven at 70℃ and dry it to constant weight to obtain a layered solid lubricating phase.
[0031] Step 4: Gradient Transition Deposition Weigh out: 27g nickel sulfate, 25g sodium hypophosphite, 17g sodium citrate, 11mL lactic acid, 2.3g sodium tungstate, 1mg thiourea, and 50mg sodium dodecyl sulfate. Mix them thoroughly and dissolve them in 1L of deionized water. Adjust the pH to 5.0 to obtain the chemical plating solution. During the plating process as follows, measure the solution pH every 5 minutes to maintain the solution pH at 5.0±0.2. Nano-silicon carbide and chemical plating solution were mixed and stirred for 40 minutes at a solid-liquid ratio of 1:3 to obtain silicon carbide premix solution; The layered solid lubricating phase and the chemical plating solution were mixed and stirred for 40 minutes at a solid-liquid ratio of 1:2 to obtain a premixed layered solid lubricating phase solution. The transition nickel support was placed in a chemical plating solution and stirred. The stirring speed was set to 300 r / min, and the temperature of the chemical plating solution was raised to 87℃. After self-deposition for 13 min, an interface locking layer with a thickness of 0.8-1.5 μm was formed on the outside of the transition nickel support. Add silicon carbide premix to the solution with a silicon carbide concentration of 2 g / L, and assist in intermittent ultrasonic dispersion. Set the ultrasonic frequency to 40 kHz, sonicate for 30 seconds every 7 min, and deposit for 25 min to form a hard load-bearing skeleton layer with a thickness of 2-4 μm on the outside of the interface locking layer. A layered solid lubricating phase premix was added to the chemical plating solution at a concentration of 1.5 g / L. After deposition for 20 min, a gradient transition synergistic layer with a thickness of 2-3 μm was formed on the outside of the hard bearing skeleton layer, thus obtaining the substrate for the bearing layer plating.
[0032] Step 5: Functional Layer Deposition Weigh out: 27g nickel sulfate, 25g sodium hypophosphite, 19g sodium citrate, 11mL lactic acid, 3.0g sodium tungstate, 0.8g nano silicon carbide, 6g layered solid lubricating phase, 1mg stabilizer, and 100mg surface wetting agent. Mix and dissolve in 1L deionized water, adjust pH to 5.0 to obtain functionalized plating solution. During the following plating process, measure the solution pH every 5 minutes to maintain the solution pH at 5.0±0.2. The substrate for the substrate coating was placed in a functionalized plating solution and stirred with intermittent ultrasonic dispersion. The stirring speed was set to 180 r / min and the ultrasonic frequency was set to 40 kHz. Ultrasonic dispersion was performed for 30 seconds every 7 minutes. The temperature of the functionalized plating solution was raised to 87℃ and deposition was carried out for 50 minutes. A solid lubricating functional layer with a thickness of 4-6 μm was formed on the outside of the substrate for the substrate coating, thus obtaining the coated modified substrate.
[0033] Step Six: Low-Temperature Heat Treatment and Pre-Run-In The coated modified carrier was placed in a nitrogen-protected atmosphere furnace, heated to 240°C, and held for 1.8 hours. After cooling to room temperature with the furnace, chain pieces and pins with a composite wear-resistant layer were obtained. After applying lubricating oil to the outside, they were assembled into a chain. The speed was set to 700 r / min, and the chain was pre-run for 40 minutes to form a composite wear-resistant layer on the chain pieces and pins, thus obtaining a high-speed chain.
[0034] Example 3 This embodiment provides a processing technology for a composite wear-resistant layer adapted to high-speed chain links and pins, including the following steps: Step 1: Matrix Pretreatment Sodium hydroxide, sodium carbonate, sodium phosphate, Span-80 and deionized water were mixed evenly at a ratio of 40g:26g:18g:0.5g:1L to obtain an alkaline degreasing solution. The alkaline degreasing solution was heated to 75°C. Chain plates and pins were added to the alkaline degreasing solution at a solid-liquid ratio of 1:10. The solution was ultrasonically dispersed for 20 minutes to obtain the degreasing matrix. Alumina particles with a particle size of 10-20μm were used as abrasives. They were mixed with deionized water at a solid-liquid ratio of 1:6 and placed in a shot peening machine. The blasting pressure was set to 0.3MPa to perform micro-blasting treatment on the degreased substrate, so that the surface roughness of the degreased substrate reached 0.35-0.45μm, thus obtaining a roughened substrate. Oleic acid imidazoline and 0.7 mol / L hydrochloric acid were mixed evenly at a ratio of 0.8 g: 1 L to obtain an acid-activated solution; The roughened matrix was completely immersed in the acid activation solution and ultrasonically dispersed for 50 seconds at room temperature. Then, the roughened matrix was removed from the acid activation solution, washed with deionized water until neutral, and transferred to a drying oven at 80°C to dry to constant weight, thus obtaining the pretreated matrix.
[0035] Step 2: Pre-plating nickel Nickel chloride and 1.7 mol / L hydrochloric acid were mixed evenly at a ratio of 260 g: 1 L to obtain a pre-plating nickel solution; The pretreated substrate was placed in a pre-plating nickel bath at 35°C for electroplating deposition, with a current density of 7 A / dm³. 2 A nickel-bonded transition layer with a thickness of 0.2-0.6 μm is formed on the surface of the pretreated substrate to obtain a transition nickel support.
[0036] Step 3: Preparation of layered solid lubricating phase Tungsten disulfide with a particle size of 1.0-1.5 μm and hexagonal boron nitride with a particle size of 0.2-0.8 μm were mixed evenly at a weight ratio of 2:1 to obtain a layered solid. Dopamine hydrochloride and deionized water were mixed and stirred to dissolve, resulting in a 2 g / L solution. The pH of the solution was adjusted to 8.5 to obtain the dopamine solution. Weigh out 10g of layered solid and 1L of dopamine solution, mix them, and stir and disperse at room temperature for 3h. Add 1.5g of nickel sulfate to the solution and stir for 15min. Add 1.5g of sodium hypophosphite to the solution and stir and disperse for 100min. Filter the solution, wash the filter cake three times with purified water and dry it. Transfer the filter cake to a drying oven at 75℃ and dry it to constant weight to obtain a layered solid lubricating phase.
[0037] Step 4: Gradient Transition Deposition Weigh out: 28g nickel sulfate, 26g sodium hypophosphite, 18g sodium citrate, 12mL lactic acid, 2.5g sodium tungstate, 1mg thiourea, and 50mg sodium dodecyl sulfate. Mix them thoroughly and dissolve them in 1L of deionized water. Adjust the pH to 5.2 to obtain the chemical plating solution. During the plating process as follows, measure the solution pH every 5 minutes to maintain the solution pH at 5.2±0.2. Nano-silicon carbide and chemical plating solution were mixed and stirred for 50 minutes at a solid-liquid ratio of 1:3 to obtain silicon carbide premix solution; The layered solid lubricating phase and the chemical plating solution were mixed and stirred for 50 min at a solid-liquid ratio of 1:2 to obtain a premixed layered solid lubricating phase solution. The transition nickel support was placed in the electroless plating solution and stirred. The stirring speed was set to 320 r / min, and the temperature of the electroless plating solution was raised to 90℃. After self-deposition for 15 min, an interface locking layer with a thickness of 0.8-1.5 μm was formed on the outside of the transition nickel support. Add silicon carbide premix to the solution with a silicon carbide concentration of 2 g / L, and use intermittent ultrasonic dispersion to assist in the process. Set the ultrasonic frequency to 50 kHz, sonicate for 40 seconds every 8 minutes, and deposit for 30 minutes to form a hard load-bearing skeleton layer with a thickness of 2-4 μm on the outside of the interface locking layer. A layered solid lubricating phase premix was added to the chemical plating solution at a concentration of 2 g / L. After deposition for 25 min, a gradient transition synergistic layer with a thickness of 2-3 μm was formed on the outside of the hard bearing skeleton layer, thus obtaining the substrate for the bearing layer plating.
[0038] Step 5: Functional Layer Deposition Weigh out: 28g nickel sulfate, 26g sodium hypophosphite, 20g sodium citrate, 12mL lactic acid, 3.2g sodium tungstate, 1g nano silicon carbide, 7g layered solid lubricating phase, 1mg stabilizer, and 100mg surface wetting agent. Mix and dissolve in 1L deionized water, adjust pH to 5.2 to obtain functionalized plating solution. During the following plating process, measure the solution pH every 5 minutes to maintain the solution pH at 5.2±0.2. The substrate for the coating layer was placed in a functionalized plating solution and stirred with intermittent ultrasonic dispersion. The stirring speed was set to 200 r / min and the ultrasonic frequency was set to 50 kHz. Ultrasonic dispersion was performed for 40 seconds every 8 minutes. The temperature of the functionalized plating solution was raised to 90℃ and deposition was carried out for 60 minutes. A solid lubricating functional layer with a thickness of 4-6 μm was formed on the outside of the substrate for the coating layer, thus obtaining the coated modified substrate.
[0039] Step Six: Low-Temperature Heat Treatment and Pre-Run-In The coated modified carrier was placed in a nitrogen-protected atmosphere furnace, heated to 250°C, and held for 2 hours. After cooling to room temperature with the furnace, chain pieces and pins with a composite wear-resistant layer were obtained. After applying lubricating oil to the outside, they were assembled into a chain. The speed was set to 800 r / min, and the chain was pre-run for 50 minutes to form a composite wear-resistant layer on the chain pieces and pins, thus obtaining a high-speed chain.
[0040] Comparative Example 1 The difference between this comparative example and Example 3 is that step two is omitted, and the pretreated matrix in step one is used instead of the transition nickel support in step four.
[0041] Comparative Example 2 The difference between this comparative example and Example 3 is that no silicon carbide premix was added in step four.
[0042] Comparative Example 3 The difference between this comparative example and Example 3 is that, in step four, no layered solid lubricating phase premix was added.
[0043] Comparative Example 4 The difference between this comparative example and Example 3 is that the segmented deposition method in step four is cancelled, and instead, nano-silicon carbide and modified layered solid lubricating phase are added to the chemical plating solution at one time for composite co-deposition. The total deposition time and the total thickness of the resulting coating are controlled to be similar to those in Example 3.
[0044] Comparative Example 5 The difference between this comparative example and Example 3 is that step five is omitted.
[0045] Comparative Example 6 The difference between this comparative example and Example 3 is that the pre-run-in step in step six is omitted.
[0046] Performance testing: The thickness of the composite wear-resistant layer of the chain and pin samples with composite wear-resistant layer prepared in Examples 1-3 and Comparative Examples 1-6 was determined according to the standard GB / T 6462-2025 "Measuring the thickness of metal and oxide coatings by microscopy". The thickness value is the average value of the composite wear-resistant layer thickness of at least 10 samples. The adhesion of the composite wear-resistant layer of the chain links and pins prepared in Examples 1-3 and Comparative Examples 1-6 was determined by the scratch-grid test in ASTM B571-2018, "Standard Procedure for Qualitative Adhesion Testing of Metallic Coatings". The Knoop hardness of the composite wear-resistant layer of the chain and pin specimens with composite wear-resistant layer prepared in Examples 1-3 and Comparative Examples 1-6 was determined according to the standard ASTM E384-2022 "Standard Test Method for Microindentation Hardness of Materials". Referring to the standard GB / T 12444-2006 "Test Methods for Wear of Metallic Materials - Test Ring-Block Sliding Wear Test", the test force was set to 200 N, the rotation speed to 1000 r / min, and the time to 60 min. The volume wear of the chain segments of the high-speed chain samples prepared in Examples 1-3 and Comparative Examples 1-6 was measured. The specific test data are shown in Table 1 below.
[0047] Table 1 - Performance Test Data of Samples
[0048]
[0049] Data Analysis: Comparative analysis of the data in Table 1 above shows that the composite wear-resistant layer thickness of the samples prepared in Examples 1-3 reached 10.1-14.2 μm, and the Knoop hardness reached 792-918 kgf / mm. 2 Volumetric wear was reduced to 0.022-0.008 mm. 3 .
[0050] In Comparative Example 1, after the pre-plated nickel layer was removed, the thickness of the composite wear-resistant layer was not much different from that in Example 3, but the adhesion was unsatisfactory, and the volumetric wear increased to 0.041 mm. 3 This indicates that although the nickel bonding transition layer is relatively thin, it plays a crucial role in the bonding between the substrate and the subsequent chemical composite coating, and can reduce the risk of peeling and flaking under high-speed friction.
[0051] Comparative Example 2, in which no silicon carbide premix was added in step four, showed a decrease in Knoop hardness to 742 kgf / mm. 2 Volumetric wear increased to 0.029 mm. 3 This indicates that after nano-silicon carbide participates in the formation of a hard load-bearing skeleton layer, it can significantly improve the load-bearing capacity and abrasive wear resistance of the composite wear-resistant layer.
[0052] Comparative Example 3, in which no layered solid lubricating phase premix was added in step four, showed an increase in Knoop hardness to 948 kgf / mm. 2 The volumetric wear reached 0.021mm. 3 This indicates that simply increasing hardness is not sufficient to meet the frictional conditions of high-speed chains. After the layered solid lubricating phase participates in the formation of a gradient transition synergistic layer, it can reduce the frictional damage of the chain.
[0053] Comparative Example 4 eliminated segmented gradient deposition, and the thickness of the composite wear-resistant layer was close to that of Example 3. However, the adhesion of the composite wear-resistant layer was unsatisfactory, and the Knoop hardness decreased to 826 kgf / mm. 2 Volumetric wear increased to 0.036 mm. 3 This invention does not simply increase the coating thickness, nor does it simply mix silicon carbide and layered solid lubricant phases into the plating solution. Instead, it improves particle distribution, interlayer transition, and anti-stripping performance through a layered structure consisting of an interface locking layer, a hard load-bearing skeleton layer, a gradient transition synergistic layer, and a solid lubricant functional layer.
[0054] Comparative Example 5: With the functional layer deposition removed, the composite wear-resistant layer thickness decreased to 8.7 μm, and the Knoop hardness increased to 982 kgf / mm. 2 Volumetric wear increased to 0.031 mm. 3 This indicates that the outer solid lubrication functional layer can provide lubrication and friction reduction during high-speed friction, enabling the composite wear-resistant layer to have both load-bearing and friction-reducing properties.
[0055] Comparative Example 6, without pre-run-in, had a composite wear-resistant layer thickness and hardness that were basically the same as in Example 3, but the volumetric wear increased to 0.018 mm. 3 This indicates that the pre-run-in treatment does not significantly change the coating thickness and hardness, but it can promote the formation of a stable lubricating contact state or transfer of a lubricating film on the friction pair surfaces of the chain links and pins, thereby further reducing initial wear under high-speed conditions.
[0056] This invention first improves the surface cleanliness and bonding activity of the substrate through alkaline degreasing, micro-spray roughening, and acid activation, and then pre-plats to form a nickel bonding transition layer. Subsequently, it utilizes dopamine to modify the WS2 / h-BN layered solid lubricating phase, and sequentially constructs an interface locking layer, a hard load-bearing skeleton layer, a gradient transition synergistic layer, and an outer solid lubricating functional layer through chemical plating, forming a composite wear-resistant structure with strong bonding, high load-bearing capacity, gradient transition, and low friction lubrication from the inside out. Finally, it undergoes low-temperature heat treatment and pre-run-in treatment to achieve a stable lubricating contact state between the chain links and the pin friction pair surfaces, thereby improving the adhesion stability, hardness, anti-stripping ability, and high-speed wear-resistant and friction-reducing performance of the composite wear-resistant layer, making it suitable for long-life operation of high-speed chains.
[0057] The above description is merely an example and illustration of the structure of the present invention. Those skilled in the art can make various modifications or additions to the specific embodiments described, or use similar methods to replace them, as long as they do not deviate from the structure of the invention or exceed the scope defined in the claims, all of which should fall within the protection scope of the present invention.
[0058] In the description of this specification, references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the invention. In this specification, illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.
[0059] The preferred embodiments of the present invention disclosed above are merely illustrative of the invention. These preferred embodiments do not exhaustively describe all details, nor do they limit the invention to specific implementations. Clearly, many modifications and variations can be made based on the content of this specification. This specification selects and specifically describes these embodiments to better explain the principles and practical applications of the invention, thereby enabling those skilled in the art to better understand and utilize the invention. The invention is limited only by the claims and their full scope and equivalents.
Claims
1. A processing technology for a composite wear-resistant layer adapted to high-speed chain links and pins, characterized in that, Includes the following steps: S1. The chain links and pins are placed in an alkaline degreasing solution for chemical degreasing, and then subjected to micro-roughening and activation treatment to obtain a pretreated matrix. S2. Place the pretreated substrate in the pre-plating nickel solution to form a nickel bonding transition layer with a thickness of 0.2-0.6 μm on the pretreated substrate to obtain a transition nickel carrier; S3. Place the transition nickel carrier in the chemical plating solution to deposit a particle-free interface locking layer, then add hard particles to the chemical plating solution to deposit a hard bearing skeleton layer, and then add a modified layered solid lubricating phase to the chemical plating solution to deposit a gradient transition layer, thus obtaining the carrier with the bearing layer plating. S4. A solid lubrication functional layer is deposited on the substrate coated with the receiving layer to obtain the coated modified substrate; S5. Heat-treat the coated modified carrier to obtain chain pieces and pins with composite wear-resistant layers. After assembling the chain pieces and pins with composite wear-resistant layers, pre-run them to obtain a high-speed chain.
2. The processing technology of the composite wear-resistant layer adapted for high-speed chain links and pins according to claim 1, characterized in that, The alkaline degreasing solution is prepared by mixing sodium hydroxide, sodium carbonate, sodium phosphate, Span-80, and deionized water in a ratio of 30-40g:20-26g:15-18g:0.3-0.5g:1L. The micro-roughening and activation treatment includes micro-spraying treatment and acid activation treatment. After micro-spraying treatment, the surface roughness of the chain links and pins reaches 0.35-0.45μm. The acid activation treatment is prepared by mixing oleic acid imidazoline and 0.5-0.7mol / L hydrochloric acid in a ratio of 0.5-0.8g:1L to obtain an acid activation solution. The chain links and pins after micro-spraying treatment are immersed in the acid activation solution, ultrasonically treated at room temperature for 30-50s, then washed with deionized water until neutral and dried.
3. The processing technology of the composite wear-resistant layer adapted for high-speed chain links and pins according to claim 1, characterized in that, The pre-plating nickel solution is prepared by mixing nickel chloride and 1.3-1.7 mol / L hydrochloric acid at a ratio of 220-260 g: 1 L. The electroplating deposition temperature for the pre-plating nickel is 25-35℃, and the current density is 5-7 A / dm³. 2 The coating thickness is 0.2-0.6μm.
4. The processing technology of the composite wear-resistant layer adapted for high-speed chain links and pins according to claim 1, characterized in that, The chemical plating solution is prepared by dissolving a mixture of nickel sulfate, sodium hypophosphite, sodium citrate, lactic acid, sodium tungstate, stabilizer, and surface wetting agent in 26-28g:24-26g:16-18g:10-12mL:2-2.5g:1mg:50mg in 1L of deionized water and adjusting the pH to 4.8-5.
2.
5. The processing technology of the composite wear-resistant layer adapted for high-speed chain links and pins according to claim 1, characterized in that, The particle-free interface locking layer deposition involves placing the transition nickel support in a chemical plating solution at a temperature of 85-90℃ and performing autocatalytic chemical deposition for 10-15 minutes at a stirring speed of 280-320 r / min, thereby forming a particle-free interface locking layer with a thickness of 0.8-1.5 μm on the outside of the nickel-bonded transition layer.
6. The processing technology of the composite wear-resistant layer adapted for high-speed chain links and pins according to claim 1, characterized in that, The hard particles are nano-silicon carbide, the thickness of the hard load-bearing skeleton layer is 2-4 μm, and the thickness of the gradient transition layer is 2-3 μm.
7. The processing technology of the composite wear-resistant layer adapted for high-speed chain links and pins according to claim 1, characterized in that, The modified layered solid lubricating phase is prepared by mixing tungsten disulfide and hexagonal boron nitride to obtain a layered solid; adding the layered solid to a dopamine solution and stirring and dispersing it at room temperature for 2-3 hours; then adding nickel sulfate and stirring for 10-15 minutes, followed by adding sodium hypophosphite and stirring and dispersing it for 80-100 minutes; and finally obtaining the modified layered solid lubricating phase after filtration, washing and drying.
8. The processing technology of the composite wear-resistant layer adapted for high-speed chain links and pins according to claim 7, characterized in that, The weight ratio of tungsten disulfide to hexagonal boron nitride is 2:1, the particle size of tungsten disulfide is 1.0-1.5 μm, and the particle size of hexagonal boron nitride is 0.2-0.8 μm; the ratio of layered solids, dopamine solution, nickel sulfate, and sodium hypophosphite is 1 g:100 mL:0.15 g:0.15 g, and the dopamine solution is an aqueous solution of dopamine hydrochloride with a concentration of 2 g / L and a pH of 8.
5.
9. The processing technology of the composite wear-resistant layer adapted for high-speed chain links and pins according to claim 1, characterized in that, The functional plating solution is a mixture of nickel sulfate, sodium hypophosphite, sodium citrate, lactic acid, sodium tungstate, nano-silicon carbide, layered solid lubricating phase, stabilizer, and surface wetting agent in a ratio of 26-28g:24-26g:18-20g:10-12mL:2.8-3.2g:0.6-1g:5-7g:1mg:100mg, dissolved in 1L of deionized water and adjusted to pH=4.8-5.2; the thickness of the solid lubricating functional layer is 4-6μm.
10. The processing technology of the composite wear-resistant layer adapted for high-speed chain links and pins according to claim 1, characterized in that, The heat treatment temperature is 230-250℃, the heat treatment is carried out under an inert gas atmosphere, and the heat treatment time is 1.5-2h; the pre-run-in speed is 600-800r / min, and the pre-run-in time is 30-50min.