Silicon carbide crystals and their preparation methods
By using SiC powder with rare earth compounds encapsulated in the center and controlling the release of rare earth elements during the growth of silicon carbide crystals, the problems of polymorphic phase transformation and inclusions in traditional methods were solved, and high-quality silicon carbide crystals with single crystal form and low dislocation density were obtained.
Patent Information
- Application Number
- CN202611543522.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-30
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional silicon carbide crystal preparation methods are prone to polymorphic phase transitions and the introduction of heterogeneous polymorphic inclusions, making it difficult to obtain silicon carbide crystals with a single crystal form and high quality.
SiC powder with rare earth compounds encapsulated in the center is used as the raw material for crystal growth. The release and volatilization of rare earth elements are controlled during the crystal growth process to ensure the uniform distribution of rare earth elements at the front of the silicon carbide crystal. Silicon carbide crystals are grown by the PVT method.
This method achieves crystal form uniformity and low dislocation density in silicon carbide crystals, improving crystal quality and stability while reducing phase transitions and defect formation.
Smart Images

Figure CN123108728A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of silicon carbide materials technology, and in particular to silicon carbide crystals and their preparation methods. Background Technology
[0002] Silicon carbide single crystals are currently the most widely used third-generation semiconductor material, possessing excellent properties such as a large bandgap, high saturated electron mobility, strong breakdown field, and high thermal conductivity. As the research and application of silicon carbide devices in power electronics, radio frequency devices, and optoelectronic devices continue to deepen and expand, the quality requirements for silicon carbide materials are also constantly increasing.
[0003] Currently, commercially available SiC single-crystal substrates mainly use 4H-SiC substrates, and their fabrication method is primarily physical vapor transport (PVT). SiC possesses over 200 polymorphs, including 3C, 4H, 6H, and 15R, with extremely small differences in formation energies between these polymorphs. This makes polymorphic phase transitions or the introduction of heteropolymorphic inclusions during crystal growth highly likely. Therefore, traditional methods for preparing silicon carbide crystals still require improvement. Summary of the Invention
[0004] Based on this, one or more embodiments of this application provide a silicon carbide crystal with a single crystal form and low dislocation density, and a method for preparing the same.
[0005] According to a first aspect of the embodiments of this application, a method for preparing silicon carbide crystals is provided, comprising the following steps:
[0006] SiC powder with a first rare earth compound encapsulated in its center is placed in the lower part of the inner cavity of the crystal growth device. A container is placed in the center of the SiC powder with the first rare earth compound encapsulated in its center, and the container contains a second rare earth compound.
[0007] The crystal growth apparatus is heated to grow silicon carbide crystals;
[0008] The first rare earth compound and the second rare earth compound each independently include Sc2O3, CeO2, La2O3, and Pr6O. 11 One or more of Nd2O3, Y2O3, LaSi2, PrSi2, NdSi2, ScSi2, YSi2 and CeSi2.
[0009] In some embodiments, the amount of the second rare earth compound added is 0.1wt% to 0.3wt% based on the mass of the SiC powder centrally encapsulating the first rare earth compound.
[0010] In some embodiments, the method for preparing the SiC powder with the first rare earth compound encapsulated in its center includes the following steps:
[0011] Carbon powder and silicon powder are mixed to obtain the first mixture;
[0012] The first mixture is subjected to a first heat treatment to obtain β-phase SiC powder;
[0013] The first mixture is mixed with the first rare earth compound to obtain the second mixture;
[0014] The second mixture is subjected to a second heat treatment to obtain α-phase SiC powder;
[0015] The α-phase SiC powder and the β-phase SiC powder are mixed to obtain a third mixture;
[0016] The third mixture is subjected to a third heat treatment to obtain SiC powder with a first rare earth compound encapsulated in its center.
[0017] In some embodiments, the preparation method satisfies at least one of the following conditions:
[0018] (1) The heating rate of the first heating treatment is 75℃ / h~80℃ / h;
[0019] (2) The temperature of the first heat treatment is 1900℃~2000℃;
[0020] (3) The protective gas for the first heat treatment includes argon;
[0021] (4) The reaction pressure of the first heat treatment is 14000 Pa to 16000 Pa;
[0022] (5) The heat treatment holding time for the first heat treatment is 24h~26h;
[0023] (6) The particle size of the β-phase SiC powder is 0.25 mm to 0.8 mm;
[0024] (7) The particle size of the α-phase SiC powder is 0.425 mm to 2 mm;
[0025] (8) The particle size of the SiC powder containing the first rare earth compound in the center is 0.85 mm to 4 mm;
[0026] (9) In the second mixture, based on the mass of the second mixture, the amount of the first rare earth compound added is 0.05wt%~8wt%;
[0027] (10) In the third mixture, the mass ratio of the α-phase SiC powder to the β-phase SiC powder is (6~8):(1~2).
[0028] In some embodiments, the second heat treatment includes the following steps: placing the second mixture in a reaction apparatus, raising the bottom temperature and top temperature of the reaction apparatus to 1850°C~1950°C, and holding the temperature for 24h~26h;
[0029] Then, the bottom temperature of the reaction device is raised to 2290℃~2300℃ and the top temperature of the reaction device is raised to 2090℃~2110℃, and kept at this temperature for 24h~26h.
[0030] In some embodiments, the third heating treatment includes the following steps: placing the third mixture at the bottom of the reaction device, raising the bottom temperature of the reaction device to 2300℃~2350℃, raising the top temperature of the reaction device to 2180℃~2200℃, and holding the temperature for 24h~26h.
[0031] In some embodiments, before placing the third mixture at the bottom of the reaction apparatus, the step further includes placing β-phase SiC powder below the third mixture.
[0032] In some embodiments, the mass ratio of the third mixture to the β-phase SiC powder is (8~9):(1~2).
[0033] In some embodiments, the preparation method satisfies at least one of the following conditions:
[0034] (1) Seed crystals for growing silicon carbide crystals include 4H-SiC;
[0035] (2) The growth temperature of silicon carbide crystal is 2150℃~2250℃;
[0036] (3) The growth rate of silicon carbide crystals is 150 μm / h to 250 μm / h;
[0037] (4) In the step of growing silicon carbide crystal, the distance between the seed crystal and the SiC powder with the first rare earth compound in the center is 50mm~100mm.
[0038] According to a second aspect of the embodiments of this application, a silicon carbide crystal is provided, which is prepared by the above-described preparation method.
[0039] Compared with traditional technologies, this application has the following advantages:
[0040] In the method for preparing silicon carbide crystals disclosed in this application, SiC powder with a first rare earth compound centrally encapsulated is used as the crystal growth raw material, and a container holding a second rare earth compound is placed at the center of the powder. During the early stage of crystal growth, the rare earth compound in the container is gradually released, and the rare earth elements are incorporated into the leading edge of the resulting silicon carbide crystal. During the middle and later stages of crystal growth, the SiC on the outer surface of the SiC powder with the first rare earth compound centrally encapsulated gradually sublimates and decomposes, exposing and volatilizing the first rare earth compound to the surface of the seed crystal. This maintains a relatively stable concentration of rare earth elements required for crystal growth in the crystal growth apparatus, thereby ensuring a uniform distribution of rare earth elements along the thickness direction at the leading edge of the silicon carbide crystal. This allows for stable growth of the silicon carbide crystal, reducing the likelihood of phase transitions and stacking faults, thus obtaining a high-quality crystal with a single crystal form. Attached Figure Description
[0041] To more clearly illustrate the technical solutions of the specific embodiments of this application, the drawings used in the description of the specific embodiments will be briefly introduced below. Obviously, the drawings described below are some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings.
[0042] Figure 1 This is a schematic diagram showing the location of the raw materials used in Example 1 of this application.
[0043] Explanation of reference numerals in the attached figures: 10, graphite crucible; 20, graphite jar; 30, CeSi2 powder; 40, SiC powder with a first rare earth compound encapsulated in the center. Detailed Implementation
[0044] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, a detailed description of specific embodiments of this application is provided. Many specific details are set forth in the following description to provide a thorough understanding of this application. However, this application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of this application. Therefore, this application is not limited to the specific embodiments disclosed below.
[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. Unless otherwise specifically stated, all raw materials, reagents, instruments, and equipment used in this application are commercially available or can be prepared by existing methods.
[0046] In this application, the terms "multiple", "various", "multiple times", "multi-dimensional", etc., unless otherwise specified, refer to a quantity greater than or equal to 2. For example, "one or more" means one or more than or equal to two.
[0047] The terms “combinations of,” “any combination of,” and “any combination of” used in this article include all suitable combinations of any two or more of the listed items.
[0048] In this document, the term "suitable" as used in phrases such as "suitable combination," "suitable method," and "any suitable method" refers to the ability to implement the technical solution of this application, solve the technical problem of this application, and achieve the expected technical effect of this application.
[0049] In this application, the terms "first aspect," "second aspect," "third aspect," "fourth aspect," etc., are used for descriptive purposes only and should not be construed as indicating or implying relative importance or quantity, nor should they be construed as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first," "second," "third," "fourth," etc., serve only as a non-exhaustive enumeration and should be understood not to constitute a closed limitation on quantity.
[0050] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.
[0051] In this application, numerical intervals (i.e., numerical ranges) are involved. Unless otherwise specified, the selected numerical distributions within the aforementioned numerical intervals are considered continuous and include the two endpoints (i.e., the minimum and maximum values) of the numerical range, as well as every value between these two endpoints. Unless otherwise specified, when a numerical interval refers only to integers within that interval, it includes the two endpoint integers of the numerical range, as well as every integer between the two endpoints. In this document, this is equivalent to directly listing every integer. For example, if t is an integer selected from 1 to 10, it means that t is any integer selected from the group of integers consisting of 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10. Furthermore, when multiple ranges are provided to describe features or characteristics, these ranges can be merged. In other words, unless otherwise specified, the ranges disclosed herein should be understood to include any and all subranges to which they are included.
[0052] Unless otherwise specified, the temperature parameters in this application are permitted to be either constant-temperature treatment or variations within a certain temperature range. It should be understood that the constant-temperature treatment allows temperature fluctuations within the precision range of the instrument control, such as ±5℃, ±4℃, ±3℃, ±2℃, or ±1℃.
[0053] In this application, "room temperature" or "normal temperature" generally refers to 4℃~35℃, for example, 20℃±5℃. In some embodiments of this application, "room temperature" or "normal temperature" refers to 10℃~30℃. In some embodiments of this application, "room temperature" or "normal temperature" refers to 20℃~30℃.
[0054] In this application, %(w / w) and wt% both represent weight percentage, %(v / v) refers to volume percentage, and %(w / v) refers to mass-volume percentage.
[0055] The traditional doping method is to directly stir and mix rare earth sources and silicon carbide powder evenly. However, in the actual growth process, even if the rare earth sources are evenly distributed in space, there is still uneven distribution in time due to the difference in melting point and sublimation rate between them and silicon carbide powder.
[0056] Some embodiments of this application provide a method for preparing silicon carbide crystals, comprising the following steps:
[0057] SiC powder with a first rare earth compound encapsulated in its center is placed in the lower part of the inner cavity of the crystal growth device. A container is placed in the center of the SiC powder with the first rare earth compound encapsulated in its center, and the container contains a second rare earth compound.
[0058] The crystal growth apparatus is heated to grow silicon carbide crystals;
[0059] The first and second rare earth compounds each independently include Sc2O3, CeO2, La2O3, and Pr6O. 11 One or more of Nd2O3, Y2O3, LaSi2, PrSi2, NdSi2, ScSi2, YSi2 and CeSi2.
[0060] Furthermore, the first rare earth compound and the second rare earth compound each independently include one or more of LaSi2, PrSi2, NdSi2, ScSi2, YSi2 and CeSi2.
[0061] Furthermore, both the first and second rare earth compounds are CeSi2.
[0062] During the silicon carbide crystal growth process, rare earth elements can be uniformly doped onto the leading edge of the silicon carbide crystal. Rare earth elements can increase the growth rate of silicon carbide crystals, make the crystal growth direction more singular and regular, and reduce the generation of impurities and defects in the crystal, thereby producing silicon carbide crystals with a singular crystal form and higher quality.
[0063] In some embodiments, the first rare earth compound and the second rare earth compound are of the same type.
[0064] In the above preparation method, in the early stage of silicon carbide crystal growth, the second rare earth compound in the container is gradually released, and the rare earth elements therein are doped into the leading edge of the silicon carbide crystal. In the middle and late stages of crystal growth, the SiC on the outer part of the SiC powder that is centrally wrapped with the first rare earth compound gradually sublimates and decomposes, so that the centrally wrapped first rare earth compound is gradually exposed and volatilized to the surface of the seed crystal, so that the concentration of rare earth elements required for crystal growth in the reaction device is kept relatively stable, thereby making the rare earth elements in the leading edge of the silicon carbide crystal uniformly distributed in the thickness direction; thus improving the problem of phase transition that is prone to occur in the middle and late stages of crystal growth.
[0065] Understandably, the container could be made of a material such as graphite, which has certain pores when heated to high temperatures, allowing the second rare earth compound contained within to slowly seep out from these pores.
[0066] In some embodiments, the container used in this application is a semi-enclosed container; further, the semi-enclosed container uses a lid without threads.
[0067] In some embodiments, the amount of the second rare earth compound added is 0.1wt% to 0.3wt%, based on the mass of the SiC powder centrally encapsulating the first rare earth compound.
[0068] As an example, based on the mass of SiC powder containing the first rare earth compound, the amount of the second rare earth compound added can be 0.1wt%, 0.2wt%, 0.3wt%, or any value within the range of any two of the above points.
[0069] In some embodiments, the method for preparing SiC powder centrally encapsulating a first rare earth compound includes the following steps:
[0070] Carbon powder and silicon powder are mixed to obtain the first mixture;
[0071] The first mixture was subjected to a first heat treatment to obtain β-phase SiC powder.
[0072] The first mixture is mixed with the first rare earth compound to obtain the second mixture;
[0073] The second mixture was subjected to a second heat treatment to obtain α-phase SiC powder;
[0074] A third mixture was prepared by mixing α-phase SiC powder and β-phase SiC powder.
[0075] The third mixture is subjected to a third heat treatment to obtain SiC powder with the first rare earth compound encapsulated in its center.
[0076] It is understandable that in the step of preparing the second mixture by mixing the first mixture with the first rare earth compound, the first rare earth compound acts as a nucleating agent, enabling the carbon powder and silicon powder to grow SiC crystals around the nucleating agent during the synthesis process.
[0077] In some embodiments, the molar ratio of carbon powder to silicon powder is (0.8~1.2):(0.8~1.2).
[0078] Furthermore, the molar ratio of carbon powder to silicon powder is 1:1.
[0079] In some embodiments, the heating rate of the first heating treatment is 75°C / h to 80°C / h.
[0080] As an example, the heating rate of the first heating treatment can be 75℃ / h, 76℃ / h, 77℃ / h, 78℃ / h, 79℃ / h, 80℃ / h, or any value within the range formed by any two of the above points.
[0081] In some embodiments, the temperature of the first heat treatment is 1900°C to 2000°C.
[0082] As an example, the temperature of the first heating treatment can be 1900℃, 1910℃, 1920℃, 1930℃, 1940℃, 1950℃, 1960℃, 1970℃, 1980℃, 1990℃, 2000℃, or any value within the range formed by any two of the above points.
[0083] In some embodiments, the protective gas for the first heat treatment includes argon.
[0084] In some embodiments, the reaction pressure of the first heat treatment is 14000 Pa to 16000 Pa.
[0085] As an example, the reaction pressure of the first heat treatment can be 14000Pa, 14500Pa, 15000Pa, 15500Pa, 16000Pa, or any value within the range formed by any two of the above points.
[0086] In some embodiments, the holding time for the first heat treatment is 24h to 26h.
[0087] As an example, the holding time for the first heat treatment can be 24h, 25h, 26h, or any value within the range formed by any two of the above points.
[0088] In some embodiments, the amount of the first rare earth compound added in the second mixture is 0.05wt% to 8wt% based on the mass of the second mixture.
[0089] As an example, in the second mixture, based on the mass of the second mixture, the amount of the first rare earth compound added can be 0.05wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, 0.5wt%, 0.55wt%, 0.6wt%, 0.65wt%, 0.7wt%, 0.75wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt%, 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, or any value within the range formed by any two of the above points.
[0090] Furthermore, in the second mixture, the amount of the first rare earth compound added is 1wt% to 2wt% based on the mass of the second mixture.
[0091] In some embodiments, the mass ratio of α-phase SiC powder to β-phase SiC powder in the third mixture is (6~8):(1~2).
[0092] As an example, in the third mixture, the mass ratio of α-phase SiC powder to β-phase SiC powder can be 6:1, 6:2, 7:1, 7:2, 8:1, 8:2, or any value within the range of any two of the above ratios.
[0093] In some embodiments, the second heating treatment includes the following steps: placing the second mixture in a reaction apparatus, raising the bottom temperature and top temperature of the reaction apparatus to 1850°C~1950°C, and holding the temperature for 24h~26h;
[0094] Then, the temperature at the bottom of the reaction apparatus is raised to 2290℃~2300℃ and the temperature at the top of the reaction apparatus is raised to 2090℃~2110℃, and kept at these temperatures for 24h~26h.
[0095] In some embodiments, the reaction pressure of the first stage of the second heat treatment is 4800 Pa to 5200 Pa.
[0096] Furthermore, the reaction pressure of the first stage of the second heat treatment is 5000 Pa.
[0097] As an example, in the first stage of the second heating treatment, the bottom temperature and top temperature of the reaction device can be 1850℃, 1860℃, 1870℃, 1880℃, 1890℃, 1900℃, 1910℃, 1920℃, 1930℃, 1940℃, 1950℃, or any value within the range formed by any two of the above points.
[0098] As an example, the holding time in the first stage of the second heat treatment can be 24h, 25h, 26h, or any value within the range formed by any two of the above points.
[0099] As an example, in the second stage of the second heating treatment, the bottom temperature of the reaction device can be 2290℃, 2291℃, 2292℃, 2293℃, 2294℃, 2295℃, 2296℃, 2297℃, 2298℃, 2299℃, 2300℃, or any value within the range formed by any two of the above points.
[0100] As an example, in the second stage of the second heat treatment, the top temperature of the reaction device can be 2090℃, 2091℃, 2092℃, 2093℃, 2094℃, 2095℃, 2096℃, 2097℃, 2098℃, 2099℃, 2100℃, 2101℃, 2102℃, 2103℃, 2104℃, 2105℃, 2106℃, 2107℃, 2108℃, 2109℃, 2110℃, or any value within the range formed by any two of the above points.
[0101] As an example, the holding time in the second stage of the second heat treatment can be 24h, 25h, 26h, or any value within the range formed by any two of the above points.
[0102] In some embodiments, the reaction pressure of the second stage of the second heat treatment is 45 Pa to 55 Pa.
[0103] Furthermore, the reaction pressure of the second stage of the second heat treatment is 50 Pa.
[0104] In some embodiments, the protective atmosphere for the second heat treatment includes an argon atmosphere.
[0105] In the first stage of the second heat treatment, holding the temperature at a relatively low temperature allows carbon powder and silicon powder to fully react and synthesize silicon carbide in the β phase. In the second stage of the second heat treatment, continuing to raise the temperature allows silicon carbide particles to grow and transform into the α phase (SiC particles can grow when the pressure is low (50 Pa) and the temperature difference between the top and bottom of the raw material is >100 °C. This is because the temperature difference creates buoyancy in the gas, which is transported towards the lower temperature. Low pressure is also conducive to gas transport. If the pressure is high, other transport resistances are blocked, which is not conducive to the growth of the raw material).
[0106] It should be noted that if the bottom temperature in the second stage is too high, the first rare earth compound may sublimate too quickly, thus increasing the difficulty of encapsulation. Furthermore, the α-phase SiC powder obtained after the second heat treatment contains the first rare earth compound, with some of it encapsulated by the α-phase SiC powder, while the remaining portion remains exposed.
[0107] In some embodiments, the third heating treatment includes the following steps: placing the third mixture at the bottom of the reaction device, raising the temperature of the bottom of the reaction device to 2300°C~2350°C, raising the temperature of the top of the reaction device to 2180°C~2200°C, and holding the temperature for 24h~26h.
[0108] As an example, the bottom temperature of the third heating treatment can be 2300℃, 2305℃, 2310℃, 2315℃, 2320℃, 2325℃, 2330℃, 2335℃, 2340℃, 2345℃, 2350℃, or any value within the range formed by any two of the above point values.
[0109] As an example, the top temperature of the third heating treatment can be 2180℃, 2181℃, 2182℃, 2183℃, 2184℃, 2185℃, 2186℃, 2187℃, 2188℃, 2189℃, 2190℃, 2191℃, 2192℃, 2193℃, 2194℃, 2195℃, 2196℃, 2197℃, 2198℃, 2199℃, 2200℃, or any value within the range formed by any two of the above points.
[0110] As an example, the holding time for the third heat treatment can be 24h, 25h, 26h, or any value within the range formed by any two of the above points.
[0111] In some embodiments, the protective atmosphere for the third heat treatment includes an argon atmosphere.
[0112] In some embodiments, the reaction pressure of the third heat treatment is 4800 Pa to 5200 Pa.
[0113] Furthermore, the reaction pressure of the third heat treatment is 5000 Pa.
[0114] In some embodiments, the particle size of the β-phase SiC powder is 0.25 mm to 0.8 mm.
[0115] As an example, the particle size of β-phase SiC powder can be 0.25 mm, 0.3 mm, 0.35 mm, 0.4 mm, 0.45 mm, 0.5 mm, 0.55 mm, 0.6 mm, 0.65 mm, 0.7 mm, 0.75 mm, 0.8 mm, or any value within the range formed by any two of the above point values.
[0116] In some embodiments, the particle size of the α-phase SiC powder is 0.425 mm to 2 mm.
[0117] As an example, the particle size of α-phase SiC powder can be 0.425 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, or 2.0 mm, or any value within the range formed by any two of the above values.
[0118] It is understandable that the third mixture contains β-phase SiC powder with relatively small particle size and α-phase SiC powder with relatively large particle size. Similar to the Ostwald ripening principle, the small-particle-size β-phase SiC powder has a high specific surface energy and is thermodynamically unstable, making it easy to sublimate during the third heat treatment. On the other hand, the large-particle-size α-phase SiC powder is stable and continues to grow during the third heat treatment, resulting in a decrease in total surface area and a reduction in the total energy of the system.
[0119] In some embodiments, before placing the third mixture at the bottom of the reaction apparatus, the step further includes placing β-phase SiC powder below the third mixture.
[0120] Understandably, the bottom temperature of the reaction device is relatively higher during the third heating process. During the heating process, the β-phase SiC powder placed under the third mixture will all sublimate, and the sublimated gas will be transported to the top where the temperature is relatively lower. During the transport process, the gas molecules will "stick" to the α-phase SiC particles along the way, which will eventually make the SiC particles larger. The α-phase SiC powder is a high-temperature stable phase and is not easy to decompose. This ensures that the first rare earth compound is well encapsulated and will not sublimate prematurely.
[0121] In some embodiments, the mass ratio of the third mixture to the β-phase SiC powder is (8~9):(1~2).
[0122] As an example, the mass ratio of the third mixture to the β-phase SiC powder can be 8:1, 8:1.5, 8:2, 8.5:1, 8.5:1.5, 8.5:2, 9:1, 9:1.5, 9:2, or any value within the range formed by any two of the above points.
[0123] In some embodiments, the particle size of the SiC powder centrally encapsulating the first rare earth compound is 0.85 mm to 4 mm.
[0124] As an example, the particle size of the SiC powder with the first rare earth compound encapsulated in the center can be 0.85 mm, 0.9 mm, 1 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, 2 mm, 2.1 mm, 2.2 mm, 2.3 mm, 2.4 mm, 2.5 mm, 2.6 mm, 2.7 mm, 2.8 mm, 2.9 mm, 3 mm, 3.1 mm, 3.2 mm, 3.3 mm, 3.4 mm, 3.5 mm, 3.6 mm, 3.7 mm, 3.8 mm, 3.9 mm, or 4 mm, or any value within the range formed by any two of the above values.
[0125] It is understandable that by controlling the particle size of the SiC powder containing the first rare earth compound within the above-mentioned range, a more stable and controllable gas phase evaporation rate and a smoother crystal growth interface can be obtained, thereby achieving better crystal quality.
[0126] In some embodiments, the method for growing silicon carbide crystals includes the PVT method.
[0127] In some embodiments, the seed crystal for growing silicon carbide crystals includes 4H-SiC.
[0128] In some embodiments, the growth temperature of the silicon carbide crystal is 2150°C to 2250°C.
[0129] As an example, the growth temperature of silicon carbide crystals can be 2150℃, 2160℃, 2170℃, 2180℃, 2190℃, 2200℃, 2210℃, 2220℃, 2230℃, 2240℃, 2250℃, or any value within the range formed by any two of the above points.
[0130] In some embodiments, the growth rate of silicon carbide crystals is 150 μm / h to 250 μm / h.
[0131] As an example, the growth rate of silicon carbide crystals can be 150 μm / h, 160 μm / h, 170 μm / h, 180 μm / h, 190 μm / h, 200 μm / h, 210 μm / h, 220 μm / h, 230 μm / h, 240 μm / h, 250 μm / h, or any value within the range formed by any two of the above points.
[0132] Understandably, during the growth of silicon carbide crystals, the silicon-rich gases such as Si and Si2C released from the silicon carbide powder have high saturated vapor pressures and high sublimation rates, leaving loose and porous carbon powder and SiC2 layers on the surface of the SiC powder raw material. As the temperature rises, the rare earth compounds encapsulated in the center of the raw material begin to be exposed and decompose and sublimate. Among them, rare earth elements volatilize to the crystal front, increasing the 4H-SiC stacking fault energy and improving the crystal phase transition; non-rare earth elements can react with the loose and porous carbon powder, reducing the generation of free carbon powder and improving the carbon encapsulation defects that occur in the later stages of crystal growth.
[0133] In some embodiments, during the step of growing silicon carbide crystals, the distance between the seed crystal and the SiC powder centrally encapsulating the first rare earth compound is 50 mm to 100 mm.
[0134] As an example, the distance between the seed crystal and the SiC powder that encapsulates the first rare earth compound can be 50mm, 55mm, 60mm, 65mm, 70mm, 75mm, 80mm, 85mm, 90mm, 95mm, 100mm, or any value within the range of any two of the above points.
[0135] Some embodiments of this application also provide a silicon carbide crystal, which is prepared using the above-described preparation method.
[0136] The silicon carbide crystals prepared by the above method have at least the advantages of single crystal form, few phase transitions, and low dislocation density.
[0137] The present application will be further described below with reference to specific embodiments and comparative examples, but these should not be construed as limiting the scope of protection of the present application. Unless otherwise specified, the raw materials involved in the following specific embodiments are all commercially available, the instruments used are all commercially available, and the processes involved are conventionally selected by those skilled in the art unless otherwise specified.
[0138] Example 1
[0139] (1) Weigh 14010g of high-purity silicon powder and 5990g of high-purity carbon powder; wherein, the high-purity carbon powder and high-purity silicon powder are mixed evenly in a molar ratio of 1:1 and the mixture is recorded as the first mixture.
[0140] (2) Take 10 kg of the first mixture and place it in a graphite crucible for the first heating treatment: the top temperature and the bottom temperature are simultaneously raised to 1950℃ at a rate of 20℃ / h, argon atmosphere is used as protective gas, the reaction pressure is controlled at 15000Pa, and the temperature is kept for 25h to obtain β phase SiC powder.
[0141] (3) After the graphite crucible has cooled to room temperature, the β phase SiC powder is crushed and sieved to obtain β phase SiC powder with a particle size between 0.25 mm and 0.8 mm for later use.
[0142] (4) Take 9.85 kg of the first mixture and mix it thoroughly with 0.15 kg of CeSi2. This mixture is called the second mixture.
[0143] (5) The second mixture was placed in a graphite crucible, and the bottom and top temperatures were simultaneously raised to 1900°C. The reaction pressure was 5000 Pa, and the temperature was maintained for 25 h. Then the bottom temperature was raised to 2295°C and the top temperature was raised to 2100°C. Argon was used as a protective gas, the reaction pressure was controlled to 50 Pa, and the temperature was maintained for 25 h to obtain α-phase SiC powder containing CeSi2.
[0144] (6) After the graphite crucible has cooled to room temperature, the α-phase SiC powder containing CeSi2 is crushed and sieved to obtain α-phase SiC powder containing CeSi2 with a particle size between 0.425 mm and 2 mm for later use.
[0145] (7) Mix 7 kg of the above-mentioned α-phase SiC powder containing CeSi2 with 1.5 kg of β-phase SiC powder and record it as the third mixture.
[0146] (8) Take another 1.5 kg of β phase SiC powder and place it at the bottom of the graphite crucible. Then place 8.5 kg of the third mixture on the β phase SiC powder. Raise the temperature of the bottom of the graphite crucible to 2320℃ and the temperature of the top to 2190℃. Use argon atmosphere as protective gas, control the reaction pressure to 5000 Pa, and keep it at the temperature for 25 h to obtain α phase SiC powder with CeSi2 wrapped in the center.
[0147] (9) After the graphite crucible has cooled to room temperature, the above-mentioned α-phase SiC powder with CeSi2 in the center is crushed and sieved to obtain α-phase SiC powder with CeSi2 in the center with a particle size between 0.85 mm and 4 mm for later use.
[0148] (10) The α-phase SiC powder with CeSi2 encapsulated in the center is loaded using the PVT method: as follows Figure 1As shown, α-phase SiC powder (40) with CeSi2 wrapped in the center was layered and filled into the bottom of a graphite crucible (10), and the layers were vibrated to compact them. A high-purity graphite canister (20) containing CeSi2 (30) was buried in the center of the SiC powder pile. The amount of CeSi2 added in the graphite canister was 0.2wt% of the α-phase SiC powder with CeSi2 wrapped in the center. After filling, SiC powder was backfilled to completely cover the canister. A 4H-SiC seed crystal with a C-plane offset of 4° was bonded and fixed to the inside of the crucible cover with a carbon-based adhesive. The C-plane of the seed crystal was facing down, and the gas phase transmission gap between the seed crystal and the upper surface of the powder was controlled to be 80mm. The crystal growth furnace was heated to 2200℃, and argon was used to adjust the pressure and maintain the gas phase stability. The furnace pressure was maintained at 500Pa, and the crystal growth rate was controlled at 200μm / h to grow silicon carbide crystals.
[0149] After the crystal growth furnace cools to room temperature, the crystal is sliced and the phase transition of the crystal in the early, middle and late stages is analyzed.
[0150] Example 2
[0151] The process is basically the same as in Example 1, except that step (4) is different: 9.2 kg of the first mixture and 0.8 kg of CeSi2 are thoroughly mixed and recorded as the second mixture.
[0152] Example 3
[0153] The process is basically the same as in Example 1, except that step (4) is different: 9.95 kg of the first mixture and 0.05 kg of CeSi2 are thoroughly mixed and recorded as the second mixture.
[0154] Example 4
[0155] The process is basically the same as in Example 1, except that step (8) is different: 10 kg of the third mixture is added directly to the graphite crucible; the bottom temperature of the graphite crucible is raised to 2320°C and the top temperature is raised to 2190°C, argon atmosphere is used as protective gas, the reaction pressure is controlled to be 5000 Pa, and the temperature is maintained for 25 h to obtain α phase SiC powder with CeSi2 wrapped in the center.
[0156] Example 5
[0157] It is basically the same as Example 1, except that CeSi2 is replaced with CeO2 in the same mass as in Example 1.
[0158] Example 6
[0159] It is basically the same as Example 1, except that CeSi2 is replaced with Sc2O3 in equal mass in Example 1.
[0160] Comparative Example 1
[0161] The process is basically the same as in Example 1, except that step (4) is different: CeSi2 is not added to the second mixture, that is, CeSi2 is not encapsulated in the SiC raw material for growing silicon carbide crystals.
[0162] The parameters of some steps in the above embodiments and comparative examples are shown in Table 1.
[0163] Table 1
[0164]
[0165] Performance testing
[0166] The number of mid-to-late stage phase transition wafers in the silicon carbide wafers prepared in the above embodiments and comparative examples was statistically analyzed using a UV-PL ultraviolet photoluminescence imager, in accordance with ISO 21820 standard; the dislocation density of the silicon carbide wafers was statistically analyzed using the molten KOH preferred etching method, in accordance with national standard GB / T 41765-2022, and the results are shown in Table 2.
[0167] Table 2
[0168]
[0169] In Table 2, TSD refers to screw dislocation, TED refers to edge dislocation, and BPD refers to base plane dislocation.
[0170] As shown in Table 2, the silicon carbide crystal prepared in Example 1 has fewer phase transition plates and a lower dislocation density, exhibiting excellent performance. In Example 2, the increased rare earth element content resulted in excess rare earth elements being doped into the SiC lattice, leading to a slight increase in the crystal dislocation density. In Example 3, the decreased rare earth element content made it impossible to maintain a uniform rare earth element concentration in the later stages of crystal growth, resulting in increased phase transitions and lattice mismatch between different SiC crystal types, further increasing the crystal dislocation density, but still meeting the application requirements of silicon carbide devices. In Example 4, the absence of β-phase SiC powder at the bottom of the third mixture resulted in the rare earth elements not being well encapsulated by the silicon carbide powder, leading to a slight increase in phase transitions in the later stages of crystal growth, but still meeting the application requirements of silicon carbide devices. In Examples 5 and 6, rare earth oxides were encapsulated inside the raw materials. In the later stages of the reaction, oxygen elements reacted with the carbon powder on the outer layer of the silicon carbide raw materials to generate CO and CO2 gases, which may cause fluctuations in the gas phase composition, thus affecting crystal defects.
[0171] In Comparative Example 1, the silicon carbide powder did not contain rare earth elements. During the middle and later stages of crystal growth, the concentration of rare earth elements decreased, resulting in severe precipitation and a significant increase in dislocation density.
[0172] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0173] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this application should be determined by the appended claims.
Claims
1. A method for preparing silicon carbide crystals, characterized in that, Includes the following steps: SiC powder with a first rare earth compound encapsulated in its center is placed in the lower part of the inner cavity of the crystal growth device. A container is placed in the center of the SiC powder with the first rare earth compound encapsulated in its center, and the container contains a second rare earth compound. The crystal growth apparatus is heated to grow silicon carbide crystals; The first rare earth compound and the second rare earth compound each independently include Sc2O3, CeO2, La2O3, and Pr6O. 11 One or more of Nd2O3, Y2O3, LaSi2, PrSi2, NdSi2, ScSi2, YSi2 and CeSi2.
2. The method for preparing silicon carbide crystals according to claim 1, characterized in that, Based on the mass of the SiC powder containing the first rare earth compound, the amount of the second rare earth compound added is 0.1wt%~0.3wt%.
3. The method for preparing silicon carbide crystals according to claim 1, characterized in that, The method for preparing the SiC powder with a first rare earth compound encapsulated in its center includes the following steps: Carbon powder and silicon powder are mixed to obtain the first mixture; The first mixture is subjected to a first heat treatment to obtain β-phase SiC powder; The first mixture is mixed with the first rare earth compound to obtain the second mixture; The second mixture is subjected to a second heat treatment to obtain α-phase SiC powder; The α-phase SiC powder and the β-phase SiC powder are mixed to obtain a third mixture; The third mixture is subjected to a third heat treatment to obtain SiC powder with a first rare earth compound encapsulated in its center.
4. The method for preparing silicon carbide crystals according to claim 3, characterized in that, The preparation method satisfies at least one of the following conditions: (1) The heating rate of the first heating treatment is 75℃ / h~80℃ / h; (2) The temperature of the first heat treatment is 1900℃~2000℃; (3) The protective gas for the first heat treatment includes argon; (4) The reaction pressure of the first heat treatment is 14000 Pa to 16000 Pa; (5) The heat treatment holding time for the first heat treatment is 24h~26h; (6) The particle size of the β-phase SiC powder is 0.25 mm to 0.8 mm; (7) The particle size of the α-phase SiC powder is 0.425 mm to 2 mm; (8) The particle size of the SiC powder containing the first rare earth compound in the center is 0.85 mm to 4 mm; (9) In the second mixture, based on the mass of the second mixture, the amount of the first rare earth compound added is 0.05wt%~8wt%; (10) In the third mixture, the mass ratio of the α-phase SiC powder to the β-phase SiC powder is (6~8):(1~2).
5. The method for preparing silicon carbide crystals according to any one of claims 3 to 4, characterized in that, The second heat treatment includes the following steps: placing the second mixture in a reaction device, raising the bottom temperature and top temperature of the reaction device to 1850℃~1950℃, and holding the temperature for 24h~26h; Then, the bottom temperature of the reaction device is raised to 2290℃~2300℃ and the top temperature of the reaction device is raised to 2090℃~2110℃, and kept at this temperature for 24h~26h.
6. The method for preparing silicon carbide crystals according to any one of claims 3 to 4, characterized in that, The third heating treatment includes the following steps: placing the third mixture at the bottom of the reaction device, raising the temperature of the bottom of the reaction device to 2300℃~2350℃, raising the temperature of the top of the reaction device to 2180℃~2200℃, and keeping it at that temperature for 24h~26h.
7. The method for preparing silicon carbide crystals according to claim 6, characterized in that, Before placing the third mixture at the bottom of the reaction apparatus, the method further includes the following step: placing β-phase SiC powder below the third mixture.
8. The method for preparing silicon carbide crystals according to claim 7, characterized in that, The mass ratio of the third mixture to the β-phase SiC powder is (8~9):(1~2).
9. The method for preparing silicon carbide crystals according to any one of claims 1 to 4, characterized in that, The preparation method satisfies at least one of the following conditions: (1) Seed crystals for growing silicon carbide crystals include 4H-SiC; (2) The growth temperature of silicon carbide crystal is 2150℃~2250℃; (3) The growth rate of silicon carbide crystals is 150 μm / h to 250 μm / h; (4) In the step of growing silicon carbide crystal, the distance between the seed crystal and the SiC powder with the first rare earth compound in the center is 50mm~100mm.
10. A silicon carbide crystal, characterized in that, It is prepared by any one of claims 1 to 9.