A cubic silicon carbide / monocrystalline silicon composite substrate, its preparation method and application

By growing a cubic silicon carbide layer with micro-nano structures on a single-crystal silicon substrate, the challenges of the crystal quality of the cubic silicon carbide layer and the formation of micro-nano structures are solved, enabling efficient heat dissipation and low-cost composite substrate applications, suitable for heat dissipation packaging of high power density semiconductor devices.

CN123108737APending Publication Date: 2026-11-17CHINA HUBEI LONGZHONG LABORATORY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611287997.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies cannot form micro/nano surface structures that can enhance interfacial heat transfer in situ while ensuring the crystal quality of the cubic silicon carbide layer, thus limiting the application of cubic silicon carbide/monocrystalline silicon composite substrates in the field of heat dissipation.

Method used

By growing a cubic silicon carbide layer with micro-nano structures on a single-crystal silicon substrate, and controlling parameters such as temperature, pressure, and reactive gas flow rate using chemical vapor deposition, the micro-nano structures are formed simultaneously, avoiding additional processing steps. Combined with mature silicon-silicon bonding technology, the bonding difficulty is reduced.

Benefits of technology

This technology enables the in-situ formation of micro/nano structures on the surface of cubic silicon carbide layers, improving interfacial heat transfer capabilities, reducing material and processing costs, enhancing bonding quality and device reliability, and making it suitable for heat dissipation packaging of high power density semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108737A_ABST
    Figure CN123108737A_ABST
Patent Text Reader

Abstract

This invention discloses a cubic silicon carbide / monocrystalline silicon composite substrate, its preparation method, and its applications. The preparation method includes growing a cubic silicon carbide layer with micro / nano structures on one side of a pretreated monocrystalline silicon substrate. This invention avoids using large-size hexagonal silicon carbide wafers as heat dissipation substrates by directly growing a cubic silicon carbide layer on one side of the monocrystalline silicon substrate, thus reducing material costs. By controlling the chemical vapor deposition conditions, this invention can simultaneously form micro / nano structures in situ during the growth of the cubic silicon carbide layer, eliminating the need for additional post-processing, thereby simplifying the process and reducing costs. The composite substrate retains the monocrystalline silicon side as the bonding surface, transforming heterogeneous material bonding into silicon-silicon homogeneous bonding. This fully utilizes mature large-size silicon-silicon bonding technology, significantly reducing bonding difficulty, improving bonding quality and yield, and eliminating thermal stress problems caused by thermal expansion coefficient mismatch, thereby improving the long-term reliability of the device.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of heat dissipation technology for semiconductor devices, and in particular to a cubic silicon carbide / monocrystalline silicon composite substrate, its preparation method, and its application. Background Technology

[0002] Silicon devices are semiconductor electronic devices made primarily of single-crystal silicon. With the continuous improvement of performance and functional requirements in modern electronic devices, the power density of silicon devices is constantly increasing. Under high-power operation, the heat generated by the device is difficult to conduct quickly to the heat dissipation medium, easily leading to an increase in internal temperature, which in turn affects the device's performance and long-term reliability. In existing technologies, a high thermal conductivity heat dissipation substrate, a heat diffusion layer, or a thermal interface material is typically placed on the back of the silicon device to improve its heat dissipation performance. Among these, silicon carbide (SiC) materials have received widespread attention in the fields of semiconductor device heat dissipation and packaging due to their high thermal conductivity, mechanical strength, thermal stability, and chemical stability. Hexagonal SiC, in particular, has relatively mature material preparation and device applications, and has the potential to be used as a component of high thermal conductivity heat dissipation substrates or composite substrates. However, directly using hexagonal SiC wafers as heat dissipation substrates for silicon devices still has the following drawbacks: firstly, the manufacturing cost of hexagonal SiC wafers is high, and the mass production capacity of large-size wafers is still limited. On the other hand, when combining hexagonal silicon carbide wafers with silicon devices or silicon substrates, wafer bonding, metal bonding, welding or other interface connection processes are usually required. Due to the differences between silicon carbide and silicon in terms of lattice structure, coefficient of thermal expansion, elastic modulus and surface chemical properties, problems such as interface stress, warping, local debonding or bonding voids are easily generated during bonding and subsequent heat treatment.

[0003] Cubic silicon carbide (SiC) is the only crystal form that can be directly grown on a silicon substrate and is compatible with existing silicon-based semiconductor processes, offering unique advantages such as low cost and large-size fabrication. By growing a cubic SiC layer on a single-crystal silicon substrate, a cubic SiC / single-crystal silicon composite substrate can be formed. This type of composite substrate utilizes the thermal conductivity of the cubic SiC layer while retaining the single-crystal silicon layer. When subsequently connected to silicon-based devices, silicon-based epitaxial wafers, or silicon-based packaging structures, mature silicon-silicon bonding processes can be used, thereby reducing the process difficulty of traditional SiC-silicon heterobonding and improving the process compatibility and interface reliability of large-size wafer-level packaging. CN 121908885 A discloses a packaging structure based on a silicon-based SiC interposer and its fabrication method. In this scheme, the cubic SiC layer serves as a component of the CoWoS packaging interposer, with its core function being signal interconnection and heat dissipation as an auxiliary function. Due to the high requirements for surface flatness of the interposer, this scheme does not involve the control of the surface morphology of the cubic SiC layer. However, for heat dissipation substrates, in addition to the thermal conductivity of the material itself, the interfacial heat transfer capacity between the substrate and the external heat dissipation medium is also a key factor determining the overall heat dissipation efficiency. Therefore, constructing micro / nano structures on the surface of the heat dissipation substrate to increase the effective heat transfer area or improve the interfacial heat transfer capacity has become a technical direction for improving heat dissipation performance. CN 118888524 A discloses a diamond / single-crystal silicon composite three-dimensional substrate, its preparation method and application. In this scheme, a micro / nano structure is formed by setting multiple protrusions on the surface of the diamond layer to further improve heat dissipation efficiency and performance. However, existing micro / nano structures usually require post-processing such as laser processing, photolithography, plasma etching, machining or chemical etching. The additional micro / nano processing steps not only increase the complexity of the process and manufacturing cost, but may also introduce problems such as surface damage, particle contamination, local stress concentration or poor structural consistency. For silicon carbide materials with high hardness and difficult processing, the above problems are particularly prominent. It can be seen that controlling the surface morphology of the cubic silicon carbide layer to form a micro / nano structure that is conducive to heat transfer has become a potential direction for technical improvement. However, in the field of silicon-based silicon carbide heteroepitaxial growth, existing research typically aims to obtain high-quality epitaxial layers that are flat, dense, and have low defects. To ensure crystal quality, the growth process usually needs to promote the full migration of reactive species on the substrate surface, allowing atoms to enter growth positions with lower energy and more reasonable lattice matching, thereby promoting two-dimensional layered growth or relatively flat step flow growth. While this type of growth control is beneficial for improving the crystallinity of the epitaxial layer, it inhibits the formation of surface micro- and nano-undulation structures. Simply changing the temperature, reaction atmosphere, or supersaturation to induce surface roughening can lead to disordered grain orientation, affecting crystal quality and thus impacting the thermal conductivity and reliability of the cubic silicon carbide layer.

[0004] Therefore, there are still significant challenges in process control to form micro-nano surface structures that can enhance interfacial heat transfer in situ while ensuring the crystal quality of the cubic silicon carbide layer, which limits the further application of cubic silicon carbide / monocrystalline silicon composite substrates in the field of heat dissipation. Summary of the Invention

[0005] The purpose of this invention is to overcome the above-mentioned technical deficiencies and propose a cubic silicon carbide / monocrystalline silicon composite substrate, its preparation method and application, thereby solving the technical problem in the prior art that it is impossible to form micro-nano surface structures that can be used to enhance interfacial heat transfer in situ while ensuring the crystal quality of the cubic silicon carbide layer.

[0006] In a first aspect, the present invention provides a method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate, comprising the following steps: A monocrystalline silicon substrate is provided, and the monocrystalline silicon substrate is cleaned and dried to obtain a pretreated monocrystalline silicon substrate; A cubic silicon carbide layer with micro-nano structures is grown on one side of a pretreated monocrystalline silicon substrate to obtain a cubic silicon carbide / monocrystalline silicon composite substrate.

[0007] In a second aspect, the present invention provides a cubic silicon carbide / monocrystalline silicon composite substrate, which is obtained by the method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate provided in the first aspect of the present invention.

[0008] Thirdly, the present invention provides an application of a cubic silicon carbide / monocrystalline silicon composite substrate, which is used in the heat dissipation structure of silicon-based semiconductor devices.

[0009] Compared with the prior art, the beneficial effects of the present invention include: This invention directly grows a cubic silicon carbide layer on one side of a single-crystal silicon substrate, avoiding the use of large-size hexagonal silicon carbide wafers as heat dissipation substrates, which helps reduce material costs. By controlling the chemical vapor deposition conditions, this invention can simultaneously form micro-nano structures in situ during the growth of the cubic silicon carbide layer, eliminating the need for additional post-processing, thereby simplifying the process and reducing costs. The composite substrate of this invention retains the single-crystal silicon side as the bonding surface, transforming heterogeneous material bonding into silicon-silicon homogeneous bonding, making full use of mature large-size silicon-silicon bonding technology, significantly reducing bonding difficulty, improving bonding quality and yield, while eliminating thermal stress problems caused by thermal expansion coefficient mismatch, and improving the long-term reliability of the device. Attached Figure Description

[0010] Figure 1 This is a schematic diagram of the process flow of one embodiment of the method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate provided by the present invention. Figure 2This is a schematic diagram of the process flow of one embodiment of the method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate provided by the present invention. Figure 3 This is an X-ray diffraction pattern of cubic silicon carbide prepared in Example 1 of this invention; Figure 4 This is a scanning electron microscope image of cubic silicon carbide prepared in Example 1 of the present invention; wherein the magnification is 2000x. Figure 5 This is the X-ray diffraction pattern of cubic silicon carbide prepared in Example 2 of this invention; Figure 6 This is a scanning electron microscope image of cubic silicon carbide prepared in Example 2 of the present invention; wherein the magnification is 5000x. Figure 7 This is the X-ray diffraction pattern of cubic silicon carbide prepared in Example 3 of the present invention; Figure 8 This is a scanning electron microscope image of cubic silicon carbide prepared in Example 3 of the present invention; wherein the magnification is 10000 times. Figure 9 This is the X-ray diffraction pattern of cubic silicon carbide prepared in Example 4 of this invention; Figure 10 This is a scanning electron microscope image of cubic silicon carbide prepared in Example 4 of the present invention; wherein the magnification is 5000x. Figure 11 This is an X-ray diffraction pattern of cubic silicon carbide prepared in Comparative Example 1 of this invention. Figure 12 This is a scanning electron microscope image of cubic silicon carbide prepared in Comparative Example 1 of the present invention; wherein the magnification is 2000x. Figure 13 This is the X-ray diffraction pattern of cubic silicon carbide prepared in Comparative Example 2 of this invention; Figure 14 This is a scanning electron microscope image of cubic silicon carbide prepared in Comparative Example 2 of the present invention; wherein the magnification is 2000x. Detailed Implementation

[0011] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0012] Among the various silicon carbide crystal forms, cubic silicon carbide is the only one that can be directly grown on a silicon substrate. This invention utilizes this characteristic to directly grow a cubic silicon carbide layer with micro / nano structures on a single-crystal silicon substrate, thereby obtaining a cubic silicon carbide / single-crystal silicon composite substrate with high thermal conductivity and tunable surface micro / nano structures. This invention employs a three-step deposition process: carbonization, high-quality deposition, and surface micro / nano structure control. During the surface micro / nano structure control process, by adjusting process parameters such as temperature, pressure, reactive gas flow rate, and deposition time, specific micro / nano structures can be formed in situ on the surface while ensuring the crystal quality of the cubic silicon carbide layer. This avoids subsequent surface micro / nano processing steps such as laser processing, photolithography, or plasma etching. Furthermore, because the composite substrate retains a single-crystal silicon layer, its subsequent connection to silicon-based devices, silicon-based epitaxial wafers, or silicon-based packaging structures can utilize mature silicon-silicon bonding processes, thereby reducing the process difficulty of traditional silicon carbide-silicon bonding and improving the process compatibility and reliability of large-size wafer-level packaging. Based on these principles, this invention is proposed.

[0013] like Figure 1 As shown, in a first aspect, the present invention provides a method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate, comprising the following steps: S1. Provide a single-crystal silicon substrate, and clean and dry the single-crystal silicon substrate to obtain a pretreated single-crystal silicon substrate; S2. A cubic silicon carbide layer with micro-nano structure is grown on one side of the pretreated monocrystalline silicon substrate to obtain a cubic silicon carbide / monocrystalline silicon composite substrate.

[0014] Cubic silicon carbide (SiC) is one of the most compatible crystal forms of SiC with silicon substrates, allowing it to be directly grown on the surface of a single-crystal silicon substrate via chemical vapor deposition (CVD). This invention uses a large-size single-crystal silicon substrate as the support base, directly depositing a cubic SiC layer with micro / nano structures on its surface. The high thermal conductivity of cubic SiC enhances the thermal diffusion capability of the composite substrate. Simultaneously, during deposition, the nucleation density, growth rate, grain size, and crystal orientation of the cubic SiC crystals are controlled by adjusting the deposition temperature, deposition pressure, reactive gas flow rate, carbon-to-silicon ratio, and deposition time. The competitive growth between different grains leads to the formation of specific micro / nano structures on the surface of the cubic SiC layer, such as lotus-shaped, pyramidal, or granular micro / nano structures. These micro / nano structures are formed synchronously with the cubic SiC layer, eliminating the need for additional laser processing, photolithography, or mechanical processing. Furthermore, the composite substrate of this invention retains the single-crystal silicon bonding surface, allowing for the use of mature silicon-to-silicon bonding processes when connecting to silicon-based chips, silicon-based epitaxial wafers, or silicon-based packaging structures. Compared with traditional direct bonding of silicon carbide wafers and silicon wafers, this invention can reduce the difficulty of bonding heterogeneous materials, reduce interface stress and bonding defects, and improve packaging reliability.

[0015] In this invention, in step S1, the single-crystal silicon substrate includes, but is not limited to, […]. <100> , <110> or <111> The crystal orientation of the single-crystal silicon wafer is 6 to 12 inches in size, including but not limited to 6 inches, 8 inches, 12 inches or other sizes, and this invention does not limit this. Single-crystal silicon wafers have mature large-size manufacturing capabilities and can be better matched with existing silicon-based semiconductor manufacturing and packaging lines.

[0016] In this invention, step S1 involves cleaning the single-crystal silicon substrate to remove particles, organic contaminants, metal ion contaminants, and the natural oxide layer from its surface. This invention does not limit the cleaning method; those skilled in the art can select one or more methods based on the actual situation, including but not limited to organic solvent cleaning, RCA cleaning, deionized water rinsing, hydrofluoric acid treatment, and plasma cleaning.

[0017] In this invention, in step S2, a chemical vapor deposition method is used to place the pretreated single-crystal silicon substrate in the process chamber of a chemical vapor deposition equipment, and to deposit and grow a cubic silicon carbide layer with a micro-nano structure on one side surface of the pretreated single-crystal silicon substrate.

[0018] Furthermore, the chemical vapor deposition method includes, but is not limited to, one of atmospheric pressure chemical vapor deposition, low pressure chemical vapor deposition, plasma-enhanced chemical vapor deposition, hot-wall chemical vapor deposition, or metal-organic chemical vapor deposition.

[0019] Furthermore, during the chemical vapor deposition process, silicon-containing reactive gases and carbon-containing reactive gases are introduced into the process chamber, causing the silicon-containing reactive gases and carbon-containing reactive gases to react on one side of the single-crystal silicon substrate and form a cubic silicon carbide layer with micro-nano structures on the surface.

[0020] Furthermore, the silicon-containing reactive gas may include one or more of the following: silane, dichlorosilane, silicon tetrachloride, trichlorosilane, trichloromethylsilane, etc.

[0021] Furthermore, the carbon-containing reactive gases may include one or more of methane, ethane, propane, ethylene, acetylene, etc.

[0022] Furthermore, the reaction atmosphere may also include a carrier gas and / or a diluent gas, wherein the carrier gas and / or diluent gas are, but are not limited to, one or more of hydrogen, argon, helium or nitrogen.

[0023] like Figure 2 As shown, in this invention, step S2 involves growing a cubic silicon carbide layer with a micro / nano structure on one side of the pretreated single-crystal silicon substrate, including: S21. Place the pretreated single-crystal silicon substrate in the process chamber of the chemical vapor deposition equipment; S22. Under the conditions of deposition temperature of 1100~1200℃ and deposition pressure of 80~120 mbar, 10~30 sccm of carbon-containing reactive gas and 80~120 slm of dilution gas are introduced to carbonize the surface of the single crystal silicon substrate for 8~12 minutes to form a carbonization transition layer or initial nucleation layer on one side of the single crystal silicon substrate. S23. Under the conditions of deposition temperature of 1200~1300℃ and deposition pressure of 80~120mbar, 5~10sccm of carbon-containing reactive gas, 80~120slm of dilution gas and 10~30sccm of carrier gas are introduced, and deposition is carried out for 25~35 minutes to form a cubic silicon carbide intermediate layer on one side surface of a single crystal silicon substrate; wherein, the carrier gas carries the silicon source into the process chamber by bubbling, and the temperature of the bubbler is 18~20℃; S24. Under deposition temperatures of 1250~1350℃ and deposition pressures of 100~200 mbar, 10~30 sccm of carbon-containing reactive gas, 80~120 slm of dilution gas, and 30~50 sccm of carrier gas are introduced, and deposition is carried out for 8~12 minutes to form micro-nano structures. Among them, the carrier gas carries the silicon source into the process chamber by bubbling, and the temperature of the bubbler is 18~20℃.

[0024] In this invention, in step S2, the micro / nano structure includes, but is not limited to, lotus-shaped, pyramid-shaped, granular, hill-shaped, island-shaped, nanoforest-like, or composite micro / nano structures. The micro / nano structures of this invention can increase the actual heat transfer area on the surface of the cubic silicon carbide layer and facilitate the spreading and contact of thermal interface materials, coolants, or phase change media on its surface, thereby improving heat dissipation efficiency. The micro / nano structures of this invention are formed simultaneously with the cubic silicon carbide layer, eliminating the need for additional laser processing, photolithography, plasma etching, or mechanical processing.

[0025] In this invention, after S2, the following steps are also included: S3. Thinning treatment is performed on the side of the single-crystal silicon substrate away from the cubic silicon carbide layer.

[0026] In this invention, after forming the cubic silicon carbide layer with micro / nano structures on its surface, the surface of the monocrystalline silicon substrate away from the cubic silicon carbide layer can be thinned according to subsequent packaging or bonding requirements to reduce the thickness of the monocrystalline silicon layer. This thinning process shortens the heat conduction path from the silicon-based semiconductor device to the cubic silicon carbide layer, thereby reducing the overall thermal resistance of the composite substrate. Simultaneously, it provides a flatter monocrystalline silicon surface, which can then serve as a bonding or packaging interface for subsequent applications.

[0027] Furthermore, after the thinning process, the thickness of the single-crystal silicon substrate is 20~50μm. This invention does not limit the method of thinning; those skilled in the art can choose according to the actual situation. For example, the thinning process can employ at least one of mechanical polishing, chemical mechanical polishing, wet etching, dry etching, or a combination thereof.

[0028] In this invention, after S2 or S3, the following is also included: S4. Provide a silicon-based semiconductor structure and connect the silicon-based semiconductor structure to the single-crystal silicon side of the cubic silicon carbide / single-crystal silicon composite substrate.

[0029] Furthermore, silicon-based semiconductor structures include, but are not limited to, one or more of the following: silicon-based devices, silicon-based epitaxial wafers, silicon-based chips, or silicon-based packaging structures.

[0030] Furthermore, the connection method is silicon-silicon bonding, specifically including but not limited to one or more of the following: direct silicon-silicon bonding, plasma-assisted silicon-silicon bonding, metal interlayer silicon-silicon bonding, hydrophilic silicon-silicon bonding, hydrophobic silicon-silicon bonding, low-temperature silicon-silicon bonding, hybrid silicon-silicon bonding, welding, or bonding. Preferably, direct silicon-silicon bonding or plasma-assisted silicon-silicon bonding is used. Since at least one side of the interface involved in the connection is a single-crystal silicon surface, this invention can utilize mature silicon-silicon bonding technology to achieve composite structure connection, avoiding direct heterogeneous bonding between silicon carbide and silicon. This helps reduce bonding difficulty, decrease interface voids, warping, and debonding defects, and improve the interface reliability of the composite heat dissipation structure.

[0031] In a second aspect, the present invention provides a cubic silicon carbide / monocrystalline silicon composite substrate, which is obtained by the method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate provided in the first aspect of the present invention.

[0032] Thirdly, the present invention provides an application of a cubic silicon carbide / monocrystalline silicon composite substrate, which is used in the heat dissipation structure of silicon-based semiconductor devices.

[0033] In this invention, when the aforementioned cubic silicon carbide / monocrystalline silicon composite substrate is used for heat dissipation of silicon-based semiconductor devices, the heat generated by the semiconductor device is first conducted to the monocrystalline silicon layer, then from the monocrystalline silicon layer to the cubic silicon carbide layer, and finally diffused to the external heat dissipation structure through the cubic silicon carbide layer. Because the cubic silicon carbide layer has high thermal conductivity, it can improve the lateral diffusion and longitudinal conduction efficiency of heat. Simultaneously, the micro-nano structures on the surface of the cubic silicon carbide layer can increase its effective contact area with thermal interface materials, coolants, or phase change media, thereby further improving the interface heat transfer capability.

[0034] In this invention, a heat dissipation structure for a silicon-based semiconductor device includes: a silicon-based semiconductor device and the aforementioned cubic silicon carbide / monocrystalline silicon composite substrate; wherein the silicon-based semiconductor device is disposed on the side of the cubic silicon carbide / monocrystalline silicon composite substrate away from the cubic silicon carbide layer.

[0035] In this invention, the cubic silicon carbide layer is located on the side away from the semiconductor device to conduct the heat generated during the operation of the semiconductor device to the external heat dissipation structure.

[0036] In this invention, silicon-based semiconductor devices include, but are not limited to, silicon-based semiconductor chips, specifically including, but not limited to, GPU chips, CPU chips, AI acceleration chips, power device chips, radio frequency chips, memory chips, or other silicon-based semiconductor chips.

[0037] In this invention, the side of the cubic silicon carbide layer furthest from the single-crystal silicon substrate is connected to a thermal interface material, a metal heat sink, a heat sink, a heat spreader, a liquid cooling plate, or a phase change heat dissipation structure. The micro / nano structures on the surface of the cubic silicon carbide layer can increase its contact area with the thermal interface material or cooling medium, and improve adhesion and heat transfer efficiency.

[0038] Example 1 (1) Pretreatment of single-crystal silicon substrate: 6-inch substrate is provided <100> Orient the monocrystalline silicon substrate, and then perform RCA cleaning and drying on the monocrystalline silicon substrate to obtain the pretreated monocrystalline silicon substrate.

[0039] (2) Growth of a cubic silicon carbide layer with micro-nano structure on the surface: Cubic silicon carbide is epitaxially grown on one side of the pretreated single crystal silicon substrate by chemical vapor deposition. Specifically, trichlorosilane is used as the silicon source, and the carrier gas H2 is used to bring the silicon source into the process chamber by bubbling. The bubbler temperature is 19°C, ethylene is used as the carbon source, and H2 is used as the dilution gas. The entire deposition process consists of three steps. First, at a deposition temperature of 1150℃ and a deposition pressure of 100 mbar, ethylene at 20 sccm and H2 at 100 slm are introduced separately as dilution gases to carbonize the surface of the monocrystalline silicon substrate for 10 minutes, forming a carbonization transition layer or initial nucleation layer on the substrate surface. Then, the deposition temperature is increased to 1250℃, the ethylene flow rate is adjusted to 7 sccm, and the H2 flow rate is 20 sccm, with deposition lasting 30 minutes to form a well-crystallized cubic silicon carbide intermediate layer on one side of the monocrystalline silicon substrate. Finally, the deposition temperature and pressure are adjusted to 1300℃ and 150 mbar, respectively, and the ethylene and H2 flow rates are adjusted to 20 sccm and 40 sccm, respectively, with deposition lasting 10 minutes to control the surface micro / nano structure. Throughout the process, unless otherwise specified, the deposition pressure and dilution gas flow rates remain consistent with the first step, at 100 mbar and 100 slm, respectively.

[0040] The aforementioned cubic silicon carbide layer and the monocrystalline silicon substrate together constitute a cubic silicon carbide / monocrystalline silicon composite substrate. X-ray diffraction (XRD) analysis was performed on the resulting cubic silicon carbide layer, and its XRD pattern is shown below. Figure 3 As shown. By Figure 3 It can be seen that the above-mentioned cubic silicon carbide layer has good crystal quality; the surface of the above-mentioned cubic silicon carbide layer away from the single crystal silicon substrate was observed by scanning electron microscopy, and the scanning electron microscopy image is shown below. Figure 4 As shown. By Figure 4 It can be seen that a lotus-shaped micro / nano structure is formed on the surface of the cubic silicon carbide layer.

[0041] (3) Thinning of the back side of the single crystal silicon substrate: After forming the cubic silicon carbide layer, the surface of the single crystal silicon substrate away from the cubic silicon carbide layer is thinned by a combination of mechanical grinding and chemical mechanical polishing, so that the thickness of the single crystal silicon substrate is controlled to about 50 μm.

[0042] (4) Cubic silicon carbide / silicon-silicon wafer bonding. Another monocrystalline silicon wafer is provided, and the monocrystalline silicon wafer is directly bonded to the thinned surface to obtain a cubic silicon carbide / monocrystalline silicon composite three-dimensional substrate.

[0043] Example 2 The preparation steps and process conditions in this embodiment are basically the same as in Example 1, except that in the third step of growing a cubic silicon carbide layer with micro-nano structures on the surface, the deposition temperature and deposition pressure are adjusted to 1350℃ and 150mbar, respectively. The remaining silicon source, carbon source, carrier gas flow rate, dilution gas flow rate, carbonization conditions, deposition time, silicon substrate thinning treatment, and subsequent silicon-silicon bonding steps are all the same as in Example 1.

[0044] Compared to Example 1, Example 2 uses a higher deposition temperature. At the higher deposition temperature, the active atoms in SiC obtain sufficient activation energy to achieve nucleation and crystal growth, resulting in improved grain size and a hexagonal pyramidal surface morphology. Its X-ray diffraction pattern and scanning electron microscope image are shown below. Figure 5 , 6 As shown, the cubic silicon carbide layer has good crystal quality and its surface exhibits a pyramid structure.

[0045] Example 3 The preparation steps and process conditions in this embodiment are basically the same as in Example 1, except that in the third step of growing a cubic silicon carbide layer with micro-nano structures on the surface, the deposition temperature and deposition pressure are adjusted to 1250℃ and 150mbar, respectively. The remaining silicon source, carbon source, carrier gas flow rate, dilution gas flow rate, carbonization conditions, deposition time, silicon substrate thinning treatment, and subsequent silicon-silicon bonding steps are all the same as in Example 1.

[0046] Compared to Example 1, Example 3 uses a lower deposition temperature. Grain nucleation and growth are closely related to the deposition temperature and pressure. Under these conditions, SiC grains grow rapidly, but the nucleus density is relatively low, promoting high-speed longitudinal growth of SiC and facilitating the formation of slender "whisker-like" crystals. Due to the higher supersaturation, the gaps between SiC whiskers are smaller. Its X-ray diffraction pattern and scanning electron microscope image are shown below. Figure 7 , 8 As shown, the cubic silicon carbide layer exhibits slightly inferior crystal quality compared to Examples 1 and 2, with its surface displaying a one-dimensional whisker-like structure.

[0047] Example 4 The preparation steps and process conditions in this embodiment are basically the same as in Example 1, except that in the third step of growing a cubic silicon carbide layer with micro-nano structures on the surface, the deposition temperature and deposition pressure are adjusted to 1250℃ and 100mbar, respectively. The remaining silicon source, carbon source, carrier gas flow rate, dilution gas flow rate, carbonization conditions, deposition time, silicon substrate thinning treatment, and subsequent silicon-silicon bonding steps are all the same as in Example 1.

[0048] Compared to Example 3, Example 4 uses a lower deposition pressure. The deposition pressure is positively correlated with the supersaturation of the precursor and is also related to nucleation during CVD growth. Under these conditions, the nucleation density of SiC is lower, but the growth rate is faster, forming a porous nanoforest-like structure. Compared to Example 3, the supersaturation of SiC growth in this example is slightly reduced, forming a porous cluster structure composed of whiskers. Its X-ray diffraction pattern and scanning electron microscope image are shown below. Figure 9 , 10 As shown, the surface of the cubic silicon carbide layer exhibits a porous structure formed by one-dimensional nanocrystal clusters.

[0049] Comparative Example 1 The preparation steps and process conditions of this comparative example are basically the same as those of Example 1, except that in the third step of growing a cubic silicon carbide layer with micro-nano structures on the surface, the deposition temperature and deposition pressure are adjusted to 1150℃ and 150mbar, respectively. The remaining silicon source, carbon source, carrier gas flow rate, dilution gas flow rate, carbonization conditions, deposition time, silicon substrate thinning treatment, and subsequent silicon-silicon bonding steps are all the same as those in Example 1.

[0050] Compared to Example 1, due to the excessively low deposition temperature, the migration ability of the reactants on the surface of the single-crystal silicon substrate was insufficient, which limited the nucleation and crystal growth of cubic silicon carbide grains. The resulting silicon carbide layer had a dense and flat surface, and its crystal quality was significantly lower than that of Examples 1 and 2. This illustrates the effect of deposition temperature on the crystal quality, surface morphology, and heat dissipation enhancement effect of the cubic silicon carbide layer. Its X-ray diffraction pattern and scanning electron microscope image are shown below. Figure 11 , 12 As shown, it exhibits low crystallinity and a flat surface.

[0051] Comparative Example 2 The preparation steps and process conditions of this comparative example are basically the same as those of Example 1, except that in the third step of growing a cubic silicon carbide layer with micro-nano structures on the surface, the deposition temperature and deposition pressure are adjusted to 1200℃ and 50mbar. The remaining silicon source, carbon source, carrier gas flow rate, dilution gas flow rate, carbonization conditions, deposition time, silicon substrate thinning treatment, and subsequent silicon-silicon bonding steps are all the same as those in Example 1.

[0052] Compared to Example 4, Comparative Example 2 used excessively low deposition pressure. Under low-pressure conditions, SiC atoms possess sufficient activation energy to achieve nucleation and crystallization even with low precursor saturation, resulting in a dense, flat structure with no obvious micro / nano structures on the surface. Its X-ray diffraction pattern and scanning electron microscope image are shown below. Figure 13 , 14 As shown, it exhibits low crystallinity and a dense surface.

[0053] Compared with existing solutions that directly use hexagonal silicon carbide wafers as heat dissipation substrates or interlayers, the present invention uses a single-sided grown 3C-SiC / Si composite substrate, which has the following advantages: (1) Ability to form surface micro / nano structures that facilitate heat transfer in situ: By controlling parameters such as temperature, pressure, gas flow rate, and deposition time during the chemical vapor deposition process, this invention can simultaneously form lotus-shaped micro / nano structures during the growth of cubic silicon carbide layers. These micro / nano structures can increase the actual heat transfer area on the surface of the cubic silicon carbide layer, improve its contact state with thermal interface materials, coolants, or phase change media, thereby further enhancing the interface heat transfer efficiency without the need for complex post-processing processes such as laser processing, photolithography, or plasma etching.

[0054] (2) Better large-size fabrication capability and cost advantage: The cubic silicon carbide of the present invention can be directly epitaxially grown on the surface of a single-crystal silicon substrate, and can utilize mature large-size silicon wafers as substrates, with good compatibility with existing silicon-based semiconductor processes. Compared with directly using hexagonal silicon carbide wafers, which are more expensive and limited in size, the present invention can reduce the dependence on large-size silicon carbide wafers, reduce material costs and processing costs, and is more suitable for wafer-level fabrication and large-scale application.

[0055] (3) It can reduce the difficulty of bonding and packaging integration: Since the cubic silicon carbide layer is only formed on one side of the monocrystalline silicon substrate, the composite substrate still retains the monocrystalline silicon side as the subsequent connection surface. After thinning the back side of the silicon substrate, it can be connected to another monocrystalline silicon wafer, silicon-based chip or silicon-based packaging structure through mature silicon-silicon bonding process, avoiding direct silicon carbide-silicon heterobonding, which helps to reduce problems such as interface voids, warpage, debonding and stress concentration, and improve the reliability of the packaging structure.

[0056] (4) Simple process and good controllability. The present invention can prepare a cubic silicon carbide heat dissipation layer on one side of a single crystal silicon substrate by chemical vapor deposition, and can simultaneously control its thickness, crystal quality and surface morphology; combined with subsequent silicon substrate thinning and silicon-silicon bonding processes, a composite heat dissipation structure with enhanced thermal conductivity, enhanced interface heat transfer and silicon-based process compatibility can be formed, which is suitable for heat dissipation packaging of GPU, CPU, AI accelerator chips and other high power density semiconductor devices.

[0057] The specific embodiments of the present invention described above do not constitute a limitation on the scope of protection of the present invention. Any other corresponding changes and modifications made in accordance with the technical concept of the present invention should be included within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate, characterized in that, Includes the following steps: A monocrystalline silicon substrate is provided, and the monocrystalline silicon substrate is cleaned and dried to obtain a pretreated monocrystalline silicon substrate; A cubic silicon carbide layer with a micro / nano structure is grown on one side of the pretreated monocrystalline silicon substrate to obtain a cubic silicon carbide / monocrystalline silicon composite substrate.

2. The method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate according to claim 1, characterized in that, The single-crystal silicon substrate is <100> , <110> or <111> Crystal-oriented monocrystalline silicon wafers, with dimensions ranging from 6 to 12 inches.

3. The method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate according to claim 1, characterized in that, Using a chemical vapor deposition method, the pretreated single-crystal silicon substrate is placed in the process chamber of a chemical vapor deposition equipment, and a cubic silicon carbide layer with a micro-nano structure is deposited and grown on one side surface of the pretreated single-crystal silicon substrate.

4. The method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate according to claim 3, characterized in that, The chemical vapor deposition method is one of atmospheric pressure chemical vapor deposition, low pressure chemical vapor deposition, plasma-enhanced chemical vapor deposition, hot-wall chemical vapor deposition, or metal-organic chemical vapor deposition; and / or, During the chemical vapor deposition process, a silicon-containing reactive gas and a carbon-containing reactive gas are introduced into the process chamber, causing the silicon-containing reactive gas and the carbon-containing reactive gas to react on one side of the surface of the single-crystal silicon substrate and form a cubic silicon carbide layer with a micro-nano structure on the surface; wherein, the silicon-containing reactive gas is one or more of silane, dichlorosilane, silicon tetrachloride, trichlorosilane, and trichloromethylsilane; the carbon-containing reactive gas is one or more of methane, ethane, propane, ethylene, and acetylene; the reaction atmosphere also includes a carrier gas and / or a diluent gas, and the carrier gas and / or diluent gas is one or more of hydrogen, argon, helium, or nitrogen.

5. The method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate according to claim 1, characterized in that, A cubic silicon carbide layer with a micro / nano structure is grown on one side of the pretreated single-crystal silicon substrate, including: The pretreated single-crystal silicon substrate is placed in the process chamber of the chemical vapor deposition equipment; Under deposition temperatures of 1100~1200℃ and deposition pressures of 80~120 mbar, carbon-containing reactive gas of 10~30 sccm and dilution gas of 80~120 slm are introduced to carbonize the surface of a single-crystal silicon substrate for 8~12 minutes. At a deposition temperature of 1200~1300℃ and a deposition pressure of 80~120mbar, 5~10sccm of carbon-containing reactive gas, 80~120slm of dilution gas and 10~30sccm of carrier gas are introduced, and deposition is carried out for 25~35 minutes; wherein, the carrier gas carries the silicon source into the process chamber by bubbling, and the temperature of the bubbler is 18~20℃; At a deposition temperature of 1250~1350℃ and a deposition pressure of 100~200 mbar, 10~30 sccm of carbon-containing reactive gas, 80~120 slm of dilution gas and 30~50 sccm of carrier gas are introduced, and deposition is carried out for 8~12 minutes; wherein, the carrier gas carries the silicon source into the process chamber by bubbling, and the temperature of the bubbler is 18~20℃.

6. The method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate according to claim 1, characterized in that, The micro / nanostructure is one or more of the following: lotus-shaped, pyramid-shaped, granular, hill-shaped, island-shaped, nanoforest-shaped, or composite micro / nanostructure.

7. The method for preparing a cubic silicon carbide / monocrystalline silicon composite substrate according to claim 1, characterized in that, After growing a cubic silicon carbide layer with micro / nano structures on one side of the pretreated single-crystal silicon substrate, the process further includes: The surface of the single-crystal silicon substrate away from the cubic silicon carbide layer is thinned; after the thinning process, the thickness of the single-crystal silicon substrate is 20~50μm; and / or, A silicon-based semiconductor structure is provided, and the silicon-based semiconductor structure is connected to the single-crystal silicon side of the cubic silicon carbide / single-crystal silicon composite substrate; the silicon-based semiconductor structure is one or more of silicon-based devices, silicon-based epitaxial wafers, silicon-based chips, or silicon-based packaging structures; the connection method is silicon-silicon bonding.

8. A cubic silicon carbide / monocrystalline silicon composite substrate, characterized in that, The cubic silicon carbide / monocrystalline silicon composite substrate is obtained by the preparation method of the cubic silicon carbide / monocrystalline silicon composite substrate according to any one of claims 1 to 7.

9. An application of the cubic silicon carbide / monocrystalline silicon composite substrate as described in claim 8, characterized in that, The cubic silicon carbide / monocrystalline silicon composite substrate is used in the heat dissipation structure of silicon-based semiconductor devices.

10. The application of the cubic silicon carbide / monocrystalline silicon composite substrate according to claim 9, characterized in that, The heat dissipation structure for the silicon-based semiconductor device includes: a silicon-based semiconductor device and the cubic silicon carbide / monocrystalline silicon composite substrate; wherein... The silicon-based semiconductor device is disposed on the side of the cubic silicon carbide / monocrystalline silicon composite substrate away from the cubic silicon carbide layer; and / or, The silicon-based semiconductor device is a silicon-based semiconductor chip; and / or, The silicon-based semiconductor device is one or more of the following: GPU chip, CPU chip, AI accelerator chip, power device chip, radio frequency chip, and memory chip; and / or, The side of the cubic silicon carbide layer away from the monocrystalline silicon substrate is connected to one or more of the following: a thermal interface material, a metal heat sink, a heat sink, a heat spreader, a liquid cooling plate, or a phase change heat dissipation structure.

Citation Information

Patent Citations

  • Diamond / monocrystalline silicon composite three-dimensional substrate and preparation method and application thereof

    CN118888524A

  • Packaging structure based on silicon-based silicon carbide intermediate layer and preparation method thereof

    CN121908885A