A flame-retardant lyocell fiber and its preparation method
By using polyurethane leveling agent and melamine polyphosphate flame retardant coating treatment during the spinning process of lyocell fiber, hydrogen bond and interfacial cross-linking network are formed, solving the problem of poor compatibility of lyocell fiber flame retardant and achieving improved high flame retardant durability and mechanical strength.
Patent Information
- Application Number
- CN202611525554.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-29
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, the flame retardant of lyocell fiber has poor interfacial compatibility with the cellulose matrix, which leads to a decrease in spinning rheology and mechanical strength. At the same time, the flame retardant is prone to migration and shedding, making it difficult to maintain flame retardant performance during frequent washing.
A leveling coating structure is formed by polyurethane leveling agent and melamine polyphosphate flame retardant. Through urethane groups, ether bonds and active end groups, hydrogen bonds and interfacial cross-linking networks are formed with cellulose and flame retardant, which improves the rheological properties of spinning solution and the dispersion uniformity of flame retardant.
It improves the interfacial cross-linking strength of the flame retardant, enhances the limiting oxygen index and mechanical strength of the fiber, and the flame retardant performance decreases by no more than 5% after 50 washes. The dry breaking strength remains above 3.5 cN/dtex, and the spinning process is stable and continuous.
Smart Images

Figure CN123108757A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of flame-retardant fiber materials, and particularly relates to a flame-retardant lyocell fiber and its preparation method. Background Technology
[0002] Lyocell fiber is a regenerated cellulose fiber produced by wet or dry-jet spinning of natural plant cellulose pulp dissolved in an aqueous solution of N-methylmorpholine-N-oxide (NMMO). It combines the moisture-wicking and skin-friendly properties of natural fibers with the high strength of synthetic fibers, and boasts a high solvent recovery rate during production. However, lyocell fiber has a limiting oxygen index (LOI) of only about 17%, classifying it as a flammable material, which significantly limits its application in protective clothing, specialty home textiles, and industrial textiles.
[0003] Currently, the main methods for imparting flame retardant properties to lyocell fibers include finishing and solution blending. Among these, finishing offers advantages such as process flexibility and ease of operation; solution blending allows flame retardants to be directly introduced into the fiber interior, giving the finished fiber better initial flame retardant properties.
[0004] However, existing solution blending modification technologies suffer from a core technical bottleneck: the interfacial compatibility between flame retardant particles and the NMMO / cellulose system is extremely poor, making it impossible to simultaneously consider the rheological properties of the spinning solution and the interfacial bonding strength of the flame retardant. This core defect manifests itself in the following two aspects:
[0005] Poor spinning rheology and structural damage: When flame retardants are directly added to high-viscosity spinning solutions, they are prone to agglomeration and phase separation, which damages the fluidity and viscosity stability of the spinning solution. This not only leads to a high breakage rate in spinning, but also causes a significant decrease in the mechanical strength of the finished fiber due to uneven dispersion of the flame retardant.
[0006] Interface bonding defects (affecting durability): The flame retardant and cellulose molecular chain lack effective interfacial cross-linking and chemical anchoring, relying only on weak physical encapsulation. During frequent water washing or alkaline washing, the flame retardant is very easy to migrate and fall off, resulting in rapid decay of flame retardant performance.
[0007] Therefore, there is an urgent need for a lyocell fiber and its preparation method that can improve the fluidity and mechanical strength of spinning solution, and enhance interfacial bonding and flame retardancy. Summary of the Invention
[0008] The technical problem this invention aims to solve is how to improve the rheological properties and dispersion uniformity of the spinning solution during the dope blending and spinning process of flame-retardant lyocell fibers, and enhance the interfacial crosslinking and bonding strength between the flame retardant and the cellulose matrix. To solve the above technical problem, this invention provides a flame-retardant lyocell fiber and its preparation method. The specific technical content is as follows:
[0009] A flame-retardant lyocell fiber, the raw materials for which are prepared, by weight, include:
[0010] N-methylmorpholine-N-oxide solution: 550–750 parts;
[0011] Cellulose pulp: 60–85 parts;
[0012] Melamine polyphosphate flame retardant: 1–3 parts;
[0013] Polyurethane leveling agent: 3–7 parts;
[0014] The mass concentration of the N-methylmorpholine-N-oxide solution was 86–88%.
[0015] Furthermore, the amount of the polyurethane leveling agent added is 4–6 parts.
[0016] Furthermore, the raw materials used in the preparation also contain at least one additive selected from silicon-based flame retardants and phosphorus-based flame retardants, with an addition amount of 1–3 parts.
[0017] Furthermore, the polyurethane leveling agent and the melamine polyphosphate flame retardant form a leveling coating structure;
[0018] The polyurethane leveling agent forms hydrogen bonds and interfacial cross-linking networks with the hydroxyl groups in the cellulose pulp and the phosphate groups in the melamine polyphosphate flame retardant through urethane groups, ether bonds and active end groups.
[0019] Furthermore, the flame-retardant lyocell fiber has an initial limiting oxygen index (LOI) ≥ 28%, and the absolute decrease in the limiting oxygen index after 50 standard washes is ≤ 5%; the dry breaking strength is ≥ 3.5 cN / dtex.
[0020] A method for preparing the aforementioned flame-retardant lyocell fiber includes the following steps:
[0021] Step 1: Pre-treat the flame retardant by mixing and stirring melamine polyphosphate with polyurethane leveling agent to obtain a leveling coated flame retardant.
[0022] Step 2: Add the leveling coated flame retardant obtained in Step 1 to an N-methylmorpholine-N-oxide solution and stir under negative pressure. Then add cellulose pulp to dissolve and distill under negative pressure to obtain a uniform spinning solution.
[0023] Step 3: The uniform spinning solution is extruded, filtered and degassed before spinning. The fiber bundle is stretched through the air gap and then enters the coagulation bath to solidify and form. After washing, oiling and drying, the finished fiber is obtained.
[0024] Furthermore, in step one, the pretreatment conditions are as follows: stirring at 20-25°C for 15-20 minutes until the system is viscous and free of bubbles.
[0025] Furthermore, in step two:
[0026] The mass concentration of the N-methylmorpholine-N-oxide solution is 86–88%;
[0027] The stirring conditions after adding the leveling coated flame retardant are: stirring under negative pressure for 30–60 minutes at a temperature of 80–100°C and a pressure of -0.08 to -0.10 MPa;
[0028] The dissolution time after adding the cellulose pulp is 60–120 minutes;
[0029] The conditions for the negative pressure distillation are: distillation at a temperature of 90–110°C under negative pressure for 2–3 hours.
[0030] Furthermore, in step three:
[0031] The spinning temperature is 90–105°C;
[0032] The coagulation bath is an aqueous solution of N-methylmorpholine-N-oxide with a mass concentration of 20–30%, and the coagulation bath temperature is 10–25°C.
[0033] The beneficial effects of flame-retardant lyocell fiber in this invention are as follows:
[0034] Significantly improved flame retardancy and durability: The polyurethane leveling agent contains polar urethane groups, ether bonds, and active end groups, which can form multiple hydrogen bonds and interfacial cross-linking networks with the hydroxyl groups of cellulose molecules and the phosphate groups of melamine polyphosphate (MPP). This structure endows the flame retardant with extremely high interfacial adhesion and chemical anchoring strength, resulting in a fiber limiting oxygen index (LOI) ≥ 28%, and an LOI decrease of ≤ 5% after 50 standard water washes, solving the problem of easy washing away by traditional flame retardants.
[0035] High mechanical strength retention: By pre-coating the MPP particles with polyurethane leveling agent, the compatibility between the flame retardant particles and the cellulose matrix is greatly improved, avoiding stress concentration and microstructural defects caused by flame retardant agglomeration, and keeping the dry breaking strength of the finished fiber above 3.5 cN / dtex.
[0036] Green, halogen-free, and environmentally friendly: It adopts a nitrogen-phosphorus synergistic halogen-free flame retardant system, which produces low smoke and no toxicity when burning, in line with the green and environmentally friendly properties of lyocell fiber itself, and expands its application in the fields of close-fitting protective clothing and home textiles.
[0037] The beneficial effects of the preparation method are as follows:
[0038] Significantly improves the rheological and leveling properties of spinning solution: MPP and polyurethane leveling agent are pre-stirred at 20–25°C to form a leveling coated flame retardant, which can significantly reduce the viscosity disturbance of the NMMO / cellulose system after the introduction of flame retardant, improve the surface tension and flow uniformity of spinning solution, and effectively avoid the phenomenon of bubble retention and uneven distribution of flame retardant in spinning solution caused by direct feeding.
[0039] The spinning process is continuous and stable: the uniform and stable spinning solution ensures smooth extrusion, filtration and degassing and air gap stretching processes, which greatly reduces the spinneret blockage rate and spinning breakage rate, and improves the spinning quality and production efficiency. Attached Figure Description
[0040] Figure 1 This is a process flow diagram for preparing flame-retardant lyocell fibers according to an embodiment of the present invention;
[0041] Figure 2 This is a schematic diagram illustrating the working mechanism of an embodiment of the present invention. Detailed Implementation
[0042] To make the objectives and technical solutions of the present invention clearer, the specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings and examples.
[0043] First, the testing and evaluation methods used in the embodiments and comparative examples of this invention will be explained:
[0044] 1. Limiting Oxygen Index (LOI) Test: The test shall be conducted in accordance with GB / T5454-1997 "Test for Burning Performance of Textiles - Oxygen Index Method".
[0045] 2. Wash fastness test: Standard washing was performed in accordance with GB / T17596-1998 "Commercial washing procedures before burning tests of textile fabrics", and the initial limiting oxygen index and the limiting oxygen index (LOI) after 50 standard washes were measured.
[0046] 3. Dry breaking strength test of fibers: The dry breaking strength (unit: cN / dtex) of the finished fibers was determined using a single fiber tensile tester in accordance with GB / T14337-2022 "Test Method for Tensile Properties of Chemical Fibers and Short Fibers".
[0047] 4. Evaluation of spinning stability and leveling: Observe the uniformity of the spinning solution flow, whether phase separation or gelation occurs, and record the breakage rate (unit: times / spindle) during continuous spinning.
[0048] The preparation process of flame-retardant lyocell fiber of this invention is as follows: Figure 1 As shown.
[0049] Example 1:
[0050] The raw material formulation in this embodiment, by weight, is as follows: 653.4 parts of 88% NMMO solution (obtained by dehydration of 1150 parts of 50% NMMO solution), 72 parts of wood pulp, 2.16 parts of melamine polyphosphate (MPP) flame retardant, and 4.32 parts of polyurethane leveling agent. The specific preparation method includes the following steps:
[0051] (1) Flame retardant pretreatment: At room temperature of 25°C, 2.16 parts of MPP flame retardant powder and 4.32 parts of polyurethane leveling agent liquid were placed in a premixed reaction vessel, and mechanical stirring was started. The stirring speed was controlled at 300–500 rpm, and stirring was carried out continuously for 18 minutes. The system was observed to gradually transform from a solid-liquid mixture into a leveling and compatible white viscous suspension, and there were no obvious residual bubbles on the surface and inside. The leveling coated flame retardant was obtained.
[0052] (2) Preparation of spinning solution: Take 1150 parts of NMMO aqueous solution with a mass concentration of 50%, turn on the heating and negative pressure stirring system, and stir under negative pressure for 45 minutes at a temperature of 90°C and a negative pressure of -0.09MPa to remove water so that the mass concentration of NMMO reaches 88% (the solution after dehydration is about 653.4 parts). Then, add all the leveling coated flame retardant obtained in step (1) into the system, and stir under negative pressure for 45 minutes at a temperature of 90°C and a negative pressure of -0.09MPa to fully disperse the coated flame retardant; then add 72 parts of dried wood pulp to the system, and stir and dissolve at 90°C for 90 minutes to achieve uniform dispersion of the coated flame retardant in the NMMO solvent, while the cellulose is completely swollen and dissolved. After dissolution, the system is heated to 100°C and distilled for 2.5 hours under a negative pressure of -0.09MPa to remove excess water and control the water content of the system, resulting in an amber-colored and uniformly flowing spinning solution.
[0053] (3) Spinning and forming: The obtained uniform spinning solution is conveyed by a screw extruder, metered by a multi-stage metering pump, and filtered and degassed by a metering filter. It is then pressed into the spinning assembly and spun out through the micro-holes of the spinneret at a spinning temperature of 98°C to form a fine stream of filaments. The fine stream of filaments is stretched and cooled by air through a 15mm long air gap zone, and then enters a coagulation bath to solidify and form. The coagulation bath is an NMMO aqueous solution with a mass concentration of 25% and a temperature controlled at 15°C. After solidification and forming, the nascent filaments are washed with multiple deionized water sprays to remove residual solvents, oiled, and dried and shaped. Finally, they are wound and packaged to obtain the flame-retardant lyocell fiber finished product.
[0054] Example 2:
[0055] The raw material formulation in this embodiment, by weight, is as follows: 653.4 parts of 88% NMMO solution (obtained by dehydration of 1150 parts of 50% NMMO solution), 72 parts of wood pulp, 1.44 parts of MPP flame retardant, 5.76 parts of polyurethane leveling agent, and 1.44 parts of silicone-based flame retardant Baliso. The specific preparation method includes the following steps:
[0056] (1) Flame retardant pretreatment: At room temperature of 20°C, 1.44 parts of MPP flame retardant powder, 1.44 parts of silicone flame retardant Baliso and 5.76 parts of polyurethane leveling agent were placed in a premixed reaction vessel and stirred thoroughly at 300–500 rpm for 15 minutes until the system was uniform and viscous and no visible bubbles were observed, thus obtaining a composite leveling coated flame retardant.
[0057] (2) Preparation of spinning solution: Take 1150 parts of NMMO aqueous solution with a mass concentration of 50% and dehydrate it under negative pressure stirring at 90°C and negative pressure of -0.09MPa until the mass concentration is 88% (about 653.4 parts). Then add the composite leveling coated flame retardant obtained in step (1) and stir for 30 minutes at 85°C and negative pressure of -0.08MPa to fully disperse the flame retardant composite. Then add 72 parts of wood pulp and keep it at 85°C to swell and dissolve for 60 minutes. After dissolution, raise the temperature to 95°C and distill and dehydrate it under negative pressure of -0.10MPa for 2.0 hours to obtain a uniform spinning solution.
[0058] (3) Spinning and forming: The spinning solution is conveyed by screw extrusion and filtered and degassed, and then extruded and spun at a spinning temperature of 98°C. The filament bundle is stretched and cooled through an air gap and then enters a coagulation bath for coagulation and forming. The coagulation bath is an NMMO aqueous solution with a mass concentration of 20% and a temperature controlled at 10°C. The nascent filament bundle is thoroughly washed with deionized water, oiled, and dried to obtain the finished fiber.
[0059] Example 3:
[0060] The raw material formula in this embodiment, by mass parts, is as follows: 653.4 parts of 88% NMMO solution (obtained by dehydration of 1150 parts of 50% NMMO solution), 72 parts of wood pulp, 2.16 parts of MPP flame retardant, 4.32 parts of polyurethane leveling agent, and 2.16 parts of phosphorus-based flame retardant SMFR-40.
[0061] The specific preparation method includes the following steps:
[0062] (1) Flame retardant pretreatment: At room temperature of 25°C, 2.16 parts of MPP flame retardant, 2.16 parts of phosphorus flame retardant SMFR-40 and 4.32 parts of polyurethane leveling agent were mixed and stirred at 300–500 rpm for 20 minutes until the system was viscous and free of bubbles, thus obtaining leveling coated flame retardant.
[0063] (2) Preparation of spinning solution: Take 1150 parts of NMMO aqueous solution with a mass concentration of 50% and dehydrate it under negative pressure stirring at 90°C and negative pressure of -0.09MPa until the mass concentration is 88% (about 653.4 parts). Then add the leveling coated flame retardant obtained in step (1) and stir for 60 minutes at 100°C and negative pressure of -0.10MPa. Then add 72 parts of wood pulp and dissolve for 120 minutes. Raise the temperature to 105°C and maintain negative pressure of -0.10MPa for distillation and dehydration for 3.0 hours to obtain a uniform spinning solution.
[0064] (3) Spinning and forming: After the spinning solution is squeezed and filtered to remove bubbles, it is spun at a spinning temperature of 98°C. The filament bundle is stretched through the air gap and then enters the coagulation bath to form. The coagulation bath is an NMMO aqueous solution with a mass concentration of 20% and a temperature of 15°C. The nascent filament bundle is washed, oiled and dried in multiple stages to obtain the finished fiber.
[0065] Comparative Example 1 (using paraffin-based leveling agents instead of polyurethane leveling agents)
[0066] The raw material formulation for this comparative example, by mass parts, is as follows: 653.4 parts of 88% NMMO solution (obtained by dehydration of 1150 parts of 50% NMMO solution), 72 parts of wood pulp, 2.16 parts of MPP flame retardant, and 4.32 parts of paraffin leveling agent. The specific preparation method is as follows:
[0067] (1) Pretreatment attempt: 2.16 parts of MPP flame retardant and 4.32 parts of paraffin leveling agent were mixed and stirred for 18 minutes at 25°C. Due to the low polarity of paraffin leveling agent, the surface wettability of the flame retardant was poor, and the compatibility of the mixture was not good.
[0068] (2) Preparation of spinning solution: Take 1150 parts of NMMO aqueous solution with a mass concentration of 50% and dehydrate it under negative pressure stirring at 90°C and -0.09MPa to a mass concentration of 88% (about 653.4 parts). Add the above mixture and stir for 45 minutes at 90°C and -0.09MPa negative pressure; then add 72 parts of wood pulp and dissolve for 90 minutes, raise the temperature to 100°C and distill under negative pressure for 2.5 hours to obtain the spinning solution.
[0069] (3) Spinning and forming: The spinning solution is extruded and spun at 98°C, and then solidified in a 15°C, 25% NMMO aqueous solution coagulation bath. After washing, oiling and drying, the finished fiber is obtained.
[0070] Comparative Example 2 (without any leveling agent added)
[0071] The raw material formulation for this comparative example, by mass parts, is as follows: 653.4 parts of 88% NMMO solution (obtained by dehydration of 1150 parts of 50% NMMO solution), 72 parts of wood pulp, and 2.16 parts of MPP flame retardant. The specific preparation method is as follows:
[0072] (1) Pretreatment not performed: The flame retardant pre-coating step was omitted.
[0073] (2) Preparation of spinning solution: Take 1150 parts of NMMO aqueous solution with a mass concentration of 50% and dehydrate it under negative pressure stirring at 90°C and negative pressure of -0.09MPa to a mass concentration of 88% (about 653.4 parts). Add 2.16 parts of pure MPP flame retardant powder without leveling agent directly to the 88% NMMO solution at 90°C and stir for 45 minutes under negative pressure of -0.09MPa at 90°C. The flame retardant powder will locally agglomerate in the polar NMMO solution. Add 72 parts of wood pulp and dissolve for 90 minutes. Heat to 100°C and distill under negative pressure for 2.5 hours to obtain spinning solution.
[0074] (3) Spinning and forming: The spinning solution is extruded and spun at 98°C, and then formed in a coagulation bath of 15°C and 25% NMMO aqueous solution. After washing, oiling and drying, the finished fiber is obtained.
[0075] The performance of the lyocell fibers prepared in Examples 1–3 and Comparative Examples 1–2 was tested, and the test results are shown in Table 1.
[0076]
[0077] Table 1
[0078] Results Analysis and Demonstration:
[0079] Comparative analysis with Comparative Example 2 (with no leveling agent added) (combined) Figure 2(Mechanism of Action and Test Data in Table 1): In Examples 1–3, the initial LOI of the finished fibers was increased to 29.0%–31.0% by introducing polyurethane leveling agents. After 50 standard washes, the LOI remained within the range of 27.5%–29.0%, with an absolute decrease in LOI of no more than 5%. The dry breaking strength remained stable above 3.5 cN / dtex, and the continuous spinning process was smooth. The mechanism of action is that the polar urethane groups and ether bonds in the polyurethane leveling agent molecular structure can form multiple interfacial hydrogen bonds and cross-linking networks with the hydroxyl groups on the cellulose macromolecular chain and the phosphate groups in the flame retardant (MPP). This cross-linking structure improves the interfacial bonding strength and fixation effect of the flame retardant particles inside the fiber, preventing physical peeling during the washing process. At the same time, the coating effect of the leveling agent improves the dispersion compatibility of the flame retardant in the matrix, reduces stress concentration points caused by the agglomeration of flame retardant particles, and thus protects the mechanical strength of the fiber itself.
[0080] Comparative analysis with Example 1, which uses paraffin-based leveling agents: Paraffin-based leveling agents are non-polar long-chain alkanes, lacking polar functional groups and active sites in their molecular structure that can effectively bind with flame retardants and the cellulose matrix. They only play a simple physical lubricating role in the system. In the highly polar and viscous NMMO / cellulose system, paraffin-based leveling agents exhibit poor compatibility with the system, easily leading to phase separation and interfacial migration precipitation, resulting in fluctuations in the viscosity of the spinning solution. During routine washing, the flame retardant lacks effective interfacial adhesion and detaches, causing the LOI to decrease to 19.5% and the dry breaking strength to decrease to 2.5 cN / dtex after washing. This comparison further confirms that the polar groups and cross-linking network of polyurethane leveling agents play a crucial role in improving rheological properties and consolidating flame retardant durability.
[0081] In summary, premixing and coating flame retardants with polyurethane leveling agents can improve the rheology and leveling uniformity of the spinning solution while enhancing the interfacial crosslinking and bonding strength of the flame retardant in the cellulose matrix, thus achieving a balance between high flame retardant durability, mechanical strength retention, and stable spinnability.
[0082] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the present invention, and all such modifications and substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A flame-retardant lyocell fiber, characterized in that, The raw materials for its preparation, by weight, include: N-methylmorpholine-N-oxide solution: 550–750 parts; Cellulose pulp: 60–85 parts; Melamine polyphosphate flame retardant: 1–3 parts; Polyurethane leveling agent: 3–7 parts; The mass concentration of the N-methylmorpholine-N-oxide solution was 86–88%.
2. The flame retardant lyocell fiber according to claim 1, characterized in that, The amount of the polyurethane leveling agent added is 4–6 parts.
3. The flame retardant lyocell fiber according to claim 1, characterized in that, The raw materials used in the preparation also include at least one additive selected from silicon-based flame retardants and phosphorus-based flame retardants, with an addition amount of 1–3 parts.
4. The flame retardant lyocell fiber according to claim 1, characterized in that, The polyurethane leveling agent and the melamine polyphosphate flame retardant form a leveling coating structure; The polyurethane leveling agent forms hydrogen bonds and interfacial cross-linking networks with the hydroxyl groups in the cellulose pulp and the phosphate groups in the melamine polyphosphate flame retardant through urethane groups, ether bonds and active end groups.
5. The flame retardant lyocell fibre according to any one of claims 1 to 4, characterized in that The flame-retardant lyocell fiber has an initial limiting oxygen index (LOI) ≥ 28%, and the absolute decrease in the limiting oxygen index after 50 standard washes is ≤ 5%; the dry breaking strength is ≥ 3.5 cN / dtex.
6. A process for the production of flame-retardant lyocell fibres as defined in any one of claims 1 to 5, characterised in that, Includes the following steps: Step 1: Pre-treat the flame retardant by mixing and stirring melamine polyphosphate with polyurethane leveling agent to obtain a leveling coated flame retardant. Step 2: Add the leveling coated flame retardant obtained in Step 1 to an N-methylmorpholine-N-oxide solution and stir under negative pressure. Then add cellulose pulp to dissolve and distill under negative pressure to obtain a uniform spinning solution. Step 3: The uniform spinning solution is extruded, filtered and degassed before spinning. The fiber bundle is stretched through the air gap and then enters the coagulation bath to solidify and form. After washing, oiling and drying, the finished fiber is obtained.
7. The process for the preparation of flame retardant lyocell fibers according to claim 6, characterized in that, In step one, the pretreatment conditions are: stirring at 20-25°C for 15-20 minutes until the system is viscous and free of bubbles.
8. A process for the preparation of flame retardant lyocell fibres according to claim 6, characterised in that, In step two: The mass concentration of the N-methylmorpholine-N-oxide solution is 86–88%; The stirring conditions after adding the leveling coated flame retardant are: stirring under negative pressure for 30–60 minutes at a temperature of 80–100°C and a pressure of -0.08 to -0.10 MPa; The dissolution time after adding the cellulose pulp is 60–120 minutes; The conditions for the negative pressure distillation are: distillation at a temperature of 90–110°C under negative pressure for 2–3 hours.
9. The process for the preparation of flame retardant lyocell fibers according to claim 6, characterized in that, In step three: The spinning temperature is 90–105°C; The coagulation bath is an aqueous solution of N-methylmorpholine-N-oxide with a mass concentration of 20–30%, and the coagulation bath temperature is 10–25°C.