A high-performance cooling and antibacterial aramid fiber and its preparation method
By introducing flexible segments and a double-layer PEI silver-locking structure into meta-aramid fibers, the problems of insufficient softness and antibacterial properties of meta-aramid fibers were solved, and the preparation of high-performance cool-feeling antibacterial fibers was realized.
Patent Information
- Application Number
- CN202611548746.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing meta-aramid fibers have insufficient durability, poor softness, and mediocre antibacterial properties when incorporating cooling powder. Furthermore, nano-silver tends to agglomerate during the spinning process, affecting spinning continuity.
By introducing 4,4′-diaminodiphenyl sulfide and 3,4′-diaminodiphenyl sulfide to copolymerize with m-phenylenediamine to form flexible segments, and combining low-temperature acyl chloride-controlled reaction with high molecular weight polyethyleneimine to lock silver ions, a bilayer structure is constructed to achieve strong interfacial bonding between the powder and the matrix.
It improves the softness, comfort, and antibacterial durability of the fiber, solves the problem of stiffness in traditional meta-aramid fibers, and ensures the stability of the spinning process and the antibacterial effect.
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-performance fibers and functional textile materials, and more specifically, to a high-performance cool-feeling antibacterial aramid fiber and its preparation method. Background Technology
[0002] Meta-aramid fibers are widely used in fire-fighting suits, arc flash protection suits, racing suits, and special industrial protective clothing due to their excellent flame retardancy, thermal stability, and electrical insulation. However, meta-aramid fibers are hydrophobic fibers, and their molecular chain structure (aromatic rings and amide bonds) results in a very low affinity for water molecules (whether in gaseous or liquid states). This leads to problems such as weak moisture absorption and wicking capacity, poor moisture transfer capacity, and low evaporative heat dissipation efficiency in the fabric materials made from them, making it difficult to meet the comprehensive needs of home textiles and smart textiles.
[0003] The prior art disclosed in CN121853201B is a method for preparing meta-aramid cooling fibers. The method involves modifying nano-jade / mica / shell with PEI to obtain an amino-modified cooling material, adding acyl chloride-terminated meta-aramid dope to form amide bonds, and then dry-jet wet-spinning. In this method, the cooling powder is added to the aramid dope in a blending manner, which needs to improve durability; moreover, the meta-aramid with the cooling powder is still relatively stiff and lacks softness; the antibacterial properties of this meta-aramid cooling fiber are also only average.
[0004] The prior art disclosed in CN117364275B is a method and apparatus for preparing antibacterial meta-aramid filaments by dry and wet spinning, which achieves antibacterial effect by combining COF-SH silver-loaded with meta-aramid dope. This method has the following drawbacks: single-function antibacterial without a cooling sensation; direct introduction of nano-silver into DMAc dope easily leads to agglomeration, reduction, and blackening; nano-silver can catalyze the hydrolysis of acyl chlorides and affect spinning continuity.
[0005] Therefore, this application is hereby submitted. Summary of the Invention
[0006] In view of this, the present invention aims to propose a high-performance cooling and antibacterial aramid fiber and its preparation method. This addresses the problems in existing technologies where cooling powder is added to the aramid solution via blending, resulting in insufficient durability; the introduction of cooling powder into meta-aramid still leads to a relatively stiff fiber; and the generally limited antibacterial properties of existing meta-aramid cooling fibers.
[0007] To achieve the above objectives, the technical solution of the present invention is implemented as follows:
[0008] A method for preparing a high-performance cooling and antibacterial aramid fiber includes the following steps:
[0009] (1) Preparation of flexible modified meta-solution;
[0010] (2) Preparation of cooling-antibacterial composite powder;
[0011] (3) Preparation of grafting blend solution;
[0012] (4) Preparation of spinning solution;
[0013] (5) Spinning;
[0014] The preparation process of the flexible modified meta-aramid solution includes dissolving a diamine monomer in a polar aprotic solvent, adding isophthaloyl chloride for low-temperature solution polycondensation, and obtaining a flexible modified meta-aramid solution; the diamine monomer is composed of m-phenylenediamine, 4,4′-diaminodiphenyl sulfide and 3,4′-diaminodiphenyl ether.
[0015] This setup successfully introduced flexible segments of ether and thioether bonds into the main chain by copolymerizing two flexible monomers, 4,4′-diaminodiphenyl sulfide (TDA) and 3,4′-ODA, with m-phenylenediamine. These groups act as molecular hinges, effectively increasing the free rotation capability of the molecular chain and reducing the crystallinity and rigidity of the polymer. This improves the softness and comfort of the fiber while maintaining the inherent flame retardancy of meta-aramid, solving the problem of the stiff feel of traditional meta-aramid and providing a matrix basis for the high filling of subsequent cooling powders.
[0016] Furthermore, the preparation process of the flexible modified meta-solution includes dissolving the diamine monomer in a polar aprotic solvent, stirring at -15 to -8°C for 0.5 to 1 hour, adding 75 to 85% isophthaloyl chloride for prepolymerization, performing low-temperature polycondensation reaction for 1 to 4 hours, adding the remaining 15 to 25% isophthaloyl chloride, and aging at 50 to 65°C for 55 to 65 minutes to obtain the flexible modified meta-solution.
[0017] This setup first utilizes low temperature and a certain amount of acyl chloride to control the reaction rate, avoiding explosive polymerization and localized overheating; then, residual acyl chloride is added to increase the degree of reaction; finally, a ripening stage at 55-65℃ is used to precisely control the molecular weight distribution and retain approximately 0.7-0.9 mol% of residual acyl chloride. This process ensures that the stock solution has a high intrinsic viscosity and also reserves active sites for subsequent grafting reactions of powders.
[0018] Furthermore, based on the total molar amount of diamine, the feeding ratio of each component is as follows: m-phenylenediamine 94-98 mol%, 4,4′-diaminodiphenyl sulfide 1-3 mol%, 3,4′-diaminodiphenyl sulfide 1-3 mol%, and the total amount of 4,4′-diaminodiphenyl sulfide and 3,4′-diaminodiphenyl sulfide does not exceed 6 mol%, and the molar ratio of isophthaloyl chloride to the total diamine is 1.001-1.02, preferably, the molar ratio of isophthaloyl chloride to the total diamine is 1.005-1.01.
[0019] This setting strictly controls the total amount of flexible monomers to no more than 6 mol%, ensuring that the rigid structure still dominates in the aramid molecular backbone. This ratio maximizes the introduction of flexible segments while ensuring that the fiber's mechanical strength and limiting oxygen index do not decrease significantly, achieving a molecular structure design that combines rigidity and flexibility.
[0020] Further, the polar aprotic solvent is one or more of N,N-dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, and hexamethylphosphoric triamine.
[0021] Further, in step (2), the preparation of the cooling-antibacterial composite powder includes the following steps:
[0022] (a) Pretreatment of cooling powder to obtain silanized cooling core;
[0023] (b) Disperse the silanized cooling core in deionized water, add high molecular weight polyethyleneimine solution, adjust the pH, stir for a period of time, then add antibacterial agent, continue stirring, centrifuge and wash with water to obtain cooling-antibacterial precursor powder;
[0024] (c) Disperse the cooling-antibacterial precursor powder in anhydrous ethanol, add low molecular weight polyethyleneimine solution and 3-aminopropyltriethoxysilane, react for a period of time, centrifuge, wash and dry to obtain cooling-antibacterial composite powder.
[0025] The high molecular weight PEI in this setup has long molecular chains that cover the powder surface and micropores like a network, and Ag is held together by N→Ag coordination bonds. + Securely locked in the inner layer to prevent Ag + The PEI is lost during subsequent organic phase processing; the low molecular weight PEI provides a high density of terminal amino groups, which act as "anchors" to react chemically with the aramid matrix. The synergistic effect of the two-layer structure ensures both long-lasting antibacterial effect and strong interfacial bonding between the powder and the matrix.
[0026] Furthermore, the antibacterial agent is selected from one or more of soluble silver salts, zinc salts, or copper salts; preferably silver nitrate, silver sulfate, silver acetate, or silver citrate; more preferably silver nitrate.
[0027] Further, the pretreatment of the cooling powder specifically involves adding the cooling powder, ethanol, and 3-aminopropyltriethoxysilane into a container, stirring evenly, refluxing at 55~65℃ for 2~4 hours, filtering, and washing with ethanol to obtain the silanized cooling core.
[0028] Furthermore, the weight ratio of cooling powder: ethanol: 3-aminopropyltriethoxysilane is 100:150~250:1~3.
[0029] Furthermore, the cooling powder is one or more of the following: nano mica, hexagonal boron nitride, nano jade, mesoporous alumina, nano alumina, aluminum nitride, and shell powder.
[0030] Furthermore, the mass ratio of the silanized cooling core: high molecular weight polyethyleneimine: AgNO3 is 1:(1.5~3):(0.02~0.05).
[0031] Further, in step (c), the mass ratio of the low molecular weight polyethyleneimine to 3-aminopropyltriethoxysilane is 1:0.2 to 1:2, preferably 1:0.5 to 1:1.
[0032] Further, in step (c), the amount of 3-aminopropyltriethoxysilane added is 0.5 to 2% of the mass of the cooling-antibacterial precursor powder.
[0033] Further, in step (3), the cooling-antibacterial composite powder is dissolved in a polar aprotic solvent, ultrasonically dispersed for a period of time, added to the flexible modified meta-solution obtained in step (1), the reaction temperature is controlled, and the mixture is stirred for a period of time to obtain a blend.
[0034] Furthermore, the ultrasonic dispersion time is 10~30 min.
[0035] Furthermore, the reaction temperature is 70~80℃, the stirring time is 0.5~1.5h, and the stirring rate is 350~450r / min.
[0036] Further, in step (4), the spinning solution is prepared by adding a monofunctional end-capping agent to the grafted blend solution to carry out the end-capping reaction, stirring the reaction at 20~30℃ for 20~40 min to obtain the spinning solution;
[0037] Further, in step (4), the spinning solution is prepared by taking a sample from the grafted blend to determine the residual acyl chloride equivalent, adding a monofunctional end-capping agent to carry out an end-capping reaction, wherein the molar amount of the monofunctional end-capping agent is 1.0 to 1.5 times the measured residual acyl chloride equivalent, stirring the reaction at 20 to 30°C for 20 to 40 minutes, reducing the residual acyl chloride mass content to <0.5%, and obtaining the spinning solution.
[0038] Furthermore, the monofunctional end-capping agent is selected from one or more of aromatic monoamines, aliphatic monoamines, and monohydroxy alcohols; preferably aniline, methanol, ethanol, or n-butanol.
[0039] Further, in step (5), the spinning process adopts dry-jet wet spinning; wherein, after end sealing, the original solution is degassed by fine filtration, extruded through a spinneret, passes through a 5-20 mm air layer and is pre-stretched in a hot state at a controlled temperature of 40-70℃, and then enters a two-stage coagulation bath for curing, and is then stretched and heat-set at 260-320℃ to obtain fibers.
[0040] Further, the spinning solution is finely filtered through a 5-25 μm filter and vacuum degassed at 30-50℃ for 2-5 h, and then the fiber is prepared using a dry-jet wet spinning process. After extrusion, the spinning solution passes through a 5-20 mm air layer and enters a primary coagulation bath, which is a mixture of polar aprotic solvent and water, wherein the mass fraction of the polar aprotic solvent is 40-60% and the temperature is 15-25℃. Subsequently, it enters a secondary coagulation bath, which is a mixture of polar aprotic solvent and water, wherein the mass fraction of the polar aprotic solvent is 10-30% and the temperature is 30-45℃. After washing and drying, it is heat-set at 260-320℃, with the total draw ratio controlled at 1.2-5.0 times, to obtain the high-performance cool-feeling antibacterial aramid fiber.
[0041] A high-performance cooling and antibacterial aramid fiber is obtained by the preparation method described above.
[0042] Compared with existing technologies, the high-performance cooling antibacterial aramid fiber and its preparation method described in this invention have the following advantages:
[0043] 1) This invention successfully introduces flexible segments of ether and thioether bonds into the main chain by copolymerizing two flexible monomers, 4,4′-diaminodiphenyl sulfide (TDA) and 3,4′-ODA, with m-phenylenediamine. These groups act as molecular hinges, effectively increasing the free rotation ability of the molecular chain and reducing the crystallinity and rigidity of the polymer. This significantly improves the softness and comfort of the fiber while maintaining the inherent flame retardancy of meta-aramid, solving the problem of the stiff feel of traditional meta-aramid and providing a matrix basis for the high filling of subsequent cooling powders.
[0044] 2) This invention utilizes low temperature and a certain amount of acyl chloride to control the reaction rate, avoiding explosive polymerization and local overheating; subsequently, residual acyl chloride is added to increase the degree of reaction; finally, through a ripening stage at 55~65℃, the molecular weight distribution is precisely controlled and approximately 0.7~0.9 mol% of residual acyl chloride is retained. This process ensures that the original solution has a high intrinsic viscosity and reserves active sites for subsequent grafting reactions of powders;
[0045] 3) In this invention, high molecular weight PEI is used to cover the powder surface and micropores, and Ag is linked through N→Ag coordination bonds. + Securely locked in the inner layer to prevent Ag +The PEI is lost during subsequent organic phase processing; the low molecular weight PEI provides a high density of terminal amino groups, which act as "anchors" to react chemically with the aramid matrix. The synergistic effect of the two-layer structure ensures both long-lasting antibacterial effect and strong interfacial bonding between the powder and the matrix. Detailed Implementation
[0046] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below.
[0047] Preparation Example 1
[0048] The preparation of the flexible modified meta-position stock solution is as follows: the diamine monomer is dissolved in N,N-dimethylacetamide (DMAc), stirred at -10℃ for 0.5h, 80% isophthaloyl chloride (IPC) is added for prepolymerization, low-temperature polycondensation reaction is carried out for 2h, and then the remaining 20% isophthaloyl chloride is added, and the temperature is raised to 55℃ for aging for 60 min to obtain the flexible modified meta-position stock solution with a viscosity of 1.75dL / g; the diamine monomer is composed of m-phenylenediamine (MPD), 4,4′-diaminodiphenyl sulfide (TDA) and 3,4′-diaminodiphenyl sulfide (3,4′-ODA).
[0049] The total molar amount of the diamine monomer is set to 1.000 mol, and its specific composition is as follows:
[0050] MPD: 0.960 mol (96 mol% of total diamine);
[0051] TDA: 0.020 mol (2 mol% of total diamine);
[0052] 3,4′-ODA: 0.020 mol (2 mol% of total diamine);
[0053] The total amount of TDA and 3,4′-ODA is 4 mol%, not exceeding 6 mol%;
[0054] The amount of IPC fed is 1.008 mol, that is, the molar ratio of IPC to total diamine R = 1.008, so that the resulting flexible modified meta-position stock solution retains about 0.8 mol% of residual acyl chloride end capping;
[0055] The monomer concentration in the reaction system is 0.95 mol / L.
[0056] Preparation Example 2
[0057] The specific steps for preparing the cooling-antibacterial composite powder are as follows:
[0058] (a): Cooling powder pretreatment: 100g of cooling powder, 200g of ethanol, and 1.5g of 3-aminopropyltriethoxysilane (APTES) were added to a container, stirred evenly, refluxed at 60℃ for 3h, filtered, and washed with ethanol to obtain silanized cooling cores; through the silanization pretreatment in step (a), highly reactive amino functional groups were introduced on the surface of the cooling powder, which not only significantly improved the dispersion stability of the powder in the organic spinning solution, but more importantly, facilitated the electrostatic adsorption of PEI and Ag in the subsequent step (b). + The coordination locking provides the necessary chemical anchors, thereby constructing a dense three-layer coating structure that ensures the long-term sustained release of silver ions.
[0059] (b): Inner layer construction: 10g of silanized cooling core was dispersed in 100g of deionized water and sonicated at 40 kHz for 20 min. 20.0g of high molecular weight polyethyleneimine (PEI) solution was added dropwise, and the pH was adjusted to 5 with acetic acid. The mixture was stirred at 300 r / min and 25℃ for 1 h to allow PEI to tightly coat the powder surface and micropores through electrostatic adsorption and hydrogen bonding. Then, 0.34g of AgNO3 solution was added, and stirring continued for 30 min. + N→Ag coordination bonds are formed with the —NH2 / —NH groups of PEI, firmly locking silver ions in the inner layer and preventing their reduction and aggregation in the organic phase. After centrifugation and washing twice with deionized water, a cooling-antibacterial precursor powder is obtained. The centrifugation rate is 8000 r / min, and the centrifugation time is 10 min. High molecular weight PEI is used to coat the powder surface and micropores, and the Ag ions are held together by N→Ag coordination bonds. + Securely locked in the inner layer to prevent Ag + The PEI is lost during subsequent organic phase processing; the low molecular weight PEI provides a high density of terminal amino groups, which act as "anchors" to react chemically with the aramid matrix. The synergistic effect of the two-layer structure ensures both long-lasting antibacterial effect and strong interfacial bonding between the powder and the matrix.
[0060] Specifically, the high molecular weight polyethyleneimine has a molecular weight of 10,000 and a mass fraction of 3 to 10 wt%, preferably 5 wt%.
[0061] Specifically, the cooling powder is a mixture of nano-mica and boron nitride in a mass ratio of 7:3, with a D50 of 0.8 μm.
[0062] Preferably, the mass fraction of the AgNO3 solution is 1 wt%.
[0063] (c): Outer layer construction: 100g of cooling-antibacterial precursor powder was dispersed in 300g of anhydrous ethanol, 2.0g of low molecular weight polyethyleneimine solution and 1.0g of APTES were added, refluxed at 60℃ for 1 h, centrifuged, washed twice with ethanol, and vacuum dried at 60℃ for 12 h to obtain cooling-antibacterial composite powder. The terminal amino groups of low molecular weight PEI are chemically bonded to the groups on the powder surface to form a dense -NH2 outer layer. The silanol groups after hydrolysis of APTES can partially condense with the amino groups on the PEI chain, stitching the loose low molecular weight PEI segments together to form a dense siloxane-polyamine hybrid network, effectively blocking Ag locked by the inner layer. + It escapes outwards, enhancing its long-lasting antibacterial properties.
[0064] Specifically, the low molecular weight polyethyleneimine has a molecular weight of 300-600 and a mass fraction of 1-5 wt%, preferably 3 wt%.
[0065] Example 1
[0066] This embodiment provides a method for preparing high-performance cooling and antibacterial aramid fiber, including the following steps:
[0067] (1) Preparation of the flexible modified meta-solution of Preparation Example 1;
[0068] (2) Preparation of the cooling-antibacterial composite powder of Example 2;
[0069] (3) Preparation of grafted blend: 3.0 g of cooling-antibacterial composite powder from Preparation Example 2 was dissolved in 20 ml of DMAc, ultrasonically dispersed at 40 kHz for 20 min, and added to the flexible modified meta-solvent obtained from Preparation Example 1. The reaction temperature was controlled at 75 °C, the stirring time was 1 h, and the stirring rate was 400 r / min to obtain the blend.
[0070] (4) Preparation of spinning solution; the residual COCl equivalent was measured to be approximately 0.003 mol; 0.31 g of aniline end-capping agent was added and stirred at 25°C for 30 min; the residual acyl chloride was reduced to <0.5% (based on the mass of the solution) to completely eliminate the risk of acyl chloride reacting with water to generate bubbles during the spinning process.
[0071] (5) Spinning and forming: After end sealing, the raw liquid is filtered through 20μm and 5μm filter cartridges in sequence, and vacuum degassed at 40℃ for 3 h to ensure that no particles block the spinneret holes. The spinning adopts dry-jet wet spinning process: the raw liquid is extruded through the spinneret, passes through a 10 mm air layer and forms a hot pre-stretch at 60℃, and then undergoes two-stage gradient coagulation bath solidification. After stretching and heat setting, the high-performance cool-feeling antibacterial aramid fiber is finally obtained. The first coagulation bath is DMAc and water with a mass ratio of 1:1 and a set temperature of 20℃. The second coagulation bath is DMAc and water with a mass ratio of 1:4 and a set temperature of 40℃. The total stretch ratio is controlled at 3.5 times, the heat setting temperature is 285℃, and the time is 2 min.
[0072] Example 2
[0073] (1) Preparation of the flexible modified meta-position stock solution of Example 1, wherein the monomer concentration of the reaction system was adjusted to 0.98 mol / L; the total molar amount of diamine monomer was still 1.000 mol, MPD was 0.958 mol (95.8 mol%), TDA was 0.021 mol (2.1 mol%), 3,4′-ODA was 0.021 mol (2.1 mol%), and the total amount of TDA and 3,4′-ODA was 4.2 mol%; the IPC feed amount was adjusted to 1.009 mol, R=1.009, and about 0.9 mol% of residual acyl chloride was retained for end capping;
[0074] (2) Preparation of the cooling-antibacterial composite powder of Example 2, wherein in step (a) the mass fraction of AgNO3 solution was adjusted to 0.8 wt% and the amount of feed was adjusted to 0.5 g; the mass fraction of high molecular weight PEI was adjusted to 6 wt%; and the mass fraction of low molecular weight PEI in step (b) was adjusted to 4 wt%.
[0075] (3) Preparation of grafted blend: Dissolve 3.2 g of cooling-antibacterial composite powder obtained in Preparation Example 2 in 20 mL of DMAc, disperse by ultrasonication at 40 kHz for 20 min, add to the flexible modified meta-position stock solution obtained in step (1), control the reaction temperature at 78℃, the stirring rate at 400 r / min, and the reaction time at 1 h to obtain the blend;
[0076] (4) Preparation of spinning solution: The residual COCl equivalent was measured to be approximately 0.0032 mol. 0.33 g of aniline end-capping agent was added and stirred at 25°C for 30 min to reduce the residual acyl chloride to <0.45% (based on the mass of the solution).
[0077] (5) Spinning and forming: After end sealing, the spinning solution is filtered through 20μm and 5μm filter elements in sequence, and vacuum degassing is performed at 40℃ for 3 h; the dry-jet wet spinning process parameters are the same as in Example 1, and finally high-performance cool-feeling antibacterial aramid fiber is obtained.
[0078] Example 3
[0079] This embodiment provides a method for preparing high-performance cooling and antibacterial aramid fiber, including the following steps:
[0080] (1) Preparation of the flexible modified meta-solution of Preparation Example 1;
[0081] The monomer concentration in the reaction system was adjusted to 0.92 mol / L.
[0082] The total molar amount of diamine monomers remains 1.000 mol, MPD is 0.962 mol (96.2 mol%), TDA is 0.019 mol (1.9 mol%), and 3,4′-ODA is 0.019 mol (1.9 mol%). The total amount of TDA and 3,4′-ODA is 3.8 mol%.
[0083] The IPC feed rate was adjusted to 1.007 mol, R=1.007, retaining approximately 0.7 mol% of residual acyl chloride for end capping;
[0084] (2) Preparation of the cooling-antibacterial composite powder of Example 2, wherein in step (a) the mass fraction of AgNO3 solution was adjusted to 0.6 wt% and the amount of feed was adjusted to 0.4 g; the mass fraction of high molecular weight PEI was adjusted to 6 wt%; and the mass fraction of low molecular weight PEI in step (b) was adjusted to 4 wt%.
[0085] (3) Preparation of grafted blend: Dissolve 2.8g of cooling-antibacterial composite powder obtained in Preparation Example 2 in 20 mL of DMAc, disperse by ultrasonication at 40 kHz for 20 min, add to the flexible modified meta-position stock solution obtained in step (1), control the reaction temperature at 72℃, the stirring rate at 400 r / min, and the reaction time at 1 h to obtain the blend;
[0086] (4) Preparation of spinning solution: The residual COCl equivalent was measured to be approximately 0.0028 mol. 0.29 g of aniline end-capping agent was added and stirred at 25°C for 30 min to reduce the residual acyl chloride to <0.55% (based on the mass of the solution).
[0087] (5) Spinning and forming: Same as in Example 1.
[0088] Comparative Example 1
[0089] Comparative Example 1
[0090] Based on Example 1, the difference lies in the preparation of the modified meta-position stock solution. Specifically, the diamine monomer is dissolved in a polar aprotic solvent, stirred at -10°C for 0.5 h, 25% isophthaloyl chloride is added for prepolymerization, low-temperature polycondensation reaction is carried out for 2 h, and then the remaining 75% isophthaloyl chloride is added, and the temperature is raised to 55°C for aging for 10 min to obtain the modified meta-position stock solution. The rest is the same as in Example 1.
[0091] Comparative Example 2
[0092] The difference between this comparative example and Example 1 is that the cooling powder pretreatment step is not included in Preparation Example 2.
[0093] Comparative Example 3
[0094] Based on Example 1, the difference is that in Preparation Example 2, the outer layer construction is not included. The inner layer construction is as follows: 10g of cooling powder is dispersed in 100ml of deionized water, sonicated at 40 kHz for 20 min, 40.0g of high molecular weight polyethyleneimine (PEI) solution is added dropwise, the pH is adjusted to 5 with acetic acid, and stirred at 300 r / min and 25℃ for 12 h. Then, 0.36g of AgNO3 solution is added, and stirring is continued for 30 min. After centrifugation and washing twice with deionized water, the cooling-antibacterial precursor powder is obtained. The rest is the same as in Example 1.
[0095] The performance of the aramid fibers prepared in Examples 1-3 and Comparative Examples 1-3 was tested. The specific test data are shown in Table 1 below, and the relevant test methods are as follows:
[0096] (1) Cooling performance test method: The test was conducted according to the national standard GB / T35263-2017.
[0097] (2) Test method for fiber breaking strength: The test shall be conducted in accordance with the test method of GB / T 14337-2008.
[0098] (3) Flame retardant performance test method: The test shall be conducted in accordance with the test method of GB / T2406.
[0099] (4) Antibacterial test method: The test shall be conducted in accordance with GB / T 20944.3-2008 "Evaluation of antibacterial properties of textiles - Part 3: Vibration method".
[0100] (5) Antibacterial stability test method: 10cm×10cm cool fiber fabric was stirred and washed in 1kg of 20℃ deionized water for 10 minutes. The washing process was repeated 50 times under the same conditions. After drying, the antibacterial performance of each fabric was tested again.
[0101] (6) Test method for silver ion concentration: Refer to GB / T 20944.3-2008 "Evaluation of antibacterial properties of textiles - Part 3: Shaking method", place the fiber sample in PBS buffer (pH 7.2), shake at 37℃ and 150 rpm for 1 h, take the supernatant and filter it through a 0.22 μm filter membrane, and determine the silver ion concentration by ICP-MS.
[0102] Table 1
[0103] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Cooling coefficient (J / (cm²·s)) 0.228 0.235 0.221 0.210 0.185 0.215 Fracture strength (cN / dtex) 4.58 4.62 4.52 3.85 4.10 4.25 Elongation at break (%) 31.5 32.8 30.2 25.4 28.5 29.0 LOI (%) 29.5 29.8 29.3 28.5 29.2 29.1 Antibacterial rate (Staphylococcus aureus, %) 99.2 99.6 99.5 93.5 95.3 96.0 Antibacterial rate (Escherichia coli, %) 99.8 99.9 99.9 90.2 92.1 91.0 Antibacterial rate (Staphylococcus aureus, %) after 50 washes 98.5 98.7 98.8 80.5 81.2 56.5 Silver ion concentration mg / L <0.05 <0.05 <0.05 0.15 0.18 0.14
[0104] As can be seen from the data in Table 1, the high-performance cooling and antibacterial aramid fibers prepared in Examples 1-3 of this invention maintain excellent mechanical properties and flame retardancy while also exhibiting significant cooling effects and long-lasting antibacterial properties. This is attributed to the synergistic effect of the double-layer PEI silver-locking structure and residual acyl chloride grafting, which ensures the firm anchoring of cooling powder and silver ions in the fiber matrix.
[0105] Comparing Example 1 with Comparative Example 1, it can be seen that if the amount of IPC added is too large and the curing time is insufficient, it will lead to uneven distribution of polymer molecular weight and excessive residual acyl chloride. This not only makes it easy to generate bubbles during spinning, but also leads to a significant decrease in the mechanical properties of the fiber. At the same time, excessive free acyl chloride may react with silver ions, affecting antibacterial stability.
[0106] Comparing Example 1 and Comparative Example 2, it can be seen that if the silanization pretreatment of the cooling powder is omitted, the interfacial bonding force between the powder and the polymer matrix decreases significantly, resulting in a reduction in the cooling factor. Furthermore, the antibacterial rate decreases drastically after washing, and the silver ion content in the solution is high after water washing. This demonstrates that the silanization pretreatment step is crucial for improving powder dispersibility, reactivity, and water washability.
[0107] Comparing Example 1 and Comparative Example 3, it can be seen that by precisely controlling the molecular weight and dosage of PEI, a triple protection system of high molecular weight PEI silver locking, low molecular weight PEI anchoring, and APTES crosslinking can be constructed.
[0108] While the present invention has been disclosed above, it is not limited thereto. Any person skilled in the art can make various modifications and alterations without departing from the spirit and scope of the invention; therefore, the scope of protection of the present invention should be determined by the scope defined in the claims.
Claims
1. A method for preparing high-performance cooling and antibacterial aramid fiber, characterized in that, Includes the following steps: (1) Preparation of flexible modified meta-solution; (2) Preparation of cooling-antibacterial composite powder; (3) Preparation of grafting blend solution; (4) Preparation of spinning solution; (5) Spinning and forming; The preparation process of the flexible modified meta-aramid solution includes dissolving a diamine monomer in a polar aprotic solvent, adding isophthaloyl chloride for low-temperature solution polycondensation, and obtaining a flexible modified meta-aramid solution; the diamine monomer is composed of m-phenylenediamine, 4,4′-diaminodiphenyl sulfide and 3,4′-diaminodiphenyl ether.
2. The preparation method according to claim 1, characterized in that, The preparation process of the flexible modified meta-solvent includes dissolving the diamine monomer in a polar aprotic solvent, stirring at -15 to -8°C for 0.5 to 1 hour, adding 75 to 85% isophthaloyl chloride for prepolymerization, performing a low-temperature polycondensation reaction for 1 to 4 hours, adding the remaining 15 to 25% isophthaloyl chloride, and aging at 50 to 65°C for 55 to 65 minutes to obtain the flexible modified meta-solvent.
3. The preparation method according to claim 1, characterized in that, Based on the total molar amount of diamine, the feeding ratio of each component is as follows: m-phenylenediamine 94-98 mol%, 4,4′-diaminodiphenyl sulfide 1-3 mol%, 3,4′-diaminodiphenyl sulfide 1-3 mol%, and the total amount of 4,4′-diaminodiphenyl sulfide and 3,4′-diaminodiphenyl sulfide does not exceed 6 mol%, and the molar ratio of isophthaloyl chloride to the total diamine is 1.001-1.
02.
4. The preparation method according to claim 1, characterized in that, The polar aprotic solvent is one or more of N,N-dimethylacetamide, N-methylpyrrolidone, dimethyl sulfoxide, N,N-dimethylformamide, and hexamethylphosphoric triamine.
5. The preparation method according to claim 1, characterized in that, In step (2), the preparation of the cooling-antibacterial composite powder includes the following steps: (a) Pretreatment of cooling powder to obtain silanized cooling core; (b) Disperse the silanized cooling core in deionized water, add high molecular weight polyethyleneimine solution, adjust the pH, stir for a period of time, then add antibacterial agent, continue stirring, centrifuge and wash with water to obtain cooling-antibacterial precursor powder; (c) Disperse the cooling-antibacterial precursor powder in anhydrous ethanol, add low molecular weight polyethyleneimine solution and 3-aminopropyltriethoxysilane, react for a period of time, centrifuge, wash and dry to obtain cooling-antibacterial composite powder.
6. The preparation method according to claim 5, characterized in that, The cooling powder is one or more of the following: nano mica, hexagonal boron nitride, nano jade, mesoporous alumina, nano alumina, aluminum nitride, and shell powder.
7. The preparation method according to claim 1, characterized in that, In step (3), the cooling-antibacterial composite powder is dissolved in a polar aprotic solvent, ultrasonically dispersed for a period of time, added to the flexible modified meta-solution obtained in (1), the reaction temperature is controlled, and the mixture is stirred for a period of time to obtain a blend.
8. The preparation method according to claim 7, characterized in that, The ultrasonic dispersion time is 10~30 min.
9. The preparation method according to claim 7, characterized in that, The reaction temperature is 70~80℃, the stirring time is 0.5~1.5h, and the stirring rate is 350~450r / min.
10. A high-performance cooling and antibacterial aramid fiber, characterized in that, It is obtained by the preparation method described in any one of claims 1 to 9.
Citation Information
Patent Citations
Method and device for preparing antibacterial meta-aramid filament by dry-wet spinning
CN117364275B
Metaposition aramid cool fiber and preparation method thereof
CN121853201B