A bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting and its preparation process
By using composite materials containing poly(L-lactic acid) and poly(D-lactic acid) and segmented stretching processes, the problems of strength, toughness, and biodegradability of sports and leisure netting materials have been solved, resulting in high-performance bio-based biodegradable sports and leisure netting.
Patent Information
- Application Number
- CN202611345211.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-01
- Publication Date
- 2026-11-17
AI Technical Summary
Existing sports and leisure netting materials cannot guarantee strength and toughness while also meeting the requirements of weather resistance and biodegradability for long-term use. Furthermore, traditional modifiers suffer from problems such as insufficient interfacial compatibility, high cost, and complex processes.
Bio-based biodegradable sports and leisure netting was prepared by using a composite material of poly(L-lactic acid), poly(D-lactic acid), bio-based polybutylene succinate, microcrystalline cellulose, epoxidized soybean oil grafted citric acid cellulose, zinc gallate complexed lignin nanoparticles, and calcium stearate through a twin-screw extruder melt blending and segmented stretching process.
It improves the material's crystallization ability, heat resistance, and dimensional stability; enhances the strength and toughness of monofilaments; improves interfacial bonding; reduces the material's hydrophilicity; enhances impact resistance and UV aging resistance; reduces melt adhesion and spinning breakage; and achieves good processing stability and biodegradability.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention belongs to the field of bio-based biodegradable polymer material modification technology, specifically relating to a bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting and its preparation process. Background Technology
[0002] Sports and leisure netting is widely used in football, volleyball, badminton, tennis, climbing, protective gear, hammocks, and outdoor recreational facilities. During use, it must withstand long-term tensile loads, ball impacts, repeated bending, net knot compression, wind vibration, and temperature and humidity changes. Existing sports and leisure netting is typically made of petroleum-based polymers such as polyethylene, polypropylene, polyamide, or polyester. While these materials offer good strength, abrasion resistance, and processing stability, they are difficult to degrade in the natural environment after disposal, easily leading to persistent plastic waste and microplastic pollution. Sports and leisure netting is characterized by its numerous mesh openings, large surface area, difficulty in recycling and sorting, and dispersed usage locations. After disposal, it easily enters soil, water bodies, or the open environment, and traditional incineration further increases energy consumption and carbon emissions. Therefore, replacing traditional petroleum-based netting materials with renewable and degradable polymers under controlled conditions has become an important direction for the green development of sports equipment and outdoor leisure products.
[0003] Polylactic acid (PLA) is mainly prepared from lactic acid obtained through the fermentation of renewable biomass. It boasts advantages such as wide availability, melt processing, good biocompatibility, and biodegradability under suitable composting conditions. Furthermore, it possesses high tensile strength and transparency, making it a promising candidate material for preparing biodegradable fibers and monofilaments for mesh fabrics. However, PLA's molecular chains are relatively rigid, resulting in significant brittleness, notch sensitivity, and insufficient impact resistance and repeated bending performance. Stress concentration easily occurs at knots, intersections, and areas impacted by spheres, leading to monofilament cracking or breakage. PLA has a slow crystallization rate and is prone to dimensional changes and creep under sustained loads after heating. During outdoor use, moisture can penetrate the amorphous regions of PLA and cause ester bond hydrolysis. Ultraviolet radiation and oxygen further promote molecular chain breakage, gradually reducing the strength and toughness of the mesh fibers. Using PLA alone is insufficient to simultaneously meet the comprehensive requirements of sports and leisure nets for knot strength, impact toughness, fatigue resistance, resistance to damp heat, resistance to ultraviolet aging, and long-term dimensional stability.
[0004] Cellulose is abundant, has low density, high specific strength, and is renewable and biodegradable. Adding microcrystalline cellulose to polylactic acid (PLA) can improve the material's rigidity and promote PLA crystallization. However, cellulose contains a large number of hydroxyl groups on its surface, making it highly hydrophilic and resulting in insufficient interfacial compatibility with PLA. During melt blending, it easily agglomerates and forms interfacial pores. The moisture adsorbed by cellulose also accelerates the hydrolytic degradation of PLA during high-temperature processing, causing a decrease in melt viscosity, a reduction in molecular weight, filament breakage, and fluctuations in spinning pressure. Existing technologies typically use free plasticizers, petroleum-based elastomers, coupling agents, UV absorbers, or ordinary lignin to improve the properties of PLA composites. However, free plasticizers are prone to migration and reduce heat resistance, petroleum-based elastomers reduce the material's bio-based properties and degradation performance, some coupling agents are costly and have complex processing conditions, and ordinary lignin has problems such as dark color, difficulty in dispersion, and insufficient interfacial bonding. Furthermore, existing research on polylactic acid cellulose composites largely focuses on ordinary injection-molded products, films, or short-term static mechanical properties, lacking systematic consideration of the continuous melt spinning, segmented drawing, heat setting, network durability, and outdoor aging performance required for sports and leisure netting monofilaments. Therefore, it is necessary to develop polylactic acid cellulose composites and their preparation processes that possess good interfacial compatibility, melt spinning stability, strength, toughness, weather resistance, thermal dimensional stability, and biodegradability. Summary of the Invention
[0005] To address the shortcomings of existing technologies, the present invention aims to provide a bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting, comprising the following components in parts by weight:
[0006] Poly(L-lactic acid) 75.0-82.0 parts, poly(D-lactic acid) 2.0-4.0 parts, bio-based polybutylene succinate 7.0-12.0 parts, microcrystalline cellulose 5.0-9.0 parts, epoxidized soybean oil-grafted citric acid cellulose 1.5-3.5 parts, zinc gallate-complexed lignin nanoparticles 0.4-1.2 parts, tributyl acetylacetonate 0.8-1.8 parts, and calcium stearate 0.2-0.5 parts.
[0007] According to a preferred embodiment of the present invention, the method for preparing the epoxidized soybean oil grafted with citric acid cellulose includes:
[0008] A1. By weight, add 90.0-110.0 parts of microcrystalline cellulose to 250.0-400.0 parts of deionized water, stir and disperse, add 18.0-30.0 parts of citric acid monohydrate and 6.0-9.0 parts of sodium hypophosphite monohydrate, stir and impregnate at 45-55℃ to obtain impregnated microcrystalline cellulose; dry the impregnated microcrystalline cellulose at 65-75℃, and then carry out solid-phase esterification at 145-160℃; after solid-phase esterification, wash with deionized water, vacuum dry, grind and vibrate sieve to obtain citric acid cellulose;
[0009] A2. Add 15.0-25.0 parts of epoxidized soybean oil and 0.3-0.8 parts of tetrabutylammonium bromide to 250.0-400.0 parts of acetone and stir to obtain an epoxidized soybean oil reaction solution. Add 90.0-110.0 parts of citric acid cellulose to a mixer. While stirring, spray the epoxidized soybean oil reaction solution into the mixer. Under vacuum conditions at 40-55℃, recover the acetone to obtain the material after acetone recovery. Under nitrogen protection, heat the material after acetone recovery to 115-130℃ for reaction. After the reaction is completed, cool, add acetone for washing, filter, and collect the filter cake. Vacuum dry, grind, and vibrate sieve the filter cake.
[0010] According to a preferred embodiment of the present invention, in step A1, the solid-phase esterification time at 145-160°C is 30-50 min.
[0011] According to a preferred embodiment of the present invention, in step A2, the reaction time at 115-130°C is 2.5-4.0 h.
[0012] According to a preferred embodiment of the present invention, the method for preparing the zinc gallate-complexed lignin nanoparticles includes:
[0013] B1. By weight, add 90.0-110.0 parts of alkali lignin and 12.0-18.0 parts of sodium hydroxide to 800.0-1200.0 parts of deionized water, stir at 45-55℃, filter, and obtain an alkaline lignin solution; under nitrogen protection, add 12.0-16.0 parts of gallic acid to the alkaline lignin solution, stir, and obtain an alkaline lignin solution containing gallic acid; dissolve 5.0-8.0 parts of zinc acetate dihydrate in 100.0-180.0 parts of deionized water to obtain an aqueous zinc acetate solution; under stirring, add the aqueous zinc acetate solution dropwise to the alkaline lignin solution containing gallic acid, adjust the pH to 11.0-12.0 with an aqueous sodium hydroxide solution, stir the reaction at 25-35℃, and obtain a zinc gallate-lignin complex dispersion;
[0014] B2. Under shearing conditions, dilute sulfuric acid is added dropwise to the zinc gallate-lignin complex dispersion to adjust the pH to 6.0-7.0, and the mixture is aged at 25-35℃. After aging, the mixture is centrifuged and washed to obtain wet complexed lignin nanoparticles. The wet complexed lignin nanoparticles are dispersed in 400.0-600.0 parts of deionized water to obtain a nanoparticle slurry. The nanoparticle slurry is spray-dried, and then ground and vibrated sieved.
[0015] According to a preferred embodiment of the present invention, in step B1, the stirring reaction time at 25-35°C is 60-120 min.
[0016] According to a preferred embodiment of the present invention, in step B2, the aging time at 25-35°C is 2.0-4.0 h.
[0017] This invention also provides a preparation process for the aforementioned bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting, comprising the following steps:
[0018] S1. Poly(L-lactic acid), poly(D-lactic acid), bio-based polybutylene succinate, microcrystalline cellulose, epoxidized soybean oil-grafted citric acid cellulose, and zinc gallate-complexed lignin nanoparticles are dried separately. 25-35% of poly(L-lactic acid), microcrystalline cellulose, epoxidized soybean oil-grafted citric acid cellulose, and 40-60% of acetylated tributyl citrate are mixed and stirred at 55-65°C to obtain a premix. The premix is then... The material is added to a twin-screw extruder, melt-blended at 175-190℃, vacuum-de-squeezed, and extruded into pellets to obtain cellulose composite masterbatch; the cellulose composite masterbatch is mixed with the remaining poly(L-lactic acid), the remaining tributyl acetyl citrate, poly(D-lactic acid), bio-based polybutylene succinate, zinc gallate complexed lignin nanoparticles, and calcium stearate, added to a twin-screw extruder, melt-blended at 180-195℃, vacuum-de-squeezed, filtered, extruded into pellets, and dried to obtain composite granules;
[0019] S2. Add the composite granules to a melt spinning machine and melt them at 185-200℃. Extrude them through the spinneret and cool and set them at 20-30℃ to obtain nascent yarn. Perform the first stage of drawing on the nascent yarn at 75-90℃, and then perform the second stage of drawing at 95-110℃. Subsequently, perform heat setting and controlled shrinkage to obtain monofilaments for orientation webs. Form the orientation webs into a web and relax and set it at 60-80℃.
[0020] According to a preferred embodiment of the present invention, in step S1, the stirring time at 55-65°C is 5-10 min.
[0021] According to a preferred embodiment of the present invention, in step S2, the heat setting temperature is 110-130°C.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] (1) This invention uses poly-L-lactic acid as the continuous phase, and forms a structurally stable stereocomposite crystal between poly-D-lactic acid and poly-L-lactic acid, thereby improving the crystallization ability, heat resistance and dimensional stability of the composite material, and reducing creep and relaxation of sports and leisure nets under continuous stress and temperature changes. Bio-based polybutylene succinate has flexible molecular chain segments, which can improve the problems of poly-L-lactic acid's high brittleness and insufficient impact resistance; microcrystalline cellulose plays a reinforcing and heterogeneous nucleation role, which is beneficial to improving the strength and rigidity of the net monofilaments. Acetyl tributyl citrate improves the melt flowability and drawing processing performance of each component, and calcium stearate reduces the friction between the material and the processing equipment, reduces melt adhesion, die buildup and monofilament surface defects, so that the composite material has good strength, toughness and processing stability.
[0024] (2) Grafting citric acid cellulose with epoxidized soybean oil can reduce the hydrophilicity and aggregation tendency of microcrystalline cellulose surface, enhance the interfacial bonding between microcrystalline cellulose and poly(L-lactic acid) and bio-based polybutylene succinate, effectively transfer external force from the poly(L-lactic acid) matrix to the microcrystalline cellulose reinforcing phase, and dissipate the concentrated stress of the network knots and impact points through the deformation of flexible fatty chain segments, thereby improving the breaking elongation, knot strength and repeated bending durability of the network monofilaments. Zinc gallate complexed lignin nanoparticles can absorb ultraviolet light, remove free radicals generated during photo-oxidation and promote poly(L-lactic acid) crystallization, slow down the photo-oxidative breakage of poly(L-lactic acid) and bio-based polybutylene succinate molecular chains, and improve the UV aging resistance and service stability of the composite material.
[0025] (3) This invention employs a process combining pre-fabrication of cellulose composite masterbatch and secondary melt blending of composite granules. This allows microcrystalline cellulose and epoxidized soybean oil-grafted citric acid cellulose to be fully dispersed in a portion of poly-L-lactic acid, and then uniformly blended with the remaining poly-L-lactic acid, poly-D-lactic acid, bio-based polybutylene succinate, zinc gallate-complexed lignin nanoparticles, tributyl acetyl citrate, and calcium stearate. This reduces microcrystalline cellulose agglomeration, melt pressure fluctuations, and spinning breakage. Segmented stretching orients the molecular chains of poly-L-lactic acid, poly-D-lactic acid, and bio-based polybutylene succinate along the monofilament axis. Heat setting and controlled shrinkage further stabilize the orientation and crystalline structure, resulting in sports and leisure netting with good tensile strength, impact resistance, fatigue resistance, damp heat resistance, and dimensional stability. It can also be gradually degraded under suitable controlled treatment conditions, reducing persistent plastic pollution caused by waste sports and leisure netting. Detailed Implementation
[0026] To facilitate understanding of the present invention, the following embodiments are provided. Those skilled in the art should understand that these embodiments are merely illustrative and should not be construed as limiting the scope of the invention.
[0027] Example 1
[0028] This embodiment provides a method for preparing a bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting, the steps of which include:
[0029] Step S1: Take sufficient amounts of poly(L-lactic acid), poly(D-lactic acid), and bio-based polybutylene succinate, and dry them at 70°C and -0.08 MPa for 8 hours; take sufficient amounts of microcrystalline cellulose, epoxidized soybean oil-grafted citric acid cellulose, zinc gallate-complexed lignin nanoparticles, and calcium stearate, and dry them at 60°C and -0.08 MPa for 8 hours; take sufficient amounts of acetylated tributyl citrate and dehydrate them at 60°C and -0.08 MPa for 4 hours; after drying, cool each material to 25°C in a desiccator and seal them for storage. Measure the moisture content using a moisture analyzer. The moisture content of bio-based polybutylene succinate, microcrystalline cellulose, epoxidized soybean oil-grafted citric acid cellulose, and zinc gallate-complexed lignin nanoparticles is no greater than 0.02%, and the moisture content of acetylthiol tributyl citrate and calcium stearate is no greater than 0.05%. Weigh out 78.50g of dried poly-L-lactic acid, 3.00g of dried poly-D-lactic acid, 9.50g of dried bio-based polybutylene succinate, 7.00g of dried microcrystalline cellulose, 2.50g of dried epoxidized soybean oil-grafted citric acid cellulose, 0.80g of dried zinc gallate-complexed lignin nanoparticles, 1.30g of dehydrated acetylthiol tributyl citrate, and 0. 0.35g calcium stearate; Take 23.55g dried poly-L-lactic acid, and add it to a high-speed mixer along with 7.00g dried microcrystalline cellulose, 2.50g dried epoxidized soybean oil-grafted citric acid cellulose, and 0.65g dehydrated acetylated tributyl citrate. Stir at 60°C and 800r / min for 7.5min to obtain a premix; Add the premix to a twin-screw extruder and melt-blend and vacuum degas at 182.5°C, screw speed 180r / min, and vacuum degree -0.08MPa. Extrude, cool, and pelletize to obtain cellulose composite masterbatch; Combine the cellulose composite masterbatch with the remaining 54.95g dried poly-L-lactic acid. The following ingredients were mixed for 5 min: cyclolactic acid, the remaining 0.65 g of dehydrated tributyl acetylacetonate, 3.00 g of dried poly(D-lactic acid), 9.50 g of dried bio-based polybutylene succinate, 0.80 g of dried zinc gallate complexed lignin nanoparticles, and 0.35 g of dried calcium stearate. The mixture was then fed into a twin-screw extruder and melt-blended under conditions of 187.5°C, screw speed of 180 r / min, and vacuum degree of -0.08 MPa. The melt was then passed through a 150 μm filtration device, extruded, cooled, and pelletized. The resulting pellets were dried at 70°C and vacuum degree of -0.08 MPa for 8 h to obtain composite pellets.
[0030] Step S2: The composite granules are added to a melt spinning machine and melted at 192.5°C. The granules are then extruded through a spinneret with a diameter of 1.15 mm and cooled and shaped in air at 25°C to obtain nascent filaments. The nascent filaments are then stretched in the first stage at 82.5°C with a draw ratio of 3.0:1, and then stretched in the second stage at 102.5°C with a draw ratio of 1.5:1. The stretched monofilaments are then tension heat-set at 120°C for 60 seconds and subjected to 5% controlled shrinkage to obtain monofilaments for oriented mesh with a diameter of 0.50 mm. The monofilaments for oriented mesh are then woven into a sports and leisure net with a mesh side length of 70 mm and relaxed and shaped at 70°C for 10 minutes to obtain a polylactic acid cellulose composite material product for bio-based biodegradable sports and leisure nets.
[0031] Preparation steps of epoxidized soybean oil grafted with citric acid cellulose:
[0032] Step A1: Add 325.0 g of deionized water to a reaction vessel equipped with a mechanical stirrer, add 100.0 g of microcrystalline cellulose at 800 rpm, and continue stirring for 20 min to ensure uniform dispersion of the microcrystalline cellulose; add 24.0 g of citric acid monohydrate and 7.5 g of sodium hypophosphite monohydrate, raise the temperature to 50°C, and stir and impregnate at 500 rpm for 45 min to obtain impregnated microcrystalline cellulose; after impregnation, do not filter, transfer all material to a drying tray, and air dry at 70°C. The material was dried for 8 hours, turning it over every 2 hours during the drying process to ensure that citric acid monohydrate and sodium hypophosphite monohydrate were evenly loaded onto the surface of the microcrystalline cellulose. The dried material was placed in a heat-resistant reaction vessel and solid-phase esterification was carried out at 152.5°C for 40 minutes. The material was then removed and cooled to 25°C. The solid-phase esterified material was washed with 1000.0g of deionized water, and the solid was collected by filtration. The solid was dried at 70°C and a vacuum of -0.08MPa for 8 hours. After grinding, the solid was passed through a vibrating sieve with a pore size of 45μm to obtain citric acid cellulose.
[0033] Step A2: Add 325.0g of acetone, then add 20.0g of epoxidized soybean oil and 0.55g of tetrabutylammonium bromide to a sealed stirring container. Stir at 400r / min for 20min to obtain a homogeneous epoxidized soybean oil reaction solution. Add 100.0g of citric acid cellulose to a mixer and stir at 600r / min. Spray the epoxidized soybean oil reaction solution evenly into the mixer within 30min. After spraying, maintain the mixer temperature at 47.5°C and the vacuum degree at -0.08MPa, stir at 300r / min, and recover the acetone. The acetone mass fraction in the material was increased to no more than 0.5%. Nitrogen gas was introduced into the mixer at a rate of 0.5 L / min, and the material was heated to 122.5°C and reacted at 300 r / min for 3.25 h. After the reaction was completed, the mixture was cooled to 25°C, and 200.0 g of acetone was added and stirred and washed for 20 min. After filtration, another 200.0 g of acetone was added and stirred and washed for 20 min. The filter cake was collected after filtration. The filter cake was dried at 70°C and under a vacuum of -0.08 MPa for 8 h. After grinding, the mixture was passed through a vibrating sieve with a pore size of 45 μm to obtain epoxidized soybean oil grafted citric acid cellulose.
[0034] Preparation steps of zinc gallate-complexed lignin nanoparticles:
[0035] Step B1: Add 100.0g of alkali lignin and 15.0g of sodium hydroxide to 1000.0g of deionized water, stir at 50°C and 500r / min for 90min, filter using a 10μm pore size filter to remove insoluble matter, and obtain an alkaline lignin solution; purge with nitrogen at 0.5L / min, add 14.0g of gallic acid to the alkaline lignin solution at 400r / min, and continue stirring for 30min to obtain an alkaline lignin solution containing gallic acid; add 6.5g of zinc acetate dihydrate to 140.0g of deionized water. In deionized water, the mixture was stirred at 25°C and 300 rpm for 15 min to obtain an aqueous solution of zinc acetate. The zinc acetate aqueous solution was then added dropwise to a lignin alkaline solution containing gallic acid over 45 min while stirring at 800 rpm. A 10% sodium hydroxide aqueous solution was prepared using 3.0 g of sodium hydroxide and 27.0 g of deionized water. The sodium hydroxide aqueous solution was added dropwise, and the pH was adjusted to 11.5. After the addition was complete, the mixture was stirred at 30°C and 600 rpm for 90 min to obtain a zinc gallate-lignin complex dispersion.
[0036] Step B2: Prepare 238.0 g of dilute sulfuric acid using 24.29 g of 98% sulfuric acid and 213.71 g of deionized water; maintain the zinc gallate-lignin complex dispersion at 30°C and shear at 3000 r / min, adding dilute sulfuric acid dropwise over 60 min to adjust the pH to 6.5; after the addition is complete, reduce the shear rate to 500 r / min and age at 30°C for 3.0 h; after aging, centrifuge at 10000 r / min for 15 min. The precipitate was collected, washed with 1000.0g of deionized water, and centrifuged again to obtain wet complexed lignin nanoparticles. All wet complexed lignin nanoparticles were dispersed in 500.0g of deionized water and sheared at 3000r / min for 20min to obtain nanoparticle slurry. The nanoparticle slurry was spray-dried at an inlet air temperature of 170°C and an outlet air temperature of 75°C. The spray-dried product was ground and passed through a vibrating sieve with a pore size of 45μm to obtain zinc gallate complexed lignin nanoparticles.
[0037] Example 2
[0038] This embodiment provides a method for preparing a bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting, the steps of which include:
[0039] Step S1: Take sufficient amounts of poly(L-lactic acid), poly(D-lactic acid), and bio-based polybutylene succinate, and dry them at 70°C and a vacuum of -0.08 MPa for 8 hours; take sufficient amounts of microcrystalline cellulose, epoxidized soybean oil-grafted citric acid cellulose, zinc gallate-complexed lignin nanoparticles, and calcium stearate, and dry them at 60°C and a vacuum of -0.08 MPa for 8 hours; take sufficient amounts of acetylated tributyl citrate and dehydrate them at 60°C and a vacuum of -0.08 MPa for 4 hours; after treatment, cool each material to 25°C in a dryer and seal for storage to allow the poly(L-lactic acid), poly(D-lactic acid), and bio-based polybutylene succinate to dry. The moisture content of alcohol esters, microcrystalline cellulose, epoxidized soybean oil-grafted citric acid cellulose, and zinc gallate-complexed lignin nanoparticles is no greater than 0.02%, and the moisture content of acetylthiol tributyl citrate and calcium stearate is no greater than 0.05%. Weigh out 75.00g of dried poly-L-lactic acid, 2.00g of dried poly-D-lactic acid, 7.00g of dried bio-based polybutylene succinate, 5.00g of dried microcrystalline cellulose, 1.50g of dried epoxidized soybean oil-grafted citric acid cellulose, 0.40g of dried zinc gallate-complexed lignin nanoparticles, 0.80g of dehydrated acetylthiol tributyl citrate, and 0.20g of dried... 18.75g of dried poly-L-lactic acid was added to a high-speed mixer along with 5.00g of dried microcrystalline cellulose, 1.50g of dried epoxidized soybean oil-grafted citric acid cellulose, and 0.32g of dehydrated acetylacetic acid tributyl ester. The mixture was stirred at 55°C and 800r / min for 5min to obtain a premix. The premix was then added to a twin-screw extruder and melt-blended and vacuum-degassed at 175°C, 180r / min, and -0.08MPa. The mixture was extruded, cooled, and pelletized to obtain cellulose composite masterbatch. The cellulose composite masterbatch was then mixed with the remaining 56.25g of dried poly-L-lactic acid. The acid, the remaining 0.48g of dehydrated acetylic acid tributyl ester, 2.00g of dried poly(D-lactic acid), 7.00g of dried bio-based polybutylene succinate, 0.40g of dried zinc gallate complexed lignin nanoparticles, and 0.20g of dried calcium stearate were mixed for 5 min and added to a twin-screw extruder. The mixture was melt-blended and vacuum-degassed at 180°C, 180 r / min, and -0.08 MPa. The melt was then passed through a 150 μm filtration device, extruded, cooled, and pelletized. The resulting pellets were dried at 70°C and -0.08 MPa for 8 h to obtain composite pellets.
[0040] Step S2: Add the composite granules to a melt spinning machine, melt them at 185°C, extrude them through a spinneret with a diameter of 0.80 mm, and cool and set them in cooling air at 20°C to obtain nascent filaments; perform the first stage of drawing at 75°C with a draw ratio of 2.5:1, and then perform the second stage of drawing at 95°C with a draw ratio of 1.3:1; perform tension heat setting of the drawn monofilaments at 110°C for 30 seconds, and perform controlled shrinkage of 3% to obtain 0.20 mm diameter oriented mesh monofilaments; weave the oriented mesh monofilaments into a sports and leisure net with a mesh side length of 20 mm, relax and set it at 60°C for 5 minutes to obtain a polylactic acid cellulose composite material product for bio-based biodegradable sports and leisure nets.
[0041] Preparation steps of epoxidized soybean oil grafted with citric acid cellulose:
[0042] Step A1: Add 250.0 g of deionized water to a reaction vessel equipped with a mechanical stirrer, add 90.0 g of microcrystalline cellulose at 800 r / min, and continue stirring for 20 min; add 18.0 g of citric acid monohydrate and 6.0 g of sodium hypophosphite monohydrate, raise the temperature to 45°C, and stir and impregnate at 500 r / min for 45 min; after impregnation, do not filter, transfer all materials to a drying tray, and dry at 65°C with forced air for 8 h, turning the material every 2 h during the drying process; perform solid-phase esterification of the dried material at 145°C for 30 min, and cool to 25°C; wash with 900.0 g of deionized water, filter and collect the solid, dry the solid at 65°C and vacuum degree -0.08 MPa for 8 h, grind and pass through a vibrating sieve with a pore size of 45 μm to obtain citric acid cellulose.
[0043] Step A2: Add 250.0g of acetone, then add 15.0g of epoxidized soybean oil and 0.30g of tetrabutylammonium bromide to a sealed stirring container. Stir at 400r / min for 20min to obtain an epoxidized soybean oil reaction solution. Add 90.0g of citric acid cellulose to a mixer and stir at 600r / min. Spray the epoxidized soybean oil reaction solution evenly into the mixer within 30min. Stir at 300r / min under conditions of 40°C and a vacuum of -0.08MPa, and recover acetone until the material is completely dissolved. The mass fraction of acetone is not greater than 0.5%; nitrogen gas is introduced at 0.5 L / min to heat the material to 115°C and react at 300 r / min for 2.5 h; after cooling to 25°C, 150.0 g of acetone is added and stirred and washed for 20 min, filtered, and then another 150.0 g of acetone is added and stirred and washed for 20 min, filtered and the filter cake is collected; the filter cake is dried at 65°C and vacuum degree -0.08 MPa for 8 h, ground and passed through a vibrating sieve with a pore size of 45 μm to obtain epoxidized soybean oil grafted citric acid cellulose.
[0044] Preparation steps of zinc gallate-complexed lignin nanoparticles:
[0045] Step B1: Add 90.0 g of alkali lignin and 12.0 g of sodium hydroxide to 800.0 g of deionized water, stir at 45°C and 500 r / min for 90 min, and filter using a 10 μm pore size filter to obtain an alkaline lignin solution; purge nitrogen gas at 0.5 L / min, add 12.0 g of gallic acid at 400 r / min, and continue stirring for 30 min; add 5.0 g of zinc acetate dihydrate to 100.0 g of deionized water, and stir at 25°C and 300 r / min... Stirring at 800 rpm for 15 min yields an aqueous solution of zinc acetate. The zinc acetate solution is then added dropwise to a lignin alkaline solution containing gallic acid over 45 min. A 10% sodium hydroxide solution is prepared using 2.0 g of sodium hydroxide and 18.0 g of deionized water. The sodium hydroxide solution is added dropwise, and the pH is adjusted to 11.0. After the addition is complete, the mixture is stirred at 25°C and 600 rpm for 60 min to obtain a zinc gallate-lignin complex dispersion.
[0046] Step B2: Prepare 184.0 g of dilute sulfuric acid using 18.78 g of 98% sulfuric acid and 165.22 g of deionized water; maintain the zinc gallate-lignin complex dispersion at 25°C and shear at 3000 r / min, adding dilute sulfuric acid dropwise over 60 min to adjust the pH to 6.0; reduce the shear rate to 500 r / min and age at 25°C for 2.0 h; after aging, centrifuge at 10000 r / min for 15 min. n. Collect the precipitate, wash the precipitate with 800.0g of deionized water and centrifuge again to obtain wet complexed lignin nanoparticles; disperse all wet complexed lignin nanoparticles in 400.0g of deionized water and shear at 3000r / min for 20min; spray dry the obtained nanoparticle slurry at an inlet air temperature of 160°C and an outlet air temperature of 70°C, grind the spray-dried product and pass it through a vibrating sieve with a pore size of 45μm to obtain zinc gallate complexed lignin nanoparticles.
[0047] Example 3
[0048] This embodiment provides a method for preparing a bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting, the steps of which include:
[0049] Step S1: Take sufficient amounts of poly(L-lactic acid), poly(D-lactic acid), and bio-based polybutylene succinate, and dry them at 70°C and a vacuum of -0.08 MPa for 8 hours; take sufficient amounts of microcrystalline cellulose, epoxidized soybean oil-grafted citric acid cellulose, zinc gallate-complexed lignin nanoparticles, and calcium stearate, and dry them at 60°C and a vacuum of -0.08 MPa for 8 hours; take sufficient amounts of acetylated tributyl citrate and dehydrate them at 60°C and a vacuum of -0.08 MPa for 4 hours; after treatment, cool each material to 25°C in a dryer and seal for storage to allow the poly(L-lactic acid), poly(D-lactic acid), and bio-based polybutylene succinate to dry. The moisture content of esters, microcrystalline cellulose, epoxidized soybean oil-grafted citric acid cellulose, and zinc gallate-complexed lignin nanoparticles is no greater than 0.02%, and the moisture content of acetylthiol tributyl citrate and calcium stearate is no greater than 0.05%. Weigh out 82.00g of dried poly-L-lactic acid, 4.00g of dried poly-D-lactic acid, 12.00g of dried bio-based polybutylene succinate, 9.00g of dried microcrystalline cellulose, 3.50g of dried epoxidized soybean oil-grafted citric acid cellulose, 1.20g of dried zinc gallate-complexed lignin nanoparticles, 1.80g of dehydrated acetylthiol tributyl citrate, and 0.50g of dried... Calcium stearate; 28.70g of dried poly-L-lactic acid, 9.00g of dried microcrystalline cellulose, 3.50g of dried epoxidized soybean oil-grafted citric acid cellulose, and 1.08g of dehydrated acetylated tributyl citrate were added to a high-speed mixer and stirred at 65°C and 800r / min for 10min to obtain a premix; the premix was added to a twin-screw extruder and melt-blended and vacuum-degassed at 190°C, screw speed 180r / min, and vacuum degree -0.08MPa, then extruded, cooled, and pelletized to obtain cellulose composite masterbatch; the cellulose composite masterbatch was then mixed with the remaining 53.30g of dried poly-L-lactic acid. The remaining 0.72g of dehydrated tributyl acetylacetonate, 4.00g of dried poly(D-lactic acid), 12.00g of dried bio-based polybutylene succinate, 1.20g of dried zinc gallate complexed lignin nanoparticles, and 0.50g of dried calcium stearate were mixed for 5 min and added to a twin-screw extruder. The mixture was melt-blended and vacuum-degassed at 195°C, 180 r / min, and -0.08 MPa. The melt was then passed through a 150 μm filtration device, extruded, cooled, and pelletized. The resulting pellets were dried at 70°C and -0.08 MPa for 8 h to obtain composite pellets.
[0050] Step S2: The composite granules are added to a melt spinning machine, melted at 200°C, extruded through a spinneret with a diameter of 1.50 mm, and cooled and shaped in air at 30°C to obtain nascent filaments; the nascent filaments are first drawn at 90°C with a draw ratio of 3.5:1, and then second drawn at 110°C with a draw ratio of 1.7:1; the drawn monofilaments are tension heat-set at 130°C for 90 s and subjected to 8% controlled shrinkage to obtain 0.80 mm diameter monofilaments for oriented mesh; the oriented mesh monofilaments are woven into a sports and leisure net with a mesh side length of 120 mm, and relaxed and shaped at 80°C for 15 min to obtain a polylactic acid cellulose composite material product for bio-based biodegradable sports and leisure net.
[0051] Preparation steps of epoxidized soybean oil grafted with citric acid cellulose:
[0052] Step A1: Add 400.0 g of deionized water to a reaction vessel equipped with a mechanical stirrer, add 110.0 g of microcrystalline cellulose at 800 r / min, and continue stirring for 20 min; add 30.0 g of citric acid monohydrate and 9.0 g of sodium hypophosphite monohydrate, raise the temperature to 55°C, and stir and impregnate at 500 r / min for 45 min; after impregnation, do not filter, transfer all materials to a drying tray, and dry at 75°C with forced air for 8 h, turning the material every 2 h during the drying process; perform solid-phase esterification of the dried material at 160°C for 50 min, and cool to 25°C; wash with 1100.0 g of deionized water, filter and collect the solid, dry the solid at 75°C and vacuum degree -0.08 MPa for 8 h, grind and pass through a vibrating sieve with a pore size of 45 μm to obtain citric acid cellulose.
[0053] Step A2: Add 400.0g of acetone, then add 25.0g of epoxidized soybean oil and 0.80g of tetrabutylammonium bromide to a sealed stirring container. Stir at 400r / min for 20min to obtain an epoxidized soybean oil reaction solution. Add 110.0g of citric acid cellulose to a mixer and stir at 600r / min. Spray the epoxidized soybean oil reaction solution evenly into the mixer within 30min. Stir at 300r / min under conditions of 55°C and a vacuum of -0.08MPa, and recover acetone until the material is... The mass fraction of acetone is no more than 0.5%; nitrogen gas is introduced at 0.5 L / min to heat the material to 130°C and react at 300 r / min for 4.0 h; after cooling to 25°C, 250.0 g of acetone is added and stirred and washed for 20 min, filtered, and then another 250.0 g of acetone is added and stirred and washed for 20 min, and the filter cake is collected; the filter cake is dried at 75°C and vacuum degree -0.08 MPa for 8 h, ground, and passed through a vibrating sieve with a pore size of 45 μm to obtain epoxidized soybean oil grafted citric acid cellulose.
[0054] Preparation steps of zinc gallate-complexed lignin nanoparticles:
[0055] Step B1: Add 110.0 g of alkali lignin and 18.0 g of sodium hydroxide to 1200.0 g of deionized water, stir at 55°C and 500 r / min for 90 min, and filter using a 10 μm pore size filter to obtain an alkaline lignin solution; purge nitrogen gas at 0.5 L / min, add 16.0 g of gallic acid at 400 r / min, and continue stirring for 30 min; add 8.0 g of zinc acetate dihydrate to 180.0 g of deionized water, and stir at 25°C and 300 r / min... Stirring at 800 rpm for 15 min yields an aqueous solution of zinc acetate. The zinc acetate solution is then added dropwise to an alkaline lignin solution containing gallic acid over 45 min. A 10% sodium hydroxide solution is prepared using 4.0 g of sodium hydroxide and 36.0 g of deionized water. The sodium hydroxide solution is added dropwise, and the pH is adjusted to 12.0. After the addition is complete, the mixture is stirred at 35°C and 600 rpm for 120 min to obtain a zinc gallate-lignin complex dispersion.
[0056] Step B2: Prepare 302.0 g of dilute sulfuric acid using 30.82 g of 98% sulfuric acid and 271.18 g of deionized water; maintain the zinc gallate-lignin complex dispersion at 35°C and shear at 3000 r / min, adding dilute sulfuric acid dropwise over 60 min to adjust the pH to 7.0; reduce the shear rate to 500 r / min and age at 35°C for 4.0 h; after aging, centrifuge at 10000 r / min for 15 min. n. Collect the precipitate, wash the precipitate with 1200.0g of deionized water and centrifuge again to obtain wet complexed lignin nanoparticles; disperse all wet complexed lignin nanoparticles in 600.0g of deionized water and shear at 3000r / min for 20min; spray dry the obtained nanoparticle slurry at an inlet air temperature of 180°C and an outlet air temperature of 80°C, grind the spray-dried product and pass it through a vibrating sieve with a pore size of 45μm to obtain zinc gallate complexed lignin nanoparticles.
[0057] Comparative Example 1
[0058] The difference between this comparative example and Example 1 is that the epoxidized soybean oil grafted with citric acid cellulose in Example 1 is replaced with an equal mass of microcrystalline cellulose, while the rest is the same as in Example 1.
[0059] Comparative Example 2
[0060] The difference between this comparative example and Example 1 is that the zinc gallate complexed lignin nanoparticles in Example 1 are replaced with an equal mass of alkali lignin, while the rest is the same as in Example 1.
[0061] Comparative Example 3
[0062] The difference between this comparative example and Example 1 is that the epoxidized soybean oil grafted citric acid cellulose and zinc gallate complexed lignin nanoparticles in Example 1 are replaced with an equal mass of poly-L-lactic acid, and the rest is the same as in Example 1.
[0063] The performance of the bio-based biodegradable polylactic acid cellulose composite materials for sports and leisure nets provided in the above embodiments and comparative examples was tested using the following methods:
[0064] The oriented nets prepared in Examples 1-3 and Comparative Examples 1-3 were tested using monofilaments and sports and leisure nets. For each test, samples were randomly taken from different locations. The samples were equilibrated for 24 hours in a standard environment with a temperature of 20°C ± 2°C and a relative humidity of 65% ± 5% before being tested.
[0065] During the fracture strength test, samples with a length of not less than 800 mm were cut from the monofilaments of each group of oriented wire mesh. The linear density of the samples was first determined. Ten samples with a length of 1000 mm were taken from each group. The effective length was measured under a pretension of 0.05 cN / dtex. The samples were weighed and the linear density was calculated according to the mass and length of the samples, with the unit being dtex. The fracture strength was tested using a constant speed elongation type strength testing machine with a clamping distance of 500 mm and a pretension of 0.05 cN / dtex. The clamping speed was determined to be 300 mm / min through a preliminary test, so that the average fracture time of the samples was controlled within 20 s ± 3 s. At least 20 valid results were obtained for each group. Results were invalid if the sample fractured within 5 mm of the clamp or if clamping slippage occurred. The fracture strength was calculated by dividing the maximum force at fracture by the linear density, with the unit being cN / dtex.
[0066] Elongation at break and fracture strength were tested simultaneously. The change in the clamp spacing when the specimen broke was recorded. The elongation at break was calculated according to the ratio of the elongation at break to the initial clamping length. The arithmetic mean of no less than 20 valid results was taken for each group.
[0067] During the nodule strength utilization rate test, a single dead knot was made in the middle of a single filament of an oriented mesh with a length of not less than 600 mm, so that the nodule was located between two clamps with a clamping distance of 250 mm. A pretension of 0.05 cN / dtex was applied, and the clamping speed was adjusted so that the average fracture time was controlled within 20 s ± 3 s. The maximum force at the nodule fracture was recorded, and no less than 20 valid results were obtained for each group. The nodule strength utilization rate was calculated by the ratio of the nodule fracture strength to the fracture strength of the nodule-free sample in the same group.
[0068] During the dry heat shrinkage test, 10 monofilaments of orientation mesh with a length of not less than 600 mm were cut from each group. Under a pretension of 0.05 cN / dtex, an effective length of 500 mm was marked. After removing the pretension, the sample was placed without tension in a forced-air drying oven at 100°C±2°C for 30 min. After taking it out, it was equilibrated in an environment with a temperature of 20°C±2°C and a relative humidity of 65%±5% for 30 min. The same pretension was reapplied and the length between the marks after treatment was measured. The dry heat shrinkage rate was calculated by dividing the difference between the length before treatment and the length after treatment by the length before treatment.
[0069] During the xenon lamp aging test to assess the retention rate of fracture strength, an oriented mesh with a length of not less than 800 mm was fixed stress-free to the sample holder of the xenon lamp aging test chamber using a monofilament. A daylight filter was used, and the irradiance at 340 nm was 0.51 W / (m²). 2 ·nm)±0.02W / (m 2 The black standard temperature was 65°C±3°C, the test chamber temperature was 38°C±3°C, and the relative humidity was 50%±10%. Each cycle included 102 minutes of continuous light exposure and 18 minutes of light exposure plus deionized water spray. After a cumulative exposure of 500 hours, the sample was taken out and equilibrated for 24 hours in an environment with a temperature of 20°C±2°C and a relative humidity of 65%±5%. At least 20 valid results were obtained according to the aforementioned fracture strength test method. The fracture strength retention rate after xenon lamp aging was calculated by the ratio of the fracture strength after aging to the fracture strength before aging.
[0070] During the 180-day biodegradation rate test under controlled composting conditions, the composite material particles of each group were ground to a particle size of no more than 2 mm. The total organic carbon content of the samples was determined. Stable and matured compost from a normally operating organic waste composting plant was used as the inoculum. The inoculum was sieved through a 10 mm sieve and the moisture content was adjusted to 50%. Each group had 3 test material containers, 3 microcrystalline cellulose reference material containers, and 3 blank containers. The effective volume of each container was no less than 2 L. The dry solids content of the test material was no less than 50.0 g and the total organic carbon content was no less than 20.0 g. The test material and inoculum dry solids were thoroughly mixed at a mass ratio of 1:6. The reference material was microcrystalline cellulose with a particle size of less than 20 μm. Only an equal amount of inoculum was added to the blank containers. Each container was placed at 58°C±2°C and continuously purged with CO2-removed and humidified air. The aeration rate was adjusted to ensure that the oxygen volume fraction in the exhaust gas was not less than 6%. The material was turned over periodically, and deionized water lost through evaporation was replenished. The CO2 released from each container was continuously measured. Records were made daily during the first week and at least twice a week thereafter. The experiment lasted for 180 days. The biodegradation rate was calculated as the ratio of the cumulative CO2 released from the test container minus the cumulative CO2 released from the blank container to the theoretical maximum CO2 release from the test material. The test results were considered valid when the average biodegradation rate of microcrystalline cellulose at 45 days was greater than 70%, the relative deviation of the cumulative CO2 released from each blank container met the requirements, and the deviation of the results from each parallel container met the requirements.
[0071] The performance test data above are shown in Table 1.
[0072] Table 1: Performance Test Results
[0073]
[0074] As can be seen from the above, the fracture strength of Examples 1-3 is 4.39-4.91 cN / dtex, which is higher than that of Comparative Examples 1-3 (3.55-4.21 cN / dtex); the elongation at break is 21.2%-25.0%, which is significantly higher than that of Comparative Examples 1-3 (10.7-19.6%); and the utilization rate of nodal strength is 73.5-79.6%, which is higher than that of Comparative Examples 1-3 (52.6-68.7%). This indicates that the present invention improves the problems of high brittleness of polylactic acid cellulose composite materials, insufficient interfacial compatibility between microcrystalline cellulose and poly-L-lactic acid, and stress concentration and premature fracture of monofilaments at nodules.
[0075] Compared with Comparative Example 1, after adding epoxidized soybean oil to graft citric acid cellulose, the tensile strength of Example 1 increased from 3.82 cN / dtex to 4.68 cN / dtex, the elongation at break increased from 13.8% to 23.4%, the utilization rate of nodular strength increased from 60.2% to 76.8%, and the dry heat shrinkage decreased from 4.8% to 2.6%. This indicates that epoxidized soybean oil grafting to citric acid cellulose can improve the dispersion state of microcrystalline cellulose in the polymer matrix, mitigate the interfacial polarity difference between cellulose and the polymer matrix, and improve the interfacial load transfer capacity and monofilament toughness through the flexible grafting structure.
[0076] Compared with Comparative Example 2, after adding zinc gallate-complexed lignin nanoparticles, the fracture strength retention rate after 500 hours of xenon lamp aging increased from 74.8% to 91.7%, an increase of 16.9 percentage points. At the same time, the fracture strength and nodule strength utilization rate also increased from 4.21 cN / dtex and 68.7% to 4.68 cN / dtex and 76.8%, respectively. This indicates that zinc gallate-complexed lignin nanoparticles can be uniformly dispersed and weaken the damage of ultraviolet radiation to polymer molecular chains. The gallic acid, zinc complex structure and lignin aromatic structure together inhibit the continuous reaction of free radicals during photo-oxidation, solving the problems of uneven dispersion, easy formation of defects and insufficient aging protection efficiency of uncomplexed alkali lignin.
[0077] Compared with Comparative Example 3, which does not contain epoxidized soybean oil-grafted citric acid cellulose and zinc gallate-complexed lignin nanoparticles, Example 1 showed a 31.8% increase in fracture strength, a 118.7% increase in elongation at break, a 46.0% increase in nodular strength utilization, a decrease in dry heat shrinkage from 5.7% to 2.6%, and an increase in fracture strength retention from 67.1% to 91.7% after 500 hours of xenon lamp aging. This demonstrates that epoxidized soybean oil-grafted citric acid cellulose and zinc gallate-complexed lignin nanoparticles have a synergistic effect in terms of interfacial compatibilization, stress dispersion, crystallization and orientation stabilization, and photo-oxidation protection.
[0078] The controlled composting biodegradation rates of Examples 1-3 were 90.8-94.1% after 180 days, maintaining good controlled composting biodegradation capacity while achieving high mechanical properties, nodule reliability, dimensional stability, and resistance to artificial aging. Although Comparative Example 1 achieved a biodegradation rate of 93.2% due to the increase in microcrystalline cellulose content, its breaking strength, elongation at break, nodule strength utilization rate, and dimensional stability all decreased significantly, indicating that simply increasing unmodified microcrystalline cellulose cannot achieve a balance between performance and degradation performance.
[0079] Therefore, this invention solves the technical problems of insufficient toughness, weak interfacial bonding of cellulose, large loss of nodular strength, easy shrinkage when heated, significant strength decay after outdoor exposure to sunlight, and difficulty in balancing durability and biodegradability in existing polylactic acid sports and leisure net materials.
Claims
1. A biobased degradable sport and leisure netting polylactic acid cellulose composite material characterized by, Includes the following components in parts by weight: Poly(L-lactic acid) 75.0-82.0 parts, poly(D-lactic acid) 2.0-4.0 parts, bio-based polybutylene succinate 7.0-12.0 parts, microcrystalline cellulose 5.0-9.0 parts, epoxidized soybean oil-grafted citric acid cellulose 1.5-3.5 parts, zinc gallate-complexed lignin nanoparticles 0.4-1.2 parts, tributyl acetylacetonate 0.8-1.8 parts, and calcium stearate 0.2-0.5 parts.
2. The bio-based degradable polylactic acid cellulose composite fiber for sports and leisure net according to claim 1, characterized in that, The preparation method of the epoxidized soybean oil grafted with citric acid cellulose includes: A1. By weight, add 90.0-110.0 parts of microcrystalline cellulose to 250.0-400.0 parts of deionized water, stir and disperse, add 18.0-30.0 parts of citric acid monohydrate and 6.0-9.0 parts of sodium hypophosphite monohydrate, stir and impregnate to obtain impregnated microcrystalline cellulose; dry the impregnated microcrystalline cellulose, and then carry out solid-phase esterification at 145-160℃; after solid-phase esterification, wash with deionized water, vacuum dry, grind and vibrate sieve to obtain citric acid cellulose; A2. Add 15.0-25.0 parts of epoxidized soybean oil and 0.3-0.8 parts of tetrabutylammonium bromide to 250.0-400.0 parts of acetone and stir to obtain an epoxidized soybean oil reaction solution. Add 90.0-110.0 parts of citric acid cellulose to a mixer. While stirring, spray the epoxidized soybean oil reaction solution into the mixer. Under vacuum conditions at 40-55℃, recover the acetone to obtain the material after acetone recovery. Under nitrogen protection, heat the material after acetone recovery to 115-130℃ for reaction. After the reaction is completed, cool, add acetone for washing, filter, and collect the filter cake. Vacuum dry, grind, and vibrate sieve the filter cake.
3. The bio-based degradable polylactic acid cellulose composite fiber for sports and leisure net according to claim 2, characterized by, In step A1, the solid-phase esterification is carried out at 145-160℃ for 30-50 minutes.
4. The bio-based degradable polylactic acid cellulose composite fiber for sports and leisure net according to claim 2, characterized by, In step A2, the reaction time is 2.5-4.0 h when the temperature is raised to 115-130℃.
5. The biobased degradable polylactic acid cellulose composite fiber for sports and leisure net according to claim 1, characterized in that, The preparation method of the zinc gallate complexed lignin nanoparticles includes: B1. By weight, add 90.0-110.0 parts of alkali lignin and 12.0-18.0 parts of sodium hydroxide to 800.0-1200.0 parts of deionized water, stir at 45-55℃, filter, and obtain an alkaline lignin solution; under nitrogen protection, add 12.0-16.0 parts of gallic acid to the alkaline lignin solution, stir, and obtain an alkaline lignin solution containing gallic acid; dissolve 5.0-8.0 parts of zinc acetate dihydrate in 100.0-180.0 parts of deionized water to obtain an aqueous zinc acetate solution; under stirring, add the aqueous zinc acetate solution dropwise to the alkaline lignin solution containing gallic acid, adjust the pH to 11.0-12.0 with an aqueous sodium hydroxide solution, stir the reaction at 25-35℃, and obtain a zinc gallate-lignin complex dispersion; B2. Under shearing conditions, dilute sulfuric acid is added dropwise to the zinc gallate-lignin complex dispersion to adjust the pH to 6.0-7.0, and the mixture is aged at 25-35℃. After aging, the mixture is centrifuged and washed to obtain wet complexed lignin nanoparticles. The wet complexed lignin nanoparticles are dispersed in 400.0-600.0 parts of deionized water to obtain a nanoparticle slurry. The nanoparticle slurry is spray-dried, and then ground and vibrated sieved.
6. The bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting according to claim 5, characterized in that, In step B1, the reaction is stirred at 25-35℃ for 60-120 minutes.
7. The bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting according to claim 5, characterized in that, In step B2, the aging time at 25-35℃ is 2.0-4.0 hours.
8. A preparation process for a bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting according to any one of claims 1-7, characterized in that the step... include: S1. Poly(L-lactic acid), poly(D-lactic acid), bio-based polybutylene succinate, microcrystalline cellulose, epoxidized soybean oil-grafted citric acid cellulose, and zinc gallate-complexed lignin nanoparticles are dried separately. 25-35% of poly(L-lactic acid), microcrystalline cellulose, epoxidized soybean oil-grafted citric acid cellulose, and 40-60% of acetylated tributyl citrate are mixed and stirred at 55-65°C to obtain a premix. The premix is then... The material is added to a twin-screw extruder, melt-blended at 175-190℃, vacuum-de-squeezed, and extruded into pellets to obtain cellulose composite masterbatch; the cellulose composite masterbatch is mixed with the remaining poly(L-lactic acid), the remaining tributyl acetyl citrate, poly(D-lactic acid), bio-based polybutylene succinate, zinc gallate complexed lignin nanoparticles, and calcium stearate, added to a twin-screw extruder, melt-blended at 180-195℃, vacuum-de-squeezed, filtered, extruded into pellets, and dried to obtain composite granules; S2. Add the composite granules to a melt spinning machine and melt them at 185-200℃. Extrude them through the spinneret and cool and set them at 20-30℃ to obtain nascent yarn. Perform the first stage of drawing on the nascent yarn at 75-90℃, and then perform the second stage of drawing at 95-110℃. Subsequently, perform heat setting and controlled shrinkage to obtain monofilaments for orientation webs. Form the orientation webs into a web and relax and set it at 60-80℃.
9. The preparation process of the bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting according to claim 8, characterized in that, In step S1, the stirring time at 55-65℃ is 5-10 minutes.
10. The preparation process of the bio-based biodegradable polylactic acid cellulose composite material for sports and leisure netting according to claim 8, characterized in that, In step S2, the heat setting temperature is 110-130℃.