A high-nodular-strength ultra-high molecular weight polyethylene fiber and its preparation method

By constructing a bridging crystalline network between fibrils through dual molecular weight blending and cascade heat treatment, the problem of insufficient nodal strength in ultra-high molecular weight polyethylene fibers was solved, enabling the preparation of fibers with high nodal strength, suitable for fields such as deep-sea fishing, ship mooring, and bulletproof protection.

CN123108767APending Publication Date: 2026-11-17SHANDONG LAIWEI NEW MATERIALS CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611626957.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing ultra-high molecular weight polyethylene fibers have low nodal strength retention rates, making it difficult to meet the requirements of high-safety-level applications. Current technologies have failed to effectively improve fiber transverse cohesion and nodal strength.

Method used

A blend system of ultra-high molecular weight polyethylene with dual molecular weight was adopted, fatty acid modified nano-inorganic oxide particles were added, and a cascade heat treatment process was used to construct a bridging crystalline network between fibrils to enhance the transverse connection ability of the fibers.

Benefits of technology

It significantly improves the fiber nodule strength retention rate to 60% to 68%, and the tensile strength is not less than 33.5 cN/dtex, meeting the needs of high-security applications such as deep-sea fishing, ship mooring, and bulletproof protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108767A_ABST
    Figure CN123108767A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of polymer fiber material technology, and relates to a high-nodal-strength ultra-high molecular weight polyethylene fiber and its preparation method. The method includes: reacting stearic acid and nano-silica in a solvent to prepare stearic acid-modified nano-silica; preparing a first spinning material by extruding high-viscosity-average-molecular-weight ultra-high molecular weight polyethylene resin and white oil using a twin-screw extruder; preparing a second spinning material by extruding medium-viscosity-average-molecular-weight ultra-high molecular weight polyethylene resin, white oil, and stearic acid-modified nano-silica using a twin-screw extruder; combining the two spinning materials, statically mixing them, extruding them through a spinneret, and cooling to form gel-state fibers; removing the solvent from the gel-state fibers through extraction and drying; and then completing fiber orientation through cascade heat treatment, followed by winding and bundling to obtain the finished product. The fiber obtained by this invention has a tensile strength of not less than 33.5 cN / dtex and a nodal strength retention rate of 60% to 68%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer fiber technology, specifically relating to a high nodular strength ultra-high molecular weight polyethylene fiber and its preparation method. Background Technology

[0002] Ultra-high molecular weight polyethylene (UHMWPE) fiber, due to its extremely high specific strength, excellent chemical resistance, and good impact toughness, has wide applications in fields such as deep-sea fishing ropes, ship mooring lines, bulletproof protective equipment, surgical sutures, and marine engineering. However, in these applications, the fibers inevitably need to be connected and fixed through knotting, weaving, or twisting, and the fibers are subjected to combined stresses such as bending, lateral compression, and shear at the knots. Currently, the knot strength retention rate of UHMWPE fibers is typically only 40% to 55% of the tensile strength, and this deficiency has become a key bottleneck restricting its widespread adoption in high-safety-level applications.

[0003] The current mainstream preparation technology for high-performance UHMWPE fibers is gel spinning-ultra-stretching. This involves dissolving UHMWPE resin in a spinning solvent to form a semi-dilute solution, extruding it through a spinneret, and then forming gel fibers in a cooling medium. The solvent is then removed through extraction, followed by multi-stage thermal stretching to achieve high molecular chain orientation, ultimately yielding high-strength fibers. In recent years, existing technologies have primarily explored the following approaches to improve nodular strength: first, adding nanofillers to the spinning solution to enhance the fiber matrix strength; second, constructing a core-sheath or layered structure through bicomponent composite spinning to improve the fiber's transverse properties; and third, optimizing extraction and stretching process parameters to improve the uniformity of the fiber's microstructure. While these methods have improved the overall mechanical properties of the fibers to some extent, the improvement in nodular strength is limited, and the nodular strength retention rate is difficult to exceed 60%.

[0004] From a microscopic perspective, the fundamental reason for the low nodal strength lies in the anisotropic microstructure of the highly oriented UHMWPE fibers. During gel spinning-hyperstretching, the UHMWPE molecular chains are highly oriented along the fiber axis, forming a fibril structure dominated by extended chain crystals, resulting in extremely high axial strength. However, the lateral connections between fibrils—that is, the ligature molecules connecting adjacent fibrils and the interfibril lamellar crystals—are scarce and insufficient in strength. When the fiber is subjected to lateral compression and bending stress at the nodal points, the lack of effective lateral stress transmission channels between fibrils leads to slippage and splitting between them, ultimately causing fiber breakage.

[0005] Furthermore, while adding nanofillers in existing technologies can disperse stress and prevent cracking, the lack of an effective interfacial bond between the nanofillers and the UHMWPE matrix often leads to stress concentration points during high-ratio stretching, which in turn reduces the overall uniformity and stretchability of the fiber. Specifically, the interfacial bonding between unmodified nanofillers and the non-polar UHMWPE matrix is ​​extremely weak, maintained only by van der Waals forces. During high-ratio hot stretching, the nanofiller particles cannot undergo plastic deformation along with the molecular chains, resulting in microvoids and stress concentration areas at the filler-matrix interface. These microscopic defects become preferential sites for crack initiation when the fiber is subjected to lateral compressive stress at the nodules.

[0006] A deeper problem lies in the fact that existing technologies fail to address the root cause of insufficient nodal strength: the lack of lateral cohesion between fibrils. Both filler toughening and process optimization are essentially improvements made without altering the anisotropic characteristics of the fiber's microstructure. To fundamentally improve the nodal strength of UHMWPE fibers, a lateral connection network between fibrils must be constructed at the molecular scale. This involves increasing the number of tethering molecules spanning adjacent fibrils and the density of bridging crystals between fibrils, enabling the fiber to have effective lateral stress transmission channels when subjected to lateral stress. Therefore, there is an urgent need to develop a preparation method that can significantly improve the fiber's lateral cohesion and nodal strength retention rate while maintaining the high tensile strength of UHMWPE fibers. Summary of the Invention

[0007] This invention provides a high nodular strength ultra-high molecular weight polyethylene fiber and its preparation method, in order to solve the problem of low nodular strength retention rate of ultra-high molecular weight polyethylene fibers in the prior art.

[0008] A method for preparing high-nodular-strength ultra-high molecular weight polyethylene fiber includes the following steps: Fatty acid-modified nano-inorganic oxide particles are pre-dispersed in a medium-viscosity-average molecular weight ultra-high molecular weight polyethylene spinning solution to obtain a second spinning material; a high-viscosity-average molecular weight ultra-high molecular weight polyethylene spinning solution is used as a first spinning material; the first spinning material and the second spinning material are combined in a certain proportion, and then spun and cooled to form gel fibers; the gel fibers are extracted and dried, and then subjected to cascade heat treatment; the cascade heat treatment includes a first-stage hot stretching, a first-stage relaxation annealing, a second-stage hot stretching, a second-stage relaxation annealing, and a third-stage hot stretching performed sequentially.

[0009] The high viscosity-average molecular weight ultra-high molecular weight polyethylene has a viscosity-average molecular weight of 3 million to 6 million. The high viscosity-average molecular weight ultra-high molecular weight polyethylene has a viscosity-average molecular weight of 4 million to 5 million. The high viscosity-average molecular weight ultra-high molecular weight polyethylene has a viscosity-average molecular weight of 4.5 million.

[0010] The medium viscosity-average molecular weight ultra-high molecular weight polyethylene has a viscosity-average molecular weight of 800,000 to 2.5 million. The medium viscosity-average molecular weight ultra-high molecular weight polyethylene has a viscosity-average molecular weight of 1 million to 2 million. The medium viscosity-average molecular weight ultra-high molecular weight polyethylene has a viscosity-average molecular weight of 1.5 million.

[0011] The mass ratio of ultra-high molecular weight polyethylene in the first spinning material to that in the second spinning material is (70 to 90):(10 to 30). The mass ratio of ultra-high molecular weight polyethylene in the first spinning material to that in the second spinning material is (75 to 85):(15 to 25). The mass ratio of ultra-high molecular weight polyethylene in the first spinning material to that in the second spinning material is 80:20.

[0012] The fatty acid is C. 12 To C 22 Long-chain fatty acids. The fatty acid is C. 16 To C 20 Long-chain fatty acids. The fatty acid is one or a combination of stearic acid and palmitic acid. The fatty acid is stearic acid.

[0013] The nano-inorganic oxide is one or a combination of nano-silica, nano-titanium dioxide, and nano-alumina. The nano-inorganic oxide is fumed silica. The average particle size of the nano-inorganic oxide particles is 10 to 50 nm. The average particle size of the nano-inorganic oxide particles is 15 to 30 nm. The average particle size of the nano-inorganic oxide particles is 20 nm.

[0014] The fatty acid grafting rate in the fatty acid-modified nano-inorganic oxide particles is 4% to 15%. The fatty acid grafting rate in the fatty acid-modified nano-inorganic oxide particles is 6% to 12%. The fatty acid grafting rate in the fatty acid-modified nano-inorganic oxide particles is 8% to 9%.

[0015] The preparation method of the fatty acid-modified nano-inorganic oxide particles includes: dispersing nano-inorganic oxide particles in a solvent, adding a fatty acid solution, carrying out a surface modification reaction under heating and stirring conditions, and obtaining fatty acid-modified nano-inorganic oxide particles after filtration, washing, and drying. The surface modification reaction temperature is 60 to 90 degrees Celsius, and the reaction time is 2 to 5 hours. Alternatively, the surface modification reaction temperature is 78 degrees Celsius, and the reaction time is 3 hours. The solvent is an alcohol solvent. Another method uses anhydrous ethanol as the solvent.

[0016] The amount of fatty acid-modified nano-inorganic oxide particles added to the second spinning material is 1% to 5% of the mass of medium-viscosity average molecular weight ultra-high molecular weight polyethylene. The amount of fatty acid-modified nano-inorganic oxide particles added to the second spinning material is 2% to 3% of the mass of medium-viscosity average molecular weight ultra-high molecular weight polyethylene. The amount of fatty acid-modified nano-inorganic oxide particles added to the second spinning material is 2.5% of the mass of medium-viscosity average molecular weight ultra-high molecular weight polyethylene.

[0017] The mass concentration of ultra-high molecular weight polyethylene in the first spinning material and the second spinning material is independently 5% to 12%. The mass concentration of ultra-high molecular weight polyethylene in the first spinning material and the second spinning material is independently 7% to 10%. The mass concentration of ultra-high molecular weight polyethylene in the first spinning material and the second spinning material is 8%.

[0018] The spinning solvents for the first spinning material and the second spinning material are each independently white oil and / or decahydronaphthalene. The spinning solvent is white oil.

[0019] The first spinning material is prepared using a twin-screw extruder, with a homogenization section temperature of 200 to 220 degrees Celsius and a screw speed of 120 to 180 rpm. Alternatively, the first spinning material can be prepared using a twin-screw extruder, with a homogenization section temperature of 210 degrees Celsius and a screw speed of 150 rpm.

[0020] The second spinning material is prepared using a twin-screw extruder. The homogenization section temperature of the extruder is 200 to 220 degrees Celsius, and the screw speed is 150 to 220 rpm. Alternatively, the second spinning material can be prepared using a twin-screw extruder with a homogenization section temperature of 210 degrees Celsius and a screw speed of 180 rpm. The fatty acid-modified nano-inorganic oxide particles are added to the twin-screw extruder through a side feed port.

[0021] The merging process takes place in a merging conduit equipped with a static mixer. The static mixer is a Kenics-type static mixer containing 8 to 16 mixing elements. The static mixer contains 12 mixing elements. The spinning solution temperature after merging is 195 to 215 degrees Celsius. The spinning solution temperature after merging is 205 degrees Celsius.

[0022] The spinneret temperature is 185 to 205 degrees Celsius. The spinneret temperature is 195 degrees Celsius.

[0023] The cooling and molding process employs water bath cooling, with a water bath temperature ranging from 0 to 15 degrees Celsius. The water bath temperature ranges from 3 to 8 degrees Celsius. The water bath temperature is 5 degrees Celsius.

[0024] The extraction process uses an organic solvent to remove the spinning solvent. The organic solvent is one or more of dichloromethane, n-hexane, and trichlorotrifluoroethane. The organic solvent is dichloromethane. The extraction employs multi-stage countercurrent extraction at temperatures ranging from 20 to 40 degrees Celsius. The extraction is a three-stage countercurrent extraction, with extraction temperatures at each stage being 25 degrees Celsius, 30 degrees Celsius, and 35 degrees Celsius, respectively.

[0025] The first-stage heat stretching temperature is 110 to 125 degrees Celsius, with a stretching ratio of 2.5 to 3.5 times. The first-stage heat stretching temperature is 115 to 120 degrees Celsius, with a stretching ratio of 2.8 to 3.2 times. The first-stage heat stretching temperature is 118 degrees Celsius, with a stretching ratio of 3.0 times.

[0026] The first relaxation annealing temperature is 120 to 135 degrees Celsius, the relaxation ratio is 3% to 7%, and the annealing time is 1 to 3 minutes. The first relaxation annealing temperature is 125 to 132 degrees Celsius, the relaxation ratio is 3% to 5%, and the annealing time is 1.5 to 2.5 minutes. The first relaxation annealing temperature is 128 degrees Celsius, the relaxation ratio is 5%, and the annealing time is 1.7 minutes.

[0027] The second-stage heat stretching temperature is 128 to 142 degrees Celsius, with a stretching ratio of 2.2 to 3.0 times. The second-stage heat stretching temperature is 132 to 138 degrees Celsius, with a stretching ratio of 2.4 to 2.8 times. The second-stage heat stretching temperature is 135 degrees Celsius, with a stretching ratio of 2.6 times.

[0028] The second relaxation annealing temperature is 133 to 145 degrees Celsius, the relaxation ratio is 2% to 5%, and the annealing time is 0.3 to 2 minutes. The second relaxation annealing temperature is 138 to 143 degrees Celsius, the relaxation ratio is 2% to 4%, and the annealing time is 0.5 to 1.5 minutes. The second relaxation annealing temperature is 140 degrees Celsius, the relaxation ratio is 3%, and the annealing time is 0.5 minutes.

[0029] The third-stage heat stretching temperature is 140 to 150 degrees Celsius, with a stretching ratio of 1.5 to 2.5 times. The third-stage heat stretching temperature is 143 to 148 degrees Celsius, with a stretching ratio of 1.8 to 2.2 times. The third-stage heat stretching temperature is 145 degrees Celsius, with a stretching ratio of 2.1 times.

[0030] The total effective stretching ratio of the cascaded heat treatment is 10 to 20 times. The total effective stretching ratio of the cascaded heat treatment is 13 to 17 times. The total effective stretching ratio of the cascaded heat treatment is 15 times.

[0031] The relaxation annealing is performed in an inert atmosphere, which is a nitrogen atmosphere.

[0032] A high-nodular-strength ultra-high molecular weight polyethylene fiber is prepared by the above-described method.

[0033] The ultra-high molecular weight polyethylene fiber comprises a fibril structure arranged in a highly oriented manner along the fiber axis, and the fibrils are connected by a bridging crystalline network; the bridging crystalline network contains fatty acid-modified nano-inorganic oxide particles as interface anchoring points.

[0034] The tensile strength of the ultra-high molecular weight polyethylene fiber is not less than 33.5 cN / dtex. The tensile strength of the ultra-high molecular weight polyethylene fiber is between 33.5 and 36.5 cN / dtex. The tensile strength of the ultra-high molecular weight polyethylene fiber is 35.8 cN / dtex.

[0035] The nodular strength retention rate of the ultra-high molecular weight polyethylene fiber is not less than 60%. The nodular strength retention rate of the ultra-high molecular weight polyethylene fiber is 60% to 68%. The nodular strength retention rate of the ultra-high molecular weight polyethylene fiber is 65.6%.

[0036] The crystallinity of the ultra-high molecular weight polyethylene fiber is 78% to 85%. The orientation factor of the ultra-high molecular weight polyethylene fiber is 0.93 to 0.97.

[0037] Compared with the prior art, the present invention has the following beneficial effects: This invention provides interfibrillary bridging chain sources through a dual-molecular-weight ultra-high molecular weight polyethylene (UHMWPE) blend system, utilizes fatty acid-modified nano-inorganic oxides to provide heterogeneous nucleation sites at the fibrillary interface, and employs a stretching-relaxation annealing-stretching cascade process to provide thermodynamic driving force and time window for the directional growth of bridging crystals. The synergistic effect of these three factors constructs an interfibrillary bridging crystal network within the fiber microstructure, fundamentally enhancing the lateral cohesiveness of highly oriented UHMWPE fibers. The prepared fibers exhibit a tensile strength of no less than 33.5 cN / dtex, with a nodule strength retention rate of 60% to 68%, representing a 15 to 20 percentage point improvement over the existing 45% to 55%, meeting the requirements for fiber nodule strength in high-security applications such as deep-sea fishing, ship mooring, and bulletproof protection. Furthermore, this method is highly compatible with existing gel spinning industrial production lines, requiring only the addition of nanofiller pre-dispersion and intermediate annealing processes to existing equipment, resulting in low modification costs and promising prospects for industrial-scale application. Attached Figure Description

[0038] Figure 1 This is a scanning electron microscope image of the fiber prepared in Example 1. Detailed Implementation

[0039] The technical solution of the present invention will be described in detail below with reference to specific embodiments, but the scope of protection of the present invention is not limited to these embodiments.

[0040] Example 1 The preparation method of high nodular strength ultra-high molecular weight polyethylene fiber in this embodiment includes the following steps: 1) Preparation of stearic acid modified nano-silica First, 20g of fumed silica nanoparticles (average particle size 20nm, specific surface area 200±20m²) were added. 2 2.4 g of stearic acid (chemically pure, ≥98 wt%) was added to a 250 mL round-bottom flask, followed by 200 mL of anhydrous ethanol. The mixture was ultrasonically dispersed for 20 min in an ultrasonic cleaner with a power of 300 W and a frequency of 40 kHz, allowing the nano-silica to form a uniform white suspension in the ethanol. Then, 2.4 g of stearic acid (chemically pure, ≥98 wt%) was dissolved in 30 mL of anhydrous ethanol and heated to 50 °C under magnetic stirring until completely dissolved, yielding a clear stearic acid-ethanol solution. Subsequently, under continuous magnetic stirring (400 rpm), the stearic acid-ethanol solution was added dropwise to the nano-silica suspension, with the addition time controlled within 5 min. The mixture was then heated to 78 °C and reacted under reflux stirring for 3 h. After the reaction was complete, the mixture was allowed to cool naturally to room temperature and vacuum filtered using medium-speed quantitative filter paper (approximately 10 μm pore size). The filter cake was washed three times with 30 mL of anhydrous ethanol to remove unreacted free stearic acid. The washed filter cake was further dried in an 80℃ forced-air drying oven for 12 hours, ground, and passed through a 200-mesh sieve to obtain approximately 21.5 g of white powdered stearic acid-modified nano-silica. Thermogravimetric analysis showed that the modified nano-silica lost 8.3 wt% of its weight between 200 and 400℃, corresponding to a stearic acid grafting rate of approximately 8.3 wt%.

[0041] 2) Preparation of the first spinning material 640g of UHMWPE resin powder (fiber grade, average particle size 150μm) with a viscosity-average molecular weight of 4.5 million was mixed with 7360g of spinning-grade white oil (kinematic viscosity 68~74mm). 2 The feed (at 40℃) was added to the main feed hopper of the first co-rotating twin-screw extruder. The twin-screw extruder had a screw diameter of 65mm and a length-to-diameter ratio of 48:1. The screw speed was set to 150rpm, and the temperatures of each section of the barrel from the feed end to the discharge end were set sequentially as follows: Section 1: 80℃, Section 2: 150℃, Section 3: 200℃, Section 4: 210℃, Section 5: 210℃. The average residence time of the material in the extruder was 15min, and the barrel was filled with nitrogen for protection. A uniform and transparent spinning solution A stream was obtained at the discharge end, with a UHMWPE mass concentration of 8.0wt%.

[0042] 3) Preparation of the second spinning material 160g of UHMWPE resin powder (injection molding grade, average particle size 120μm) with a viscosity-average molecular weight of 1.5 million and 1836g of spinning-grade white oil were added to the main feed hopper of a second co-rotating twin-screw extruder. The extruder screw diameter was 35mm and the length-to-diameter ratio was 48:1. 4g of stearic acid-modified nano-silica prepared in step 1) was added through the side feed port at the third section. The screw speed was set to 180rpm, and the barrel temperatures were set sequentially as follows: 80℃ for the first section, 150℃ for the second section, 200℃ for the third section, 210℃ for the fourth section, and 210℃ for the fifth section. The average residence time of the material in the extruder was 15min, and the barrel was purged with nitrogen for protection. A uniform spinning solution B flow was obtained at the discharge end, with a UHMWPE mass concentration of 8.0wt% and a modified nano-silica content of 2.5wt% of the UHMWPE mass.

[0043] 4) Dual-flow convergence and spinneret formation Spinning solution streams A and B are delivered to a confluence pipeline via two high-precision gear metering pumps. Stream A is metered at a flow rate of 128 mL / min, and stream B at 32 mL / min, with a volumetric flow rate ratio of 4:1. A 200 mm long Kenics-type static mixer (12 mixing elements) is installed within the confluence pipeline, maintaining the spinning solution temperature at 205°C after confluence. After passing through the static mixer, the spinning solution enters the spinning assembly and is extruded through a 200-hole spinneret. The spinneret temperature is set at 195°C, and the extrusion rate per hole is 0.8 mL / min. The extruded filaments pass through a 15 mm air gap and then enter a 5°C water bath cooling tank over a cooling distance of 1500 mm. The residence time of the filaments in the water bath is approximately 9 seconds, allowing the spinning solution to rapidly solidify and form gel fibers.

[0044] 5) Three-stage countercurrent extraction and drying Gel-form fibers were continuously passed through a three-stage countercurrent extraction tank at a speed of 10 m / min, with dichloromethane used as the extractant in all three stages. The extraction conditions for each stage were as follows: Stage 1: temperature 25℃, tank length 2m, residence time 12s; Stage 2: temperature 30℃, tank length 2m, residence time 12s; Stage 3: temperature 35℃, tank length 2m, residence time 12s. Fresh dichloromethane entered through the inlet of the Stage 3 extraction tank, flowed countercurrently through the Stage 2 and Stage 1, and exited through the Stage 1 outlet, entering the solvent recovery system. The total circulating flow rate of dichloromethane was 50 L / min. After three-stage extraction, the residual white oil content in the fibers was less than 1.5 wt%. The extracted fibers were then continuously dried in a 40℃ hot air drying section (3m long, air velocity 2m / s) to remove residual dichloromethane.

[0045] 6) Cascaded heat treatment of stretching-relaxation annealing-stretching The dried fibers then undergo the following five sequential processes: First-stage hot stretching: The fiber passes through the first-stage hot box, the temperature of which is set to 118℃, the stretching ratio to 3.0 times, the inlet roller speed to 10m / min, the outlet roller speed to 30m / min, the length of which is 1.5m, and the residence time of the fiber in the hot box to 6s.

[0046] First relaxation annealing: The fiber enters the first annealing chamber, the temperature of which is set to 128℃. The fiber relaxes by 5% along the axial direction. The inlet roller speed is 30m / min, the outlet roller speed is 28.5m / min, the length of the annealing chamber is 0.8m, and the residence time of the fiber in the annealing chamber is about 1.7min. The annealing atmosphere is nitrogen protection.

[0047] Second-stage hot stretching: The fiber enters the second-stage hot box, the temperature is set at 135℃, the stretching ratio is 2.6 times, the inlet roller speed is 28.5m / min, the outlet roller speed is 74.1m / min, the length of the hot box is 2.0m, and the residence time is about 2.2s.

[0048] Second relaxation annealing: The fiber enters the second annealing chamber, the temperature is set to 140℃, the fiber relaxes by 3% along the axial direction, the inlet roller speed is 74.1m / min, the outlet roller speed is 71.9m / min, the annealing chamber length is 0.6m, the residence time is about 0.5min, and the annealing atmosphere is nitrogen protection.

[0049] Third-stage hot stretching: The fiber enters the third-stage hot box, with the temperature set at 145℃, a stretch ratio of 2.1, an inlet roller speed of 71.9 m / min, an outlet roller speed of 151.0 m / min, a box length of 2.5 m, and a residence time of approximately 1.4 s. The total effective stretch ratio is approximately 3.0 × 0.95 × 2.6 × 0.97 × 2.1 ≈ 15.0 times.

[0050] 7) Bundle and tie the silk threads After the third stage of stretching, the fibers are coated with 0.3wt% (by weight of the fiber) of silicone-based antistatic oil through an oiling device, and then wound into shape at a speed of 151.0 m / min through a winding device with the winding tension controlled at 1.5 cN / dtex, to obtain high nodular strength ultra-high molecular weight polyethylene fibers.

[0051] The properties of the obtained fibers were tested using an Instron 5967 universal testing machine according to the GB / T 19975 standard method. The clamp spacing was 250 mm, the tensile speed was 250 mm / min, the test temperature was 23±2℃, and the relative humidity was 50±5%. The average value of 20 fiber samples was taken for each group. The nodular strength was tested using the single-knot method. The test results are as follows: fineness 1756 dtex, tensile strength 35.8 cN / dtex, coefficient of variation of tensile strength 3.2%, elongation at break 2.7%, coefficient of variation of elongation 3.5%, tensile modulus 1368 cN / dtex, coefficient of variation of tensile modulus 3.8%, nodular strength 23.5 cN / dtex, nodular strength retention rate 65.6%, coefficient of variation of nodular strength 4.6%.

[0052] Example 2 The preparation method of high nodular strength ultra-high molecular weight polyethylene fiber in this embodiment is basically the same as that in Example 1, except that: in step 6), the first relaxation annealing temperature is adjusted from 128°C to 123°C, and the second relaxation annealing temperature is adjusted from 140°C to 136°C. All other raw material formulations, preparation conditions and operation steps are exactly the same as in Example 1.

[0053] The obtained fibers were subjected to performance tests using the same test methods and conditions as in Example 1. The test results are as follows: fineness 1762 dtex, tensile strength 35.5 cN / dtex, tensile strength coefficient of variation 3.5%, elongation at break 2.8%, elongation coefficient of variation 3.8%, tensile modulus 1345 cN / dtex, tensile modulus coefficient of variation 4.0%, nodular strength 21.8 cN / dtex, nodular strength retention rate 61.4%, nodular strength coefficient of variation 5.0%.

[0054] Example 3 The preparation method of high nodular strength ultra-high molecular weight polyethylene fiber in this embodiment is basically the same as that in Example 1, except that the temperature of the three-stage hot stretching in step 6) is changed. The first-stage stretching temperature is adjusted from 118℃ to 125℃, the second-stage stretching temperature is adjusted from 135℃ to 140℃, and the third-stage stretching temperature is adjusted from 145℃ to 148℃. The stretching ratio (3.0 times / 2.6 times / 2.1 times), annealing conditions (128℃ / 140℃) and other parameters are completely consistent with those in Example 1.

[0055] The obtained fibers were subjected to performance tests using the same test methods and conditions as in Example 1. The test results are as follows: fineness 1748 dtex, tensile strength 34.6 cN / dtex, coefficient of variation of tensile strength 3.8%, elongation at break 2.5%, coefficient of variation of elongation 4.0%, tensile modulus 1402 cN / dtex, coefficient of variation of tensile modulus 4.2%, nodular strength 22.4 cN / dtex, nodular strength retention rate 64.7%, coefficient of variation of nodular strength 5.2%.

[0056] Example 4 The preparation method of high-nodular-strength ultra-high molecular weight polyethylene fiber in this embodiment is basically the same as that in Example 1, except that: in step 2), the viscosity-average molecular weight of the high viscosity-average molecular weight UHMWPE resin is adjusted from 4.5 million to 4 million, while the amount remains 640g; in step 3), the viscosity-average molecular weight of the medium viscosity-average molecular weight UHMWPE resin is adjusted from 1.5 million to 2 million, while the amount remains 160g. The mass ratio of high molecular weight to medium molecular weight UHMWPE remains 80:20, and all other raw material formulations, modified nano-silica dosages, preparation conditions, and operating steps are exactly the same as in Example 1.

[0057] The obtained fibers were subjected to performance tests using the same test methods and conditions as in Example 1. The test results are as follows: fineness 1760 dtex, tensile strength 33.9 cN / dtex, coefficient of variation of tensile strength 3.6%, elongation at break 2.9%, coefficient of variation of elongation 3.6%, tensile modulus 1298 cN / dtex, coefficient of variation of tensile modulus 4.1%, nodular strength 22.0 cN / dtex, nodular strength retention rate 64.9%, coefficient of variation of nodular strength 4.8%.

[0058] Example 5 The preparation method of high-nodular-strength ultra-high molecular weight polyethylene (UHMWPE) fiber in this embodiment is basically the same as that in Example 1, except that: in step 2), the amount of high viscosity-average molecular weight UHMWPE resin is adjusted from 640g to 680g, and the amount of white oil is adjusted accordingly to 7820g to maintain the UHMWPE mass concentration at 8.0wt%; in step 3), the amount of medium viscosity-average molecular weight UHMWPE resin is adjusted from 160g to 120g, and the amount of white oil is adjusted accordingly to 1380g to maintain the UHMWPE mass concentration at 8.0wt%, and the amount of modified nano-silica is adjusted to 3g to maintain its proportion of 2.5wt% of the medium molecular weight UHMWPE mass. The mass ratio of high molecular weight to medium molecular weight UHMWPE is adjusted from 80:20 to 85:15. In step 4), the flow rate of the A-flow metering pump is adjusted to 136mL / min, the flow rate of the B-flow metering pump is adjusted to 24mL / min, and the volumetric flow rate ratio is adjusted accordingly. The remaining preparation conditions and operating steps are exactly the same as in Example 1.

[0059] The obtained fibers were subjected to performance tests using the same test methods and conditions as in Example 1. The test results are as follows: fineness 1750 dtex, tensile strength 36.2 cN / dtex, coefficient of variation of tensile strength 3.0%, elongation at break 2.6%, coefficient of variation of elongation 3.4%, tensile modulus 1395 cN / dtex, coefficient of variation of tensile modulus 3.6%, nodular strength 22.3 cN / dtex, nodular strength retention rate 61.6%, coefficient of variation of nodular strength 4.9%.

[0060] Example 6 The preparation method of high-nodular-strength ultra-high molecular weight polyethylene fiber in this embodiment is basically the same as that in Example 1, except that the amount of stearic acid in step 1) is adjusted from 2.4g to 1.2g, while the remaining modification steps remain unchanged. Thermogravimetric analysis showed that the stearic acid grafting rate of the modified nano-silica was approximately 4.5wt%. In step 3), the amount of modified nano-silica added remains 4g, and all other raw material formulations, preparation conditions, and operating steps are exactly the same as in Example 1.

[0061] The obtained fibers were subjected to performance tests using the same test methods and conditions as in Example 1. The test results are as follows: fineness 1758 dtex, tensile strength 35.4 cN / dtex, coefficient of variation of tensile strength 3.4%, elongation at break 2.8%, coefficient of variation of elongation 3.7%, tensile modulus 1352 cN / dtex, coefficient of variation of tensile modulus 3.9%, nodular strength 21.5 cN / dtex, nodular strength retention rate 60.7%, coefficient of variation of nodular strength 5.3%.

[0062] Comparative Example 1 The preparation method of the high nodular strength ultra-high molecular weight polyethylene fiber in this comparative example includes the following steps: The difference between this comparative example and Example 1 is that: a dual molecular weight UHMWPE blend system is not used; only a single high viscosity-average molecular weight UHMWPE resin is used. All other raw material formulations, preparation conditions, and operating steps are exactly the same as in Example 1.

[0063] Raw material list and specifications: (1) High viscosity-average molecular weight UHMWPE resin: viscosity-average molecular weight 4.5 million, fiber grade, powder, average particle size 150 micrometers. Dosage: 800g.

[0064] (2) Spinning grade white oil: kinematic viscosity (40 degrees Celsius) 68 to 74 mm 2 / s, pour point below -12 degrees Celsius, colorless and odorless. Dosage: 9200g.

[0065] (3) Stearic acid modified nano-silica: Prepared according to the same method as step 1) of Example 1. Dosage: 4g.

[0066] (4) Dichloromethane: Industrial grade, content not less than 99.5%. Dosage: Continuously supplied to the extraction process.

[0067] Preparation steps: Step 1) Preparation of stearic acid modified nano silica: exactly the same as step 1) in Example 1.

[0068] Step 2) Preparation of spinning material: 800g of UHMWPE resin powder with a viscosity-average molecular weight of 4.5 million, 4g of stearic acid-modified nano-silica, and 9200g of spinning-grade white oil were added to a co-rotating twin-screw extruder. The screw diameter was 65 mm, the length-to-diameter ratio was 48:1, and the screw speed was 150 rpm. The temperatures of each section of the barrel from the feed end to the discharge end were set sequentially as follows: Section 1: 80°C, Section 2: 150°C, Section 3: 200°C, Section 4: 210°C, and Section 5: 210°C. The average residence time of the material in the extruder was 15 minutes, and the barrel was purged with nitrogen for protection. The spinning solution obtained at the discharge end had a UHMWPE mass concentration of 8.0% and a modified nano-silica content of 0.5% of the PE mass.

[0069] Step 3) Spinning: The spinning solution is delivered to the spinning assembly via a gear metering pump and extruded through a 200-hole spinneret at a temperature of 195 degrees Celsius. The extrusion rate per hole is 0.8 mL / min. The extruded filaments pass through a 15 mm air gap and then enter a water bath cooling tank at a temperature of 5 degrees Celsius for a cooling distance of 1500 mm, forming gel-like fibers.

[0070] Step 4) Three-stage countercurrent extraction: exactly the same as step 5) in Example 1.

[0071] Step 5) Cascaded heat treatment of "stretching-relaxation annealing-stretching": exactly the same as step 6) of Example 1, that is, the first stage of hot stretching is 118 degrees Celsius, 3.0 times, the first relaxation annealing is 128 degrees Celsius, relaxation is 5%, 1.7 minutes, the second stage of hot stretching is 135 degrees Celsius, 2.6 times, the second relaxation annealing is 140 degrees Celsius, relaxation is 3%, 0.5 minutes, and the third stage of hot stretching is 145 degrees Celsius, 2.1 times.

[0072] Step 6) Winding: exactly the same as step 7) in Example 1.

[0073] The test conditions were exactly the same as in Example 1.

[0074] Test results: Fineness: 1748 dtex Tensile strength: 34.2 cN / dtex Elongation at break: 2.5% Tensile modulus: 1380 cN / dtex Nodule strength: 18.8 cN / dtex Nodule strength retention rate: 55.0% Comparative Example 2 The preparation method of the high nodular strength ultra-high molecular weight polyethylene fiber in this comparative example includes the following steps: The difference between this comparative example and Example 1 is that stearic acid-modified nano-silica is not added, while all other raw material formulations (dual molecular weight blend system), preparation conditions, and operating steps are exactly the same as in Example 1.

[0075] Raw material list and specifications: (1) High viscosity-average molecular weight UHMWPE resin: viscosity-average molecular weight 4.5 million, fiber grade, powder, average particle size 150 micrometers. Dosage: 640g.

[0076] (2) Medium viscosity-average molecular weight UHMWPE resin: viscosity-average molecular weight 1.5 million, injection molding grade, powder, average particle size 120 micrometers. Dosage: 160g.

[0077] (3) Spinning grade white oil: kinematic viscosity (40 degrees Celsius) 68 to 74 mm 2 / s, pour point below -12 degrees Celsius, colorless and odorless. Dosage: 9200g.

[0078] (4) Dichloromethane: Industrial grade, content not less than 99.5%. Dosage: Continuously supplied to the extraction process.

[0079] Preparation steps: Step 1) Preparation of the first spinning material (A stream): exactly the same as Step 2) in Example 1. 640g of UHMWPE resin powder with a viscosity-average molecular weight of 4.5 million and 7360g of spinning-grade white oil were added to the first co-rotating twin-screw extruder, and the process parameters were exactly the same as in Example 1.

[0080] Step 2) Preparation of the second spinning material (B stream): 160g of UHMWPE resin powder with a viscosity-average molecular weight of 1.5 million and 1840g of spinning-grade white oil were added to a second co-rotating twin-screw extruder, without adding stearic acid-modified nano-silica. The screw diameter was 35 mm, the length-to-diameter ratio was 48:1, the screw speed was 180 rpm, and the temperature of each section of the barrel was exactly the same as in Step 3) of Example 1. The mass concentration of UHMWPE in the B stream was 8.0%.

[0081] Step 3) Dual-flow convergence and spinneret formation: exactly the same as step 4) in Example 1.

[0082] Step 4) Three-stage countercurrent extraction: exactly the same as step 5) in Example 1.

[0083] Step 5) "Stretch-Relaxation Annealing-Stretch" cascade heat treatment: exactly the same as Step 6) in Example 1.

[0084] Step 6) Winding: exactly the same as step 7) in Example 1.

[0085] The test conditions were exactly the same as in Example 1.

[0086] Test results: Fineness: 1760 dtex Tensile strength: 35.2 cN / dtex Elongation at break: 2.8% Tensile modulus: 1350 cN / dtex Nodule strength: 20.5 cN / dtex Nodule strength retention rate: 58.2% Comparative Example 3 The preparation method of the high nodular strength ultra-high molecular weight polyethylene fiber in this comparative example includes the following steps: The difference between this comparative example and Example 1 is that the "stretching-relaxation annealing-stretching" cascade process is not used. Instead, a continuous three-stage hot stretching process without intermediate relaxation annealing steps is used. All other raw material formulations (dual molecular weight blend system, stearic acid modified nano-silica), preparation conditions and operating steps are exactly the same as in Example 1.

[0087] Raw material list and specifications: exactly the same as in Example 1, including: (1) High viscosity-average molecular weight UHMWPE resin: viscosity-average molecular weight 4.5 million, fiber grade, powder, average particle size 150 micrometers. Dosage: 640g.

[0088] (2) Medium viscosity-average molecular weight UHMWPE resin: viscosity-average molecular weight 1.5 million, injection molding grade, powder, average particle size 120 micrometers. Dosage: 160g.

[0089] (3) Spinning grade white oil: kinematic viscosity (40 degrees Celsius) 68 to 74 mm 2 / s, pour point below -12 degrees Celsius, colorless and odorless. Dosage: 9200g.

[0090] (4) Stearic acid modified nano-silica: Prepared using the same method as step 1) of Example 1. Dosage: 4g.

[0091] (5) Dichloromethane: Industrial grade, content not less than 99.5%. Dosage: Continuously supplied to the extraction process.

[0092] Preparation steps: Step 1) Preparation of stearic acid modified nano silica: exactly the same as step 1) in Example 1.

[0093] Step 2) Preparation of the first spinning material (A stream): exactly the same as step 2) in Example 1.

[0094] Step 3) Preparation of the second spinning material (B stream): exactly the same as step 3) in Example 1.

[0095] Step 4) Dual-flow convergence and spinneret formation: exactly the same as step 4) in Example 1.

[0096] Step 5) Three-stage countercurrent extraction: exactly the same as step 5) in Example 1.

[0097] Step 6) Continuous three-stage hot stretching: The dried fibers are sequentially subjected to the following three tandem stretching processes, eliminating the two relaxation annealing steps in Example 1: First stage of hot stretching: hot box temperature 118 degrees Celsius, stretching ratio 3.0 times, inlet roller speed 10 m / min, outlet roller speed 30 m / min, hot box length 1.5 m.

[0098] Second-stage hot stretching: hot box temperature 135 degrees Celsius, stretching ratio 2.6 times, inlet roller speed 30 m / min, outlet roller speed 78 m / min, hot box length 2.0 m.

[0099] Third-stage hot stretching: hot box temperature 145 degrees Celsius, stretching ratio 2.1 times, inlet roller speed 78 m / min, outlet roller speed 163.8 m / min, hot box length 2.5 m.

[0100] The total stretch ratio is 3.0 × 2.6 × 2.1 = 16.4 times.

[0101] Step 7) Winding: exactly the same as step 7) in Example 1, except the winding speed is adjusted to 163.8 m / min.

[0102] The test conditions were exactly the same as in Example 1.

[0103] Test results: Fineness: 1740 dtex Tensile strength: 36.5 cN / dtex Elongation at break: 2.4% Tensile modulus: 1410 cN / dtex Nodule strength: 19.2 cN / dtex Nodule strength retention rate: 52.6% Experimental content The performance test data of Examples 1 to 3 and Comparative Examples 1 to 3 are summarized in Table 1. The test conditions were uniform: tensile strength and elongation were determined according to the GB / T 19975 standard method using an Instron 5967 universal testing machine with a clamp spacing of 250 mm, a tensile speed of 250 mm / min, a test temperature of 23±2 degrees Celsius, and a relative humidity of 50±5%. The average value of 20 fiber samples was taken for each test group. Nodal strength was tested using the single-knot method, i.e., a simple knot was tied in the middle of the fiber before tensile testing, under the same conditions as above. The scanning electron microscope image of the fiber obtained in Example 1 is shown below. Figure 1 As shown.

[0104] Table 1 Summary of performance test data for both examples and comparative examples

[0105] Note: The data in Example 3 in Table 1 are based on the description of Example 3 in the technical solution, that is, the first stage tensile temperature is increased to 125 degrees Celsius, the second stage tensile temperature is increased to 140 degrees Celsius, and the third stage tensile temperature is increased to 148 degrees Celsius. The other parameters are the same as in Example 1.

[0106] As shown in Table 1, the tensile strength of Examples 1 to 3 is not less than 34.8 cN / dtex, the nodular strength is not less than 21.8 cN / dtex, and the nodular strength retention rate is not less than 61.4%. Among them, Example 1 has the highest nodular strength retention rate, reaching 65.6%.

[0107] Comparative Example 1 used only a single high viscosity-average molecular weight UHMWPE resin without employing a dual molecular weight blend system. Its nodal strength was 18.8 cN / dtex, and the nodal strength retention rate was 55.0%, representing a decrease of 4.7 cN / dtex and 10.6 percentage points compared to Example 1, respectively. This demonstrates that viscosity-average molecular weight UHMWPE, as a bridging chain source, plays a crucial role in enhancing fiber transverse cohesion and nodal strength.

[0108] Comparative Example 2 used a dual molecular weight blend system but without the addition of stearic acid-modified nano-silica. Its nodule strength was 20.5 cN / dtex, and the nodule strength retention rate was 58.2%, which were 3.0 cN / dtex and 7.4 percentage points lower than those in Example 1, respectively. This indicates that stearic acid-modified nano-silica, as an interfacial heterogeneous nucleation site, is indispensable for guiding the efficient formation of bridging crystals.

[0109] Although Comparative Example 3 employed both a dual molecular weight blend system and stearic acid-modified nano-silica, it omitted the intermediate relaxation annealing step. Its nodular strength was 19.2 cN / dtex, with a nodular strength retention rate of only 52.6%, the lowest among all comparative examples, representing a decrease of 4.3 cN / dtex and 13.0 percentage points compared to Example 1. Notably, Comparative Example 3 exhibited a tensile strength of 36.5 cN / dtex, slightly higher than Example 1. This is because the continuous three-stage hot stretching without relaxation annealing resulted in a higher total stretch ratio (16.4 times compared to approximately 15.0 times in Example 1), and a higher degree of molecular chain axial orientation. However, the lack of a bridging crystallization formation time window provided by relaxation annealing meant that even with bridging chain sources and interfacial nucleation sites, the bridging crystallization network could not be effectively constructed, resulting in severely insufficient transverse cohesion of the fibers. The nodular strength retention rate was even lower than that of Comparative Example 1, which only lacked the dual molecular weight blend design. This result strongly demonstrates the decisive role of the "stretch-relaxation annealing-stretch" cascade process in the construction of bridging crystalline networks, and also verifies the strict coupling dependency between the three innovative designs—all three are indispensable, and the absence of any single one leads to a significant decrease in nodule strength.

Claims

1. A method for preparing high-nodular-strength ultra-high molecular weight polyethylene fiber, characterized in that, Includes the following steps: 1) Stearic acid and fumed silica nanoparticles were reacted in a solvent to carry out a surface modification reaction, resulting in stearic acid-modified silica nanoparticles; 2) A high viscosity-average molecular weight UHMWPE resin is mixed with white oil and extruded through a screw extruder to obtain spinning solution A; a medium viscosity-average molecular weight UHMWPE resin, white oil, and the stearic acid-modified nano-silica are mixed and extruded through a screw extruder to obtain spinning solution B; the high viscosity-average molecular weight UHMWPE resin has a viscosity-average molecular weight of 4 million to 5 million, and the medium viscosity-average molecular weight UHMWPE resin has a viscosity-average molecular weight of 1 million to 2 million; the mass ratio of the high viscosity-average molecular weight UHMWPE resin to the medium viscosity-average molecular weight UHMWPE resin is (75-85):(15-25); the stearic acid-modified nano-silica is pre-dispersed in the spinning solution B, and its addition amount is 1.5% to 3.5% of the mass of the medium viscosity-average molecular weight UHMWPE resin; the mass concentration of UHMWPE in the spinning solution A and spinning solution B is independently 6% to 10%. 3) After the spinning solution A stream and spinning solution B stream are combined and mixed, they are extruded through a spinneret and cooled to obtain gel-state fibers; 4) After extraction and drying, the gel-state fiber is subjected to first-stage hot stretching, first-stage relaxation annealing, second-stage hot stretching, second-stage relaxation annealing and third-stage hot stretching in sequence to obtain the high-nodular-strength ultra-high molecular weight polyethylene fiber.

2. The preparation method according to claim 1, characterized in that, In step 1), the average particle size of the fumed silica nanoparticles is 15–30 nm, and the specific surface area is 180–220 m². 2 / g; the mass ratio of stearic acid to nano silica is (8-15):100; the surface modification reaction temperature is the ethanol reflux temperature, and the reaction time is 2-4 hours; the stearic acid grafting rate of the stearic acid modified nano silica is 6%-12%.

3. The preparation method according to claim 1, characterized in that, In step 3), the combined spinning solution is mixed by a static mixer, the temperature of the spinning solution is 200-210℃, the temperature of the spinneret is 190-200℃, and the extruded filaments are cooled and shaped in a cooling medium at a temperature of 0-10℃ after passing through an air gap.

4. The preparation method according to claim 1, characterized in that, In step 4), the temperature of the first stage of hot stretching is 115-120℃, and the stretching ratio is 2.8-3.2 times; the temperature of the second stage of hot stretching is 132-138℃, and the stretching ratio is 2.4-2.8 times; the temperature of the third stage of hot stretching is 143-148℃, and the stretching ratio is 1.8-2.2 times.

5. The preparation method according to claim 1, characterized in that, In step 4), the temperature of the first relaxation annealing is 125-132℃, the axial relaxation amount is 3%-5%, and the annealing time is 1.5-2.5 minutes; the temperature of the second relaxation annealing is 138-143℃, the axial relaxation amount is 2%-4%, and the annealing time is 0.5-2 minutes.

6. The preparation method according to claim 1, characterized in that, In step 4), the extraction is carried out using dichloromethane for multi-stage countercurrent extraction at an extraction temperature of 25-35°C. After extraction, the residual white oil content in the fiber is less than 1.5%. The total effective stretch ratio of the three-stage hot stretching is 13-17 times.

7. A high-nodular-strength ultra-high molecular weight polyethylene fiber, characterized in that, The fiber is prepared by the preparation method according to any one of claims 1 to 6; the fiber comprises an axially oriented fibril structure formed by high viscosity-average molecular weight UHMWPE and an interfibril bridging crystalline network formed by medium viscosity-average molecular weight UHMWPE, as well as stearic acid modified nano-silica distributed at the fibril interface; the tensile strength of the fiber is not less than 33.5 cN / dtex, and the nodule strength retention rate is 60% to 68%.

8. The high-nodular-strength ultra-high molecular weight polyethylene fiber as described in claim 7, characterized in that, The fiber has a crystallinity of 78%–85% and an orientation factor of 0.93–0.97; the content of nano-silica in the fiber, calculated as SiO2, is 0.15%–0.35%; the bridging crystal connects adjacent fibrils at an angle of 15°–45° to the fiber axis.