A method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fibers
By melt spinning a mixture of polyacrylonitrile and polyimide and performing segmented pre-oxidation treatment, the processability and mechanical properties of polyacrylonitrile pre-oxidized fibers were solved, resulting in high-strength, flame-retardant pre-oxidized fibers suitable for high-end textiles and composite materials.
Patent Information
- Application Number
- CN202611355604.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-17
AI Technical Summary
Existing pre-oxidized polyacrylonitrile fibers have defects in processability and mechanical properties, making it difficult to meet the needs of high-end applications. Furthermore, when PI is combined with PAN materials, there are problems with poor dispersion uniformity and microphase separation.
A mixture of polyacrylonitrile and polyimide is melt-spun and pre-oxidized in stages to form a core-sheath structure. The cyano groups of polyimide participate in the cyclization reaction to improve the flame retardant properties and mechanical strength of the fiber.
It has achieved the preparation of high-strength, low-cost pre-oxidized fibers with excellent flame retardant properties and mechanical strength, meeting the application requirements of high-end textiles.
Abstract
Description
Technical Field
[0001] This application relates to a method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber, belonging to the field of polyacrylonitrile filament technology. Background Technology
[0002] Polyacrylonitrile (PAN) pre-oxidized fibers, with their excellent flame retardancy, high temperature resistance, acid and alkali corrosion resistance, low production cost, and outstanding cost-effectiveness, are widely used in many fields such as flame-retardant textile materials, high-temperature dust removal filter materials, carbon / carbon composite materials, and activated carbon fiber precursors, making them one of the important materials in industrial protection and high-end composite materials. However, existing pure PAN pre-oxidized fibers have many inherent performance defects, which greatly limit their high-end application scenarios: On the one hand, PAN raw materials have poor processability and are difficult to spin into finished products. Currently, wet spinning, dry-jet wet spinning, and dry spinning processes all rely on large amounts of organic solvents such as N,N-dimethylformamide and dimethyl sulfoxide, resulting in organic solvent pollution, high raw material and environmental treatment costs, and high energy consumption. While melt spinning does not require organic solvents and avoids problems such as solvent pollution and residual defects, PAN materials have inherent processing limitations. Their melting temperature is much higher than their thermal decomposition temperature, making it impossible to achieve melt spinning under conventional process conditions. This greatly restricts the widespread application of melt spinning technology in PAN fiber preparation.
[0003] On the other hand, it has poor mechanical properties, with low overall strength and high brittleness. Nascent PAN fibers are prone to phase separation and structural defects in the coagulation bath. Residual organic solvents inside the fibers form micropores and voids during the pre-oxidation process, further deteriorating the mechanical strength and structural uniformity of the pre-oxidized fibers. During stress processing and actual service, the fibers are prone to excessive oxidation fragments and residue shedding, which seriously affects the appearance integrity and service stability of textiles, and significantly reduces the application value of PAN pre-oxidized fibers in the field of high-end flame-retardant textiles.
[0004] Polyimide (PI) is a high-performance polymer material with an imide ring in its main chain. It possesses excellent comprehensive properties, exhibiting superior resistance to high and low temperatures, aging, and chemical stability. Furthermore, its tensile strength and structural stability far surpass those of traditional PAN materials. Currently, PI films, PI fibers, and other derivative products are widely used in aerospace, precision protection, and high-end insulation fields, and are recognized as high-performance structural and functional materials. Combining PI with PAN materials can achieve complementary performance, balancing excellent mechanical properties, low cost, and functionality, making it highly valuable for research and application. However, we have discovered two major drawbacks in the composite process: firstly, the poor uniformity of PI dispersion leads to uneven fiber strength; secondly, during the high-temperature pre-oxidation stage, microphase separation easily occurs between PI and pre-oxidized PAN, further reducing fiber strength. Summary of the Invention
[0005] In view of this, this application provides a method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber, which is not only simple and efficient in preparation, but also produces fibers with excellent flame retardant properties and mechanical strength.
[0006] Specifically, this application is implemented through the following scheme: A method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber, comprising the following steps: Step 1: After mixing polyacrylonitrile A and polyimide evenly, polyacrylonitrile B is added to obtain a mixture of polyacrylonitrile and polyimide. Polyacrylonitrile A is a copolymer formed by acrylonitrile and a second monomer, and polyacrylonitrile B is a pure acrylonitrile polymer. Step 2: After the polyacrylonitrile and polyimide mixture is melt-spun at a temperature below 200°C, it is then wound to obtain PAN fibers. Step 3, segmented pre-oxidation of PAN fibers: The temperature of the first stage of pre-oxidation is 210-230℃ and the duration is 0.5-1.0h; the temperature of the second stage of pre-oxidation is 250-260℃ and the duration is 0.5-1.0h, to obtain pre-oxidized polyacrylonitrile fibers.
[0007] Furthermore, as a preferred option: In step one, The mass ratio of polyacrylonitrile A, polyacrylonitrile B, and polyimide is 10-20:85-65:5-15, and preferably 15:75:10.
[0008] In the polyacrylonitrile A, the second monomer accounts for 10-15% of the mass of the two materials, aiming to lower the melting point of polyacrylonitrile, and is not limited to a specific type. More preferably, the second monomer is any one of vinyl acetate, ethyl vinyl ether, methyl acrylate, and butyl acrylate.
[0009] The weight-average molecular weight of the polyacrylonitrile A is 2.0 × 10⁻� 4 ~3.0×10 4 More preferably 2.0×10 4 ~2.87×10 4 More preferably 2.3×10 4 ~2.5×10 4 .
[0010] The particle size D50 of the polyacrylonitrile A is 20-30 μm, preferably 25 μm.
[0011] The weight-average molecular weight of the polyacrylonitrile B is 5.0 × 10⁻� 4 ~7.0×10 4Further optimization of 5.7×10 4 ~6.86×10 4 More preferably 6.0×10 4 ~6.5×10 4 .
[0012] The polyimide is a BPDA-PDA-ODA-DABN quaternary copolymer, namely, a polymer obtained by copolymerizing 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), p-phenylenediamine (PDA), 4,4'-diphenyl ether diamine (ODA), and bis(dodecyl)dimethylammonium bromide (DABN) in a molar ratio of 0.8:0.5:0.3:0.2, with a number average molecular weight of 50,000 to 55,000 g / mol.
[0013] The particle size D50 of the polyimide powder is 5-10 μm, preferably 5 μm.
[0014] The particle size D50 of the polyacrylonitrile B is 20-30 μm, preferably 25 μm.
[0015] The melting point of the polyacrylonitrile and polyimide mixture is 180–193°C.
[0016] In step two, The melt spinning is performed using a twin-screw melt spinning machine.
[0017] The melt spinning temperature is 170–200°C, and the melt spinning screw speed is 30–50 r / min. More preferably, the melt spinning temperature is 185°C, and the melt spinning screw speed is 40 r / min.
[0018] The winding speed is 400-600 m / min.
[0019] The working principle and beneficial effects of this application are summarized as follows: (1) Polyacrylonitrile A and B are powders with a D50 of 20-30 μm, and polyimide powder is powder with a particle size of 5-10 μm. During the mixing process, the three are conducive to the uniform distribution of polyimide in polyacrylonitrile.
[0020] (2) Using polyacrylonitrile A with a smaller weight average molecular weight to blend with polyacrylonitrile B and polyimide with a larger weight average molecular weight for melt spinning can not only lower the melting point of the mixture to below 200°C for melt spinning; under the high temperature of the pre-oxidation stage, polyacrylonitrile A can also migrate to the fiber surface to participate in chemical reactions such as cyclization, dehydrogenation, oxidation and cross-linking, so that the pre-oxidation degree of the fiber surface is significantly greater than that of the fiber interior, promoting the formation of the core-sheath structure. While giving the fiber excellent flame retardant properties, it reduces the damage to the fiber strength. Moreover, since the melt rheological properties of polyacrylonitrile A are better than those of polyacrylonitrile B, it is easy to wet and spread on the polyimide surface during melt spinning, thereby effectively avoiding the aggregation of polyimide powder.
[0021] (3) The polyimide side chain used in the mixture contains cyano groups, which participate in the cyclization reaction of polyacrylonitrile during the pre-oxidation process and improve the compatibility between polyimide and polyacrylonitrile through valence bonds, thereby improving the strength of the fiber.
[0022] (4) By segmented pre-oxidation, pre-oxidized fibers with a distinct core-sheath structure are obtained, which meets the requirement that flame-retardant textiles only require the fiber surface to have flame-retardant functional properties. Specifically: during the first stage of pre-oxidation, polyacrylonitrile A with a lower weight-average molecular weight migrates to the fiber surface. During the migration to the fiber surface, it does not generate pores inside the fiber, that is, polyacrylonitrile A does not have a significant impact on the fiber strength; during the second stage of pre-oxidation, polyacrylonitrile A with a lower weight-average molecular weight rapidly participates in the pre-oxidation reaction on the fiber surface, forming a dense sheath layer with significant flame-retardant effect on the fiber surface. Detailed Implementation
[0023] To make the technical problems, technical solutions, and beneficial effects to be solved by this application clearer, the technical solutions of this application will be further described in detail below with reference to specific examples in the embodiments of this application. It should be understood that the specific embodiments described herein are only used to explain this application and are not intended to limit the technical solutions of this application. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.
[0024] Example 1
[0025] This embodiment provides a method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fibers, the steps of which are as follows: Step 1: By mechanical stirring, 15 parts by weight of particles with a particle size D50 = 25 μm and a weight-average molecular weight of 2.35 × 10⁻⁶ were mixed. 4 After mixing polyacrylonitrile A powder with 10 parts by weight of polyimide powder with a particle size D50 = 5 μm and homogeneous, 75 parts by weight of polyimide powder with a particle size D50 = 25 μm and a weight average molecular weight of 6.56 × 10⁻⁶ was added. 4Polyacrylonitrile B powder was stirred and mixed evenly to obtain a mixture of polyacrylonitrile and polyimide. The melting point of this mixture was determined to be 185℃.
[0026] Polyacrylonitrile A is a copolymer of acrylonitrile and a second monomer, specifically vinyl acetate, with a feed percentage of 8.5%. Polyimide is a quaternary copolymer of BPDA-PDA-ODA-DABN.
[0027] Step 2: Melt spinning using a twin-screw melt spinning machine: Heat the twin-screw melt spinning machine to 185℃, preheat for 30 minutes, adjust the screw speed to 40 r / min, add the mixture of polyacrylonitrile and polyimide, and wind at a speed of 450 m / min to obtain PAN fibers.
[0028] Step 3, segmented pre-oxidation: The parameters for the first stage of pre-oxidation are 210℃ for 1.0h and the parameters for the second stage of pre-oxidation are 260℃ for 0.5h, to obtain polyacrylonitrile pre-oxidized fibers.
[0029] In the above process: The structural formula of polyimide (PI) is: .
[0030] The structural formula of polyacrylonitrile pre-oxidized fiber is: .
[0031] The strength of PAN fiber is 67.7 cN / tex, and the coefficient of variation of strength is 0.15; the strength of pre-oxidized fiber PANOF is 63.9 cN / tex, and the limiting oxygen index is 28.9%.
[0032] Example 2
[0033] This embodiment has the same setup as Embodiment 1, except that the step-by-step mixing in step one is replaced with a single-step mixing, that is: Polyacrylonitrile A powder (15 parts by weight, particle size D50 = 25 μm, weight average molecular weight 2.35 × 10⁻⁶) 4 Polyimide powder (10 parts by weight, particle size D50 = 5 μm), polyacrylonitrile B (75 parts by weight, particle size D50 = 25 μm, weight average molecular weight 6.56 × 10⁻⁶), and polyimide powder (10 parts by weight, particle size D50 = 5 μm, weight average molecular weight 6.56 × 10⁻⁶). 4 The powder is simultaneously put into a mixer for mechanical stirring to obtain a mixture of polyacrylonitrile and polyimide.
[0034] The strength of PAN fiber is 58.7 cN / tex, and the coefficient of variation of strength is 0.39; the strength of PANOF is 55.8 cN / tex, and the limiting oxygen index is 27.9%.
[0035] Compared to Example 1, the strength of the fiber filament prepared by one-step mixing is significantly lower than that of the sample prepared by two-step mixing, and the coefficient of variation of the former is significantly greater than that of the latter. This is because, in one-step mixing, polyimide and polyacrylonitrile A are not easily uniformly distributed in polyacrylonitrile B, and polyimide and polyacrylonitrile A are not easily mixed uniformly, which leads to the easy aggregation of polyimide during melt spinning. In two-step mixing, firstly, polyimide and polyacrylonitrile A are uniformly mixed, and then the mixture is mixed with polyacrylonitrile B, resulting in uniform mixing of the three components; secondly, during melt spinning, the polyacrylonitrile A melt with a lower weight-average molecular weight is easily wetted and spread on the surface of polyimide, thus effectively avoiding the aggregation of polyimide powder. Therefore, the fiber prepared by two-step mixing has higher strength and better uniformity.
[0036] Example 3
[0037] This embodiment has the same setup as Example 1, except that the polyimide is replaced with a BPDA-PDA-ODA terpolymer, which is a polymer obtained by copolymerizing 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), p-phenylenediamine (PDA), and 4,4'-diphenyl ether diamine (ODA) in a mass ratio of 0.8:0.5:0.3, with a number average molecular weight of 52000 g / mol.
[0038] The strength of PAN fiber is 67.1 cN / tex, and the coefficient of variation of strength is 0.17; the strength of PANOF is 55.7 cN / tex, and the limiting oxygen index is 28.1%.
[0039] Compared to Example 1, the strength of pre-oxidized fibers prepared by melt spinning BPDA-PDA-ODA terpolymer as the polyimide was significantly lower than that of pre-oxidized fibers prepared by melt spinning BPDA-PDA-ODA-DABN quaternary copolymer as the polyimide. This is because the thermodynamic compatibility between BPDA-PDA-ODA terpolymer and polyacrylonitrile is poor, leading to phase separation during pre-oxidation and resulting in lower fiber strength. The BPDA-PDA-ODA-DABN quaternary copolymer contains cyano groups in its side chains, which can react with the cyano groups in polyacrylonitrile during pre-oxidation to form valence bonds, effectively suppressing phase separation and imparting good strength to the fibers.
[0040] Example 4
[0041] The setup in this embodiment is the same as in Embodiment 1, except that the weight-average molecular weights of polyacrylonitrile A and polyacrylonitrile B are shown in Table 1.
[0042] Table 1: Effect of different weight-average molecular weights on the melting point of polyacrylonitrile / polyimide mixtures and corresponding PAN fibers .
[0043] As shown in Table 1, when the weight-average molecular weight of polyacrylonitrile B is maintained at 6.56 × 10⁻⁶... 4 At this point, the melting point and strength of the polyacrylonitrile-polyimide mixture and the fiber filament both gradually increase with the increase of the weight-average molecular weight of polyacrylonitrile A, but the strength is relatively low at a weight-average molecular weight of 2.87 × 10⁻⁶. 4 ~3.29×10 4 It maintained a value above 66.6 cN / tex, and the weight-average molecular weight of polyacrylonitrile A was 2.35 × 10⁻⁶. 4 The melting point reaches a maximum of 67.7 cN / tex. While a lower melting point is more favorable for melt spinning, the strength of the fiber filament is lower. Meanwhile, when the weight-average molecular weight of polyacrylonitrile A is maintained at 2.35 × 10⁻⁶... 4 At that time, the melting point of the mixture and the strength of the fiber filaments both gradually increased with the increase of the viscosity-average molecular weight of polyacrylonitrile B.
[0044] During the above experiments on weight-average molecular weight, we found that when the melting temperature exceeds 200℃ (as shown in items 4 and 8 in Table 1), polyacrylonitrile undergoes a small amount of decomposition. Considering both melting point and fiber filament strength, the optimal melting point of the polyacrylonitrile / polyimide mixture should be controlled within the range of 180–193℃, and the corresponding weight-average molecular weight of polyacrylonitrile A is preferably controlled at 2.35 × 10⁻⁶. 4 Left and right, such as: 2.0×10 4 ~2.87×10 4 The weight-average molecular weight of polyacrylonitrile B is preferably controlled at 6.56 × 10⁻⁶. 4 Left and right, such as: 5.7×10 4 ~6.86×10 4 .
[0045] Example 5
[0046] This embodiment has the same setup as Embodiment 1, except that: polyacrylonitrile A ( m A ), Polyacrylonitrile B ( m B ), polyimide ( m C The mass ratio of 15:75:10 has been replaced as shown in Table 2.
[0047] Table 2: Effects of different compositions on the melting point and fiber properties of polyacrylonitrile and polyimide mixtures .
[0048] As shown in Table 2 and Example 1, with the increase of the mass percentage of polyacrylonitrile A, the melting point of the polyacrylonitrile / polyimide mixture gradually decreases, the strength of the pre-oxidized fiber filaments shows a trend of first increasing and then decreasing, and the limiting oxygen index gradually increases. This is because, as the mass percentage of polyacrylonitrile A increases, its blocking effect on the polyacrylonitrile B molecular chains is enhanced, and the melting point of the polyacrylonitrile / polyimide mixture decreases. Furthermore, during pre-oxidation, polyacrylonitrile A, with its lower weight-average molecular weight, can migrate to the fiber surface and participate in chemical reactions such as cyclization, dehydrogenation, oxidation, and cross-linking, forming a dense protective layer on the fiber surface and slowing down the oxidation reaction inside the fiber. When the mass percentage of polyacrylonitrile A is low, the protective layer on the fiber surface has a weak protective effect on the fiber interior, resulting in lower strength. When its mass percentage is high, although the protection on the fiber surface provides good protection for the fiber interior, a small amount remains inside the fiber, affecting the fiber strength. The limiting oxygen index mainly depends on the degree of oxidation of the fiber surface.
[0049] Meanwhile, with the mass ratio of polyacrylonitrile A to polyacrylonitrile B remaining constant at 1:5, as the mass percentage of polyimide increased from 5% to 10%, 15%, and 20%, the melting point of the mixture gradually decreased from 189℃ to 185℃, 182℃, and 181℃, respectively. The strength of the pre-oxidized fiber filaments showed a trend of first increasing and then decreasing, while the limiting oxygen index remained unchanged. This is because as the mass percentage of polyimide increases, its blocking effect on the polyacrylonitrile molecular chains strengthens, lowering the melting point of the polyacrylonitrile / polyimide mixture. Due to the inherent high strength properties of polyimide, it has a reinforcing effect on polyacrylonitrile. However, at higher mass percentages of polyimide, aggregation may occur, and the orderly arrangement of polyacrylonitrile molecular chains may also be hindered, thus reducing the strength of the polyacrylonitrile fibers.
[0050] Example 6
[0051] This embodiment has the same setup as Embodiment 1, except that the segmented pre-oxidation in step three is replaced by a single-stage pre-oxidation, i.e., the PAN fibers are pre-oxidized at 260°C for 1 hour.
[0052] The strength of PAN fiber is 67.7 cN / tex, and the coefficient of variation of strength is 0.15; the strength of PANOF is 56.6 cN / tex, and the limiting oxygen index is 29.2%.
[0053] Compared to Example 1, the strength of the single-stage pre-oxidized fiber was significantly lower than that of the two-stage pre-oxidized fiber, while the limiting oxygen index showed no significant difference. This is because, during high-temperature one-step oxidation, firstly, the cyclization reaction erupts instantaneously, and the exothermic reaction cannot dissipate in time, leading to localized overheating inside the fiber and causing fiber degradation; secondly, it accelerates the phase separation of polyacrylonitrile and polyimide at high temperatures, weakening the interfacial bonding between the two phases.
[0054] The above-described embodiments are merely illustrative of several feasible implementations of the present invention, and their descriptions are relatively specific and detailed. However, they should not be construed as limiting the scope of the present invention, nor are the embodiments intended to limit the scope of protection in the claims of the present invention. For those skilled in the art, various modifications and improvements can be made without departing from the concept of the present invention. All equivalent implementations or changes that do not depart from the present invention should be included in the technology of the present invention.
Claims
1. A method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber, characterized in that, The steps are as follows: Step 1: After mixing polyacrylonitrile A and polyimide evenly, polyacrylonitrile B is added to obtain a mixture of polyacrylonitrile and polyimide. Polyacrylonitrile A is a copolymer formed by acrylonitrile and a second monomer, and polyacrylonitrile B is a pure acrylonitrile polymer. Step 2: After the polyacrylonitrile and polyimide mixture is melt-spun at a temperature below 200°C, it is then wound to obtain PAN fibers. Step 3, segmented pre-oxidation of PAN fibers: The temperature of the first stage of pre-oxidation is 210-230℃ and the duration is 0.5-1.0h; the temperature of the second stage of pre-oxidation is 250-260℃ and the duration is 0.5-1.0h, to obtain pre-oxidized polyacrylonitrile fibers.
2. The method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber according to claim 1, characterized in that: The mass ratio of polyacrylonitrile A, polyacrylonitrile B, and polyimide is 10-20:85-65:5-15.
3. The method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber according to claim 1, characterized in that: In the polyacrylonitrile A, the second monomer accounts for 10-15% of the total mass of the two materials.
4. The method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber according to claim 1, characterized in that: The weight-average molecular weight of the polyacrylonitrile A is 2.0 × 10⁻⁶. 4 ~3.0×10 4 The weight-average molecular weight of polyacrylonitrile B is 5.0 × 10⁻⁶. 4 ~7.0×10 4 .
5. The method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber according to claim 1, characterized in that: The particle size D50 of the polyacrylonitrile A is 20-30 μm, the particle size D50 of the polyacrylonitrile B is 20-30 μm, and the particle size D50 of the polyimide powder is 5-10 μm.
6. The method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber according to claim 1, characterized in that: The polyimide is a quaternary copolymer of BPDA-PDA-ODA-DABN.
7. The method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber according to claim 1, characterized in that: The melting point of the polyacrylonitrile and polyimide mixture is 180–193°C.
8. The method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber according to claim 1, characterized in that: The melt spinning temperature is 170–200°C, and the melt spinning screw speed is 30–50 r / min.
9. The method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber according to claim 1, characterized in that: The winding speed is 400-600 m / min.
10. The method for preparing high-strength melt-spun polyacrylonitrile pre-oxidized fiber according to claim 1, characterized in that: The weight-average molecular weight of polyacrylonitrile A is 2.0 × 10⁻⁶. 4 ~2.87×10 4 The weight-average molecular weight of polyacrylonitrile B is 5.7 × 10⁻⁶. 4 ~6.86×10 4 The melt spinning temperature was 185℃, and the melt spinning screw speed was 40 r / min.