A method for preparing composite yarn of STF / liquid silica-modified pre-oxidized staple fiber yarn and para-aramid filament yarn
The method of preparing core-sheath composite yarn by combining STF/liquid silica-modified pre-oxidized short fiber yarn with para-aramid filament has solved the shortcomings of single fiber materials in terms of flame retardancy and cut resistance, and achieved a multi-functional synergistic performance improvement of the yarn, which is suitable for high-end protective textiles.
Patent Information
- Application Number
- CN202611462257.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-17
AI Technical Summary
Single-fiber materials cannot simultaneously achieve both flame retardancy and cut resistance. Existing fibers are insufficient in terms of heat aging resistance and UV aging resistance, making it difficult to meet the comprehensive performance requirements of protective fabrics in complex service environments.
A composite yarn of pre-oxidized short fiber yarn modified with STF/liquid silica gel and para-aramid filament yarn is prepared by shear thickening liquid treatment and liquid silica gel finishing to form a core-sheath structure. Combined with phosphorus-based halogen-free flame retardant, the multifunctional synergistic properties of the fiber are achieved.
It significantly improves the mechanical properties and aging resistance of composite yarns, solves the problems of yarns feeling sticky, easily falling off and migrating after conventional treatment, and provides an ideal material solution for high-end protective textiles.
Smart Images

Figure CN123108797A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite yarn technology, and more specifically, to a method for preparing a composite yarn of STF / liquid silica-modified pre-oxidized staple fiber yarn and para-aramid filament. Background Technology
[0002] Currently, flame-retardant protective materials mostly utilize modified aramid, flame-retardant polyester, and carbon fiber as raw materials. These materials typically possess good thermal stability and flame-retardant properties. In the field of cut resistance, high-strength, high-modulus fibers such as para-aramid and ultra-high molecular weight polyethylene are widely used, as their excellent mechanical properties make them outstanding in cut resistance. However, a single type of fiber often struggles to simultaneously achieve both flame retardancy and cut resistance. While para-aramid fibers possess high strength and modulus, they still have certain shortcomings in heat aging resistance and UV aging resistance. Polyacrylonitrile-based pre-oxidized fibers exhibit intrinsic flame retardancy and good thermal stability, but their mechanical properties are relatively weak, making it difficult to meet the load-bearing capacity and damage resistance requirements of high-level protection when used alone. Therefore, single-fiber materials have significant limitations in multi-functional protection and cannot meet the actual needs of comprehensive performance of protective fabrics in complex service environments. Thus, combining the excellent properties of pre-oxidized fibers with those of para-aramid, thereby overcoming the performance bottleneck of single materials, and preparing composite yarns with excellent comprehensive performance will have broad application prospects. Summary of the Invention
[0003] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing composite yarn of STF / liquid silica-modified pre-oxidized short fiber yarn and para-aramid filament.
[0004] To achieve the above objectives, the present invention adopts the following technical solution:
[0005] A method for preparing a composite yarn of STF / liquid silica-modified pre-oxidized staple fiber yarn and para-aramid filament includes the following steps:
[0006] (1) SiO2 is dispersed in polyethylene glycol to prepare a shear thickening solution;
[0007] (2) Mix component A and component B of liquid silica gel, add phosphorus-based halogen-free flame retardant and anhydrous ethanol, mix evenly to obtain flame-retardant liquid silica gel slurry; use shear thickening liquid to perform a first sizing treatment on pre-oxidized short fiber yarn, dry and adjust humidity balance, then use flame-retardant liquid silica gel slurry for a second sizing treatment, dry and adjust humidity balance again to obtain STF / liquid silica gel modified pre-oxidized short fiber yarn;
[0008] (3) Using para-aramid filament as the core yarn and STF / liquid silica-modified pre-oxidized short fiber yarn as the outer yarn, multiple strands of STF / liquid silica-modified pre-oxidized short fiber yarn are continuously wrapped on the surface of the core yarn in a spiral manner through a hexagonal rotary braiding machine to obtain a core-shell structure composite yarn of STF / liquid silica-modified pre-oxidized short fiber yarn and para-aramid filament.
[0009] The present invention is further configured such that, in step (1), the SiO2 content in the shear thickening liquid is 2.5-12.5 wt%.
[0010] The present invention is further configured such that, in step (1), the average particle size of SiO2 is 7-12 nm and the average molecular weight of polyethylene glycol is 200-400.
[0011] The present invention is further configured such that, in step (2), the concentration of liquid silicone in the flame-retardant liquid silicone slurry is 1-9 wt%, and the amount of phosphorus-based halogen-free flame retardant added is 1% of the total mass of liquid silicone A component and B component.
[0012] The present invention is further configured such that, in step (2), the sizing speed for the first sizing and the second sizing is 10-50 m / min.
[0013] The present invention is further configured such that, in step (2), the sizing rate of the first sizing is 6.8-90.5%, and the sizing rate of the second sizing is 1.9-25.4%.
[0014] The present invention is further configured such that, in step (2), the drying temperature after the first sizing and the second sizing treatment is 60°C.
[0015] The present invention is further configured such that, in step (3), 6-12 strands of STF / liquid silicone modified pre-oxidized short fiber yarn are wrapped on the surface of the core yarn.
[0016] In summary, the present invention has the following beneficial effects:
[0017] This invention achieves the effective preparation of a core-sheath composite yarn consisting of an "STF / liquid silicone pre-oxidized short fiber yarn covering layer - para-aramid central skeleton layer" through synergistic modification of STF and phosphorus-based halogen-free flame retardant liquid silicone and hexagonal continuous rotary weaving technology. By introducing phosphorus-based halogen-free flame retardant into the outer layer of the pre-oxidized short fiber yarn, it solves the problems of sticky hand feel, easy shedding and migration of yarn after conventional STF treatment. At the same time, it significantly improves the mechanical properties and aging resistance of the composite yarn, and helps to achieve multi-functional synergy of flame retardancy, cut resistance and wear resistance of the fabric, providing an ideal material solution for high-end protective textiles. Attached Figure Description
[0018] Figure 1 SEM images of different staple fiber yarns ( Figure 1 (a) to Figure 1 (d) SEM images of pre-oxidized short fiber yarn (unmodified), STF / liquid silica-modified pre-oxidized short fiber yarn prepared in Example 1, STF-modified pre-oxidized short fiber yarn prepared in Comparative Example 1, and liquid silica-modified pre-oxidized short fiber yarn prepared in Comparative Example 2, in order.
[0019] Figure 2 The graph shows the significant abrasion resistance analysis results of the pre-oxidized short fiber yarn (unmodified), the STF / liquid silica gel modified pre-oxidized short fiber yarn prepared in Example 1, and the STF modified pre-oxidized short fiber yarn prepared in Comparative Example 1 (in the graph, the control group corresponds to the pre-oxidized short fiber yarn, the shear thickening liquid group corresponds to the STF modified pre-oxidized short fiber yarn, and the shear thickening liquid + liquid silica gel group corresponds to the STF / liquid silica gel modified pre-oxidized short fiber yarn containing phosphorus-based halogen-free flame retardant).
[0020] Figure 3 The graph shows the strength (breaking strength) retention rate decay of para-aramid filament and composite yarn prepared in Example 1 under ultraviolet aging.
[0021] Figure 4 The graph shows the rate of decrease in the breaking strength retention of para-aramid filament and the composite yarn prepared in Example 1 under heat aging. Detailed Implementation
[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0023] The composite yarn of STF / liquid silica-modified pre-oxidized short fiber yarn and para-aramid filament of the present invention is prepared according to the following steps:
[0024] (1) Preparation of shear thickening fluid: SiO2 is dispersed in polyethylene glycol, stirred evenly, and then ultrasonicated and degassed to obtain a shear thickening fluid with SiO2 content of 2.5-12.5wt% (average particle size of SiO2 is 7-12nm, average molecular weight of polyethylene glycol is 200-400); or SiO2 is added to polyethylene glycol, and then decaglycerol-perillic acid mPEG grafted oligomer is added, stirred evenly, and then ultrasonicated and degassed to obtain a shear thickening fluid with SiO2 content of 2.5-12.5wt% and decaglycerol-perillic acid mPEG grafted oligomer content of 0.6-1.3wt%.
[0025] (2) Mix component A and component B of liquid silica gel, add phosphorus-based halogen-free flame retardant at 1% of the total mass of components A and B of liquid silica gel, then add anhydrous ethanol to dilute and mix evenly to prepare a flame-retardant liquid silica gel slurry with a liquid silica gel mass concentration of 1-9wt%; use shear thickening liquid to perform a first sizing treatment on pre-oxidized short fiber yarn (sizing speed is 10-50m / min, sizing rate is 6.8-90.5%), dry (60℃), and adjust humidity balance, then use flame-retardant liquid silica gel slurry for a second sizing treatment (sizing speed is 10-50m / min, sizing rate is 1.9-25.4%), dry (60℃) and adjust humidity balance again to obtain STF / liquid silica gel modified pre-oxidized short fiber yarn;
[0026] (3) Using para-aramid filament as the core yarn and STF / liquid silica-modified pre-oxidized short fiber yarn as the outer yarn, multiple strands (preferably 6-12 strands) of STF / liquid silica-modified pre-oxidized short fiber yarn are continuously wrapped on the surface of the core yarn in a spiral manner using a hexagonal rotary braiding machine (spindle speed is 500-800 r / min, pitch is 8-12 mm, braiding angle is 14-38°) to obtain a core-sheath structure composite yarn of STF / liquid silica-modified pre-oxidized short fiber yarn and para-aramid filament.
[0027] Example 1: Preparation of STF / liquid silica-modified pre-oxidized staple fiber yarn
[0028] (1) Preparation of shear thickening fluid (STF): SiO2 (silica A200 purchased from Zhejiang Lijie Chemical Co., Ltd., with an average particle size of 7nm) was added to PEG400 in batches under stirring. After stirring evenly, the mixture was ultrasonically treated at 25°C for 30 min (power 300W). The dispersion was then placed in a vacuum oven at 70°C for 1 h to degas, resulting in a shear thickening fluid with a SiO2 content of 12.5wt%.
[0029] (2) Mix component A and component B of liquid silicone at a mass ratio of 1:1. Component A is mainly vinyl polysiloxane and component B is mainly hydrogen polysiloxane. The liquid silicone is actually liquid adhesive GA2640 produced by Shenzhen Zhengan Organosilicon Materials Co., Ltd. Subsequently, a phosphorus-based halogen-free flame retardant (dimethyl methylphosphonate) was added at 1% of the total mass of liquid silica gel components A and B, and stirred thoroughly. Anhydrous ethanol was then added for dilution and mixed evenly to prepare a flame-retardant liquid silica gel slurry with a liquid silica gel mass concentration of 5%. The pre-oxidized short fiber yarn (also known as polyacrylonitrile pre-oxidized fiber, purchased from Zhejiang Jili New Material Co., Ltd., specification 29tex×2) was subjected to a first sizing treatment using a shear thickening liquid (sizing speed 20m / min, sizing rate 90.5%), dried at 60℃, and then placed in a standard atmospheric environment at 20±2℃ and relative humidity (65±2)% for 24h to adjust to humidity equilibrium. Subsequently, a second sizing treatment was performed using the flame-retardant liquid silica gel slurry (sizing speed 20m / min, sizing rate 10.2%), dried at 60℃, and then placed in a standard atmospheric environment at 20±2℃ and relative humidity (65±2)% for 24h to adjust to humidity equilibrium again, resulting in STF / liquid silica gel modified pre-oxidized short fiber yarn.
[0030] (3) Using para-aramid filament (purchased from Sinochem High Performance Fiber Materials Co., Ltd., 1684.8 dtex / 1000F) as the core yarn and STF / liquid silica modified pre-oxidized short fiber yarn as the outer yarn, six strands of STF / liquid silica modified pre-oxidized short fiber yarn are continuously wrapped in a spiral manner on the surface of the core yarn drawn out from the hollow spindle by a hexagonal rotary braiding machine (spindle speed is 800 r / min, pitch is 8 mm, braiding angle is 33.41°) to obtain a core-sheath structure STF / liquid silica modified pre-oxidized short fiber yarn and para-aramid filament composite yarn with a linear density of 619 tex and a diameter of 1.68 mm.
[0031] Comparative Example 1
[0032] STF-modified pre-oxidized short fiber yarn was prepared according to Example 1, except that step (2) was: the pre-oxidized short fiber yarn (also known as polyacrylonitrile-based pre-oxidized fiber) was sized with a shear thickening liquid (sizing speed was 20 m / min, sizing rate was 90.5%), dried at 60°C and then placed in a standard atmospheric environment at 20±2°C and relative humidity (65±2)% for 24 hours to adjust the humidity.
[0033] Comparative Example 2
[0034] Liquid silica-modified pre-oxidized short fiber yarn was prepared according to Example 1, except that step (2) was as follows: component A and component B of liquid silica were mixed at a mass ratio of 1:1, anhydrous ethanol was added and mixed evenly to prepare a liquid silica slurry with a concentration of 5%; the liquid silica slurry was used for sizing treatment (sizing speed of 20m / min, sizing rate of 10.2%), dried at 60℃ and then placed in a standard atmospheric environment of 20±2℃ and relative humidity of (65±2)% for 24h to adjust the humidity.
[0035] Performance testing and results analysis:
[0036] (1) SEM images of pre-oxidized staple fiber yarn (unmodified), STF / liquid silica-modified pre-oxidized staple fiber yarn prepared in Example 1, STF-modified pre-oxidized staple fiber yarn prepared in Comparative Example 1, and liquid silica-modified pre-oxidized staple fiber yarn prepared in Comparative Example 2 are shown below. Figure 1 As shown in the figure. From the figure, we can see that:
[0037] 1.1 The surface of the pre-oxidized short fiber yarn exhibits a significant longitudinal groove structure. The fiber surface is generally smooth with no obvious impurities attached. This unique groove structure provides a natural "anchor point" for the physical adsorption of subsequent functional fluids, which is beneficial to increasing the contact area between STF particles and fibers and the mechanical interlocking ability.
[0038] 1.2 Compared with pre-oxidized staple fiber yarn, the surface of STF-modified pre-oxidized staple fiber yarn is no longer smooth, but uniformly covered with a dense layer of nanoparticles. More importantly, the nano-SiO2 particles not only cover the fiber protrusions, but also fill a large amount of the longitudinal grooves on the fiber surface. This "filling-covering" mode significantly improves the micro-roughness of the fiber surface. During dynamic impact, these hard nanoparticles will act as "friction enhancers", greatly increasing the sliding resistance between yarns. This is the structural basis for the shear thickening effect of composite yarn.
[0039] 1.3 A continuous and smooth polymer film is formed on the fiber surface of the pre-oxidized staple fiber yarn modified with liquid silica gel. Liquid silica gel exhibits good wettability on the pre-oxidized staple fiber yarn, and some liquid silica gel penetrates into the fiber bundle, bonding the individual fibers together. This elastomer film can bind the loose fibers, limit their excessive slippage, and thus help improve the fiber breaking elongation.
[0040] 1.4 The surface of STF / liquid silicone modified pre-oxidized short fiber yarn exhibits a unique particle-reinforced elastomer encapsulation structure. Specifically, the nanoparticles in the STF are tightly encapsulated by an outer translucent liquid silicone film, forming a microscopic state similar to "embedding," which is consistent with... Figure 1Compared to the exposed STF particles in (b), this structure effectively solves the defects of liquid STF being prone to loss and moisture absorption during long-term use. At the same time, the liquid silica gel layer serves as the continuous phase, and the STF particles serve as the dispersed phase. Together with the fiber matrix, they form a stable ternary interface. This structure not only retains the frictional synergistic effect of the STF particles, but also utilizes the elastic recovery force of the liquid silica gel layer to maintain the integrity of the structure, providing an ideal microstructure for achieving excellent impact resistance.
[0041] (2) The mechanical properties of the pre-oxidized staple yarn and the STF / liquid silica gel modified pre-oxidized staple yarn prepared in Example 1 were tested using the electronic single yarn strength tester YM065SS of Suzhou Electronic Instruments Co., Ltd., according to GB / T 3916-2013 "Determination of breaking strength and elongation at break of single yarn in packaged textiles (CRE method)". (The spacing was set to 500 mm, the stretching speed was 500 mm / min, and the pre-tension was set to 0.5 ± 0.1 cN / tex; before the test, the samples were placed under standard atmospheric conditions for 24 h to equilibrate. Each group of samples was tested 60 times, and the average value was taken). The test results are shown in Table 1.
[0042] Table 1
[0043]
[0044] (3) The abrasion resistance of pre-oxidized staple yarn, STF / liquid silica gel modified pre-oxidized staple yarn prepared in Example 1, and STF modified pre-oxidized staple yarn prepared in Comparative Example 1 were tested using an FFZ622 yarn abrasion tester manufactured by Wenzhou Fangyuan Instrument Co., Ltd., according to the standard FZ / T 01058-2004 "Test Method for Abrasion Resistance of Yarn - Grinding Roller Method". Before the test, the samples were placed under standard atmospheric conditions for 24 hours to equilibrate. During the test, the yarn was installed on the instrument clamping device according to the standard, and the sample was continuously rubbed against the grinding roller until the sample broke. The number of abrasion resistance tests was recorded. Each group of samples was tested 5 times, and the average value was taken. The results of the abrasion resistance significance analysis are shown in the figure. Figure 2 .
[0045] Depend on Figure 2 It can be seen that the abrasion resistance of the control group (unmodified pre-oxidized staple yarn) was mainly concentrated between 60 and 90 cycles, with a median of approximately 75 cycles. This indicates that the pre-oxidized staple yarn is more prone to fiber wear and structural damage under repeated friction, and its abrasion resistance is relatively low. In contrast, after treatment with the shear thickening solution, the overall abrasion resistance of the fibers increased, with values generally ranging from 70 to 120 cycles, and a median of approximately 90 cycles. Significance analysis results showed a highly significant difference between the control group and the shear thickening solution group (STF-modified pre-oxidized staple yarn). (p < 0.001). This result indicates that the introduction of shear thickening liquid can improve the fiber's resistance to frictional damage to a certain extent. The reason for this phenomenon is related to the rheological properties of the shear thickening liquid under shearing action. When the fiber surface is subjected to friction or shearing, the viscosity of the system increases rapidly, and an instantaneous structural network is formed between the internal particles, thereby generating a certain "support" or "locking" effect between the fibers. This structure can increase the frictional resistance between fibers and reduce the slippage of yarns during friction, thus improving the overall abrasion resistance of the fabric. After further liquid silica gel treatment on the basis of shear thickening liquid, the abrasion resistance of the STF / liquid silica gel modified pre-oxidized short fiber yarn samples still showed an upward trend, with the abrasion resistance mainly distributed between 75 and 115 times, and the median value was about 95 times. It also showed a significant difference compared with the control group. (p < 0.001). This result indicates that liquid silicone finishing further enhances the wear resistance of fibers to a certain extent. This is because liquid silicone forms a relatively continuous flexible film layer on the fiber surface. On the one hand, it can improve the bonding stability between fibers and reduce fiber shedding during friction. On the other hand, liquid silicone has certain elastic characteristics, which can play a role in buffering and dispersing stress during friction, thereby slowing down the wear of fibers.
[0046] (4) Mechanical properties and UV aging resistance of para-aramid filament and composite yarn prepared in Example 1 were tested. The test results are shown in Table 2 and Figure 3 The mechanical properties were tested according to GB / T 19975-2005 "Test Method for Tensile Properties of High-Strength Fiber Filaments", using a Shimadzu AG-X PLUS 100KN universal testing machine. Before testing, the samples were conditioned for 24 hours under standard atmospheric conditions of (20±2)℃ and (65±2)% relative humidity. During testing, the yarn samples were installed straight between the upper and lower clamps of the testing machine to avoid twisting or initial additional tension. The clamping distance was set to 500 mm, and the tensile speed was set to 500 mm / min. After the test started, the samples were uniformly stretched along the axial direction until they broke, and parameters such as breaking strength and elongation at break were recorded. Each group of samples was tested 10 times, and the average value was taken as the final test result. The mechanical properties of each group of yarns were compared and analyzed in combination with the data dispersion. The UV aging resistance was tested according to GB / T 31899-2015 standard using a TH8071 UV aging test chamber from Dongguan Tianhai Instrument Co., Ltd. A UVA-340 fluorescent UV lamp was used, with an irradiance set to 0.89 W / (m²). 2·nm)@340nm, blackboard temperature 60℃, exposed to sunlight for 8 hours, then condensed at blackboard temperature 50℃ for 4 hours. For samples with different aging times, their breaking strength was tested, and the UV aging strength retention rate was calculated.
[0047] Table 2
[0048]
[0049] From Table 2 and Figure 3 It can be seen that the strength retention rate of the composite yarn of STF / liquid silica modified pre-oxidized short fiber yarn and para-aramid filament decreased relatively slowly during the entire aging process, and the overall decay curve was more gentle, showing better stability and repeatability. After 120h aging, its strength retention rate still reached 85.90%, which was 25.51% higher than that of para-aramid filament, indicating that the composite structure can significantly delay the mechanical property decay caused by ultraviolet aging.
[0050] The main reason for the above differences lies in the different ways in which the two groups of yarns are affected by ultraviolet radiation: the molecular chain of para-aramid fiber contains a large number of amide bonds (-CO-NH-), which are highly sensitive to ultraviolet radiation. Under ultraviolet excitation, the amide bonds are prone to photo-oxidative cracking, resulting in cracking of the fiber surface, darkening of color, and a sharp decline in mechanical properties, which severely limits its long-term service capability in outdoor environments. When para-aramid filament is directly exposed to the ultraviolet environment as a single load-bearing material, the fiber surface is irradiated first. As the irradiation time increases, surface damage gradually accumulates and is transmitted to the interior, causing the fiber load-bearing unit to be continuously weakened, thus the strength retention rate decreases significantly. For composite yarns, the pre-oxidized short fiber yarn, acting as the outer sheath, provides significant shielding protection for the core aramid fiber. On one hand, the pre-oxidized outer layer increases the propagation path of ultraviolet light before it reaches the core yarn and weakens the direct intensity of ultraviolet radiation through interlayer fiber blocking. On the other hand, the pre-oxidized yarn itself has a darker color and a more stable pre-oxidized structure, possessing light absorption and energy dissipation capabilities to a certain extent, thus reducing the ultraviolet radiation load directly borne by the core aramid fiber. Since the core load-bearing yarn is not directly exposed to a high-intensity ultraviolet environment for extended periods, the decay of its molecular structure and load-bearing capacity is significantly delayed, allowing the composite yarn to maintain a high strength retention rate during aging. Furthermore, the presence of the outer sheath makes the light exposure conditions of the core yarn more uniform, reducing local aging differences. Therefore, the test fluctuations between composite yarn samples are smaller, exhibiting higher stability.
[0051] (5) The heat aging resistance of para-aramid filament and the composite yarn prepared in Example 1 was characterized by a combination of heat exposure and mechanical property retention rate using a muffle furnace (model BTF-1400C-Ⅱ) manufactured by Anhui Beiyike Equipment Technology Co., Ltd. During the test, the samples were exposed to hot air in a muffle furnace at a set temperature for 10 minutes. After treatment, they were removed and cooled to room temperature, then conditioned according to the standard atmospheric conditions specified in GB / T 6529-2008. After conditioning, the tensile strength of the samples was tested, and the tensile strength of the aged samples was compared with that of the unaged samples to calculate the strength retention rate (the higher the strength retention rate, the smaller the mechanical property decay of the yarn after heat exposure, and the better its heat aging resistance). The test results are shown in Table 3 and... Figure 4 .
[0052] Table 3
[0053]
[0054] From Table 3 and Figure 4 It is evident that the breaking strength of both yarns gradually decreases with increasing heat treatment temperature, but the rate and pace of decrease differ significantly, indicating that their response mechanisms to high-temperature environments are not identical. In contrast, although the absolute breaking strength of the composite yarn at room temperature is only 53.10 cN / tex, significantly lower than that of para-aramid filament, its strength retention after heat aging is superior, especially exhibiting better thermal stability within the medium-low to medium-high temperature range. Its mechanical properties are significantly less sensitive to temperature increases than those of single aramid filament. The main reason for these differences lies in the different structural compositions and heating methods of the two yarns. Para-aramid filament is a single-fiber system, directly exposed to hot air during heat aging. The fiber surface is more susceptible to the combined effects of heat and oxygen, leading to surface structure deterioration and gradually affecting overall load-bearing performance. In contrast, the composite yarn uses a core-sheath composite structure, with a pre-oxidized short fiber outer layer and an aramid load-bearing component inner layer. Pre-oxidized yarn itself has good heat resistance and stability. During heating, it can form a relatively stable protective layer on the outside, slowing down the direct transfer of heat and oxygen to the aramid core and reducing the degree to which the aramid core yarn is directly exposed to the high-temperature oxidizing environment. Therefore, it can delay the thermal aging process of the aramid core to a certain extent. In addition, the presence of the outer layer can also provide structural constraint and support to the core layer, reducing the damage to the load-bearing unit caused by local stress concentration under high temperature conditions, so that the composite yarn maintains a high degree of mechanical integrity after heat treatment.
[0055] (6) The composite yarn of Example 1 was woven into a fabric (warp density 16 threads / 10cm, weft density 44 threads / 10cm), and its abrasion resistance, cut resistance, tensile strength and flame retardancy were tested. The results are shown in Table 4.
[0056] Abrasion resistance test: A Martindale abrasion and pilling resistance tester (model MARTINDALE) from Rochester International Ltd., UK, was used. The pressure was set to (9±0.2) kPa, and the unit mass was selected as (300±30) g / m³. 2 The abrasive was tested on circular specimens with a diameter of 38 mm or more.
[0057] Cutting resistance test: The sample with a length of (120±10) mm and a width of (120±10) mm was cut in the radial direction at a cutting speed of 10 m / min, and the number of cycles T when the hole just appeared was recorded.
[0058] Tensile property testing: The tensile properties of the samples were tested using a Shimadzu AG-X plus 100KN universal testing machine. Before testing, the samples were conditioned for 24 hours under standard atmospheric conditions of (20±2)℃ and (65±2)% relative humidity. During testing, rectangular samples with dimensions of 120 mm × 40 mm were cut along the warp direction of the fabric and clamped flat between the upper and lower clamps of the testing machine. The test parameters were set as follows: clamping distance 100 mm, tensile speed 100 mm / min. During the test, the samples were continuously stretched along the warp direction until fracture, and the breaking strength and maximum elongation at break were recorded. Each group of samples was tested 5 times, and the average value was taken as the final test result for that group of samples.
[0059] Flame retardant performance: Tests were conducted according to GB / T 5455-2014 "Determination of Vertical Destruction Length, Afterflame and Residual Flame Time of Textiles," using a YG851A vertical combustion performance tester from Zhejiang Sangongjiang Instrument Co., Ltd. Before testing, the samples were conditioned for 24 hours under standard atmospheric conditions of (20±2)℃ and (65±2)% relative humidity. Samples of the specified dimensions were cut according to the standard requirements and vertically clamped onto the combustion test apparatus. During ignition, a specified flame was applied to the lower end of the sample for a certain period. After the flame was removed, the afterflame time, smoldering time, and destruction length of the sample were recorded. Each group of samples was tested at least five times, and the average value of all test results was taken as the final result for evaluating the flame retardant performance of the fabric.
[0060] Table 4
[0061]
[0062] Example 2
[0063] The STF / liquid silica-modified pre-oxidized short fiber yarn and para-aramid filament composite yarn were prepared according to the method of Example 1. The difference is that a novel functional additive, decaglycerol-perillic acid mPEG grafted oligomer, was added to the shear thickening liquid in step (1). Specifically, SiO2 was added to PEG400 in batches under stirring, followed by the addition of decaglycerol-perillic acid mPEG grafted oligomer. After stirring evenly, the mixture was ultrasonically treated at 25°C for 30 min, and then the dispersion was placed in a vacuum oven at 70°C for 1 h to degas, resulting in a shear thickening liquid with a SiO2 content of 12.5 wt% and a decaglycerol-perillic acid mPEG grafted oligomer content of 1.1 wt%.
[0064] The preparation method of decaglycerol-perillic acid mPEG grafted oligomer is as follows:
[0065] (a) Add decaglycerol (purchased from Shanghai Jizhi Biochemical Technology Co., Ltd.) and perillic acid (added at a molar ratio of hydroxyl groups in decaglycerol to carboxyl groups in perillic acid of 1:0.25) to the reactor. Add the catalyst p-toluenesulfonic acid (0.1% of the total mass of decaglycerol and perillic acid) and xylene (20% of the total mass of decaglycerol and perillic acid). Reflux the reaction at 130°C for 4 hours under nitrogen protection. After the reaction is completed, cool the temperature to 65°C and add an equal volume of 65°C deionized water to the system for washing. Allow the mixture to stand and separate the organic phase. Remove the xylene at 75°C and a vacuum degree <5kPa to obtain decaglycerol-perillic acid oligomer.
[0066] (b) Add decaglycerol-perillic acid oligomer and methoxyPEG carboxylic acid (mPEG-COOH, purchased from Aladdin Reagent Company, catalog number C163407) to a reaction vessel (the molar ratio of hydroxyl groups in decaglycerol-perillic acid oligomer to carboxyl groups in mPEG-COOH is 1:0.15). Add anhydrous dichloromethane (3 times the total mass of the reactants), 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride (1.1 times the molar equivalent of mPEG-COOH) and DMAP (4-dimethylaminopyridine, 0.2 times the molar equivalent of mPEG-COOH). Under nitrogen protection, react at 0°C for 1 h, then raise to room temperature (25±2°C) and continue stirring for 8 h. After the reaction was completed, the product was washed twice with 0.1 mol / L citric acid aqueous solution (to remove the EDC byproduct urea derivative), then washed with saturated sodium bicarbonate until neutral, washed once with saturated brine, dried overnight with anhydrous sodium sulfate, filtered, and the filtrate was evaporated under reduced pressure below 40°C to remove dichloromethane, yielding decaglycerol-perillic acid mPEG grafted oligomer.
[0067] The test results of UV aging resistance, heat aging resistance, abrasion resistance, cut resistance, elongation and flame retardancy of the composite yarn prepared in Example 2 are shown in Tables 5 and 6.
[0068] Table 5
[0069]
[0070] Table 6
[0071]
[0072] The above description is merely a preferred embodiment of the present invention. The scope of protection of the present invention is not limited to the above embodiments. All technical solutions falling within the scope of the present invention's concept are within the scope of protection of the present invention. It should be noted that for those skilled in the art, any improvements and modifications made without departing from the principles of the present invention should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a composite yarn of STF / liquid silica-modified pre-oxidized staple fiber yarn and para-aramid filament, characterized in that, Includes the following steps: (1) SiO2 is dispersed in polyethylene glycol to prepare a shear thickening solution; (2) Mix component A and component B of liquid silica gel, add phosphorus-based halogen-free flame retardant and anhydrous ethanol, mix evenly to obtain flame-retardant liquid silica gel slurry; use shear thickening liquid to perform a first sizing treatment on pre-oxidized short fiber yarn, dry and adjust humidity balance, then use flame-retardant liquid silica gel slurry for a second sizing treatment, dry and adjust humidity balance again to obtain STF / liquid silica gel modified pre-oxidized short fiber yarn; (3) Using para-aramid filament as the core yarn and STF / liquid silica-modified pre-oxidized short fiber yarn as the outer yarn, multiple strands of STF / liquid silica-modified pre-oxidized short fiber yarn are continuously wrapped on the surface of the core yarn in a spiral manner through a hexagonal rotary braiding machine to obtain a core-shell structure composite yarn of STF / liquid silica-modified pre-oxidized short fiber yarn and para-aramid filament.
2. The method for preparing a composite yarn of STF / liquid silica-modified pre-oxidized staple fiber yarn and para-aramid filament according to claim 1, characterized in that, In step (1), the SiO2 content in the shear thickening liquid is 2.5-12.5 wt%.
3. The method for preparing a composite yarn of STF / liquid silica-modified pre-oxidized staple fiber yarn and para-aramid filament according to claim 1, characterized in that, In step (1), the average particle size of SiO2 is 7-12 nm and the average molecular weight of polyethylene glycol is 200-400.
4. The method for preparing a composite yarn of STF / liquid silica-modified pre-oxidized staple fiber yarn and para-aramid filament according to claim 1, characterized in that, In step (2), the concentration of liquid silicone in the flame-retardant liquid silicone slurry is 1-9 wt%, and the amount of phosphorus-based halogen-free flame retardant added is 1% of the total mass of liquid silicone components A and B.
5. The method for preparing a composite yarn of STF / liquid silica-modified pre-oxidized staple fiber yarn and para-aramid filament according to claim 1, characterized in that, In step (2), the sizing speed for both the first and second sizing processes is 10-50 m / min.
6. The method for preparing a composite yarn of STF / liquid silica-modified pre-oxidized staple fiber yarn and para-aramid filament according to claim 1, characterized in that, In step (2), the sizing rate of the first sizing is 6.8-90.5%, and the sizing rate of the second sizing is 1.9-25.4%.
7. The method for preparing a composite yarn of STF / liquid silica-modified pre-oxidized staple fiber yarn and para-aramid filament according to claim 1, characterized in that, In step (2), the drying temperature after the first and second sizing processes is 60℃.
8. The method for preparing a composite yarn of STF / liquid silica-modified pre-oxidized staple fiber yarn and para-aramid filament according to claim 1, characterized in that, In step (3), 6-12 strands of STF / liquid silicone modified pre-oxidized short fiber yarn are wrapped around the core yarn surface.