A method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence with wearing comfort

By combining low-temperature dyeing and low-damage combing processes with optimized weaving parameters, the performance differences and weaving problems in the blending of luminescent fibers and wool fibers were solved, resulting in the production of highly efficient luminescent, comfortable, and well-feeling luminescent wool worsted fabrics, which enhances the product's market competitiveness and sustainability.

CN123108809APending Publication Date: 2026-11-17SHANDONG LUJIANA TEXTILE & GARMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611187632.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing blending processes for luminescent fibers and wool fibers suffer from problems such as large differences in fiber properties, weaving jams, yarn slippage, uneven fabric density, and reduced breathability and moisture permeability. Coating and composite processes result in poor luminescence durability and stuffy, stiff fabrics. Traditional dyeing processes damage the soft texture of wool and reduce luminescence efficiency.

Method used

By using low-temperature dyeing, low-damage combing, low-tension weaving, and wrinkle-resistant and comfortable finishing of wool and luminous nylon fibers, a high-efficiency luminescent and comfortable luminous wool worsted fabric is prepared. Low-temperature dyeing treatment reduces fiber damage, and combined with low-damage combing and optimized weaving parameters, yarn quality and fabric performance are ensured.

Benefits of technology

This has resulted in a glow-in-the-dark wool worsted fabric with excellent luminescence performance, a comfortable feel, and a high-end appearance. It has solved the weaving problems caused by differences in fiber properties, maintained the soft texture and luminescence efficiency of wool, met the requirements of green manufacturing, and enhanced the product's market competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108809A_ABST
    Figure CN123108809A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing a glow-in-the-dark wool worsted fabric that combines high-efficiency luminescence with wearing comfort, relating to the field of worsted wool fabric preparation technology. Addressing the application limitations of functional glow-in-the-dark wool fabrics, the proposed method includes: using wool fibers and glow-in-the-dark nylon fibers as raw materials, and performing independent low-temperature dyeing treatments separately; performing separate / mixed carding on the dyed wool fibers and glow-in-the-dark nylon fibers using a low-damage carding process, followed by sequential roving, spinning, winding, and steaming / twisting processes to produce three types of yarns: blended, pure wool, and pure glow-in-the-dark nylon; using the blended yarns for weaving or interlacing wool yarn as warp and glow-in-the-dark nylon yarn or blended yarn as weft, with the loom using preset weaving parameters to produce a grey fabric; after the grey fabric undergoes a wrinkle-resistant and comfort finishing process, a finished fabric with nighttime luminescence function and elastic wrinkle-resistant properties is finally obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of worsted wool fabric preparation technology, specifically a method for preparing luminescent worsted wool fabric that combines high-efficiency luminescence with comfortable wear. Background Technology

[0002] With the upgrading of people's lifestyles, the market demand for functional textiles continues to rise. Developing fabrics that combine aesthetics, comfort, and safety features (such as nighttime visual warnings) has become an important development trend in the textile industry. Currently, luminescent fiber technology has formed a relatively mature technical system. Its core preparation process includes key steps such as rare-earth phosphorescent powder modification, luminescent functional masterbatch preparation, and core-sheath composite melt spinning. The market offers a wide variety of luminescent fiber products, covering luminescent staple fibers, filaments, embroidery threads, and finished luminescent fabrics, widely used in home decoration, outdoor clothing, safety protection, and other fields. Meanwhile, a new generation of intelligent luminescent fabrics is gradually being implemented. These fabrics use a composite structure of an optical luminescent layer and a fabric substrate, possessing excellent properties such as waterproofing, mildew resistance, and UV resistance. They can achieve intelligent adjustment of brightness and lighting modes via a wireless controller, significantly improving functionality and practicality.

[0003] Currently, the mainstream processes for applying luminescent fibers to textiles in the industry are mainly divided into two categories: (a) directly using commercially available mature luminescent yarns (such as Lumira luminescent yarn) for weaving, sewing, or embroidery; and (b) attaching luminescent functional materials to the surface of ordinary fabrics through finishing methods such as surface coating and lamination. In addition, in the wool textile field, to meet the functional requirements of outdoor scenarios, the industry has conducted relevant research, attempting to blend and interweave functional yarns with wool yarns to improve the outdoor adaptability of wool fabrics. However, current application solutions still have significant technical shortcomings: In the direct fiber blending process, the mechanical, frictional, and shrinkage properties of luminescent fibers differ greatly from those of conventional textile fibers, which can easily lead to problems such as weaving jamming, yarn slippage, uneven fabric density, and poor finished product smoothness; the coating composite process forms a dense film on the fabric surface, which significantly sacrifices the breathability and moisture permeability of the fabric, resulting in stuffy and stiff wear. At the same time, the coating has limited adhesion and is easy to fall off after washing and rubbing, resulting in poor luminescence durability and color fastness; and the traditional dyeing and high-temperature setting finishing processes for wool fabrics not only easily damage the soft texture and elasticity of the natural protein fibers of wool, but the high-temperature environment can also cause the fluorescence of the luminescent materials to quench, significantly reducing the luminescence efficiency. In severe cases, it can lead to permanent loss of luminescence in the fabric, which greatly restricts the industrial application of luminescent wool functional fabrics. Summary of the Invention

[0004] This invention addresses the needs and shortcomings of current technological development by providing a method for preparing luminescent wool worsted fabric that combines high-efficiency luminescence with comfortable wear.

[0005] The present invention provides a method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence with wearing comfort. The technical solution adopted to solve the above-mentioned technical problems is as follows: A method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence with wearing comfort, the method comprising the following steps: Step 1, Raw material selection and dyeing: Wool fiber and luminous nylon fiber are used as raw materials, and each is subjected to independent low-temperature dyeing treatment; Step 2, Spinning: The dyed wool fibers and luminous nylon fibers are mixed and combed using a low-damage combing process to obtain a mixed sliver. Then, the sliver is spun into a blended yarn by sequentially passing through roving, spinning, winding, steaming and twisting processes. The dyed wool fibers and luminous nylon fibers were separately combed using a low-damage combing process to produce wool tops and luminous nylon tops. The two types of tops were then separately processed through roving, spinning, winding, steaming and twisting processes to produce pure wool yarn and pure luminous nylon yarn, respectively. Step 3, Weaving: The fabric is woven using blended yarns with pre-set weaving parameters of "low tension, low speed, and small opening" on the loom to produce the greige fabric; or, the fabric is woven by interlacing wool yarn as warp yarns and luminous nylon yarn or blended yarns as weft yarns with pre-set weaving parameters of "low tension, low speed, and small opening" on the loom to produce the greige fabric. Among them, the blended yarn or pure luminous nylon yarn used in the weaving process adopts a separate heddle threading and reed threading method, while optimizing the amplitude of the back beam swing mechanism and the side support device to reduce frictional damage to the blended yarn or pure luminous nylon yarn. Step 4: After the greige fabric undergoes a wrinkle-resistant and comfort finishing process, a finished fabric with nighttime luminescence and elastic wrinkle-resistant properties is finally obtained.

[0006] Optionally, the diameter of the wool fibers involved is in the range of 15μm-23μm.

[0007] Optionally, the luminous nylon fiber involved is a functional fiber made by blending polyamide as a matrix, incorporating rare earth long afterglow luminescent materials, and using a masterbatch blending melt spinning process; its core characteristics are that after absorbing light for 10–30 minutes, it can continue to glow in the dark for more than 4–10 hours, and has the properties of being non-radioactive, washable, recyclable, and having multi-color light effects.

[0008] Optionally, perform step 1, using wool reactive dyes or neutral dyes to perform low-temperature dyeing treatment on wool fibers. The specific process is as follows: In the dyeing machine, add water at 40℃-45℃, add formic acid to adjust the pH of the dye bath to 5.5-6, add dyeing defoamer and run continuously for 4min-8min; use wool reactive dyes or neutral dyes, and dye at 80℃-85℃ under the action of leveling agent; after dyeing, there is no need to drain the dye bath, directly add alkali and detergent to the original dye bath for two alkali washes, followed by sequential washing with hot water at 55℃-60℃ for 8min-12min, washing with cold water at 45℃-50℃ for 4min-8min, and acid neutralization treatment; control the dyeing bath ratio at 1:5, and the dyeing time is 3-4 hours.

[0009] Alternatively, step 1 can be performed, using a specified acidic dye to perform low-temperature dyeing treatment on the luminous nylon fiber. The specific process is as follows: First, pre-treat the fiber at 38℃-42℃ with 0.5% FFA auxiliary agent and drain the liquid and change the water. Then, start dyeing at 30℃ under neutral pH conditions of 7-7.5. Add leveling agent sequentially and run for 4-7 minutes, followed by dyeing for 8-12 minutes. The dyeing temperature should not exceed 80℃ throughout the process, and the amount of dye should be controlled within 0.5% owf. The heating process is as follows: heat the fiber from 30℃ to 70℃ at a uniform rate of 1℃ / min, hold for 8-12 minutes, then heat it to 80℃ at a rate of 0.8℃ / min and hold for 8-12 minutes. In the later stage of dyeing, add acetic acid to adjust the pH to an acidic environment of 5-6, hold for 20-30 minutes to complete the color fixation, and finally cool and wash with water.

[0010] Optionally, in step 2, the dyed wool fibers and luminous nylon fibers are mixed and combed in a dry weight ratio of 50:50 to obtain a mixed sliver, which is then spun into a blended yarn through roving, spinning, winding, steaming and twisting processes.

[0011] Optionally, in step 2, a low-damage combing process with preset "closed-number needles, small spacing, low speed, small feed, and small draft" is adopted. The spinning process ensures yarn strength and evenness by optimizing the size of the collector, machine speed, and twist parameters; The winding process reduces strength loss at the twist joint by optimizing winding untwisting and splicing parameters, thereby reducing yarn hairiness and yarn defects.

[0012] Optionally, in step 2, during the production of blended yarn, pure wool yarn, and pure luminous nylon yarn, a segmented double steaming process is used to set the twist of the yarn. This segmented double steaming process involves first steaming the yarn tassels, then steaming the winding yarn. For blended yarns, the first steaming temperature is controlled at 75℃ and held for 20 minutes, and the second steaming temperature is controlled at 85℃ and held for 30 minutes. For pure wool yarn and pure luminous nylon yarn, the first steaming temperature is controlled at 70℃ and held for 10 minutes, and the second steaming temperature is controlled at 80℃ and held for 30 minutes.

[0013] Optionally, the wrinkle-resistant and comfort finishing processes involved include, in sequence: raw repair, dyeing machine elastic treatment, low-damage singeing, flat washing, wool washing, shearing, light ironing, and light steaming; among which: The dyeing machine was subjected to elastic treatment in a water bath at 40℃-45℃ and pH 6-6.5, running at a speed of 25 m / min for 120 min. The low-damage singeing process is as follows: first, the greige fabric is cleaned to remove spinning and weaving auxiliaries, and then singeing is performed. The singeing speed is 110-130 m / min, and the distance between the burner and the fabric surface is 10-14 cm. The temperature for light ironing is controlled at 100℃-120℃, and the tension of the guide belt is set to 50%. The steaming temperature is controlled at 115℃-120℃, the pressure at 0.6 bar, and the processing time at 90-100 seconds.

[0014] The present invention provides a method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence with wearing comfort. Compared with the prior art, the advantages of this method are: 1. This invention uses wool fiber and luminous nylon fiber as raw materials, and through four operations, including short-time low-temperature low-damage dyeing, high-efficiency low-damage spinning, high-count lightweight and high-elastic weaving, and wrinkle-resistant and comfortable finishing, a functional worsted wool fabric for outdoor use is prepared. This fabric can retain the natural oiliness, fluffiness and soft hand feel of wool to the greatest extent. 2. This invention uses wool fiber and luminescent nylon fiber as raw materials. The wool fiber and luminescent nylon fiber undergo low-temperature dyeing treatment, significantly reducing the damage rate of wool fiber from the traditional 6.3% to 1-2.6%, while maximizing the preservation of the luminescent properties of the luminescent nylon fiber (high brightness retention rate). A low-damage carding process is employed, combined with roving, spinning, winding, and steaming / twisting processes, to spin blended yarns, wool yarns, and luminescent nylon yarns respectively. Low tension, low speed, and small opening weaving parameters are used to produce the grey fabric, solving the problem of yarn shrinkage differences and ensuring... To ensure a smooth fabric surface, during weaving, a process with separate reeding, low tension, low speed, and small opening is adopted for blended yarns and luminescent nylon yarns. The swing amplitude of the back beam and the edge support device are also improved to effectively overcome technical problems such as multiple yarn breaks and uneven fabric surface caused by the blending of different fibers, thereby improving weaving efficiency and production stability. Anti-wrinkle and comfort finishing technology is developed to give the fabric excellent elasticity, wrinkle resistance and comfortable hand feel without compromising its luminescent function. The final result is an ultralight wool worsted fabric with excellent luminescence performance, comfortable hand feel, high-end appearance, durability and suitability for outdoor and personalized fashion fields. 3. This invention combines luminous function with the comfort and luxurious feel of high-grade worsted wool fabric, solving the problems of poor hand feel and low fastness of traditional luminous fabrics. The product not only glows in the dark, but also maintains the inherent high-quality characteristics of wool fabric, such as fluffiness, softness, elasticity, and natural luster. It features low damage, short process, and low liquor ratio. Compared with traditional processes, it saves about 69% of water, 14% of electricity, and 20% of steam. The first-pass dyeing qualification rate reaches over 99.2%, which is in line with the modern green manufacturing and sustainable development concept. 4. The finished fabric prepared by this invention breaks through the limitations of traditional application areas of wool fabrics, providing new material options for high-end outdoor sports, fashion leisure, safety protection (such as fire protection, traffic, and night work) clothing and home decoration, significantly enhancing the market competitiveness and added value of the products. Attached Figure Description

[0015] Appendix Figure 1 This is a nighttime luminescence effect image of the finished fabric obtained by this invention; Appendix Figure 2 This is a process curve diagram of the low-temperature dyeing treatment of wool fibers using reactive dyes for wool in this invention; Appendix Figure 3 This is a process curve diagram of the low-temperature dyeing treatment of wool fibers using neutral dyes in this invention; Appendix Figure 4 This is a low-temperature dyeing process curve of luminescent nylon fiber in this invention. Detailed Implementation

[0016] Example 1: This example proposes a method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence with wearing comfort. The method includes the following steps: Step 1, Raw material selection and dyeing: Wool fiber and luminous nylon fiber (the legal name of the national standard for the textile industry, "FZ / T 54102-2022 Luminous Chemical Fiber") are used as raw materials, and are subjected to independent low-temperature dyeing treatments respectively.

[0017] When preparing luminous worsted wool fabric: ① The diameter of the wool fibers is in the range of 15μm-23μm, and Australian superfine Merino wool fibers with a fiber diameter of 16.5μm are specifically selected.

[0018] ②Luminous nylon fiber is a functional fiber made by blending polyamide (nylon) as the matrix, incorporating rare earth long afterglow luminescent materials, and using a masterbatch blending melt spinning process; its core characteristic is that after absorbing light for 10–30 minutes, it can continue to glow in the dark for more than 4–10 hours, and has the characteristics of being non-radioactive, washable, recyclable, and having multi-color light effects.

[0019] Step 1.1: Low-temperature dyeing treatment of wool fibers using wool reactive dyes. The specific process is as follows: In the dyeing machine, water is added at 40℃, and 1.6% formic acid is added to adjust the pH of the dye bath to 5.5-6. Then, the dyeing defoamer FFA (Deli Xiao FFA, a textile dyeing-specific defoamer, a polyether compound silicone-free defoaming system) is added and the machine is run continuously for 5 minutes. Wool reactive dyes (such as Lanasol CE series) are used, and dyeing is performed at 80℃-85℃ under the action of a leveling agent (such as Millerland LTD 2%). After dyeing, there is no need to drain the dye bath; simply add 2% alkali (such as soda ash) and detergent WPS directly to the existing dye bath. Two alkaline washes were performed at 2% (first alkaline treatment at 80℃ for 15-20 minutes; after draining the first alkaline treatment, water was directly added for the second alkaline treatment, with 1% alkali and 2% detergent). Subsequent washing included hot water at 55℃-60℃ for 8-12 minutes, cold water at 45℃-50℃ for 4-8 minutes, and acid neutralization. The dyeing bath ratio was controlled at 1:5, and the dyeing time was 3-4 hours. Specific low-temperature dyeing procedures can be found in the appendix. Figure 2 , Figure 2 In the diagram, A represents defoamer FFA, run for 5 minutes; B represents leveling agent Millerland LTD 2% and dye, run for 5 minutes; and C represents wool reactive dye, run for 5 minutes and then raise the temperature.

[0020] It should be noted that conventional reactive dyeing processes for wool typically use a 98℃ dyeing temperature. After dyeing, post-treatment involves rinsing with drained water and adding fresh water with an alkali agent to adjust the pH. This post-treatment requires repeated rinsing, resulting in high water, electricity, and gas costs. The low-temperature dyeing process in this step utilizes a highly efficient leveling agent to promote low-temperature swelling of wool fibers, lowering the dyeing temperature. Furthermore, it prioritizes soaping auxiliaries in post-treatment, enabling direct alkali addition without draining water, reducing the number of rinsing cycles and improving post-treatment efficiency. Compared to the traditional 98℃ dyeing process, this low-temperature dyeing process reduces wool fiber damage from 6.3% to 1-2.6%, shortens dyeing time to 3-4 hours, reduces the liquor ratio from 1:20 to 1:5, reduces soft water consumption by 30%, electricity consumption by approximately 15%, steam consumption by approximately 27%, increases production efficiency by 25%, and raises the first-pass dyeing yield to over 99.2%.

[0021] It should be added that neutral dyes can also be used to perform low-temperature dyeing treatment on wool fibers, the process of which is as follows: Figure 3As shown: In the dyeing machine, water is introduced at 40℃, and 0.5-1% of defoamer FFA (Deli Xiao FFA textile dyeing special defoamer, polyether compound silicone-free defoaming system) is added. The temperature is raised to 50℃ and run for 5 minutes. Then, water is introduced for rinsing, and the temperature is lowered to 35-40℃. 1% acetic acid is added to adjust the pH of the dye bath to 5.5-6. The leveling agent TOP (Hunsmay Albegal SET, trade name Albegal SET, a hermaphroditic wool leveling agent) and neutral dyes (such as Lanna Sauté series) are added. Dyeing is carried out at 80℃-85℃ under the action of the agent. Subsequently, hot water washing at 55℃-60℃ is performed for 5-8 minutes, followed by cold water washing at 45℃-50℃ for 4-8 minutes. The dyeing bath ratio is controlled at 1:5, and the dyeing time is 2-3 hours. Figure 3 In the diagram, A represents 0.5-1% of defoamer FFA, heated to 50℃ and run for 5 minutes; B represents leveling agent; and C represents neutral dye. After running for 5 minutes, the temperature is increased.

[0022] In the process of low-temperature dyeing of wool fibers using neutral dyes, in order to reduce damage to wool fibers, dyeing at 85°C is achieved by selecting a dyeing leveling agent (such as Huntsman Albegal SET, a hermaphroditic wool leveling agent). This reduces the damage to wool fibers caused by high temperatures, improves the production efficiency of subsequent processes, and reduces energy consumption by about 20% and increases efficiency by 15%.

[0023] It's important to add that when performing low-temperature dyeing on wool fibers, neutral dyes are typically used for light-colored wool fibers, while reactive dyes are used for dark-colored wool fibers. The terms "light-colored wool" and "dark-colored wool" align with common understanding.

[0024] Step 1.2: Low-temperature dyeing treatment of luminescent nylon fibers is performed using a specified acid dye (such as DyStar's "Tianlong A2R" series or Huntsman's "Lanna Satto PA" series). The specific process is as follows: First, pretreatment with 0.5% FFA auxiliary agent at 38℃-42℃ is performed, followed by draining and water replacement. Dyeing begins at 30℃ under neutral pH conditions of 7-7.5. Leveling agent is added sequentially and the dyeing process is repeated for 5 minutes, followed by the addition of the specified acid dye (such as DyStar's "Tianlong A2R" series or Huntsman's "Lanna Satto PA" series) for 10 minutes. The total dyeing temperature does not exceed 80℃, and the dye dosage is controlled at 0.5%. Within owf; the heating process is as follows: heat from 30℃ to 70℃ at a uniform rate of 1℃ / min, hold for 10 minutes, then heat to 80℃ at a rate of 0.8℃ / min and hold for 10 minutes; in the later stage of dyeing, add acetic acid to adjust the pH value to an acidic environment of 5-6, hold for 20-30 minutes to complete the color fixation, and finally cool and wash with water. This low-temperature dyeing process uses neutral starting point, slow temperature increase and subsequent acid adjustment to promote dyeing, ensuring even dyeing and color fastness, while the luminance retention rate can reach more than 60% (compared to untreated).

[0025] To obtain the low-temperature staining process described in step 1.2, the following experiments are required.

[0026] (1) Verify the effect of dye bath temperature on the luminescence properties of luminescent nylon fiber. The luminescent nylon fiber was placed in a dye cup, and soft water was added at a bath ratio of 1:10 and sealed. The dyeing sample machine was set to keep warm at 60℃, 70℃, 80℃, 90℃, 100℃ and 105℃ for 30 min respectively. After washing and drying, it was placed in a standard D65 lamp box for 5 min and the luminescence brightness was observed in a dark room. The luminescence brightness of the untreated luminescent nylon fiber was taken as 100%. The experimental results are shown in Table 1 below.

[0027] Table 1. Effect of dye bath temperature on the luminescence properties of luminescent nylon fibers

[0028] This experiment shows that the luminescence of luminescent nylon fibers changes when the temperature exceeds 90℃. The higher the temperature, the greater the decrease in luminescence. Since the dyeing temperature of conventional nylon fibers is generally 90℃-105℃, optimizing the dyeing process to keep the dyeing temperature below 90℃ is the key to maintaining its luminescence performance. To this end, this embodiment selects suitable nylon dyes for low-temperature dyeing, namely DyStar's Tianlong series and Huntsman's Lanner Satter PA series, and conducts further dyeing experiments.

[0029] (2) Verify the effect of different colored dyes on the luminescence properties of luminescent nylon fibers. Small samples were dyed with 0.1% of different colored dyes, kept at 80℃ for 30 min, washed and dried after dyeing, and irradiated in a standard D65 lamp box for 5 min. The changes in luminescence brightness were observed in a dark room, with the luminescence brightness of untreated luminescent nylon fibers as 100%. The experimental results are shown in Table 2 below.

[0030] Table 2. Effects of different colored dyes on the luminescent properties of luminescent nylon fibers

[0031] The experiment shows that different colored dyes have a significant impact on the luminescence properties of luminescent nylon fibers. Yellow has a smaller impact, while blue has the largest impact. Furthermore, the overall effect of the Tianlong series of bright colors is less than that of the Lanna Sato PA series of dark colors.

[0032] (3) Verification of the effect of dye dosage on the luminescent properties of luminescent nylon fiber. Tianlong Red A2R dye was used at dosages of 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, and 0.5% respectively, with a liquor ratio of 1:10. The dyeing was carried out at 80℃ for 30 min, followed by rinsing and drying. The fibers were then irradiated in a standard D65 lamp box for 5 min and observed in a dark room. The luminescence brightness of untreated luminescent nylon fiber was taken as 100%, and the dyeing K / S value was tested. The experimental results are shown in Table 3 below.

[0033] Table 3 Effect of dye dosage on the luminescent properties of luminescent nylon fiber

[0034] As can be seen from Table 3, the luminescence performance of luminescent nylon fiber gradually decreases with the increase of dye dosage. When the dye dosage is greater than 0.5%, the luminescence performance of luminescent nylon fiber is severely damaged. Therefore, both color and luminescence performance should be considered in fabric design.

[0035] Taking all the above factors into account, a low-temperature dyeing process for luminous nylon was developed, and its specific curve is shown in the figure. Figure 4 As shown. Figure 4 In the instructions, A indicates the addition of 0.5% FFA and pretreatment at 40℃; B indicates dyeing at 30℃ and pH 7-7.5; C indicates the addition of leveling agent and running for 5 minutes; D indicates the addition of a specified acid dye (such as DyStar "Tianlong A2R" series or Huntsman "Lanna Sat PA" series), running for 10 minutes, and then heating; E indicates the addition of acetic acid to adjust the pH to 5-6.

[0036] Based on the low-temperature dyeing process implemented in this step, it was found that the first-pass dyeing qualification rate of luminous nylon fiber reached over 99.2%, and the unit product soft water, electricity, and steam consumption were reduced by approximately 69%, 14%, and 20% respectively compared to the conventional method. The number of employees per unit was reduced by more than half (from 35 to 16), reflecting the concept of "short time, low consumption, and low damage".

[0037] Step 2, Spinning: The dyed wool fibers and luminous nylon fibers are mixed and combed using a low-damage combing process to obtain a mixed sliver. The sliver is then spun into a blended yarn by sequentially passing it through roving, spinning, winding, steaming, and twisting processes. The dyed wool fibers and luminous nylon fibers are mixed and combed in a dry weight ratio of 50:50.

[0038] Of course, in actual production, in order to ensure the feel of the fabric and the inherent characteristics of wool, the dry weight of wool fibers should not be less than 50%. The blending ratio of luminous nylon fibers directly determines the strength of the fabric's luminous properties and can be flexibly adjusted according to the luminous use requirements of the finished fabric.

[0039] This step employs a low-damage combing process characterized by "closely spaced needles, small spacing, low speed, small feed rate, and small draft." For example, the defelting machine uses a small spacing of 40mm-45mm and a low speed of 140rpm-160rpm; the combing machine uses a small spacing of 20mm-35mm and a low speed of 120rpm-140rpm; the head needles use closely spaced needles, controlling the draft ratio to 6.5 times (small draft), a low speed of 140 rpm, and a small feed rate; the weight of the sliver exiting the last needle is controlled at 20±0.5g / m, the wool pellet index of the blended sliver is controlled at no more than 1.0 pellet / gram, and the wool flakes are 0.

[0040] The spinning process in this step ensures yarn strength and evenness by optimizing the size of the collector, spinning speed, and twist parameters. For example, taking 52 / 1Nm blended yarn as an example, by matching and optimizing the collector opening specifications, spinning speed, and twist parameters, and coordinating with 4mm spacer blocks for control, the optimal process scheme is: collector opening 8, spinning speed 7800rpm, and twist 800 twists / meter. This parameter combination can effectively improve yarn strength and evenness. The 52 / 1Nm yarn produced under this process has an average strength of 136cN, a USTER evenness CV% of 13.52, 42 fine places / km and 25 thick places / km, respectively, and a hairiness index of 2.1, resulting in stable and reliable yarn quality.

[0041] The winding process reduces strength loss at the twisting point and reduces yarn hairiness and yarn defects by optimizing winding untwisting and splicing parameters (such as 3 times of blowing twist, splicing strength of 3N, overlap length of 4mm, and untwisting time of 2 seconds).

[0042] In the process of producing blended yarn, a segmented two-stage steaming process is used to set the twist of the yarn. The segmented two-stage steaming process involves first steaming the yarn tassels, and then steaming the winding yarn. For blended yarns, the first steaming temperature is controlled at 75℃ and held for 20 minutes, and the second steaming temperature is controlled at 85℃ and held for 30 minutes.

[0043] After the steaming process is completed, the various indicators of the blended yarn are tested. Once the quality is qualified, it enters the weaving process. The process parameters for weaving can be corrected and guided. The quality control indicators of blended yarn are shown in Table 4 below.

[0044] Table 4 Control Indicators for Blended Yarns

[0045] Step 3, Weaving: Blended yarns are used for weaving. Optimax rapier looms are used with low tension (e.g., 22gf-23gf), low speed (e.g., 450rpm), and small opening (e.g., heddle angle 300°-310°) to produce the greige fabric.

[0046] In this process, the blended yarn is threaded separately using heddles and reeds. The amplitude of the back beam swing mechanism and the side support device are optimized to reduce frictional damage to the blended yarn. Specifically, the amplitude of the back beam swing mechanism can be optimized by reducing the spring diameter and lengthening the swing rod. For example, reducing the back beam spring diameter from 7mm to 5mm and lengthening the swing rod by 6cm increases the amplitude to 15mm, effectively reducing warp tension during weft insertion. The side support device can be optimized by milling the support plate deeper and increasing the wrap angle. For instance, milling 3mm away from the support plate near the side support in the original structure and modifying the bracket increases the adjustment range of the side support and the wrap angle to the fabric, thus solving the problems of weft yarn breakage and yarn snagging by the needle ring. Furthermore, weft tension control can be improved by manufacturing a thinner weft tension sheet (from 0.1mm to 0.06mm), reducing the weft insertion tension from 90cN to 60cN, ensuring gentle weft tension.

[0047] Step 4: After the greige fabric undergoes a wrinkle-resistant and comfort finishing process, a finished fabric with nighttime luminescence and elastic wrinkle-resistant properties is finally obtained.

[0048] The anti-wrinkle and comfort finishing processes include, in sequence: raw repair, dyeing machine elastic treatment, low-damage singeing, flat washing, wool washing, shearing, light ironing, and light steaming; among which: The elastic treatment of the dyeing machine was carried out in a water bath at 40℃-45℃ and pH 6-6.5 at a speed of 25m / min for 120 minutes; after the elastic treatment, the weft elastic elongation of the greige fabric increased from 6-7% to 10-13%. The low-damage singeing process is as follows: first, the greige fabric is cleaned to remove spinning and weaving auxiliaries, and then singeing is performed. The singeing speed is 110-130m / min, and the distance between the burner and the fabric surface is 10-14cm. Light ironing temperature is controlled at 100℃-120℃, and the belt tension is set at 50%; light steaming temperature is controlled at 115℃-120℃, pressure is 0.6 bar, and processing time is 90-100 seconds; using light ironing and light steaming processes to replace traditional strong ironing and steaming can maximize the preservation of the wool fibers' fluffiness, softness, and oiliness while ensuring dimensional stability and luster.

[0049] In specific implementation, the eight core processes of raw fabric repair, dyeing machine elastic treatment, low-damage singeing, flat washing, washing, shearing, light ironing, and light steaming need to be refined, and supporting transitional processes need to be added. The complete process flow is as follows: Greige fabric → Raw repair → Dyeing machine elastic treatment → Width opening → First drying → First brushing → Low-damage singeing → Flat washing and boiling → Second drying → Semi-finished product inspection → Finishing → High-speed airflow washing → Second brushing → Shearing → First ironing (light ironing and shaping) → First steaming (light steaming and shaping) → Third drying (simultaneous impregnation with softener and antistatic agent) → Second ironing (light ironing and shaping) → Oiling → Second steaming (light steaming and shaping).

[0050] The key process parameters for each step are set as follows: 1. Low-damage singeing: operating speed 120m / min, oil pressure 20mm, air pressure 10bar, singeing interval 12cm, using a one-forward-one-reverse singeing process; 2. Flat washing and boiling: operating speed 25m / min, washing temperature 98℃, dye bath pH controlled at 6, guide roller tension 1.5bar; 3. High-speed airflow washing: main fan frequency 80%, exhaust fan frequency 90%, airflow temperature 85℃, using hot air circulation washing mode; 4. Shearing: operating speed 15m / min, fabric feeding method three-forward-one-reverse, first shearing interval 0.8mm, second, third, and fourth shearing intervals are all 0.5mm; 5. First light ironing (ironing fabric 1): ironing temperature 100℃, guide belt tension 50bar. 6. First light steaming (steamed fabric 1): Steam temperature 120℃, steam pressure 0.6 bar, steaming time 100s, fabric tension 80Kg, pressure roller pressure 4 bar, using an inside-out steaming method; 7. Third drying (functional additive padding): Padding solution contains softener 40g / L and antistatic agent 40g / L, machine speed 25m / min, drying temperature 130℃; 8. Second light ironing (ironing fabric 2): Ironing temperature 120℃, belt tension 50 bar, machine speed 18m / min; 9. Second light steaming (steamed fabric 2): Steam temperature 115℃, steam pressure 0.6 bar, steaming time 90s, fabric tension 80Kg, pressure roller pressure 4 bar, using an inside-out steaming method.

[0051] Example 2: This example proposes a method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence with wearing comfort. The method includes the following steps: Step 1, Raw material selection and dyeing: Wool fiber and luminous nylon fiber (the legal name of the national standard for the textile industry, "FZ / T 54102-2022 Luminous Chemical Fiber") are used as raw materials, and are subjected to independent low-temperature dyeing treatments respectively.

[0052] When preparing luminous worsted wool fabric: ① The diameter of the wool fibers is in the range of 15μm-23μm, and Australian superfine Merino wool fibers with a fiber diameter of 16.5μm are specifically selected.

[0053] ②Luminous nylon fiber is a functional fiber made by blending polyamide (nylon) as the matrix, incorporating rare earth long afterglow luminescent materials, and using a masterbatch blending melt spinning process; its core characteristic is that after absorbing light for 10–30 minutes, it can continue to glow in the dark for more than 4–10 hours, and has the characteristics of being non-radioactive, washable, recyclable, and having multi-color light effects.

[0054] The process of independently dyeing wool fibers and luminous nylon fibers in this step is the same as described in step 1 of Example 1, and will not be repeated here.

[0055] Step 2, Spinning: The dyed wool fibers and luminous nylon fibers are separately combed using a low-damage combing process to produce wool tops and luminous nylon tops; the two types of tops are then separately processed through roving, spinning, winding, steaming and twisting processes to produce pure wool yarn and pure luminous nylon yarn, respectively.

[0056] The process of obtaining pure wool yarn and pure luminous nylon yarn in this step is the same as the description of obtaining blended yarn in step 2 of Example 1, with the only difference being: In the process of producing pure wool yarn and pure luminous nylon yarn, a segmented double steaming process is used to set the twist of the yarn. The segmented double steaming process involves steaming the yarn spools first, followed by steaming the winding yarn. For pure wool yarn and pure luminous nylon yarn, the first steaming temperature is controlled at 70℃ and held for 10 minutes, and the second steaming temperature is controlled at 80℃ and held for 30 minutes.

[0057] After the steaming process is completed, the indicators of pure wool yarn and pure luminous nylon yarn are tested. After the quality is qualified, it enters the weaving process. The process parameters of the weaving machine can be corrected and guided. The control indicators of pure wool yarn and pure luminous nylon yarn are shown in Table 5 below.

[0058] Table 5 Control Indicators for Pure Wool Yarn and Pure Luminous Nylon Yarn

[0059] In Table 5, "pure yarn" specifically refers to pure wool yarn and pure luminous nylon yarn.

[0060] Step 3, Weaving: Wool yarn is used as the warp and luminous nylon yarn is used as the weft for interlacing and weaving. An Optimax rapier loom is used with low tension (e.g., 22gf-23gf), low speed (e.g., 450rpm), and small opening (e.g., heddle flattening time main axis angle 300°-310°) to produce the greige fabric.

[0061] The pure luminous nylon yarn is threaded using separate heddles and reeds. The amplitude of the back beam swing mechanism and the side support device are optimized to reduce frictional damage to the pure luminous nylon yarn. Specifically, the amplitude of the back beam swing mechanism can be optimized by reducing the spring diameter and lengthening the swing rod. For example, reducing the back beam spring diameter from 7mm to 5mm and lengthening the swing rod by 6cm increases the amplitude to 15mm, effectively reducing warp tension during weft insertion. The side support device can be optimized by milling the support plate deeper and increasing the wrap angle. For example, milling 3mm away from the support plate near the side support in the original structure and modifying the bracket increases the adjustment range of the side support and the wrap angle to the fabric, thus solving the problems of weft yarn breakage and yarn snagging by the needle ring. Furthermore, weft tension control can be improved by manufacturing a thinner weft tension sheet (from 0.1mm to 0.06mm), reducing the weft insertion tension from 90cN to 60cN, ensuring gentle weft tension.

[0062] Step 4: After the greige fabric undergoes a wrinkle-resistant and comfort finishing process, a finished fabric with nighttime luminescence and elastic wrinkle-resistant properties is finally obtained.

[0063] The process of obtaining the finished fabric in this step is the same as that described in step 4 of Example 1, and will not be repeated here.

[0064] Example 3: This example proposes a method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence with wearing comfort. The method includes the following steps: Step 1, Raw material selection and dyeing: Wool fiber and luminous nylon fiber (the legal name of the national standard for the textile industry, "FZ / T 54102-2022 Luminous Chemical Fiber") are used as raw materials, and are subjected to independent low-temperature dyeing treatments respectively.

[0065] When preparing luminous worsted wool fabric: ① The diameter of the wool fibers is in the range of 15μm-23μm, and Australian superfine Merino wool fibers with a fiber diameter of 16.5μm are specifically selected.

[0066] ②Luminous nylon fiber is a functional fiber made by blending polyamide (nylon) as the matrix, incorporating rare earth long afterglow luminescent materials, and using a masterbatch blending melt spinning process; its core characteristic is that after absorbing light for 10–30 minutes, it can continue to glow in the dark for more than 4–10 hours, and has the characteristics of being non-radioactive, washable, recyclable, and having multi-color light effects.

[0067] The process of independently dyeing wool fibers and luminous nylon fibers in this step is the same as described in step 1 of Example 1, and will not be repeated here.

[0068] Step 2, Spinning: The dyed wool fibers and luminous nylon fibers are mixed and carded using a low-damage carding process to obtain a mixed sliver. This sliver is then spun through roving, spinning, winding, steaming, and twisting processes to produce the blended yarn. The dyed wool fibers and luminous nylon fibers are mixed and carded at a dry weight ratio of 50:50. However, in actual production, to ensure the fabric's feel and the inherent properties of wool, the dry weight percentage of wool fibers should not be less than 50%. The proportion of luminous nylon fibers directly determines the strength of the fabric's luminescence and can be flexibly adjusted according to the luminescence requirements of the finished fabric. The dyed wool fibers are individually combed using a low-damage combing process to produce wool tops; the wool tops are then processed through roving, spinning, winding, steaming, and twisting processes to produce pure wool yarn.

[0069] The process of obtaining blended yarn in this step is the same as the description of obtaining blended yarn in step 2 of Example 1. The process of obtaining pure wool yarn in this step is the same as the description of obtaining pure wool yarn in step 2 of Example 2, and will not be repeated here.

[0070] After the steaming process is completed, various indicators of blended yarn and pure wool yarn are tested. After the quality is qualified, it enters the weaving process. The process parameters of the weaving machine can be corrected and guided. The control indicators of blended yarn and pure wool yarn are shown in Table 4 and Table 5.

[0071] Step 3, Weaving: Wool yarn is used as the warp and blended yarn as the weft for interlacing and weaving. An Optimax rapier loom is used with low tension (e.g., 22gf-23gf), low speed (e.g., 450rpm), and small opening (e.g., heddle flattening time main axis angle 300°-310°) to produce the greige fabric.

[0072] The process of obtaining the grey fabric in this step is similar to the description of step 3 in Example 1, and will not be repeated here.

[0073] Step 4: After the greige fabric undergoes a wrinkle-resistant and comfort finishing process, a finished fabric with nighttime luminescence and elastic wrinkle-resistant properties is finally obtained.

[0074] The process of obtaining the finished fabric in this step is the same as that described in step 4 of Example 1, and will not be repeated here.

[0075] In summary, after the finished fabrics were prepared based on the methods described in Examples 1, 2, and 3, a subjective evaluation of the finished fabrics was conducted, as shown in Table 6.

[0076] Table 6 Subjective Style Evaluation of Finished Fabrics

[0077] Next, objective performance tests were conducted on the finished fabric: ① Safety and protection function: The fabric emits a soft and uniform glow at night or in low-light environments, successfully achieving the luminous warning function; all color fastness indicators performed excellently, especially the dry / wet rubbing fastness, which reached level 4-5 and level 4 (the first-class product standard is ≥4 and ≥3), meeting the requirements for high-durability outdoor wear. ② Physical and protective properties: a) Tensile strength: 196N in the warp and 182N in the weft (2 / 2 twill product), far exceeding the indicators of ordinary lightweight fabrics, ensuring abrasion resistance and durability; b) Wrinkle recovery angle: The warp and weft recovery angles reached 322 degrees (measured in the same product), far exceeding the superior product standard (≥270 degrees), demonstrating excellent wrinkle recovery ability; c) Elasticity and style: Through the combination of weaving and finishing processes, the product achieves excellent elasticity and stretch; ③ Weight and thickness: The finished product belongs to the ultra-lightweight category, which is in line with the "ultra-light" product positioning. It should be added that, taking 50 / 50 blended products as an example, ultralight products with a weight of less than 150g / m², usually in the range of 100-130g / m², can be defined as ultralight.

[0078] After the finished fabrics were prepared according to the methods described in Examples 1, 2 and 3, the finished fabrics were tested respectively. The test results of various indicators are shown in Table 7, and the safety performance test indicators are shown in Table 8.

[0079] Table 7 Test Results of Various Indicators of Finished Fabric

[0080] The finished fabric meets the following safety standards: formaldehyde content was not detected, pH value was 6.7, which fully complies with the OEKO-TEX Standard 100 eco-textile standard requirements, proving that the preparation method described in this embodiment is environmentally friendly and safe.

[0081] Table 8 Safety Performance Test Indicators of Finished Fabrics

[0082] In summary, the test results show that the finished fabric manufactured using the methods described in the three examples not only achieves the high-end texture and comfort of wool fabrics but also integrates excellent nighttime luminescence. The finished fabric's conventional colorfastness (dry / wet rubbing resistance ≥4) and physical properties meet the requirements of GB / T26382-2011 "Combed Wool Fabrics" (Superior Grade) and have passed OEKO-TEX Standard 100 eco-textile certification. The fabric continuously emits light in low-light environments, combining commercial value with outdoor safety protection.

[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence with wearing comfort, characterized in that, The method includes the following steps: Step 1, Raw material selection and dyeing: Wool fiber and luminous nylon fiber are used as raw materials, and each is subjected to independent low-temperature dyeing treatment; Step 2, Spinning: The dyed wool fibers and luminous nylon fibers are mixed and combed using a low-damage combing process to obtain a mixed sliver. Then, the sliver is spun into a blended yarn by sequentially passing through roving, spinning, winding, steaming and twisting processes. The dyed wool fibers and luminous nylon fibers were separately combed using a low-damage combing process to produce wool tops and luminous nylon tops. The two types of tops were then separately processed through roving, spinning, winding, steaming and twisting processes to produce pure wool yarn and pure luminous nylon yarn, respectively. Step 3, Weaving: The fabric is woven using blended yarns with pre-set weaving parameters of "low tension, low speed, and small opening" on the loom; or, wool yarn is used as the warp and luminous nylon yarn or blended yarn is used as the weft for interlacing weaving with pre-set weaving parameters of "low tension, low speed, and small opening" on the loom to produce the greige fabric. Among them, the blended yarn or pure luminous nylon yarn used in the weaving process adopts a separate heddle threading and reed threading method, while optimizing the amplitude of the back beam swing mechanism and the side support device to reduce frictional damage to the blended yarn or pure luminous nylon yarn. Step 4: After the greige fabric undergoes a wrinkle-resistant and comfort finishing process, a finished fabric with nighttime luminescence and elastic wrinkle-resistant properties is finally obtained.

2. The method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence and wearing comfort according to claim 1, characterized in that, The diameter of wool fibers ranges from 15μm to 23μm.

3. The method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence and wearing comfort according to claim 1, characterized in that, Luminous nylon fiber is a functional fiber made by blending polyamide with rare earth long afterglow luminescent materials and using a masterbatch melt spinning process. Its core characteristics are that it can continue to glow in the dark for more than 4–10 hours after absorbing light for 10–30 minutes. It is non-radioactive, washable, recyclable, and has multi-color light effects.

4. The method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence and wearing comfort according to claim 1, characterized in that, Step 1 involves low-temperature dyeing of wool fibers using reactive or neutral wool dyes. The specific process is as follows: In the dyeing machine, water is introduced at 40℃-45℃, formic acid is added to adjust the pH of the dye bath to 5.5-6, and after adding a dyeing defoamer, the machine is run continuously for 4-8 minutes. Reactive or neutral wool dyes are then used, and dyeing is performed at 80℃-85℃ under the action of a leveling agent. After completion, there is no need to drain the dye bath. Add alkali and detergent directly to the original dye bath for two alkali washes, followed by washing with hot water at 55℃-60℃ for 8-12 minutes, washing with cold water at 45℃-50℃ for 4-8 minutes, and acid neutralization treatment. The staining bath ratio should be controlled at 1:5, and the staining time should be 3-4 hours.

5. The method for preparing a luminescent wool worsted fabric with both high-efficiency luminescence and wearing comfort according to claim 4, characterized in that, Step 1 involves low-temperature dyeing of luminescent nylon fibers using a specified acidic dye. The specific process is as follows: First, pre-treat the fibers at 38℃-42℃ with 0.5% FFA auxiliaries, then drain and change the water. Dyeing begins at 30℃ under neutral pH conditions of 7-7.

5. Leveling agent is added sequentially and the dye is run for 4-7 minutes, followed by 8-12 minutes of dyeing. The dyeing temperature does not exceed 80℃ throughout the process, and the amount of dye used is controlled within 0.5% owf. The heating process involves uniformly increasing the temperature from 30℃ to 70℃ at a rate of 1℃ / min, holding for 8-12 minutes, then increasing the temperature again to 80℃ at a rate of 0.8℃ / min and holding for 8-12 minutes. In the later stages of dyeing, acetic acid is added to adjust the pH to an acidic environment of 5-6, and the dye is fixed for 20-30 minutes. Finally, the fibers are cooled and washed with water.

6. The method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence and wearing comfort according to claim 1, characterized in that, In step 2, the dyed wool fibers and luminous nylon fibers are mixed and combed in a dry weight ratio of 50:50 to obtain a mixed wool top, which is then spun into a blended yarn through roving, spinning, winding, steaming and twisting processes.

7. The method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence and wearing comfort according to claim 6, characterized in that, Step 2 involves employing a low-damage combing process characterized by "closed-number needles, small spacing, low speed, small feed rate, and small drafting". The spinning process ensures yarn strength and evenness by optimizing the size of the collector, machine speed, and twist parameters; The winding process reduces strength loss at the twist joint by optimizing winding untwisting and splicing parameters, thereby reducing yarn hairiness and yarn defects.

8. The method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence and wearing comfort according to claim 1, characterized in that, In step 2, during the production of blended yarn, pure wool yarn, and pure luminous nylon yarn, a segmented double steaming process is used to set the twist of the yarn. This process involves steaming the yarn tassels first, followed by steaming the winding yarn. For blended yarns, the first steaming temperature is controlled at 75℃ and held for 20 minutes, and the second steaming temperature is controlled at 85℃ and held for 30 minutes. For pure wool yarn and pure luminous nylon yarn, the first steaming temperature is controlled at 70℃ and held for 10 minutes, and the second steaming temperature is controlled at 80℃ and held for 30 minutes.

9. The method for preparing a luminescent wool worsted fabric that combines high-efficiency luminescence and wearing comfort according to claim 1, characterized in that, The anti-wrinkle and comfort finishing processes include, in sequence: raw repair, dyeing machine elastic treatment, low-damage singeing, flat washing, wool washing, shearing, light ironing, and light steaming; among which: The dyeing machine was subjected to elastic treatment in a water bath at 40℃-45℃ and pH 6-6.5, running at a speed of 25 m / min for 120 min. The low-damage singeing process is as follows: first, the fabric is cleaned to remove spinning and weaving auxiliaries, and then singeing is performed. The singeing speed is 110-130 m / min, and the distance between the burner and the fabric surface is 10-14 cm. The temperature for light ironing is controlled at 100℃-120℃, and the tension of the guide belt is set to 50%. The steaming temperature is controlled at 115℃-120℃, the pressure at 0.6 bar, and the processing time at 90-100 seconds.