A carbon fiber composite felt mixture for carding and felting and a method for preparing the composite felt.

By employing liquid-phase mixing and functional pre-modification, the problems of uneven mixing of multi-component fibers, electrostatic hazards, and lengthy processes have been solved, achieving uniform fiber mixing and production line stability. This technology is applicable to fields such as automotive interiors and building insulation.

CN123108833APending Publication Date: 2026-11-17JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610997008.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-06
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing multi-component fiber mixing processes suffer from problems such as uneven mixing due to fiber density differences, lengthy processes with multiple feed ports, fragmentation during functionalization, and electrostatic hazards in the production line, and there is a lack of effective solutions.

Method used

The fiber is pretreated by liquid phase mixing, antistatic modifier is introduced and the synergistic effect of thickening agent and nonionic dispersant is utilized to achieve uniform mixing of fiber through liquid phase suspension system. In the agglomeration process, low melting point thermal bonding fiber is used to form dot-like weak bond, and the fiber is directly fed into the carding machine through a single feed port.

Benefits of technology

It improves the uniformity of fiber mixing, solves the static electricity problem, simplifies the process, and improves product quality consistency and production efficiency. It is applicable to fields such as automotive interiors and building insulation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108833A_ABST
    Figure CN123108833A_ABST
Patent Text Reader

Abstract

This invention discloses a carbon fiber composite felt mixture for carding and felting, and a method for preparing the composite felt, belonging to the field of functional felt technology. First, multiple fibers containing carbon fibers and low-melting-point thermally bonded fibers undergo surface modification pretreatment, such as antistatic treatment. Then, these fibers are added to a liquid-phase suspension system containing a thickening agent and a non-ionic dispersant, utilizing the liquid medium to overcome density differences and achieve uniform mixing. Next, the mixed suspension is dried and agglomerated, and the surface of the low-melting-point thermally bonded fibers is slightly softened through two-stage heating, forming weak point bonds to lock in uniform fiber distribution. Finally, the mixture is fed into a carding machine through a single inlet, and the composite felt is obtained through carding, layup, and needle punching consolidation. By synergistically applying liquid-phase mixing and functional pre-modification, the problem of uneven mixing caused by density differences in multi-component fibers is solved, simplifying the process flow and endowing the felt with antistatic, flame-retardant, and antibacterial functions, improving product consistency and production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of nonwoven fabric and functional felt preparation technology, specifically relating to a mixture for carding felt making and a process for preparing carbon fiber composite felt. Background Technology

[0002] Needle-punched felt is an important product in the nonwoven fabric field, widely used in automotive interiors, building insulation, industrial filtration, medical and health, aerospace and other fields. With the increasing demands on felt performance from downstream applications, multi-component fiber composite technology has become a core means to improve the overall performance of felt. By mixing different types of fibers (such as carbon fiber, polyester, polypropylene, flame-retardant fibers, low-melting-point thermal bonding fibers, etc.) in specific proportions, felt can simultaneously meet functional requirements such as strength, elasticity, thermal bonding, and flame retardancy.

[0003] However, existing multi-component fiber blending processes have the following significant technical problems:

[0004] First, airflow mixing methods cannot solve the density difference problem. Traditional airflow opening and mixing boxes rely on airflow to carry and mix fibers, but differences in fiber density (such as carbon fiber density of 1.82 g / cm³ and polypropylene density of 0.91 g / cm³) result in different airflow carrying capacities. Lighter fibers float while heavier fibers sink, causing fiber stratification and uncontrolled proportions, resulting in uneven product composition and large performance fluctuations.

[0005] Second, the multi-inlet direct feeding method is a lengthy process. Traditional solutions require separate openers, storage boxes, feeders, and corresponding inlets for each fiber component, resulting in large equipment investment, a large footprint, and numerous process nodes. Deviations in flow control at each inlet can easily lead to discrepancies between the actual and designed mixing ratios. Furthermore, because each component follows an independent channel before entering the carding machine, the mixing depth between fibers is insufficient, and the fiber web may still exhibit component segregation after carding.

[0006] Third, functionalization treatment and blending processes are separated. In existing processes, functionalization treatments such as antistatic and flame retardant treatments are usually completed in the spinning stage or the finishing stage after felting, which is independent of the blending process. Modification in the spinning stage is limited by the fiber type and the compatibility of the modifying agent, while the finishing process has defects such as insufficient agent penetration depth, uneven distribution and poor durability. In addition, neither of these processes can achieve unified functionalization of multi-component fibers during blending.

[0007] Fourth, static electricity issues are prominent at the front end of the production line. Many chemical fibers (especially polyester and polypropylene) are prone to generating a large amount of static electricity during the carding process due to high-speed friction of machine parts. This can cause fibers to become entangled in rollers, doffers, and other machine parts, leading to production accidents such as tangling and wire breakage, reducing production efficiency and product quality, and posing certain safety hazards.

[0008] Fifth, the risk of secondary stratification still exists in the carding stage after liquid-phase mixing. Although liquid-phase mixing can ensure the uniform distribution of fibers of different densities in a suspended state, after drying and clumping, they enter the carding machine. Under the centrifugal force, airflow, and needle action generated by the high-speed rotation of the cylinder, lightweight fibers (such as polypropylene, with a density of 0.91 g / cm³) will stratify. 3 Heavy fibers (such as polyester and carbon fiber, with a density of 1.38–1.82 g / cm³) tend to float to the upper layer of the fiber web. 3 These components tend to deposit in the lower layers, causing component segregation to reappear in the carded fiber web, thus partially negating the homogenization effect of liquid-phase mixing during the carding process. Current processes lack effective solutions to this secondary segregation problem.

[0009] In summary, existing multi-component fiber felt-making technology has significant shortcomings in terms of mixing uniformity, process flow length, functional integration, and production stability. Therefore, a new process solution is needed that can solve the above problems from the source of mixing. Summary of the Invention

[0010] To address the core technical problems in existing multi-component fiber blending felting processes, such as uneven mixing due to density differences, lengthy processes with multiple feed ports, fragmented functionalization treatments, and static electricity hazards in the production line, this invention provides a blend preparation process for carding felting. By using a liquid-phase mixing method, it fundamentally overcomes the constraint of density differences on mixing uniformity and organically integrates functionalization modification with the mixing process. This allows the precursor fiber clusters to possess target functions such as antistatic properties, flame retardancy, and antibacterial properties before entering the carding machine. Finally, the fibers are directly fed into the carding felting production line through a single feed port, significantly simplifying the process and improving product quality consistency.

[0011] The technical solution of this invention is as follows:

[0012] A method for preparing a carbon fiber composite felt mixture for carding and felting includes the following steps:

[0013] (1) Fiber functionalization pretreatment: The surfaces of various fiber raw materials containing carbon fiber, low-melting-point thermal bonding fiber, and at least one chemical fiber, regenerated fiber, and functional fiber are modified respectively. At the same time, antistatic modifiers are introduced so that the fibers have antistatic properties before entering the mixing stage. The mixing ratio of each fiber component in the fiber raw material is adjusted according to the performance requirements of the final felt material. The low-melting-point thermal bonding fiber refers to a low-melting-point fiber with thermal bonding function that can soften on the surface and form inter-fiber bonding points after being heated. Its softening point is 90-180℃ and its proportion is 5-10 wt%.

[0014] (2) Liquid phase mixing: The pretreated fibers are added to a liquid phase suspension system containing a thickening agent and a nonionic dispersant in a designed ratio. The liquid phase suspension system is a water-based suspension or a low-boiling-point alcohol suspension. The amount of thickening agent is 0.005 to 0.05 wt% of the total mass of the suspension, and the amount of nonionic dispersant is 0.01 to 0.5 wt% of the total mass of the suspension. The buoyancy and dispersion of the liquid phase medium are used to overcome the fiber density difference and achieve uniform mixing to obtain a precursor mixed suspension.

[0015] (3) Agglomeration treatment: The precursor mixed suspension is dried and agglomerated. The drying temperature is 5-15°C below the softening point of the low melting point thermal bonding fiber, so that the surface of the thermal bonding fiber forms a weak bond at the intersection with other fibers, and the fibers of different densities are fixed in a uniform distribution state during liquid phase mixing, so as to obtain a mixed fiber agglomeration that can be directly used for carding machine feeding, namely the carbon fiber composite felt mixture used for carding felt making.

[0016] Preferably, the chemical fiber in step (1) is selected from one or more of polyester (PET), polypropylene (PP), nylon (PA), and acrylic (PAN); the regenerated fiber is selected from one or more of modal, viscose fiber, or lyocell fiber; the functional fiber is selected from one or more of conductive fiber and flame-retardant fiber; and the low-melting-point thermal bonding fiber is selected from one or more of core-sheath type bicomponent thermal bonding fiber, side-by-side type bicomponent thermal bonding fiber, and low-melting-point copolyester thermal bonding fiber, with a softening point of 100-140°C.

[0017] Preferably, the fiber length of the fiber raw material in step (1) is controlled between 20 and 100 mm.

[0018] Preferably, the antistatic modifying agent in step (1) is one or more of a permanent quaternary ammonium salt-based antistatic agent or a phosphate ester-based antistatic agent, and the surface resistance of the fiber after treatment is ≤10 Ω·cm. 9 Ω; Further optimization of permanent quaternary ammonium salt-based antistatic agents, which can form a durable conductive layer on the fiber surface, unaffected by washing. This treatment process can be carried out simultaneously with liquid phase mixing, which can eliminate the problem of static electricity accumulation in the carding process from the source and ensure the continuous and stable operation of the production line.

[0019] In step (1), one or more of the following can be introduced simultaneously: flame retardant (such as phosphorus-nitrogen synergistic flame retardant, aluminum hydroxide microparticles, etc.), antibacterial agent (such as nano silver, quaternary ammonium salt-based antibacterial agent, organosilicon quaternary ammonium salt, etc.), phase change energy storage material (such as microcapsule phase change wax, etc.), far-infrared emitting powder (such as zirconium oxide, alumina-based far-infrared ceramic powder, etc.) and negative ion powder (such as tourmaline powder, etc.) and compounded with antistatic modifying agent. The amount of flame retardant attached after flame retardant modification is 2 to 15 wt% of the fiber mass, and the amount of antibacterial agent attached after antibacterial modification is 0.5 to 2 wt% of the fiber mass.

[0020] Preferably, the thickening agent in step (2) is selected from one or more of hydroxyethyl cellulose (HEC), polyethylene glycol (PEG), guar gum, methyl cellulose (MC) or xanthan gum; the above thickening agents are all non-ionic or weakly polar polymers that do not chemically adsorb or covalently react with the fiber surface, and can be completely removed or remain in a harmless amount after drying or sheet forming, without affecting the subsequent combing performance and functional modification effect of the fiber.

[0021] More preferably, the nonionic dispersant is Triton X-100 at a concentration of 0.01~0.1 wt%, and the thickening agent is HEC at a concentration of 0.01~0.05 wt%. Through the synergistic effect of these two agents, fibers of different densities are fully unbundled and dispersed, preventing fiber bundle aggregation and sedimentation, and there is no risk of incompatibility with cationic functionalized modifiers (such as quaternary ammonium salt antistatic agents).

[0022] Preferably, the liquid phase mixing in step (2) is carried out in a mixing tank equipped with a spiral stirrer and an ultrasonic dispersion device; the stirring speed is 100-800 rpm, the ultrasonic power is 100-1000 W, and the ultrasonic time is 3-30 min.

[0023] Preferably, the drying and agglomeration in step (3) involves drying the filtered mixed fiber material in a hot air circulating oven until the moisture content is ≤0.05% to form fiber clumps. This process is divided into two stages: the first stage involves drying at 50-90°C until the moisture content is ≤0.05%, and the second stage involves heating to 5-15°C below the softening point of the low melting point thermal bonding fiber and holding for 10-30 minutes. This allows the surface of the thermal bonding fiber to form point-like weak adhesion at the points of contact with other fibers, fixing fibers of different densities in a uniform distribution state during liquid phase mixing, thus achieving thermal bonding pre-locking. This weak adhesion can be gradually disintegrated under the action of the carding machine needles without affecting the opening and carding effect.

[0024] The present invention also provides a carbon fiber composite felt mixture for carding felt production prepared by the above method.

[0025] The present invention also provides a method for preparing carbon fiber composite felt from the mixture, the method comprising the following steps: feeding the mixture into a carding machine through a single inlet, and sequentially carding, laying up, reinforcing layer bonding, needle punching and consolidation, and winding to obtain the finished carbon fiber composite felt.

[0026] Preferably, the carding machine is one of a single-roller carding machine, a double-roller carding machine, or a random web-forming carding machine, and the carding speed is 20-120 m / min;

[0027] A pre-opening and blending device is installed at the front end of the carding machine inlet. This device consists of a low-speed needle roller opening chamber (needle roller speed 20-80 rpm), a flow equalization guide plate, and a feeding curtain. The mixed fiber clumps are first gently opened into uniform fiber bundles under the action of the low-speed needle roller, avoiding segregation caused by uneven local density of the fiber clumps when directly fed into the high-speed cylinder. The flow equalization guide plate evenly spreads the opened fiber bundles to the full width, and the feeding curtain feeds them into the carding machine at a uniform speed. Compared with direct feeding, after treatment by the pre-opening and blending device, the local deviation of each component of the carded output fiber web can be further reduced to ≤3%, effectively bridging the secondary loss of liquid phase mixing uniformity caused by density differences during the carding stage.

[0028] The layup is performed using a mesh laying machine, employing either cross-laying or parallel-laying methods.

[0029] The reinforcing layer is laminated using a reinforcing layer lamination device, where a non-woven fabric or other reinforcing layer is stacked. The reinforcing layer is one of the following: non-woven fabric, woven fabric, knitted fabric, or unidirectional fiber mesh fabric, with a basis weight of 10–80 g / m². 2 It is combined with carded fiber web by laying it on top and bottom or sandwiching it in the middle to improve the dimensional stability and tear resistance of the felt.

[0030] The needle acupuncture process parameters are: needle density 50-300 needles / cm² 2 The needle puncture depth is 5-20mm, the feed speed is 1-10m / min, and the pre-needling and main needle puncture are at least two processes, which are completed by the pre-needling machine and the main needle puncture machine respectively.

[0031] The beneficial effects of this invention are:

[0032] This invention introduces liquid-phase suspension mixing technology into the multi-component fiber mixing process. The liquid-phase suspension system refers to a liquid medium with suitable viscosity that can uniformly disperse fibers of different densities without stratification and sedimentation, is easy to remove in subsequent processes, and does not affect the physical and mechanical properties and functional modification effects of the fibers. By utilizing the balanced buoyancy and dispersion effect of this medium on fibers of different densities, the uniform blending of each component fiber is achieved in a precise ratio, solving the problem of fiber stratification and uncontrolled ratio in air-flow mixing methods.

[0033] This invention introduces functionalized modifiers before or during liquid-phase mixing, enabling fibers to undergo surface functionalization in a liquid environment. This forms a precursor mixture preparation process that integrates fiber mixing and functional enhancement. It not only solves the prominent problem of static electricity at the front end of the production line, but also allows for various functionalization treatments. The resulting fiber bundles can be directly used as a single feed source for the carding machine, replacing the traditional multi-component independent feeding scheme. This solves the problem of insufficient mixing depth between fibers and component segregation in the fiber web after carding, where various fiber raw materials pass through independent channels before entering the carding machine.

[0034] This invention also introduces low-melting-point thermal bonding fibers into the fiber raw materials. During the drying process, the low-melting-point thermal bonding fibers are used to soften easily by heating them until their surface softens slightly. This causes them to form weak point bonds at the cross-contact points with other fibers, fixing the various fibers in a uniform distribution state during liquid phase mixing. This overcomes the risk of secondary delamination that still exists in the carding stage.

[0035] This invention, through the synergistic application of liquid-phase mixing and functional pre-modification, achieves significantly better uniformity of felt components (local deviation ≤5%) than the traditional multi-inlet airflow feeding scheme (deviation 12-18%). Antistatic, flame-retardant, and antibacterial properties can be imparted in one step during the liquid-phase mixing stage, eliminating the need for post-processing. The single-inlet scheme reduces the number of front-end equipment on the production line by approximately 60%, and the number of process nodes is reduced from 7-10 independent multi-component channels to 3-4, significantly improving production efficiency and product quality consistency. It is suitable for the large-scale production needs of functional felt materials in fields such as automotive interiors, building insulation, industrial filtration, and medical and health protection. Attached Figure Description

[0036] Figure 1 This is a schematic diagram of the felt-making process of the present invention. Detailed Implementation

[0037] The present invention will be further described below with reference to embodiments, but the scope of protection of the present invention is not limited thereto.

[0038] Example 1 (Antistatic Multi-component Functional Felt Material)

[0039] B1, Fiber raw material pretreatment: Weigh 5cm of short-cut carbon fiber (density 1.82g / cm³). 3 60 parts, polypropylene staple fiber (density 0.91 g / cm³) 3 30 parts of low-melting-point thermal bonding fiber and 10 parts of core-sheath bicomponent polyester thermal bonding fiber (in this embodiment, core-sheath type bicomponent polyester thermal bonding fiber is used, the sheath is copolyester (Co-PET), the core is polyethylene terephthalate (PET), the softening point is about 110℃, the length is 51mm, 4D), the fiber length is 51mm, and they are dried in an oven at 60℃ for 2h to remove the oil on the fiber surface to ensure the effect of subsequent liquid phase modification.

[0040] B2, Liquid-phase functionalized mixing: Prepare 30L of an aqueous suspension containing 0.025wt% HEC, add 0.05wt% Triton X-100, and stir evenly at 400rpm. Add the three types of dried fibers to the mixing tank simultaneously, followed by the addition of a quaternary ammonium salt permanent antistatic agent (3wt% of the total fiber mass). Turn on the ultrasonic disperser (500W power) and ultrasonically disperse for 15min to fully unbundle and uniformly mix the three types of fibers, while the antistatic agent adheres to the fiber surface to complete the functionalized modification.

[0041] B3, Agglomeration Processing: The mixed fiber suspension is filtered and dehydrated through an 80-mesh filter and placed in a hot air circulating dryer using a two-stage drying process: the first stage involves drying at 80℃ for 2 hours until the moisture content is ≤0.05%; the second stage involves heating to 108℃ and holding for 20 minutes, causing slight softening of the surface of the low-melting-point thermal bonding fibers in the system, forming point-like weak adhesion at the cross-contact points with carbon fiber and polypropylene fiber, fixing the three fibers in a uniform distribution state during liquid-phase mixing. After cooling, a fluffy and uniform antistatic functionalized pre-locked mixed fiber agglomeration with a moisture content ≤0.03% is obtained.

[0042] B4, Carding and Felt Making: The mixed fiber bundles are first fed into a pre-opening and equalizing device (low-speed needle roller speed 40 rpm), gently opened and evenly spread to the feeding curtain via a flow equalization guide plate, and then continuously fed into a double roller carding machine (carding speed 50 m / min) through a single feed port. After opening and carding, a uniform fiber web is formed; then it is laid in 8 layers by a cross-laying machine to achieve the target weight (approximately 300 g / m²). 2 The fiber layer consists of a fiber layer; a 20g / m² polypropylene (PP) spunbond nonwoven fabric is laid on both the top and bottom surfaces of the fiber layer as a reinforcing layer; and the surface is pre-needled (needle-punching density 80 needles / cm²). 2 The process involves two consolidation steps: a main needle punch (15mm deep) and a main needle punch (200 needles / cm², 10mm deep). Finally, the material is rolled up to obtain the finished antistatic functional felt.

[0043] The obtained felt material has a weight of 320 g / m². 2 Thickness 4.5mm, surface resistivity ≤5×10 8 Ω, with local content deviation of each component fiber ≤4%, suitable for anti-static applications such as automotive interiors and precision electronic equipment packaging.

[0044] Example 2 (Flame-retardant functional felt material)

[0045] B1, fiber raw material pretreatment: Weigh 50 parts of 5cm short carbon fiber, 40 parts of flame-retardant polyester (PET) short fiber, and 10 parts of low melting point thermal bonding fiber (in this example, a core-sheath type bicomponent polyester thermal bonding fiber with a softening point of about 130℃ is used), with a fiber length of 38-51mm, and dry in an oven at 60℃ for 2 hours.

[0046] B2, Liquid-phase functionalized mixing: Prepare 30L of an aqueous suspension containing 0.025wt% HEC, add 0.05wt% Triton X-100, and stir at 400rpm until homogeneous. Add the three types of fibers simultaneously to the mixing tank, along with phosphorus-nitrogen synergistic flame retardant (FR-6, 8wt% of the total fiber mass) and aluminum hydroxide micropowder (4wt%). Perform ultrasonic dispersion (600W, 20min) to ensure thorough dispersion of the fibers and uniform bonding with the flame retardant, thus completing the liquid-phase flame retardant modification.

[0047] B3, Agglomeration Processing: The mixed fiber suspension is filtered and dehydrated through an 80-mesh filter and placed in a hot air circulating dryer using a two-stage drying process: the first stage involves drying at 80℃ for 2 hours until the moisture content is ≤0.05%; the second stage involves heating to 125℃ and holding for 20 minutes, causing slight softening of the surface of the low-melting-point thermal bonding fibers in the system, forming weak point-like bonds at the cross-contact points with carbon fiber and polyester fiber, fixing the three fibers in a uniform distribution state during liquid-phase mixing. After cooling, a fluffy and uniform flame-retardant functionalized pre-locked mixed fiber agglomeration with a moisture content ≤0.03% is obtained.

[0048] B4, Carding and Felt Making: Mixed fiber bundles are fed into a double roller carding machine through a single inlet (carding speed 50m / min), and 12 layers of cross-laid web are laid (target weight approximately 500g / m²). 2 The top and bottom layers are each reinforced with a 30g / m² flame-retardant nonwoven fabric layer, and then pre-needled (100 needles / cm², 18mm depth) and main needle-punched (250 needles / cm²). 2 (12mm deep) Solidify and rewind to finish the product.

[0049] The resulting felt has a weight of 540g / m², a thickness of 7.5mm, an LOI (Limiting Oxygen Index) of ≥32%, meets the B1 flame retardant standard, and has a local deviation of ≤4.5% for each fiber component. It is suitable for applications such as building insulation and sound absorption felt, and flame retardant felt for rail transit interiors.

[0050] Example 3 (Multifunctional composite felt material: antistatic + flame retardant + antibacterial)

[0051] B1, Fiber raw material pretreatment: Weigh 50 parts of 5cm short-cut carbon fiber, 30 parts of polypropylene short fiber, and Modal fiber (density 1.50g / cm³). 315 parts of low-melting-point thermal bonding fiber and 5 parts of low-melting-point copolyester thermal bonding fiber (in this embodiment, low-melting-point copolyester thermal bonding fiber with a softening point of about 110°C) were used. The fiber length was 38-64 mm and the fiber was dried at 60°C for 2 hours.

[0052] B2, Liquid-phase functionalized mixing: Prepare 35L of water-based suspension containing 0.030wt% HEC and 0.06wt% Triton X-100. Add the four types of fibers to the mixing tank, and add quaternary ammonium salt antistatic agent (3wt%), phosphorus nitrogen flame retardant (6wt%) and organosilicon quaternary ammonium salt antibacterial agent (1wt%) in sequence. Disperse by ultrasonication (power 700W, time 25min). The three functionalized agents synergistically adhere to the fiber surface, achieving a one-time liquid-phase imparting of antistatic, flame retardant and antibacterial triple functions.

[0053] B3, Agglomeration Processing: The mixed fiber suspension is filtered and dehydrated through an 80-mesh filter and placed in a hot air circulating dryer using a two-stage drying process: the first stage involves drying at 80℃ for 2 hours until the moisture content is ≤0.05%; the second stage involves heating to 105℃ and holding for 20 minutes, causing slight softening of the surface of the low-melting-point thermal bonding fibers in the system, forming point-like weak bonds at the cross-contact points with carbon fiber, polypropylene, and modal fibers, fixing the three fibers in a uniform distribution state during liquid-phase mixing. After cooling, a fluffy, uniform, and multifunctional pre-locked mixed fiber agglomerate with antistatic, flame-retardant, and antibacterial properties, with a moisture content of ≤0.03%, is obtained.

[0054] B4, Carding and Felt Making: Feed into a carding machine with a single inlet (carding speed 40m / min), cross-lay 10 layers (target weight approximately 400g / m²), with an intermediate interlayer of 25g / m². 2 The non-woven reinforcing layer is needle-punched and consolidated (pre-needle-punching 80 needles / cm², main needle-punching 220 needles / cm²) and then rolled up.

[0055] The obtained felt material has a weight of 430 g / m². 2 Thickness 5.8mm, surface resistivity ≤8×10 8 Ω, LOI≥29%, antibacterial rate (Escherichia coli / Staphylococcus aureus)≥99%, component local deviation≤4%, suitable for high-functionality integrated scenarios such as medical and health protection, public transportation seat felt, etc.

[0056] Comparative Example 1 (Traditional airflow mixing multi-port feeding scheme)

[0057] Using the same proportions as in Example 1, 5cm chopped carbon fibers, polypropylene staple fibers, and low-melting-point thermal bonding fibers were fed into the three feed inlets of the carding machine through separate opening-storage box-feeding machine channels, with a flow rate ratio controlled at 60:30:10. The carding speed was 60m / min, and the web laying and needle punching parameters were the same as in Example 1. No reinforcing layer was added, and the felt was directly wound up to obtain the material.

[0058] Test results: The local content deviation of each fiber component in the felt material reached 12-18%, which is significantly higher than ≤4% in Example 1; during the production process, the polypropylene fiber repeatedly wrapped around the roller due to static electricity accumulation, and the machine was stopped twice for treatment; the surface resistance of the felt material was >10¹²Ω, and it did not have antistatic function; flame retardant and antibacterial properties were also not provided.

[0059] Table 1 Comparison of key performance characteristics of felt materials in each embodiment and comparative example

[0060] Performance indicators Example 1 Example 2 Example 3 Comparative Example 1 Local deviation of components (%) ≤4 ≤4.5 ≤4 12~18 Surface resistivity (Ω) <![CDATA[≤5×10 8 ]]> — <![CDATA[≤8×10 8 ]]> >10¹² LOI(%) — ≥32 ≥29 — Antibacterial rate (%) — — ≥99 —

[0061] Through the synergistic application of liquid-phase mixing and functional pre-modification, the uniformity of felt components (local deviation ≤5%) in each embodiment of the present invention is significantly better than that of the traditional multi-inlet airflow feeding scheme (deviation 12-18%). Antistatic, flame-retardant, antibacterial and other functional properties can be imparted in one step during the liquid-phase mixing stage without the need for post-processing. The single feed port scheme reduces the number of front-end equipment in the production line by about 60%, and the number of process nodes is reduced from 7-10 independent channels of multiple components to 3-4, which significantly improves production efficiency and product quality consistency.

[0062] The above embodiments and comparative examples are provided to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be easily made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments and comparative examples, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A method for preparing a carbon fiber composite felt mixture for carding and felting, characterized in that, Includes the following steps: (1) Fiber functionalization pretreatment: The surfaces of various fiber raw materials containing carbon fiber, low-melting-point thermal bonding fiber, and at least one chemical fiber, regenerated fiber, and functional fiber are modified respectively. At the same time, antistatic modifiers are introduced so that the fibers have antistatic properties before entering the mixing stage. The mixing ratio of each fiber component in the fiber raw material is adjusted according to the performance requirements of the final felt material. The low-melting-point thermal bonding fiber refers to a low-melting-point fiber with thermal bonding function that can soften on the surface and form inter-fiber bonding points after being heated. Its softening point is 90-180℃ and its proportion is 5-10 wt%. (2) Liquid phase mixing: The pretreated fibers are added to a liquid phase suspension system containing a thickening agent and a nonionic dispersant in a designed ratio. The liquid phase suspension system is a water-based suspension or a low-boiling-point alcohol suspension. The amount of thickening agent is 0.005 to 0.05 wt% of the total mass of the suspension, and the amount of nonionic dispersant is 0.01 to 0.5 wt% of the total mass of the suspension. The buoyancy and dispersion of the liquid phase medium are used to overcome the fiber density difference and achieve uniform mixing to obtain a precursor mixed suspension. (3) Agglomeration treatment: The precursor mixed suspension is dried and agglomerated. The drying temperature is 5-15°C below the softening point of the low melting point thermal bonding fiber, so that the surface of the thermal bonding fiber forms a weak bond at the intersection with other fibers, and the fibers of different densities are fixed in a uniform distribution state during liquid phase mixing, so as to obtain a mixed fiber agglomeration that can be directly used for carding machine feeding, namely the carbon fiber composite felt mixture used for carding felt making.

2. The method for preparing carbon fiber composite felt mixture for carding and felting according to claim 1, characterized in that, The chemical fiber mentioned in step (1) is selected from one or more of polyester, polypropylene, nylon, and acrylic; the regenerated fiber is selected from one or more of modal, viscose fiber, or lyocell fiber; the functional fiber is selected from one or more of conductive fiber and flame retardant fiber; the low melting point thermal bonding fiber is selected from one or more of core-sheath type bicomponent thermal bonding fiber, parallel type bicomponent thermal bonding fiber, and low melting point copolyester thermal bonding fiber, and its softening point is 100-140℃.

3. The method for preparing carbon fiber composite felt mixture for carding and felting according to claim 1, characterized in that, The fiber length of the fiber raw material mentioned in step (1) is controlled between 20 and 100 mm.

4. The method for preparing carbon fiber composite felt mixture for carding and felting according to claim 1, characterized in that, The antistatic modifier mentioned in step (1) is one or more of a permanent quaternary ammonium salt-based antistatic agent or a phosphate ester-based antistatic agent, and the surface resistance of the fiber after treatment is ≤10. 9 Ω; In step (1), one or more of the following can be introduced simultaneously: flame retardant, antibacterial agent, phase change energy storage material, far-infrared emitting powder and negative ion powder, and compounded with antistatic modifier. The amount of flame retardant after flame retardant modification is 2 to 15 wt% of the fiber mass, and the amount of antibacterial agent after antibacterial modification is 0.5 to 2 wt% of the fiber mass.

5. The method for preparing carbon fiber composite felt mixture for carding and felting according to claim 1, characterized in that, The thickening agent mentioned in step (2) is selected from one or more of hydroxyethyl cellulose, polyethylene glycol, guar gum, methyl cellulose or xanthan gum.

6. The method for preparing carbon fiber composite felt mixture for carding and felting according to claim 1, characterized in that, The liquid phase mixing in step (2) is carried out in a mixing tank equipped with a spiral stirrer and an ultrasonic dispersion device; the stirring speed is 100-800 rpm, the ultrasonic power is 100-1000 W, and the ultrasonic time is 3-30 min.

7. The method for preparing carbon fiber composite felt mixture for carding and felting according to claim 1, characterized in that, The drying and agglomeration process described in step (3) involves drying the filtered mixed fiber material in a hot air circulating oven until the moisture content is ≤0.05% to form fiber clumps. This process is divided into two stages: the first stage involves drying at 50-90℃ until the moisture content is ≤0.05%, and the second stage involves heating to 5-15℃ below the softening point of the low melting point thermal bonding fiber and holding for 10-30 minutes. This allows the surface of the thermal bonding fiber to form point-like weak adhesion at the points of contact with other fibers, fixing fibers of different densities in a uniform distribution state during liquid phase mixing, thus achieving thermal bonding pre-locking. This weak adhesion can be gradually disintegrated under the action of the carding machine needles without affecting the opening and carding effect.

8. A carbon fiber composite felt mixture for carding and felting, prepared by the method described in any one of claims 1 to 7.

9. A method for preparing carbon fiber composite felt using the mixture as described in claim 8, characterized in that, The method involves the following steps: the mixture is fed into a carding machine through a single inlet, and then sequentially carded, laid up, reinforced layer compounded, needle-punched and consolidated, and wound up to obtain the finished carbon fiber composite felt.

10. The method for preparing carbon fiber composite felt according to claim 9, characterized in that, The carding machine is one of a single-roller carding machine, a double-roller carding machine, or a random web-forming carding machine, with a carding speed of 20-120 m / min; A pre-opening and blending device is set at the front end of the carding machine feed inlet. The pre-opening and blending device includes a low-speed needle roller opening chamber and a flow equalization guide plate. The low-speed needle roller rotates at 20-80 rpm to gently open the mixed fiber bundles. The flow equalization guide plate evenly spreads the opened fiber bundles to the full width of the feeding curtain. The reinforcing layer is one of non-woven fabric, woven fabric, knitted fabric, or unidirectional fiber mesh fabric, with a basis weight of 10-80 g / m². 2 It is combined with the carded fiber web by laying it on top and bottom or sandwiching it in the middle; The needle acupuncture process parameters are: needle density 50-300 needles / cm² 2 The needle insertion depth is 5-20 mm, the feed speed is 1-10 m / min, and the pre-needling and main needle insertion are completed at least twice.