Nonwoven fabrics, nonwoven laminates and articles

By using composite fibers and embossing processes to enhance the bulk and visual appeal of spunbond nonwoven fabrics, the softness and urine management issues of existing spunbond nonwoven fabrics in diapers are solved, making it suitable for high-end diapers and hygiene products.

CN123108844APending Publication Date: 2026-11-17TORAY ADVANCED MATERIALS KOREA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611341930.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-07-09
Filing Date
2021-07-07
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing spunbond nonwoven fabrics lack sufficient fluffiness and visual appeal when manufacturing diapers, resulting in reduced softness. They also tend to cause urine residue and leakage when in contact with a baby's skin, failing to meet the demands of the high-end diaper market.

Method used

By employing composite fiber technology, a crimped nonwoven fabric is formed by mixing first and second propylene-based polymers. Combined with embossing and deep embossing processes, the bulk and visual appeal of the nonwoven fabric are improved, and a three-dimensional shape is formed on the surface.

Benefits of technology

It achieves improved fluffiness and visual appeal of nonwoven fabrics, enhances comfort when in contact with baby's skin, reduces urine residue and leakage, and is suitable for high-end diapers and hygiene products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

A nonwoven fabric, a nonwoven laminate, and an article are disclosed. The disclosed nonwoven fabric has a sieving function value of 2.0% to 65.9% as expressed by the following mathematical formula 1: [Mathematical Formula 1] Sieving function value (%) = (final weight of powder remaining on the nonwoven fabric after sieving test) / (initial weight of powder used for sieving test) × 100.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of Chinese patent application No. 202180048343.3, filed on July 7, 2021, entitled "Nonwoven Fabric, Nonwoven Laminated Articles and Articles". Technical Field

[0002] A nonwoven fabric, a nonwoven laminate, and an article are disclosed. More specifically, a nonwoven fabric, a nonwoven laminate, and an article with improved bulk and visual appeal are disclosed. Background Technology

[0003] The final physical properties of nonwoven fabrics depend on the method of web formation and bonding.

[0004] In existing spunbond nonwoven fabric manufacturing processes, a web is formed through individual spinning or core-sheath type composite spinning. The resulting web has a simple, non-curling structure and is combined with a heated calender to form a relatively thin nonwoven fabric.

[0005] In the manufacture of diapers, thinner nonwoven fabrics are used as top and bottom sheets. However, compared to short-fiber hot-air nonwoven fabrics that are formed by carding and bonded by hot air, they suffer from a significant decrease in softness due to reduced bulk.

[0006] Furthermore, because the fabric does not curl during web formation, its fluffiness decreases. This results in a larger area of ​​the diaper directly contacting the baby's skin during manufacturing. Additionally, there is little extra space between the nonwoven fabric and the ADL (Aquisition Distribution Layer) during lamination, leading to urine residue remaining in part of the top layer during urination, causing redness or rashes on the baby's buttocks. There is also the problem of urine leaking outside the diaper.

[0007] In addition, as the market for hygiene products such as diapers becomes more premiumized, existing spunbond nonwovens have limitations in terms of improving fluffiness and visual appeal to provide differentiation. Summary of the Invention

[0008] Technical issues

[0009] One embodiment of the present invention provides a nonwoven fabric with improved bulk and visual appeal.

[0010] Another embodiment of the present invention provides a nonwoven laminate article comprising two or more of the said nonwoven fabrics.

[0011] Another embodiment of the invention provides an article comprising the aforementioned nonwoven laminate.

[0012] Technical solution

[0013] This invention provides a nonwoven fabric,

[0014] It has sieve function values ​​ranging from 2.0% to 65.9%, expressed by the following mathematical formula 1:

[0015]

Mathematical Formula 1

[0016] Sieving function value (%) = (final weight of powder remaining on the nonwoven fabric after sieving test) / (initial weight of powder used for sieving test) × 100.

[0017] The sieve function value of the nonwoven fabric can be from 2.0% to 15.7%.

[0018] In the nonwoven fabric, the average size of the pores can be from 0.411 mm to 0.833 mm.

[0019] The absorption rate of the nonwoven fabric can be from 2.0 seconds to 11.4 seconds.

[0020] The nonwoven fabric can have a hand feel measurement of 3.1 g to 5.1 g in the longitudinal (MD) direction and 1.0 g to 2.3 g in the transverse (CD) direction.

[0021] The compressive strength of the nonwoven fabric can be from 3.4 cN to 6.4 cN.

[0022] Another aspect of the present invention provides a nonwoven laminate product.

[0023] It has a two- or more-layered structure, and at least one of the layers is the nonwoven fabric.

[0024] The nonwoven fabric may be a spunbond nonwoven fabric, and the nonwoven laminate may be configured such that the spunbond nonwoven fabric is exposed only on one side of the two outer layers.

[0025] In another aspect, the present invention provides an article,

[0026] It includes the nonwoven laminated product.

[0027] The items may be diapers, absorbent materials, disposable sanitary products, defecation products, sidegathers, support layers, or top sheets.

[0028] Beneficial effects

[0029] The nonwoven fabric according to one embodiment of the present invention not only has excellent bulkiness, but also has a differentiated visual appeal, thus providing a high-end image. Detailed Implementation

[0030] The following describes in detail a nonwoven fabric according to an embodiment of the present invention.

[0031] The nonwoven fabric according to one embodiment of the present invention can have a sieve function value of 2.0% to 65.9% as expressed by the following mathematical formula 1:

[0032]

Mathematical Formula 1

[0033] Sieving function value (%) = (final weight of powder remaining on the nonwoven fabric after sieving test) / (initial weight of powder used for sieving test) × 100.

[0034] When the sieving function value is between 2.0% and 65.9%, nonwoven fabrics with improved bulk and visual appeal can be obtained.

[0035] For example, the sieve function value of the nonwoven fabric can be from 2.0% to 15.7%. When the sieve function value is from 2.0% to 15.7%, a nonwoven fabric with improved bulk and visual appeal, as well as improved absorbency and processability, can be obtained.

[0036] In the nonwoven fabric, the average size of the pores can be from 0.411 mm to 0.833 mm.

[0037] In addition, the absorption rate of the nonwoven fabric can be from 2.0 seconds to 11.4 seconds.

[0038] In addition, the hand feel tester measurement value of the nonwoven fabric in the longitudinal direction (MD) can be 3.1 g to 5.1 g, and the hand feel tester measurement value in the transverse direction (CD) can be 1.0 g to 2.3 g.

[0039] In addition, the compressive strength of the nonwoven fabric can be from 3.4 cN to 6.4 cN (centinewton).

[0040] The nonwoven fabric may include crimped composite fibers (hereinafter referred to as "composite fibers").

[0041] The composite fiber may include a first propylene-based polymer and a second propylene-based polymer.

[0042] The melting point of the second propylene polymer, as measured by differential scanning calorimetry (DSC), can be 30°C or higher than that of the first propylene polymer.

[0043] The ratio of the melt index (MFR: test temperature 230°C, load 2.16 kg) of the first propylene polymer and the second propylene polymer, as measured according to ASTM D1238 (second propylene polymer / first propylene polymer), can be greater than or equal to 1.5.

[0044] For example, the melting point of the first propylene polymer may be 30°C to 60°C or 30°C to 100°C higher than the melting point of the second propylene polymer.

[0045] For example, the melt index ratio (second propylene polymer / first propylene polymer) may be 1.7 to 2.0, 1.7 to 3.0, or 1.7 to 4.0.

[0046] The first propylene polymer and the second propylene polymer are uniformly mixed or arranged to actually occupy their respective regions within the cross-section of the composite fiber and continuously elongated along the length direction. At least one component of the first propylene polymer and the second propylene polymer can continuously form at least a portion of the outer peripheral surface along the length direction of the composite fiber.

[0047] The first propylene-based polymer and the second propylene-based polymer may each independently use a homopolymer of propylene or propylene as the main structural unit component, and may be copolymers of propylene with one, two or more of α-olefins having 2 to 20, preferably 2 to 8, carbon atoms, such as ethylene, 1-butene, 1-pentene, 1-hexene, 1-octene, and 4-methyl-1-pentene. For example, the first propylene-based polymer and the second propylene-based polymer may each independently be a homopolymer or a propylene-ethylene random copolymer having an ethylene unit component content of 0 mol% to 10 mol% and an MFR of 20 g / 10 min to 200 g / 10 min.

[0048] In particular, since a nonwoven fabric comprising composite fibers with excellent bulk and softness can be obtained, the first propylene-based polymer can be a propylene homopolymer, the second propylene-based polymer can be a random copolymer of propylene and a small amount of ethylene, and the content of the ethylene unit component can be less than or equal to 10 mol%, for example, from 1 mol% to 10 mol%. Furthermore, the content of the ethylene unit component is determined by 13C-NMR spectroscopy using conventional methods.

[0049] In addition to the propylene-based polymer component as the main component, the first propylene-based polymer may further include 1% to 5% by weight of a nucleating agent, thereby the crystallization temperature of the first propylene-based polymer may be 19°C or higher than the crystallization temperature of the second propylene-based polymer.

[0050] The melting point of the first propylene-based polymer can be in the range of 120°C to 175°C, and the melting point of the second propylene-based polymer can be in the range of 110°C to 155°C. Furthermore, as mentioned above, the difference in melting points between the two components can be greater than or equal to 30°C, 30°C to 60°C, or 30°C to 100°C.

[0051] The nonwoven fabric may include 70 to 90 parts by weight of fibers formed by spinning the first propylene polymer and 10 to 30 parts by weight of fibers formed by spinning the second propylene polymer.

[0052] The nonwoven fabric has an OPU of less than or equal to 0.7%, and therefore the nonwoven fabric can have a rewetting index of less than or equal to 5.0 and a water durability absorption of less than 10 seconds.

[0053] The hydrophilic agent may include wax emulsions, active softeners, organosilicon compounds, surfactants, or combinations thereof. The organosilicon compound may include amino-containing organosilicones, oxidized alkenyl-containing organosilicones, or combinations thereof. The surfactant may include anionic surfactants such as carboxylate anionic surfactants, sulfonate anionic surfactants, sulfate anionic surfactants, and phosphate anionic surfactants (particularly alkyl phosphate salts); polyol monofatty acid esters such as dehydrated sorbitol fatty acid esters, diethylene glycol monostearate, diethylene glycol monooleate, glyceryl monostearate, glyceryl monooleate, and propylene glycol monostearate; N-(3-oleoyloxy-2-hydroxypropyl)diethanolamine; polyoxyethylene hydrogenated castor oil; and polyoxyethylene sorbitol beeswax. Nonionic surfactants such as polyoxyethylene sorbitol sesquistearate, polyoxyethylene monooleate, polyoxyethylene sorbitol sesquistearate, polyoxyethylene glycerol monooleate, polyoxyethylene monostearate, polyoxyethylene monolaurate, polyoxyethylene monooleate, polyoxyethylene hexadecyl ether, and polyoxyethylene lauryl ether; cationic surfactants such as quaternary ammonium salts, amine salts, or amines; aliphatic derivatives of secondary or tertiary amines containing carboxyl groups, sulfonates, and sulfates, or aliphatic derivatives of heterocyclic secondary or tertiary amines; or combinations thereof.

[0054] Specifically, the hydrophilic agent can be a nonionic hydrophilic agent.

[0055] The nonionic hydrophilic agent may include organosilicon compounds such as amino-containing organosilicon and oxidized alkenyl-containing organosilicon; polyol monofatty acid esters such as dehydrated sorbitol fatty acid ester, diethylene glycol monostearate, diethylene glycol monooleate, glyceryl monostearate, glyceryl monooleate, and propylene glycol monostearate; N-(3-oleoxy-2-hydroxypropyl)diethanolamine, polyoxyethylene hydrogenated castor oil, polyoxyethylene sorbitan beeswax, polyoxyethylene sorbitol sesquistearate, polyoxyethylene monooleate, polyoxyethylene sorbitol sesquistearate, polyoxyethylene glyceryl monooleate, polyoxyethylene monostearate, polyoxyethylene monolaurate, polyoxyethylene monooleate, polyoxyethylene hexadecyl ether, and polyoxyethylene lauryl ether; or combinations thereof.

[0056] More specifically, the nonionic hydrophilic agent may include a surfactant (i.e., a nonionic surfactant) with a solid content greater than or equal to 90% by weight.

[0057] The average diameter of the composite fiber can be from 1 μm to 50 μm.

[0058] The first propylene-based polymer and the second propylene-based polymer can be manufactured using a highly stereoregular polymerization catalyst.

[0059] The highly stereoregular polymerization catalyst may include a diester catalyst, a succinic acid catalyst, a metallocene catalyst, or a combination thereof.

[0060] In addition to the propylene-based polymer component as the main component, the first propylene-based polymer further includes the nucleating agent, which can increase the crystallization temperature of the first propylene-based polymer so that it is different from the crystallization temperature of the second propylene-based polymer, thereby improving the thickness of the nonwoven fabric caused by curling, and further improving the softness and fluffiness of the nonwoven fabric.

[0061] The nucleating agent may include granular additives, self-assembling nucleating agents, reactive nucleating agents, or combinations thereof. The granular additives may include sodium benzoate, titanium dioxide, silicon dioxide, nanoclay, sodium salts, calcium titanate, metal oxides, metal hydroxides, or combinations thereof. The self-assembling nucleating agents may include bis(p-methylbenzyl)sorbitol, dibenzyl sorbitol, monomethylbenzyl sorbitol (MBS), bis(p-methylbenzyl)sorbitol, their derivatives, or combinations thereof. The reactive nucleating agent may include metal salts, 4-biphenylcarboxylic acid, 4-biphenylmethanol, adipic acid, or combinations thereof.

[0062] Nonwoven fabrics comprising the composite fibers can be obtained by conventional composite melt spinning methods without the use of special equipment; for example, they can be spunbond nonwoven fabrics manufactured by superior spunbonding.

[0063] The following describes in detail a method for manufacturing a nonwoven fabric according to an embodiment of the present invention.

[0064] A method for manufacturing nonwoven fabric according to an embodiment of the present invention may include the following steps:

[0065] S10, the first propylene-based polymer and the second propylene-based polymer are melted in each region at a temperature of 180°C to 250°C using the same extruder to form a melt;

[0066] S20, the melt is discharged through a spinneret with a separate spinning nozzle; and

[0067] S30, each melt being discharged through a diffuser.

[0068] In addition, the method for manufacturing the nonwoven fabric may further include step S40, which adds mechanical properties to the nonwoven fabric formed in step S30 by embossing using heated embossing rollers or by high-temperature ventilated heat welding.

[0069] For example, the embossing process can be performed under conditions where the adhesion ratio (i.e., embossing area ratio) is less than or equal to 13%, and the non-embossed unit area is greater than or equal to 0.2 mm², for example, between 0.2 mm² and 0.7 mm². Here, the non-embossed unit area refers to the maximum area of ​​the square inscribed within the smallest unit of non-embossed area surrounded by embossed portions. When embossing is performed under the above-mentioned conditions, a nonwoven fabric with further increased bulk can be obtained while maintaining the desired nonwoven fabric strength.

[0070] The adhesion rate and non-embossed unit area can be adjusted by changing the embossing pattern.

[0071] After the embossing process, the nonwoven fabric may include embossed and non-embossed portions. The embossed portion may include a plurality of unit embossed pattern portions of open embossing type arranged continuously at the same or different intervals.

[0072] In addition, the area of ​​each embossed pattern included in the unit embossed pattern portion can be from 0.2 mm² to 0.7 mm².

[0073] In addition, the method for manufacturing the nonwoven fabric may further include step S50, in which the nonwoven fabric formed in step S40 is supplied to a post-processing device and a deep embossed shape is added to it by a processing roller, thereby providing a three-dimensional shape on the surface of the nonwoven fabric.

[0074] In step S50, the processing rollers of the post-processing equipment can be configured to perform deep embossing at 10 to 50 holes per inch to give the nonwoven fabric a thickness of 0.3 mm to 0.7 mm. Through this post-processing in step S50, the softness and bulkiness of the final manufactured nonwoven fabric can be further improved.

[0075] The nonwoven fabric of the composite fiber may further include 0.01% to 3% by weight of a fatty acid amide having 5 to 25 carbon atoms, based on the total weight of the nonwoven fabric.

[0076] The fatty acid amide can act as a slip agent.

[0077] The fatty acid amide may include oleamide, erucamide, stearamide, or a combination thereof.

[0078] In addition to the first and second propylene-based polymers, the composite fiber may contain other components as needed without prejudice to the purpose of the invention. These other components may include known heat stabilizers, weather stabilizers, various stabilizers, antistatic agents, antiblocking agents, antifogging agents, fillers, dyes, pigments, natural oils, synthetic oils, waxes, or combinations thereof.

[0079] The stabilizer may include antioxidants such as 2,6-di-tert-butyl-p-cresol (BHT), phenolic antioxidants such as tetra[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, alkyl esters of β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, and 2,2'-oxamidobis[ethyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], fatty acid metal salts such as zinc stearate, calcium stearate, and 1,2-hydroxycalcium stearate, polyol fatty acid esters such as glyceryl monostearate, glyceryl distearate, pentaerythritol monostearate, pentaerythritol distearate, and pentaerythritol tripearate, or combinations thereof.

[0080] The filler may include silica, diatomaceous earth, alumina, titanium dioxide, magnesium oxide, pumice powder, hollow pumice spheres, aluminum hydroxide, magnesium hydroxide, basic magnesium carbonate, dolomite, calcium sulfate, potassium titanate, barium sulfate, calcium sulfite, talc, clay, mica, asbestos, calcium silicate, montmorillonite, bentonite, graphite, aluminum powder, molybdenum sulfide, or combinations thereof.

[0081] The aforementioned propylene-based polymer, along with any other components used as needed, can be mixed using known methods.

[0082] The composite fiber can be a mono, core / sheath, side-by-side, or sandwitch type composite fiber.

[0083] The following describes in detail a nonwoven laminate product according to an embodiment of the present invention.

[0084] According to one embodiment of the present invention, a nonwoven laminate is a laminate having a structure of at least two or more layers, wherein at least one layer may be the aforementioned nonwoven fabric.

[0085] The nonwoven laminated product may include spunbond nonwoven fabric in the nonwoven fabric.

[0086] For example, the nonwoven fabric of the crimped composite fiber can be a spunbond nonwoven fabric, and the nonwoven laminate can be configured such that the spunbond nonwoven fabric is exposed only on one side of the two outer layers.

[0087] Furthermore, the nonwoven laminate can be formed by laminating four spunbond nonwoven fabrics, in which case the uniformity (CV%) of the nonwoven laminate can be less than or equal to 3%. In this specification, "uniformity (CV%)" refers to the percentage of the weight deviation of the 30 test pieces divided by the average weight of the plurality of test pieces after the nonwoven laminate is cut into 30 test pieces of 1㎡ size.

[0088] The thickness of the nonwoven laminate formed by stacking four spunbond nonwoven fabric layers can be greater than or equal to 0.02 mm, the number of curls greater than or equal to 10 curls / 10 mm, the adhesion rate less than or equal to 13%, and the MD stiffness, which represents the softness of the nonwoven laminate, can be less than or equal to 40 mm. In this specification, "MD stiffness" refers to the bending deformation of the nonwoven laminate in the mechanical direction (i.e., the degree of bending of the nonwoven laminate).

[0089] The following describes in detail an article according to an embodiment of the present invention.

[0090] Articles according to one embodiment of the present invention include the above-described nonwoven laminate articles.

[0091] The items may be diapers, absorbent materials, disposable sanitary products, defecation products, sidegathers, support layers, or top sheets.

[0092] When the article is a diaper, the hydrophilic agent impregnation amount (OPU: Oil Pick-UP) of the nonwoven laminate is less than or equal to 0.7%, so when applied to the top layer of the diaper, the durable water absorption rate can be less than or equal to 10 seconds.

[0093] The amount of hydrophilic agent impregnation (OPU) can be calculated according to the following mathematical formula 1.

[0094]

Mathematical Formula 1

[0095] OPU (%) = (W1-W0) / W0×100

[0096] In the formula, W0 is the weight of the nonwoven laminate without hydrophilic agent, and W1 is the weight of the nonwoven laminate with hydrophilic agent. Furthermore, in the mathematical formula 1, W1 is the weight of the nonwoven laminate without hydrophilic agent plus the weight of the solid component of the hydrophilic agent.

[0097] The present invention will now be described in detail through embodiments. These embodiments are intended to further describe the present invention in detail, but the scope of the present invention is not limited thereto.

[0098] Example 1: Manufacturing nonwoven fabric

[0099] First, 88 parts by weight of a first propylene-based polymer and 12 parts by weight of a second propylene-based polymer are melted in each region of the same extruder at a temperature of 180°C to 250°C to form a melt. Then, each melt is discharged through a spinneret with a separate spinning nozzle. The discharged melt is then discharged through a diffuser with a cross-sectional shape. Mechanical properties are then added to the formed nonwoven fabric by embossing using heated embossing rollers. Then, as a post-processing step, the formed nonwoven fabric is supplied to a post-processing device, where it is given a deep embossed shape by processing rollers, thereby providing a three-dimensional shape on the surface of the nonwoven fabric. During this post-processing, the processing rollers are maintained at 137°C. The processing rollers of the post-processing device are equipped with a first roller having multiple pins and a second roller having multiple holes formed at positions corresponding to the pins on the first roller, thereby providing a three-dimensional shape on the surface of the nonwoven fabric through deep embossing with perforated holes. The first propylene-based polymer is a propylene homopolymer (LG Chem, H7700), and the second propylene-based polymer is an elastic random copolymer of ethylene and polypropylene (Exxon Mobile Vistamaxx7020, ethylene unit content: 15.0 mol%).

[0100] Example 2: Manufacturing nonwoven fabric

[0101] Except that the processing rollers were kept at 130°C during the post-processing, the nonwoven fabric was manufactured using the same method as in Example 1.

[0102] Example 3: Manufacturing nonwoven fabric

[0103] Except that the processing rollers were kept at 120°C during the post-processing, the nonwoven fabric was manufactured using the same method as in Example 1.

[0104] Example 4: Manufacturing nonwoven fabric

[0105] Except that the processing rollers were kept at 127°C during the post-processing, the nonwoven fabric was manufactured using the same method as in Example 1.

[0106] Comparative Example 1: Manufacturing Nonwoven Fabrics

[0107] Except that the processing rollers were kept at 140°C during the post-processing, the nonwoven fabric was manufactured using the same method as in Example 1.

[0108] Comparative Example 2: Manufacturing Nonwoven Fabrics

[0109] Except that the processing rollers were kept at 100°C during the post-processing, the nonwoven fabric was manufactured using the same method as in Example 1.

[0110] Evaluation example: Evaluating the physical properties of nonwoven fabrics

[0111] The physical properties of each nonwoven fabric manufactured in Examples 1 to 4 and Comparative Examples 1 to 2 were evaluated using the following methods, and the results are shown in Table 1 below.

[0112] (1) Screening function value: Measured according to the following method.

[0113] 1) Prepare the sample material (non-woven fabric, size 175 mm × 150 mm).

[0114] 2) Measure the weight at the bottom of the collector.

[0115] 3) Place the sample between the sieve collector and the bottom of the collector, and secure it with a rubber ring.

[0116] 4) Assemble the sieve collector, sample, and collector bottom (equipment name: AS200Analytical Sieve Shakers, made in Germany) fixed with rubber rings into the equipment.

[0117] 5) Accurately weigh 20 g of glass bead powder (manufacturer: Mondi Lembacel Betheniville) using a balance and pour it into a sieve collector. The particle size distribution of the glass bead powder is as follows:

[0118] The content of particles with a diameter of 0.045 mm to 0.060 mm is 3.1% by weight.

[0119] The content of particles with a diameter of 0.061 mm to 0.075 mm is 10.9% by weight.

[0120] The content of particles with a diameter of 0.076 mm to 0.090 mm is 14.1% by weight.

[0121] The content of particles with a diameter of 0.091 mm to 0.105 mm was 39.9%.

[0122] The content of particles with a diameter of 0.106 mm to 0.120 mm was 28.1%.

[0123] The content of particles with a diameter of 0.121 mm to 0.135 mm is 3.1% by weight, and

[0124] The content of particles with a diameter of 0.136 mm to 0.150 mm is 0.8% by weight.

[0125] 6) Measure the weight at the bottom of the separator (= powder + bottom of separator).

[0126] 7) Calculate the sieving function value according to the following formula 1:

[0127] (Final weight remaining on the nonwoven fabric) / (20 g) × 100

[0128] ={20 g - (weight of collector bottom after test - weight of collector bottom before test)} / 20 g × 100

[0129] (2) Thickness (mm): Measured according to the block thickness measurement method (KSK 0506 method). The thickness of nonwoven fabric is an indicator of bulkiness.

[0130] (3) Average size of holes: The average size of the major and minor axes was measured in mm using an optical microscope at 25x magnification. The average size of the holes in the nonwoven fabric is a visual indicator.

[0131] (4) Absorbance: Measured according to WSP 70.3.

[0132] (5) Hand feel tester measurement (g): Measured according to WSP 90.3. The hand feel tester measurement value of nonwoven fabric is an indicator of softness.

[0133] (6) Compressive strength: Measured according to JIS P 8126. The compressive strength of nonwoven fabric is another indicator of its softness.

[0134] [Table 1]

[0135]

[0136] In addition, the required physical properties of the nonwoven fabric that meet the purpose of this invention are shown in Table 2 below.

[0137] [Table 2]

[0138]

[0139] Referring to Tables 1 and 2 above, the nonwoven fabrics manufactured in Examples 1 to 4 satisfy all the physical properties required for nonwoven fabrics that meet the objectives of the present invention. In contrast, the nonwoven fabrics manufactured in Comparative Examples 1 to 2 do not satisfy at least one of the physical properties required for nonwoven fabrics that meet the objectives of the present invention.

[0140] Although the invention has been described with reference to embodiments, these are merely exemplary, and those skilled in the art will understand that various modifications and equivalent embodiments can be made therefrom. Therefore, the true scope of protection of the invention should be determined by the technical concept of the appended claims.

Claims

1. A nonwoven fabric having a plurality of pores formed thereon and having a sieving function value of 2.0% to 65.9% as expressed by the following mathematical formula 1, wherein the thickness of the nonwoven fabric is 0.3 to 0.7 mm: 【Mathematical Formula 1】 Sieving function value (%) = (Final weight of powder remaining on the nonwoven fabric after sieving test) / (Initial weight of powder used for sieving test) × 100 The nonwoven fabric comprises crimped composite fibers, which include a first propylene-based polymer and a second propylene-based polymer. The melting point of the second propylene-based polymer, as measured by differential scanning calorimetry (DSC), is at least 30°C higher than that of the first propylene-based polymer. Furthermore, the ratio of the melt flow rate (MFR) of the first propylene-based polymer to the second propylene-based polymer (second propylene-based polymer / first propylene-based polymer), as measured according to ASTM D1238 (measurement temperature 230°C, load 2.16 kg), is at least 1.

5. The sieving function value was determined after sieving tests using glass beads with the following particle size distribution: The content of particles with a diameter of 0.045 mm to 0.060 mm is 3.1% by weight. The content of particles with a diameter of 0.061 mm to 0.075 mm was 10.9% by weight. The content of particles with a diameter of 0.076 mm to 0.090 mm was 14.1% by weight. The content of particles with a diameter of 0.091 mm to 0.105 mm was 39.9%. The content of particles with a diameter of 0.106 mm to 0.120 mm was 28.1%. The content of particles with a diameter of 0.121 mm to 0.135 mm was 3.1% by weight, and The content of particles with a diameter of 0.136 mm to 0.150 mm is 0.8% by weight. wherein The average size of the holes is between 0.411 mm and 0.833 mm.

2. The nonwoven fabric according to claim 1, wherein The sieving function value ranges from 2.0% to 15.7%.

3. The nonwoven fabric according to claim 1, wherein Its absorption time is 2.0 seconds to 11.4 seconds.

4. The nonwoven fabric according to claim 1, wherein Its longitudinal tactile tester measurements ranged from 3.1 g to 5.1 g, and its transverse tactile tester measurements ranged from 1.0 g to 2.3 g.

5. The nonwoven fabric according to claim 1, wherein Its compressive strength ranges from 3.4 cN to 6.4 cN.

6. A nonwoven laminated article having a two- or more-layer structure, wherein at least one layer is a nonwoven fabric according to any one of claims 1 to 6.

7. The nonwoven laminate product according to claim 6, wherein, The nonwoven fabric is a spunbond nonwoven fabric, and the nonwoven laminate is configured such that the spunbond nonwoven fabric is exposed only on one side of the two outer layers.

8. An article comprising a nonwoven laminate according to claim 7.

9. The article of claim 8, wherein, The items are diapers, absorbent materials, disposable sanitary products, defecation supplies, side pleats, support layers, or top sheets.