A plasma modification device and modification process integrated into a polyarylate melt spinning production line

By integrating plasma modification equipment and processes into the polyarylate melt spinning production line, the problems of process interruption and inert protection in TLCP fiber modification have been solved, achieving efficient and continuous fiber modification, improving interfacial bonding performance and bulk strength, and meeting the performance requirements of high-end composite materials.

CN123108924APending Publication Date: 2026-11-17JIANGXI LIDE FIBER CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611563737.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing TLCP fiber modification technologies suffer from fragmented processes, lack of inert protection, limited methods, and an inability to balance interfacial properties and bulk strength, making it difficult to meet the performance requirements of high-end composite materials.

Method used

The plasma modification device, integrated into the polyaryl ester melt spinning production line, utilizes an integrated process including an adaptive tension yarn guiding mechanism, a nitrogen micro-positive pressure plasma activation chamber, a nano-auxiliary agent ultrasonic atomization blending unit, and a constant temperature hot air curing module. This process enables the fiber to be activated and cured in situ under an inert atmosphere, avoiding high-temperature oxidation and embrittlement, and improving interfacial bonding performance.

Benefits of technology

It achieves efficient and continuous fiber modification, improves production efficiency and yield, retains high fiber strength, significantly improves interfacial bonding performance, has low environmental cost, and strong adaptability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108924A_ABST
    Figure CN123108924A_ABST
Patent Text Reader

Abstract

This invention discloses a plasma modification device and process integrated into a polyarylate melt spinning production line. The device is directly connected to the outlet of the hot drawing and setting machine via a standard flange. Along the yarn feeding direction, it sequentially and in series includes an adaptive tension yarn feeding guide mechanism, a nitrogen micro-positive pressure low-temperature plasma activation chamber, a nano-auxiliary agent ultrasonic atomization blending unit, a constant temperature hot air curing module, and a trace waste gas recovery and purification unit. These units are seamlessly connected to form a continuous channel without any breaks or exposed filaments. The heat-set TLCP filament is directly fed into the device, undergoes sequential plasma activation under nitrogen protection, ester-nano composite agent atomization coating, and hot air curing, and is then directly wound up, achieving continuous spinning-modification. Compared to unmodified filament, the modified fiber maintains excellent bulk strength while significantly improving its interfacial bonding performance with epoxy resin, making it suitable for the continuous preparation of high-end reinforcing fibers for aerospace and military insulation applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-performance chemical fiber technology, specifically relating to a plasma modification device and modification process integrated into a polyarylate melt spinning production line. Background Technology

[0002] Thermotropic liquid crystal polyarylate (TLCP) filaments possess excellent properties such as high strength, high modulus, high temperature resistance, and low dielectric constant, making them a core reinforcing material for lightweight load-bearing components in aerospace and high-frequency communication substrates. However, the strong chemical inertness, lack of active functional groups, and low surface free energy of TLCP fibers result in insufficient interfacial bonding with matrix resins such as epoxy resin and bismaleimide resin. This leads to the interlaminar shear strength of the composite material failing to meet the requirements of high-end applications. Therefore, surface modification treatment of TLCP fibers is necessary to improve their interfacial compatibility with the resin matrix.

[0003] Existing surface modification technologies mainly fall into two categories: solvent grafting and plasma treatment. For example, CN113788975A uses an organic amine solvent combined with ultraviolet grafting to perform offline batch impregnation treatment of finished fibers. While this can introduce specific functional groups, the process is disconnected from the main spinning line, requiring repeated winding and transfer of fibers, resulting in low production efficiency and high environmental disposal costs due to the large amount of organic solvents used. Another example is CN113737510A, which employs a cold plasma treatment scheme. The equipment is located independently of the spinning production line, and the fibers also require offline secondary feeding and processing. Furthermore, surface roughening and activation are only performed in an air atmosphere, lacking inert gas protection. During high-temperature treatment, the fibers are prone to oxidation and embrittlement. After activation, there is a lack of auxiliary agent coating and immediate curing, and the introduced polar groups experience time-dependent decay, with activity decreasing over time. These methods are simplistic, relying solely on solution grafting or plasma roughening, lacking the synergistic effect of in-situ curing with auxiliary agents, and thus offering limited interface improvement. Other methods, such as surface coating and sizing, and high-energy irradiation, are also offline processes that cannot be continuously integrated with the spinning main line. Repeated unwinding and rewinding of the fiber bundle can easily cause fuzz and surface damage, making it difficult to balance interfacial performance and bulk strength. In summary, existing TLCP fiber modification technologies suffer from four main drawbacks: fragmented processes, lack of inert protection, limited methods, and poor adaptability. The strength retention rate and interfacial improvement of modified fibers are both at a low level, making it difficult to balance interfacial bonding performance and fiber bulk strength, and thus failing to meet the high-performance requirements of military composite materials.

[0004] Therefore, there is an urgent need for an in-situ continuous modification scheme that can be directly connected to the polyarylate melt spinning production line, complete plasma activation and immediate in-situ solidification under the protection of an inert atmosphere, and is compatible with high-speed continuous spinning. Summary of the Invention

[0005] The purpose of this invention is to provide a plasma modification device and modification process integrated into a polyaryl filament melt spinning production line, in order to solve the problems in the existing polyaryl filament surface modification, such as the modification process being separated from the spinning process and requiring offline winding and transportation, lack of inert atmosphere protection leading to high-temperature filament oxidation and embrittlement, single modification method making it difficult to balance interface performance and bulk strength, lack of in-situ curing after activation leading to activity decay, and easy filament deviation and breakage at high speeds, while also achieving the collection and purification of trace amounts of waste gas.

[0006] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0007] This invention provides a plasma modification process integrated into a polyarylate melt spinning production line, comprising the following steps:

[0008] S1. The heat-set TLCP filament is fed from the discharge end of the box roller integrated hot air circulation stretching and setting machine into the plasma modification device through the standard flange interface. The adaptive tension feeding guide mechanism automatically maintains the constant tension of the filament bundle and synchronizes it with the feeding speed of the spinning main line through a closed-loop control system composed of an online tension sensor and a damping adjustable guide roller. No winding or transfer operation is performed throughout the process.

[0009] S2. The long filament bundle enters the nitrogen micro-positive pressure plasma activation chamber at a constant speed through the adaptive tension wire feeding guide mechanism. Dry nitrogen is introduced into the chamber to maintain micro-positive pressure and air is isolated by sealing the wire guide holes through the inlet and outlet. Plasma activation treatment is carried out under nitrogen inert protection to obtain the activated filament bundle.

[0010] S3. The activated filament bundles continuously enter the ultrasonic atomization and blending unit of nano-auxiliaries, so that the ester-nano composite additives are uniformly attached to the surface of the filament bundles.

[0011] S4. The fiber bundles with the additives attached then enter the constant temperature hot air curing module for in-situ curing to obtain modified fiber bundles.

[0012] S5. After modification, the filament bundles are directly fed into the finished product winding section to produce high interfacial bonding polyarylate filaments in one go; the trace amounts of auxiliary decomposition gases generated in each unit cavity are collected by the trace waste gas recovery and purification unit and discharged after being harmlessly adsorbed by activated carbon.

[0013] Optionally, the adaptive tension guiding mechanism in S1 consists of a closed-loop control system composed of multiple sets of adjustable damping guide rollers and online tension sensors. The online tension sensors detect and feedback the yarn tension in real time. The closed-loop control system compares the measured tension value with the set tension value and adjusts the damping of the adjustable damping guide rollers according to the deviation, so as to keep the yarn tension constant and thus keep the yarn speed in the modification device synchronized with the yarn speed of the spinning main line. Since the yarn needs to pass through multiple series cavities in sequence, the yarn resistance of each unit is different, and the tension is prone to accumulate along the way and generate local stress concentration. Through this closed-loop control mechanism, tension fluctuations can be compensated in real time when the yarn speed changes, eliminating yarn deviation and local stress concentration during high-speed yarn feeding, effectively avoiding yarn breakage caused by tension fluctuations, and ensuring speed matching and stable synchronous operation between the modification device and the spinning main line.

[0014] Optionally, the nitrogen micro-positive pressure low-temperature plasma activation chamber in S2 is a fully enclosed chamber structure with sealed guide holes at its inlet and outlet to prevent nitrogen leakage and air backflow. The chamber is connected to a nitrogen supply pipeline to continuously supply dry nitrogen to maintain a micro-positive pressure and prevent external air from seeping in. The sealed guide holes effectively maintain the airtightness of the chamber while allowing the fiber bundle to pass smoothly. The oxygen-free environment created by the dry nitrogen can prevent oxidative embrittlement of TLCP fibers during high-temperature activation, ensuring the stable preservation of the fiber's strength.

[0015] Optionally, the nitrogen micro-positive pressure low-temperature plasma activation chamber in S2 is equipped with a low-temperature plasma generator, which generates high-energy N2 from the low-temperature nitrogen plasma. + Excited nitrogen molecules, electrons, and other active particles bombard the fiber surface, causing the ester and CO bonds in the polyarylate molecular chain to break and generate hydroxyl and carboxyl active functional groups, while also producing active surface free radicals.

[0016] Optionally, the power of the low-temperature plasma generator described in S2 is 1000~1600W.

[0017] Optionally, the ultrasonic atomization blending unit for nano-additives described in S3 has an ultrasonic atomization nozzle built in, which is used to uniformly atomize the additive mixture and spray it onto the activated filament surface. The ultrasonic atomization method can break the additive mixture into micron-sized droplets, so that the additives form a uniform thin layer coating on the filament surface, effectively avoiding problems such as additive dripping and uneven coating in traditional dip coating or spraying methods, and ensuring batch stability and uniformity of the modification effect.

[0018] Optionally, the additive mixture in S3 is a mixture of ester compatibilizer and nano antioxidant, wherein the ester compatibilizer is one or more of epoxy modified fatty acid ester and aromatic polyester compatibilizer; the nano antioxidant is one or more of nano cerium dioxide and nano zinc oxide, and the average particle size of the nano antioxidant is 20~80nm; the mass ratio is ester compatibilizer: nano antioxidant = (70~90):(10~30); further, the mass ratio is (80~90):(10~20).

[0019] Optionally, the constant-temperature hot air curing module in S4 has a constant-temperature circulating hot air duct for rapidly curing the modified layer formed by the auxiliary agent on the fiber surface. The hot air temperature is linked to the yarn feed speed to ensure complete curing without damaging the fiber itself. Since the polar groups introduced by plasma activation have a time-dependent decay, setting the atomization coating and hot air curing in series immediately after the activation process allows the auxiliary agent to form a film and lock it in before the activity decays, so that the activation effect and the auxiliary agent coating form a synergy rather than a simple succession.

[0020] Optionally, the hot air temperature of the constant temperature hot air curing module in S4 is 275~285℃; further, the hot air temperature is 275~280℃.

[0021] Optionally, the trace waste gas recovery and purification unit described in S5 is connected to the sealed cavity of each unit to collect the decomposition gas of the additives and discharge it after adsorption by activated carbon. This invention does not use organic solvents throughout the process; the waste gas contains only trace amounts of volatile organic compounds produced by the decomposition of ester additives, which can be discharged in compliance with standards after adsorption by activated carbon. It eliminates the need for a complex exhaust gas treatment system, has low environmental disposal costs, is easy to operate, and has good feasibility for industrial application.

[0022] Optionally, in step S1, the wire feeding speed is 50~120m / min, and further, the wire feeding speed is 50~100m / min.

[0023] Optionally, in step S2, the nitrogen micro-positive pressure is 0.04~0.06 kPa; further, the nitrogen micro-positive pressure is 0.04~0.05 kPa.

[0024] Optionally, in step S2, the activation dwell time is 3-8 seconds; further, the activation dwell time is 5-8 seconds.

[0025] This invention provides a plasma modification device integrated into a polyarylate melt spinning production line, comprising:

[0026] The device is directly connected to the outlet of the hot drawing and shaping machine via a standard flange. Along the direction of the filament bundle, it is sequentially sealed and connected in series with an adaptive tension wire guiding mechanism, a nitrogen micro-positive pressure low-temperature plasma activation chamber, a nano-additive ultrasonic atomization blending unit, a constant temperature hot air curing module, and a trace waste gas recovery and purification unit.

[0027] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0028] 1. Improved production efficiency and yield, highly integrated process: Direct connection to the spinning main line eliminates intermediate processes such as winding, transfer, and secondary feeding, avoiding surface scratches and fuzz defects caused by repeated winding and unwinding in offline processes, resulting in a significant improvement in product quality.

[0029] 2. Near-zero mechanical property degradation and improved high-temperature oxidation: The slight positive pressure of nitrogen can effectively isolate external air and inhibit high-temperature oxidation and embrittlement, thus maintaining the basic strength of the bulk material and improving the problem of mechanical property degradation during the high-temperature modification of TLCP.

[0030] 3. Synergistic improvement in interfacial bonding performance, superior to single modification: The synergistic effect of plasma activation and in-situ co-curing of additives significantly improves the interfacial bonding strength compared to single plasma roughening and single solvent grafting schemes.

[0031] 4. Green and solvent-free, significantly reducing environmental costs: No alcohols, ketones, or amines are used throughout the process. Only trace amounts of ester auxiliaries are atomized. Waste gas can be discharged in compliance with standards after simple activated carbon adsorption. The environmental treatment cost is lower than that of wet offline processes. There is no solvent residue, and the fiber's high temperature resistance and aging resistance do not decline.

[0032] 5. Strong adaptability to production lines: The device can be directly connected to the discharge port of the integrated hot air circulation stretching and setting machine through a standard flange interface. It can achieve in-situ connection using the existing equipment interface without modifying the core equipment of the front spinning and back spinning, or adding offline winding and unwinding and transfer mechanisms. It can directly build a continuous modification channel on the existing production line and has good adaptability to production lines with different production capacity scales. Attached Figure Description

[0033] Figure 1 This is a schematic diagram of the overall docking and assembly of the plasma modification device and the hot drawing and shaping machine. The diagram shows the standard flange docking interface and the series sequence of each unit. Among them, the adaptive tension wire feeding guide mechanism is 1; the nitrogen micro-positive pressure plasma activation chamber is 2; the nano-additive ultrasonic atomization blending unit is 3; the constant temperature hot air curing module is 4; and the trace waste gas recovery and purification unit is 5.

[0034] Figure 2 This is a cross-sectional structural diagram of the internal cavity, wire guide, and atomization unit of the modification device; the diagram shows the nitrogen inlet, plasma electrode, atomization nozzle, sealed wire guide hole, and multiple wire guide rollers.

[0035] Figure 3 A schematic diagram of the complete process flow and linkage control logic for in-situ continuous modification of polyarylate spinning.

[0036] Figure 4Schematic diagram of a plasma modification structure device;

[0037] The above figures include the following reference numerals:

[0038] 1. Adaptive tension wire guiding mechanism; 1-1. Damped adjustable guide roller; 1-2. Online tension sensor; 2. Plasma activation chamber; 2-1. Sealed guide hole; 2-2. Plasma electrode; 2-3. Nitrogen inlet; 2-4. Reversible guide roller; 3. Nano-additive ultrasonic atomization blending unit; 3-1. Ultrasonic atomization nozzle; 4. Constant temperature hot air curing module; 5. Micro-waste gas recovery and purification unit; 5-1. Exhaust fan; 5-2. Activated carbon adsorption box; 6. Hot drawing and setting machine; 7. Wire bundle; 8. Standard flange; 9. Finished product winding. Detailed Implementation

[0039] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Unless otherwise defined, the technical or scientific terms used herein should have the ordinary meaning understood by those skilled in the art. The terms "comprising" and similar expressions used herein mean that the element or object preceding the word covers the element or object listed after the word and its equivalents, but does not exclude other elements or objects.

[0040] In this invention, the following embodiments are provided to better illustrate the invention and are not intended to limit the scope of the invention. Unless otherwise specified, the materials, reagents, etc., used in the following embodiments are commercially available.

[0041] I. Testing and Characterization Methods

[0042] The modified filaments obtained in the various embodiments and comparative examples of this invention were tested and characterized using the following methods:

[0043] Breaking strength and breaking strength retention rate: Determined according to GB / T14344 "Test Method for Tensile Properties of Chemical Fiber Filaments". Breaking strength is calculated according to the following formula, and the result is expressed as cN / dtex:

[0044]

[0045] In the formula, σ: fracture strength, cN / dtex; F: fracture force, cN; T t Linear density, dtex.

[0046] The tensile strength retention rate was calculated using the same batch of unmodified TLCP precursor yarn (Comparative Example 8, 29.5 cN / dtex) as a benchmark, according to the following formula:

[0047]

[0048] In the formula, R: fracture strength retention rate, %; σ m σ0: Breaking strength of modified filament, cN / dtex; σ0: Breaking strength of unmodified filament, cN / dtex.

[0049] Surface oxygen-containing functional group content: X-ray photoelectron spectroscopy (XPS) was used to test the fiber surface. Charge correction was performed using the C1s binding energy of contaminated carbon (284.8 eV). Peak fitting of the C1s spectrum was performed to quantitatively obtain the relative content of oxygen-containing functional groups such as hydroxyl and carboxyl groups. The relative content multiple of surface-active groups was calculated using the following formula:

[0050] In the formula, K: the relative content multiple of the active group; A m : Relative content of oxygen-containing functional groups on the surface of modified fiber, %; A0: Relative content of oxygen-containing functional groups on the surface of unmodified filament in the same batch.

[0051] Fiber-epoxy resin interfacial bond strength: The interfacial bond performance between the single fiber and the E51 / DDM epoxy resin system was determined using the micro-bond test and calculated according to the following formula:

[0052]

[0053] In the formula, τ: interfacial bond strength (characterized by interfacial shear strength IFSS), MPa; F max ‎: Maximum debonding force, N; d‎: Fiber diameter, mm; l: Fiber embedding length in resin microdroplets, mm.

[0054] Percentage increase in interfacial bond strength:

[0055]

[0056] In the formula, Δτ: percentage increase in bond strength, %; τ m τ0: Interfacial bond strength of modified fiber, MPa; τ0: Interfacial bond strength of unmodified precursor fiber in the same batch, MPa.

[0057] Interlaminar shear strength: A unidirectional composite material was prepared by combining modified fibers with E51 / DDM epoxy resin; the interlaminar shear strength of the composite material was tested according to the ASTM D2344 short beam method; the composite material preparation process and fiber volume fraction were exactly the same as the control group, and the strength was calculated using the following formula:

[0058]

[0059] In the formula, T: interlaminar shear strength, MPa; P: maximum load at specimen failure, in N; b: specimen width, mm; h: specimen thickness, mm.

[0060] The percentage increase in interlaminar shear strength is calculated using the following formula, based on unidirectional composites prepared from the same batch of unmodified TLCP precursor fibers:

[0061]

[0062] In the formula, ΔT: percentage increase in interlaminar shear strength, %; T m T0: Interlaminar shear strength of the modified fiber composite material, MPa; T0: Interlaminar shear strength of the unmodified precursor fiber composite material in the same batch, MPa.

[0063] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments:

[0064] See Figure 1 and Figure 2 The modification device is directly connected to the discharge port of the integrated hot air circulation stretching and setting machine via a standard flange. Along the direction of the filament bundle, the adaptive tension feeding guide mechanism 1, the nitrogen micro-positive pressure plasma activation chamber 2, the nano-auxiliary agent ultrasonic atomization blending unit 3, and the constant temperature hot air curing module 4 are sequentially sealed and connected in series. The trace waste gas recovery and purification unit 5 is connected to each unit chamber through the exhaust pipe. Each unit is sealed and connected, and the filament bundle has no breaks or exposed parts from feeding to discharging.

[0065] The system comprises: 1) a closed-loop control system consisting of four sets of adjustable damping guide rollers and two sets of online tension sensors, with the two sets of tension sensors located at the feed and discharge ends respectively; 2) a fully enclosed structure with sealed guide holes at the inlet and outlet, and multiple guide rollers within the cavity. The filament bundle reciprocates through the plasma zone within the cavity, and the effective processing length is changed by adjusting the number of reciprocating passes, thereby adjusting the activation residence time at a given wire feed speed; the electrodes of the low-temperature plasma generator are symmetrically positioned on both sides of the filament bundle; 3) two sets of built-in ultrasonic atomizing nozzles are symmetrically positioned on the upper and lower sides of the filament bundle to atomize the additives. The mixed liquid is atomized into micron-sized droplets and uniformly sprayed onto the surface of the fiber bundle. The atomization amount is adjusted in conjunction with the fiber feeding speed. 4 is a constant temperature hot air duct with a duct temperature of 275~285℃, which heats and solidifies the additives attached to the fiber surface to form a modified layer. The hot air circulation volume is adjusted in conjunction with the fiber feeding speed. 5 includes an exhaust fan, exhaust duct, and activated carbon adsorption box. The exhaust duct is connected to chambers 2, 3, and 4 respectively. The trace amounts of waste gas formed by the volatilization of a small amount of unreacted low molecular weight components in each chamber are introduced into the activated carbon adsorption box for purification before being discharged. Each chamber is maintained at a set micro-positive pressure.

[0066] The operating procedure for this device is as follows:

[0067] Connect this device to the outlet of the hot stretching and setting machine 6 via the standard flange 8, and check whether the adaptive tension wire guide mechanism 1, plasma activation chamber 2, ultrasonic atomization blending unit 3, and constant temperature hot air curing module 4 are tightly connected to ensure that the wire bundle channel is uninterrupted and without any exposed parts.

[0068] The filament bundle 7 is threaded through the following path: hot stretching and setting machine 6, standard flange 8, adaptive tension wire guide mechanism 1, around the damping adjustable guide roller 1-1, and the online tension sensor 1-2 is connected to the closed-loop control system, plasma activation chamber (2), enters through the sealed guide hole 2-1, around the return guide roller 2-4 to the ultrasonic atomizing blending unit 3, corresponding to the ultrasonic atomizing nozzle 3, constant temperature hot air curing module 4 to the finished product winding 9.

[0069] Turn on the induced draft fan 5-1, confirm that the pipeline is unobstructed, the activated carbon adsorption box 5-2 is effective, and the exhaust gas discharge channels of each chamber are open.

[0070] Example 1:

[0071] S1. The heat-set TLCP filament is fed from the discharge end of the box roller integrated hot air circulation stretching and setting machine into the plasma modification device through the standard flange interface. The closed-loop control system composed of online tension sensor and damping adjustable guide roller automatically maintains the constant tension of the filament bundle, so that the filament bundle in the modification device runs synchronously with the spinning main line at a feeding speed of 50m / min, without any winding or transfer operations throughout the process.

[0072] S2. The long filament bundle enters 2 at a uniform speed through the adaptive tension wire guiding mechanism. The cavity is continuously circulated with 0.05KPa dry nitrogen to maintain a slight positive pressure and the air is isolated by sealing the wire guide holes through the inlet and outlet. Under the inert protection of nitrogen, a 1200W plasma generator is turned on for activation treatment. The activation dwell time is 5s. The surface of the filament bundle is uniformly bombarded and active functional groups such as hydroxyl and carboxyl groups are introduced to obtain the activated filament bundle.

[0073] S3. The activated filament bundle continuously enters 3, and the built-in ultrasonic atomizing nozzle atomizes the auxiliary agent mixture evenly and sprays it onto the surface of the filament bundle. The ester compatibilizer is selected from epoxy-modified soybean fatty acid ester; the nano antioxidant is selected from nano cerium dioxide with an average particle size of 50nm. After mixing at a mass ratio of 85:15, the mixture is ultrasonically dispersed for 30 minutes to obtain a uniform and stable auxiliary agent mixture. The atomization amount is adjusted in conjunction with the filament feeding speed to ensure that the ester-nano composite auxiliary agent is uniformly attached to the surface of the filament bundle.

[0074] S4. The fiber bundle with the additive attached then enters 4 and completes the in-situ curing of the additive through a 280℃ constant temperature circulating hot air duct. The hot air temperature and the fiber feeding speed are linked and matched to ensure complete curing without damaging the fiber body, thus obtaining the modified fiber bundle.

[0075] S5. After modification, the filament bundles are directly fed into the finished product winding section to produce high interfacial bonding polyarylate filaments in one go; the trace amounts of additive decomposition gases generated in each unit cavity are collected by 5 and discharged after being harmlessly adsorbed by activated carbon.

[0076] The above S1~S5 processes ran continuously and stably for 72 hours. During the yarn feeding process, the adaptive tension yarn feeding guide mechanism adjusted the yarn tension in real time, and there were no deviation or yarn breakage faults.

[0077] Performance testing: The relative content of surface active groups in the modified fiber reached 3.1 times; the bonding strength with epoxy resin increased by 46%, and the interlaminar shear strength increased by 32%; the fiber breaking strength was 29.2 cN / dtex, the strength retention rate reached 98.9%, and there was no oxidation damage.

[0078] Example 2:

[0079] The difference between this embodiment and Embodiment 1 lies in the adjustment of process parameters: the modification device is connected to the discharge port of the integrated hot air circulating stretching machine via a standard flange, and the cavity is purged with 0.05 kPa dry nitrogen to maintain a slight positive pressure; the plasma generator has a power of 1400 W; the additive is a mixture with a mass ratio of epoxy-modified soybean fatty acid ester to nano-cerium dioxide of 85:15, and the hot air module is kept at a constant temperature of 280°C. The remaining steps and operating conditions are the same as in Embodiment 1.

[0080] Continuous operation: The production line feeds yarn at a speed of 80m / min, the yarn bundle is activated by plasma and stays for 4s, the atomization agent increases the atomization amount in conjunction with the yarn feed speed, the agent evenly coats the yarn bundle, and the hot air cures it simultaneously; the equipment runs stably for 72 hours without deviation or yarn breakage.

[0081] Performance testing: The relative content of surface active groups in the modified fiber reached 2.7 times, the bonding strength with epoxy resin increased by 41%, and the interlaminar shear strength increased by 29%; the fiber breaking strength was 29.0 cN / dtex, the strength retention rate was 98.3%, and there was no obvious oxidation damage.

[0082] Example 3:

[0083] The difference between this embodiment and Embodiment 1 lies in the adjustment of process parameters: the modification device is connected to the discharge port of the integrated hot air circulating stretching machine via a standard flange, and the cavity is purged with 0.06 kPa dry nitrogen to maintain a slight positive pressure; the plasma generator has a power of 1600 W; the additive is a mixture of epoxy-modified soybean fatty acid ester and nano-cerium dioxide at a mass ratio of 80:20, and the hot air module is kept at a constant temperature of 285°C. The remaining steps and operating conditions are the same as in Embodiment 1.

[0084] Continuous operation: The production line feeds at a speed of 120m / min, and the filament bundle is activated by plasma for 3 seconds. The system linkage increases the atomization amount and hot air circulation volume to ensure the coating and curing effect of the additives. The equipment runs stably for 48 hours continuously, and the adaptive tension mechanism automatically compensates for tension fluctuations, preventing deviation and filament breakage.

[0085] Performance testing: The relative content of surface active groups in the modified fiber reached 2.3 times, the bonding strength with epoxy resin increased by 37%, and the interlaminar shear strength increased by 26%; the fiber breaking strength was 28.8 cN / dtex, and the strength retention rate was 97.6%, which met the mass production indicators.

[0086] Example 4:

[0087] The difference between this embodiment and Embodiment 1 lies in the adjustment of process parameters: the modification device is connected to the discharge port of the integrated hot air circulating stretching machine via a standard flange, and the cavity is purged with 0.04 kPa dry nitrogen to maintain a slight positive pressure; the plasma generator has a power of 1000 W; the additive is a mixture of epoxy-modified soybean fatty acid ester and nano-cerium dioxide at a mass ratio of 90:10, and the hot air module is kept at a constant temperature of 275°C. The remaining steps and operating conditions are the same as in Embodiment 1.

[0088] Continuous operation: The production line feed speed is 50m / min, and the fiber bundle plasma activation residence time is 8s to reduce the atomization rate and extend the reaction time between the additives and the fiber surface; the equipment runs stably for 72 hours continuously, and the fiber bundle runs smoothly.

[0089] Performance testing: The modified fiber exhibits a 3.6-fold increase in the relative content of surface active groups, a 51% increase in bond strength with epoxy resin, and a 36% increase in interlaminar shear strength. The fiber's breaking strength is 29.4 cN / dtex, with a strength retention rate of 99.6%, making it suitable for military composite material components with extremely high requirements for interfacial performance.

[0090] Comparative Example 1:

[0091] This comparative example uses the organic amine solvent + ultraviolet grafting method disclosed in CN113788975A to perform offline batch impregnation treatment of the finished fibers, using an organic amine and coupling agent solvent system.

[0092] Performance testing: Under the same raw material conditions, the bond strength between the treated fiber and epoxy resin increased by 27%, the interlaminar shear strength increased by 25%, the fiber breaking strength was 26.0 cN / dtex, and the strength retention rate was 88.1%; the single batch treatment cycle was 12 hours, and the environmental treatment cost of waste liquid and waste gas was high.

[0093] Comparative Example 2:

[0094] This comparative example adopts the offline cold plasma treatment scheme disclosed in CN113737510A, which involves no nitrogen protection, no auxiliary agent curing, and offline processing with secondary fiber feeding.

[0095] Performance testing: Under the same fiber specifications and test conditions, the bonding strength between the fiber and epoxy resin only increased by 18%, the interlaminar shear strength increased by 15%, the fiber breaking strength was 26.7 cN / dtex, the strength retention rate was 90.5%, and there was obvious oxidative embrittlement; the transfer process caused filament loss, and the improvement in interface strength was far lower than that of the present invention.

[0096] Comparative Example 3:

[0097] The difference between this comparative example and Example 1 is that: the flange is directly connected to the outlet of the hot drawing and shaping machine, nitrogen gas introduction is eliminated, and the cavity is connected to the outside air; the plasma generator power is 1400W; the ratio of epoxy-modified soybean fatty acid ester to nano-cerium dioxide is 85:15, and the curing temperature is 280℃. Except for the above adjustments, the remaining steps and operating conditions are the same as in Example 1.

[0098] Continuous operation: wire feed speed 80m / min, plasma activation dwell time 4s, atomization and hot air curing unit turned on; a small number of monofilaments break and produce fuzz during equipment operation.

[0099] Performance testing: The fiber showed obvious high-temperature oxidation and embrittlement, and slight yellowing appeared on the fiber surface; the bonding strength with epoxy resin increased by 33%, and the interlaminar shear strength increased by 21%; the fiber breaking strength was 25.1 cN / dtex, and the strength retention rate was 85.1%.

[0100] Comparative Example 4:

[0101] The difference between this comparative example and Example 1 is that: the flange is directly connected to the outlet of the hot drawing and shaping machine; nitrogen gas at 0.04 kPa is introduced into the cavity to maintain a slight positive pressure; the ultrasonic atomizing nozzle is removed, and there is no additive spraying process; the plasma generator power is 1000W, and the hot air module is 275°C. Except for the above adjustments, the remaining steps and operating conditions are the same as in Example 1.

[0102] Continuous operation: wire feed speed 50m / min, plasma activation dwell time 8s, after plasma activation the wire bundle directly enters the hot air module for processing and then is wound up.

[0103] Performance testing: The relative content of surface active groups on the modified fiber reached 3.4 times; relying solely on plasma roughening activation without the synergistic effect of grafting and curing with additives, the bonding strength with epoxy resin increased by 19%, and the interlaminar shear strength increased by 14%; the fiber breaking strength was 29.3 cN / dtex, and the strength retention rate was 99.3%.

[0104] Comparative Example 5:

[0105] The difference between this comparative example and Example 1 is that the constant temperature hot air curing module is removed, and the filament bundle is directly wound up after passing through the ultrasonic atomization blending unit for nano-additives, without undergoing hot air curing treatment. Apart from the above adjustments, all other steps and operating conditions are the same as in Example 1.

[0106] Continuous operation: yarn feed speed 50m / min, nitrogen micro-positive pressure 0.05KPa, plasma power 1200W, activation dwell time 5s, epoxy modified soybean fatty acid ester: nano-cerium dioxide mass ratio 85:15. During operation, the surface additives of the yarn bundle did not cure, the yarn bundle surface became sticky after winding, and the surface active groups underwent time-dependent decay after 24 hours of storage.

[0107] Performance testing: The relative content of surface active groups in the modified fiber reached 2.9 times; the bonding strength with epoxy resin increased by 24%; the interlaminar shear strength increased by 18%; the breaking strength was 29.1 cN / dtex, and the strength retention rate was 98.6%.

[0108] Comparative Example 6:

[0109] The difference between this comparative example and Example 1 is that the ultrasonic atomizing nozzle in the ultrasonic atomizing blending unit for nano-additives is replaced with a conventional pressure spray nozzle. Apart from the above adjustments, all other steps and operating conditions are the same as in Example 1.

[0110] Continuous operation: The yarn feed speed is 50m / min, and the total supply of additives is consistent with that in Example 1. During operation, additive dripping occurs, local additive accumulation in the yarn bundle, local coating loss, and poor batch uniformity.

[0111] Performance testing: The relative content of surface active groups in the modified fiber reached 3.0 times; the bonding strength with epoxy resin increased by 31%; the interlaminar shear strength increased by 22%; the breaking strength was 28.9 cN / dtex, and the strength retention rate was 98.0%; the test data of different fiber bundles showed large dispersion.

[0112] Comparative Example 7:

[0113] The difference between this comparative example and Example 1 is that the closed-loop control system of the adaptive tension wire guide mechanism is removed, and only the ordinary fixed guide roller is retained, without tension sensors or damping automatic adjustment. Apart from the above adjustments, the remaining steps and operating conditions are the same as in Example 1.

[0114] Continuous operation: Wire feeding speed 50m / min; due to the accumulation of wire feeding resistance in each series cavity along the process, the wire bundle tension fluctuates continuously. After 12 hours of operation, the wire bundle deviates and some wires break, making it impossible to achieve 72 hours of continuous and stable production.

[0115] Performance testing: The samples were intact filament bundles without broken fibers; the relative content of surface active groups in the modified fibers reached 3.0 times; the bonding strength with epoxy resin increased by 44%; the interlaminar shear strength increased by 30%; the breaking strength was 27.2 cN / dtex, and the strength retention rate was 92.2%; some samples had fuzz and stress damage.

[0116] Comparative Example 8: Blank Control Group

[0117] TLCP filaments, directly heat-set without the treatment of this modification device, do not undergo plasma activation, additive coating, or curing processes. This comparative example serves as the basis for calculating various relative indicators: the relative content multiple of its surface-active groups is recorded as 1; the improvement rate of its bond strength with epoxy resin and the improvement rate of its interlaminar shear strength are both 0; the fiber breaking strength is 29.5 cN / dtex, and the breaking strength retention rate is recorded as 100%.

[0118] The performance test results of the above embodiments and comparative examples are shown in Table 1.

[0119] Table 1: Performance test results of the examples and comparative examples

[0120] project Relative content multiple of surface-active groups Bond strength with epoxy resin increased by % Interlaminar shear strength increased by % Fracture strength cN / dtex Strength retention rate % Example 1 3.1 46 32 29.2 98.9 Example 2 2.7 41 29 29.0 98.3 Example 3 2.3 37 26 28.8 97.6 Example 4 3.6 51 36 29.4 99.6 Comparative Example 1 — 27 25 26.0 88.1 Comparative Example 2 — 18 15 26.7 90.5 Comparative Example 3 — 33 21 25.1 85.1 Comparative Example 4 3.4 19 14 29.3 99.3 Comparative Example 5 2.9 24 18 29.1 98.6 Comparative Example 6 3.0 31 22 28.9 98.0 Comparative Example 7 3.0 44 30 27.2 92.2 Comparative Example 8 1.0 0 0 29.5 100

[0121] Note: Comparative Examples 1 and 2 were offline processes, and Comparative Example 3 focused on examining oxidation attenuation. No quantitative characterization of surface functional groups was performed in any of them.

[0122] Based on the above analysis, Examples 1-4 all achieved a comprehensive effect of strength retention rate ≥97.5%, epoxy resin bond strength improvement ≥37%, and interlaminar shear strength improvement ≥26% under different process parameters, and all could operate continuously and stably, indicating that the device and process of the present invention have good adaptability and reliability in a wide speed range of 50~120m / min. Among them, Example 4 has the best comprehensive performance, with a relative content multiple of surface active groups of 3.6, a bond strength improvement of 51%, an interlaminar shear strength improvement of 36%, and a strength retention rate of 99.6%, meeting the high-specification customization requirements of military applications.

[0123] Compared with the blank control group, the offline solvent grafting process of Comparative Example 1 had a single batch cycle of 12 hours and the fiber breakage retention rate decreased by 11.9%; the offline single plasma solution of Comparative Example 2 decreased the fiber breakage strength by 9.5% and the fiber-epoxy resin bond strength increased by only 18%. Comparative Examples 3-7 were used to remove or replace key units in the device of the present invention one by one. The results showed that the performance of each unit was significantly deteriorated, proving that each unit is indispensable: Comparative Example 3 only removed nitrogen protection, and the strength retention rate dropped to 85.1%, and the fibers showed oxidative embrittlement and yellowing; Comparative Example 4 only removed the ultrasonic atomization unit and did not co-cur with additives. Although the strength retention rate still reached 99.3%, the bond strength improvement dropped sharply to 19% and the interlaminar shear strength improvement dropped to 14%, falling back to the level of the single plasma scheme; Comparative Example 5 removed the hot air curing module, and the bond strength improvement dropped to 24%, and the active groups decayed with storage time, and the surface of the filament became sticky; Comparative Example 6 replaced ultrasonic atomization with ordinary pressure spraying, and the bond strength improvement dropped to 31%, and the batch dispersion increased significantly; Comparative Example 7 removed the tension closed-loop control, and after 12 hours of operation, the fibers deviated and broke, and it could not maintain 72 hours of continuous production, and the strength retention rate dropped to 92.2%. It is evident that nitrogen micro-positive pressure protection maintains the strength of the main body, in-situ co-curing of additives enhances the interfacial performance, hot air curing locks in the synergistic effect, ultrasonic atomization ensures batch uniformity, and tension closed-loop ensures continuous operation stability. These five mechanisms have different mechanisms of action and are irreplaceable to each other, together constituting the comprehensive technical effect of this invention: high interface, high strength retention, and long-term stability.

[0124] Therefore, this invention achieves online synergy of plasma activation, ultrasonic atomization of nano-additives, and constant-temperature hot air curing, supplemented by nitrogen micro-positive pressure protection and adaptive tension closed-loop control. This enables the modified TLCP filament to effectively improve interfacial bonding strength and interlaminar shear strength while maintaining bulk strength. This improves upon the problems of incompatibility between interfacial modification and bulk strength damage, fragmented offline processes, low efficiency, and heavy pollution in existing technologies. It is suitable for the continuous and large-scale preparation of high-end reinforcing fibers for aerospace and military insulation.

[0125] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make many possible variations and modifications to the technical solutions of the present invention using the methods and techniques disclosed above, or modify them into equivalent embodiments with equivalent changes, without departing from the spirit and technical essence of the present invention. Therefore, any simple modifications, equivalent substitutions, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solutions of the present invention shall still fall within the protection scope of the technical solutions of the present invention.

Claims

1. A plasma modification process integrated into a polyarylate melt spinning production line, characterized in that, Includes the following steps: S1. The heat-set thermotropic liquid crystal polyarylate filament is fed from the discharge end of the box roller integrated hot air circulation stretching and setting machine into the plasma modification device through the standard flange interface. The adaptive tension wire guiding mechanism (1) automatically maintains the constant tension of the filament bundle and synchronizes it with the wire speed of the spinning main line through a closed-loop control system composed of an online tension sensor and a damping adjustable guide roller. No winding and transfer operations are performed throughout the process. S2. The long filament bundle enters the nitrogen micro-positive pressure plasma activation chamber (2) at a uniform speed through the adaptive tension wire guiding mechanism. Dry nitrogen is introduced into the chamber to maintain micro-positive pressure and air is isolated by sealing the wire guide holes through the inlet and outlet. Plasma activation treatment is carried out under nitrogen inert protection to obtain the activated filament bundle. S3. The activated filament bundle continuously enters the ultrasonic atomization blending unit (3) of the nano-auxiliary agent, so that the ester-nano composite agent is uniformly attached to the surface of the filament bundle. S4. The filament bundles with the additives attached are then placed into the constant temperature hot air curing module (4) for in-situ curing to obtain modified filament bundles. S5. After modification, the filament bundles are directly fed into the finished product winding section to produce high interfacial bonding polyarylate filaments in one go. The trace amounts of auxiliary decomposition gas generated by each unit cavity are collected by the trace amount of waste gas recovery and purification unit (5) and discharged after being harmlessly adsorbed by activated carbon.

2. The modification process according to claim 1, characterized in that, The adaptive tension feeding guide mechanism described in S1 consists of a closed-loop control system composed of multiple sets of damping adjustable guide rollers and online tension sensors. The online tension sensors detect and feed back the tension of the yarn bundle in real time. The closed-loop control system compares the measured tension value with the set tension value and adjusts the damping of the damping adjustable guide rollers according to the deviation, so as to keep the yarn bundle tension constant. This ensures that the running speed of the yarn bundle in the modification device is synchronized with the yarn feeding speed of the spinning main line, avoiding yarn bundle accumulation and loosening or excessive tension that could lead to deviation and yarn breakage.

3. The modification process according to claim 1, characterized in that, The nitrogen micro-positive pressure low-temperature plasma activation chamber described in S2 is a fully enclosed chamber structure with sealing guide wire holes at its inlet and outlet; the chamber is connected to a nitrogen supply pipeline to continuously supply dry nitrogen to maintain micro-positive pressure and prevent external air from seeping in.

4. The modification process according to claim 1, characterized in that, The nitrogen micro-positive pressure low-temperature plasma activation chamber in S2 is equipped with a low-temperature plasma generator; the power of the low-temperature plasma generator is 1000~1600W.

5. The modification process according to claim 1, characterized in that, The ultrasonic atomization blending unit for nano-auxiliaries described in S3 has an ultrasonic atomization nozzle built in, which is used to uniformly atomize the auxiliary mixture and spray it onto the surface of the activated filament bundle; the auxiliary mixture is a mixture of ester compatibilizer and nano antioxidant, and its mass ratio is ester compatibilizer: nano antioxidant = (70~90):(10~30).

6. The modification process according to claim 1, characterized in that, The constant temperature hot air curing module described in S4 has a constant temperature circulating hot air duct for rapidly curing fiber surface additives to form a modified layer; the hot air temperature of the constant temperature hot air curing module is 275~285℃.

7. The modification process according to claim 1, characterized in that, The trace waste gas recovery and purification unit described in S5 is connected to the sealed cavity of each unit and is used to collect the decomposed gas of the additives and then discharge it after adsorption by activated carbon.

8. The modification process according to claim 1, characterized in that, The atomization volume of the ultrasonic atomizing nozzle and the hot air temperature of the constant temperature hot air curing module are both adjusted in conjunction with the wire feeding speed.

9. The modification process according to claim 1, characterized in that, The wire feeding speed in step S1 is 50~120m / min; the nitrogen micro-positive pressure in step S2 is 0.04~0.06KPa; and the activation residence time is 3~8s.

10. A plasma modification device integrated into a polyarylate melt spinning production line, characterized in that, It includes an adaptive tension wire guiding mechanism (1) that is sealed and connected in series along the wire bundle direction, a nitrogen micro-positive pressure low-temperature plasma activation chamber (2), a nano-additive ultrasonic atomization blending unit (3), a constant temperature hot air curing module (4), and a trace amount of waste gas recovery and purification unit (5). The feed end of the adaptive tension wire guide mechanism (1) is directly connected to the discharge port of the hot drawing and setting machine (6) through a standard flange (8); the adaptive tension wire guide mechanism (1) includes a damping adjustable guide roller (1-1) and an online tension sensor (1-2). The nitrogen micro-positive pressure low-temperature plasma activation chamber (2) has sealed guide wire holes (2-1) at its inlet and outlet. The chamber is equipped with a plasma electrode (2-2), a nitrogen inlet (2-3), and a folding guide wire roller (2-4). The plasma electrode (2-2) is symmetrically distributed on both sides of the wire bundle. The folding guide wire roller (2-4) causes the wire bundle to fold back and forth in the chamber to adjust the activation residence time. The ultrasonic atomization blending unit (3) for nano-additives has built-in ultrasonic atomization nozzles (3-1), which are symmetrically arranged on the upper and lower sides of the filament bundle. The constant temperature hot air curing module (4) has a constant temperature circulating hot air duct; The trace waste gas recovery and purification unit (5) includes an exhaust fan (5-1) and an activated carbon adsorption box (5-2). Each unit is tightly connected, and the filament bundle (7) is uninterrupted and exposed from feeding to discharging. The modified filament bundle directly enters the finished product winding (9).

Citation Information

Patent Citations

  • Cold-state plasma polymer surface treatment method

    CN113737510A

  • Surface treatment method of LCP (Liquid Crystal Polymer) material

    CN113788975A