Uniform enhancement method for surface nano-implantation structure modification of organic multifilament fibers

By subjecting PAN multifilament fibers to bending and widening using multiple sets of rollers, the problem of nanoparticles being difficult to penetrate was solved, achieving uniform modification inside the multifilament fibers and improving the modification effect.

CN123108928APending Publication Date: 2026-11-17YANTAI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611010629.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

During the liquid-phase nano-modification process of PAN multifilament fibers, nanoparticles have difficulty penetrating deep into the fiber interior, resulting in uneven modification and affecting the modification efficiency.

Method used

Multiple sets of rollers are used to bend and widen PAN multifilament fibers in different directions, which generates compressive stress in the fibers and promotes the penetration of nanoparticles. Combined with appropriate temperature control and roller design, uniformity is ensured.

Benefits of technology

The uniformity of nano-modification within PAN multifilament fibers was achieved, improving the performance consistency and stability of the modified multifilament fibers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108928A_ABST
    Figure CN123108928A_ABST
Patent Text Reader

Abstract

This invention relates to the field of carbon fiber preparation technology and discloses a method for enhancing the uniformity of nanostructure modification on the surface of organic multifilament fibers. Through the design of the physical structure, the PAN multifilament is bent under tension, generating compressive stress in the bending area. When the compressive stress exceeds the slip limit of the monofilaments in the multifilament, the monofilaments slip along the stress field direction, causing the entire multifilament to deform. During the above process, the position of the monofilaments changes, dynamically generating sufficient interfilament gaps, allowing nanoparticles in the modification solution to permeate, thereby promoting the penetration of nanoparticles into the interior of the multifilament fibers. In this way, the multifilament PAN fibers, especially the interior of the multifilament fibers, can obtain a more uniform nano-modification effect, thus making the modified multifilament fibers more consistent and stable in performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for uniform enhancement of the surface of polyacrylonitrile multifilament nanostructure modification, belonging to the field of carbon fiber preparation technology. Background Technology

[0002] Physical modification of PAN (polyacrylonitrile) fibers, particularly the construction of effective nanostructures on their surface and the deep integration of these structures with the PAN fibers, can yield modified carbon fibers with nano-implanted structures during subsequent carbonization, thereby significantly enhancing the interfacial properties of carbon fiber composites. The relatively simple and easily industrialized liquid-phase nanomodification process of PAN has become an important method for preparing nano-modified PAN fibers as precursors for nano-modified carbon fibers. However, PAN multifilaments are composed of a large number of tightly aggregated PAN monofilaments. In the liquid phase environment, nanoparticles easily bind to the outer PAN fibers of the multifilament, while the tightly packed monofilaments act like a filter, making it difficult for nanoparticles to penetrate the deeper fibers of the multifilament. This ultimately leads to uneven modification of the PAN multifilament, especially within the fiber itself, where the nanoparticle concentration is often lower than designed, thus reducing the modification efficiency. Summary of the Invention

[0003] To address the issue of uneven modification of multifilament fibers, this invention proposes a method for enhancing the uniformity of PAN multifilament surface nano-implantation structure modification.

[0004] PAN multifilament fibers are introduced into a modification solution tank via guide wheels. The tank contains multiple sets of roller assemblies, each consisting of two or more parallel rollers. The rollers' function is to bend the multifilament fibers under tension, creating compressive stress in the bending area. When this compressive stress exceeds the slippage limit of the individual filaments, the filaments slip along the stress field, causing overall deformation of the multifilament. To achieve this effective overall deformation, the roller diameter should be 10-8000 times the fiber thickness, preferably 2-20 mm. The rollers can be either smooth rods or rotating shafts; rotating shafts are preferred to minimize negative impacts on the fibers. If smooth rods are used, the surface roughness of the surface in contact with the fiber should not exceed 1.5.

[0005] Because the modification solution in the modification solution tank contains PAN solvent, which dissolves the surface of the PAN monofilament fibers, causing them to become adhesive, any physical disturbance will affect the plastic deformation of the adhesive surface of the PAN fibers. Therefore, the intervention of the roller group on the multifilament fibers should be as upstream as possible in the multifilament travel direction. Thus, the horizontal multifilaments carried by the guide rollers first enter the horizontal roller group, where they bend the multifilament fibers vertically, causing the fibers to widen for the first time. The length of the multifilament fiber from the moment it is immersed in the modification solution to the moment it reaches the first roller of the horizontal roller group should be less than 40% of the total length of the multifilament fiber immersed in the modification solution. During the first widening process of the multifilament fiber, a certain number of monofilament fibers undergo positional changes, creating sufficient inter-filament gaps, allowing nanoparticles in the modification solution to permeate, thereby promoting the penetration of nanoparticles into the interior of the multifilament fiber.

[0006] After passing through the horizontal roller group, the multifilament fibers enter the second roller group, where they undergo a second broadening process in a different direction. To prevent single fiber bundles that were not dispersed during the first broadening from remaining bundled as single fibers during the second broadening, the direction of the second broadening should be as perpendicular as possible to the first broadening. Therefore, the angle between the roller direction in the second roller group and the roller direction in the horizontal roller group is 20°-160°, with 90° being preferred. During the bending process in the second roller group, the single filaments recombine and are broadened again. Both of these processes cause a new relative positional change in a large number of single filaments, thereby further releasing nanoparticles into the interior of the multifilament fibers.

[0007] As can be predicted from the modification process, a viscose-like surface begins to form on the surface of the monofilament fiber upon entering the modification solution. This viscose-like surface gradually thickens as the fiber remains in the solution until it detaches from the solution, at which point the thickness reaches the modification process standard, achieving optimal integration of nanoparticles. Therefore, nanoparticles should first be released into the multifilament fiber, allowing them to gradually adhere and integrate onto the viscose-like surface. Consequently, the length of the multifilament fiber from the last roller of the horizontal roller group to the second roller group should be less than 20% of the total length of the multifilament fiber immersed in the modification solution.

[0008] The multifilament fibers should undergo a re-stacking of monofilament fibers as they move from the first roller group to the second roller group. To prevent the multifilament fibers from twisting as a whole from the first roller group to the second roller group, thus reducing the stacking effect of the monofilament fibers, the distance between the first roller of the second roller group and the last roller of the first roller group should be less than 10 times the width of the multifilament fiber ribbon, preferably 1-20 mm. To achieve the same purpose of re-stacking monofilament fibers in the above process, a limiting structure such as a roller group can be added after the first roller group or before the second roller group. The method of adding a limiting structure such as a roller group to achieve the above-mentioned equivalent re-stacking effect of multifilament fibers is also within the scope of protection of this invention.

[0009] After the multifilament fiber is stretched in two different directions as described above, a relatively uniform nano-surface can generally be obtained. However, roller groups can be added to further improve the uniformity. The principle is that the stretching direction of the added roller group is at an angle of 20°-160° with the stretching direction of the previous roller group, with 90° being the best.

[0010] To further promote the diffusion of nanoparticles in the above process, based on the technical solutions proposed above, increasing the temperature of the modified solution should also be within the scope of protection of this invention.

[0011] Based on the technical objective of this invention, in order to achieve the goal of causing the multifilament to bend under the action of multifilament tension, thereby generating compressive stress in the bending area, and when the compressive stress is greater than the slippage limit of the monofilament in the multifilament, the monofilament will slip along the stress field direction, thereby causing the multifilament to deform as a whole, all physical structures with the same effect as the roller assembly technology described in this invention are also within the scope of protection of this invention.

[0012] The beneficial effects of this invention are that, through the design of the physical structure, the PAN multifilament is bent under tension, generating compressive stress in the bending region. When the compressive stress exceeds the slippage limit of the monofilaments, the monofilaments slip along the stress field direction, causing overall deformation of the multifilament. During this process, the monofilament fibers change position, dynamically creating sufficient interfilament gaps, allowing nanoparticles in the modified solution to permeate, thereby promoting the penetration of nanoparticles into the interior of the multifilament fibers. In this way, the multifilament PAN fibers, especially the interior of the multifilament fibers, can achieve a more uniform nano-modification effect, resulting in more consistent and stable properties of the modified multifilament fibers. Attached Figure Description

[0013] Figure 1 This is a schematic diagram of the operation process of the present invention.

[0014] The markings in the diagram are as follows: 1-1, front liquid guide roller; 2, PAN multifilament; 3, modified solution tank; 4-1, horizontal roller group No. 1 roller; 4-2, horizontal roller group No. 2 roller; 4-3, horizontal roller group No. 3 roller; 5-1, second roller group No. 1 roller; 5-2, second roller group No. 2 roller; 5-3, second roller group No. 3 roller.

[0015] Figure 2 These are photos showing the effects of using the invention before and after.

[0016] The figures are labeled as follows: 1-a / 1-b are photos of 12KPAN multifilaments modified with carbon nanotubes without using this technology, and 2-a / 2-b are photos of carbon nanotube-modified PAN multifilaments prepared using the same modification process and equipment after using this technology. Detailed Implementation

[0017] The technical solution of the present invention will now be clearly and completely described with reference to the accompanying drawings. One example is as follows:

[0018] 12K PAN multifilament fibers are introduced into the modification solution tank via guide wheels. The modification solution tank contains two sets of roller assemblies, each consisting of three parallel rollers with a diameter of 5mm. The rollers are bearing shafts with a surface roughness of 0.5.

[0019] The horizontal multifilament fibers carried by the guide rollers first enter the horizontal roller assembly. The horizontal roller assembly bends the multifilament fibers vertically, causing the multifilament fibers to widen for the first time. The length of the multifilament fiber from the moment it is immersed in the modification solution to the moment it reaches the first roller of the horizontal roller assembly is 10% of the total length of the multifilament fiber immersed in the modification solution.

[0020] After passing through the horizontal roller group, the multifilament fibers enter the second roller group, where they undergo a second widening process in a different direction. The roller direction in the second roller group forms a 90° angle with the roller direction in the horizontal roller group. The length of the multifilament fiber from the last roller in the horizontal roller group to the second roller group is 20% of the total length of the multifilament fiber immersed in the modification solution. The first roller in the second roller group is 10 mm away from the last roller in the first roller group.

[0021] To further promote the diffusion of nanoparticles in the above process, the temperature of the modified solution was maintained at 30 degrees Celsius.

[0022] Figure 2 Photographs 1-a and 1-b show 12KPAN multifilaments modified with carbon nanotubes without this technology. It can be seen that the carbon nanotubes in the black areas are not evenly distributed on the surface of the multifilaments, resulting in varying shades of color. In contrast, Figure 2In Figures 2-a and 2-b, carbon nanotube-modified PAN multifilaments were prepared using the same modification process and equipment after applying this technology. It can be seen that the color distribution is more uniform compared to before the application of this technology.

Claims

1. A method for enhancing the uniformity of organic multifilament fiber surface nano-implanted structure modification, characterized in that, PAN multifilament fibers are guided into a modification solution tank via guide wheels. The tank contains multiple sets of roller assemblies, each consisting of two or more parallel rollers. The roller diameter is 10-8000 times the thickness of the multifilament fiber. The rollers can be smooth rods or rotating shafts; if smooth rods are used, the surface roughness of the surface in contact with the fiber should not exceed 1.

5. Following the horizontal multifilament fibers carried by the guide wheels, they first enter the horizontal roller assemblies. These roller assemblies bend the multifilament fibers vertically, causing the fibers to widen for the first time. The length of the multifilament fiber from the moment it enters the modification solution to the first roller in the horizontal roller assemblies should be less than 40% of the total length of the multifilament fiber immersed in the modification solution. After passing through the horizontal roller assemblies, the multifilament fibers enter the second roller assemblies, where they undergo a second widening in another direction. The angle between the roller direction in the second roller assemblies and the roller direction in the horizontal roller assemblies is 20°-160°. The multifilament fibers then... The length between the last roller of the horizontal roller group and the second roller group should be less than 20% of the total length of the multifilament fiber immersed in the modification solution. From the first roller group to the second roller group, the multifilament fiber should undergo re-stacking of monofilament fibers. To avoid overall twisting of the multifilament fiber from the first roller group to the second roller group, which would reduce the stacking effect of the monofilament fibers, any one or a combination of the following two technical solutions can be used: The first solution is that the distance between the first roller of the second roller group and the last roller of the first roller group is less than 10 times the width of the multifilament fiber ribbon; the second solution is to add a roller group or other limiting structure after the first roller group or before the second roller group. Alternatively, more roller groups can be added to further improve uniformity. The principle is that the angle between the widening direction of the added roller group and the widening direction of the previous roller group should be 20°-160°. To further promote the diffusion of nanoparticles in the above process, based on the proposed technical solutions, the temperature of the modification solution can be increased. Based on the technical objective of this invention, in order to achieve the goal of causing the multifilament to bend under the action of multifilament tension, thereby generating compressive stress in the bending area, and when the compressive stress is greater than the slippage limit of the monofilament in the multifilament, the monofilament will slip along the stress field direction, thereby deforming the multifilament as a whole, that is, all physical structures with the same effect as the roller assembly technology described in this invention.