A corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire, its preparation method and application
By performing surface activation treatment and interfacial transition coating on UHMWPE fibers, the problem of insufficient coating adhesion of UHMWPE fibers in marine environments was solved, achieving high-strength bonding between fibers and coatings and wear-resistant and corrosion-resistant effects.
Patent Information
- Application Number
- CN202611166200.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-03
- Publication Date
- 2026-11-17
AI Technical Summary
UHMWPE fibers experience a decrease in strength in marine environments, and their high surface inertness leads to insufficient coating adhesion, making it difficult to form effective functional coatings.
UHMWPE fibers are surface activated to form an interfacial transition coating, and then a protective coating is formed on the outside of the fiber. The coating contains silicon carbide, Ti3C2Tx MXene nanosheets and silane coupling agents to improve interfacial adhesion.
It enhances the interfacial compatibility and bonding strength between the fiber and the coating, reduces the risk of coating peeling during bending and friction, and improves the resistance to seawater corrosion.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention relates to a corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire, its preparation method and application, belonging to the field of high-performance fiber composite material technology. Background Technology
[0002] Ultra-high molecular weight polyethylene (UHMWPE) fiber has advantages such as low density, high specific strength, and impact resistance, and has been used in fishing nets, protective materials, and high-strength ropes. However, in marine environments, UHMWPE fibers are affected by seawater immersion and impact, which reduces their overall strength. Furthermore, due to the high surface inertness and low surface energy of UHMWPE fibers, their adhesion to coatings, resins, rubber, or adhesive layers is insufficient, making it difficult to form appropriate functional coatings on their surface. Summary of the Invention
[0003] The purpose of this invention is to provide a corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene (UHMWPE) wire, its preparation method, and its application. First, the fiber bundle is surface-treated, then an interface transition coating is formed on its surface, and then a protective coating with wear-resistant and corrosion-resistant particles is formed outside the interface transition coating to solve the problems of poor interfacial bonding, easy peeling of coating, and insufficient weather resistance of existing UHMWPE fibers.
[0004] To achieve the above objectives, the technical solution adopted by the present invention is as follows: A method for preparing corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire includes the following steps: After surface activation treatment, UHMWPE fiber bundles are immersed in a transitional coating solution, and then removed and dried after immersion. UHMWPE fiber bundles with a transition coating on their surface are impregnated in a protective coating solution, followed by curing and heat setting. The protective coating solution contains corrosion-resistant and wear-resistant particles, including silicon carbide and Ti3C2T adhering to the silicon carbide. x MXene nanosheets and grafted onto silicon carbide and / or Ti3C2T x Silane coupling agent on MXene nanosheets.
[0005] Preferably, the transition coating liquid comprises the following components by mass content: 2-8 wt% maleic anhydride-grafted polyethylene, 3-10 wt% waterborne polyurethane, 0.2-1 wt% silane coupling agent, and the balance being water.
[0006] Preferably, the surface activation treatment is oxygen plasma treatment or corona treatment.
[0007] Preferably, the immersion time in the transition coating solution is 1-5 min; after immersion, the drying conditions are: 60-80℃, 5-10 min.
[0008] Preferably, the protective coating liquid comprises the following components by weight: 50-70 parts of polyurea prepolymer, 30-50 parts of polyurethane elastomer, 1-5 parts of polytetrafluoroethylene micro powder, 5-10 parts of anti-corrosion and wear-resistant particles, 0.5-2 parts of silicone antifouling additive, and 0.2-1 parts of antioxidant.
[0009] Preferably, the immersion time in the protective coating liquid is 2-10 minutes.
[0010] Preferably, after immersion in the protective coating, the curing conditions are: 70-90℃, 20-30min; the heat setting conditions are: 85-100℃, under tension of 5-10% of the breaking strength of UHMWPE fiber bundles, 15-30min.
[0011] Preferably, the method for preparing the corrosion-resistant and wear-resistant particles is as follows: silicon carbide microparticles are calcined at 400-600℃ for 1-3 hours, then immersed in a mixed acid solution of concentrated sulfuric acid and hydrogen peroxide at a volume ratio of 3:1, treated at 70-90℃ for 0.5-2 hours, washed and dried, dispersed in a polydiallyldimethylammonium chloride solution, stirred for 2-4 hours, and washed and dried to obtain positively charged modified silicon carbide microparticles; Modified silicon carbide microparticles with Ti3C2T x MXene dispersion mixture, wherein modified silicon carbide microparticles and Ti3C2T x The mass ratio of MXene was (1-5):1. After adjusting the pH to 6-8, the mixture was stirred at room temperature for 30-60 minutes. After centrifugation and washing, the composite particles were obtained. The obtained composite particles are dispersed in anhydrous ethanol, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane, accounting for 5-10% of the mass of the composite particles, is added. The mixture is then stirred at 60-80℃ for 4-8 hours, washed, and vacuum dried.
[0012] A corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire is prepared by any of the above methods.
[0013] Application of corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire prepared by any of the above methods in marine aquaculture products (deep-sea aquaculture cage netting, enclosure netting, stitching thread, and wind and wave resistant connecting rope).
[0014] The beneficial effects of this invention are as follows: The problems of strong surface inertness and insufficient adhesion to coatings in UHMWPE fibers are addressed through surface activation treatment and interfacial transition. Surface activation treatment introduces oxygen-containing polar groups onto the UHMWPE fiber surface and forms a certain micro-rough structure, thereby improving the fiber surface energy and its wettability to the transition coating liquid, providing polar interaction sites and physical anchoring sites for the transition coating. The maleic anhydride-grafted polyethylene in the transition coating forms good interfacial compatibility with the UHMWPE fiber through polyethylene segments, and enhances the interfacial interaction between the maleic anhydride and waterborne polyurethane and silane coupling agent through the maleic anhydride polar groups. Waterborne polyurethane imparts good flexibility and continuity to the transition coating, while the silane coupling agent helps improve the bonding strength between the transition coating and the outer polyurea / polyurethane protective coating. Thus, the transition coating forms an interface bonding layer between the UHMWPE fiber bundle and the outer protective coating, with a gradual transition in composition and performance. This can alleviate the interface stress concentration caused by differences in polarity, compatibility, and mechanical properties between the flexible UHMWPE fiber and the protective coating, improve the adhesion and structural integrity of the protective coating, and reduce the risk of coating cracking, peeling, and detachment during bending, knotting, stretching, and repeated friction of the wire.
[0015] The corrosion-resistant and wear-resistant particles added to the protective coating provide a pressure-resistant and wear-resistant skeleton through a silicon carbide hard core, while MXene nanosheets provide physical shielding and interlayer slip friction reduction. Combined with the solid lubricating effect of polytetrafluoroethylene micropowder in the protective coating, the surface roughness of the wire is significantly reduced after repeated friction. Simultaneously, the two-dimensional lamellar labyrinth effect of MXene extends the penetration path of corrosive media. Combined with the high density of the polyurea / polyurethane matrix, this endows the wire with excellent seawater corrosion resistance. After aging in artificial seawater and salt spray environments, its tensile strength retention rate is significantly higher than that of ordinary UHMWPE wire. Detailed Implementation
[0016] Example 1: This example provides a method for preparing corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire, including the following steps: S1, preparation of activated SiC; Place 5g of nano-SiC powder in a crucible and put it into a muffle furnace. Heat the crucible to 500℃ at a heating rate of 5℃ / min, hold for 2 hours, and then let it cool naturally to room temperature. Then measure 75mL of concentrated sulfuric acid (98%) and 25mL of hydrogen peroxide (30%) into a beaker and mix them (volume ratio 3:1). Stir slowly and let it cool to room temperature.
[0017] The calcined SiC powder was then added to the above mixed acid solution, heated in a water bath to 80°C, and magnetically stirred for 1 hour. After treatment, the powder was washed with deionized water by centrifugation until the pH reached 6. The product was collected and then vacuum dried at 60°C for 12 hours to obtain activated SiC.
[0018] 5g of activated SiC was ultrasonically dispersed in 250mL of deionized water at 400W under ice bath conditions. Then, 12.5mL of a 20wt% polydiallyldimethylammonium chloride solution was added to the suspension. The mixture was magnetically stirred at room temperature for 3 hours. After stirring, the precipitate was collected by centrifugation and washed three times with deionized water. The product was dried in a vacuum drying oven at 60℃ for 12 hours, and then ground to obtain PDDA@SiC for later use.
[0019] S2, MXene(Ti3C2T) x Preparation of nanosheets; Add 40 mL of HCl solution (9 mol / L) to a polytetrafluoroethylene beaker. Weigh 2 g of LiF and slowly add it to the HCl solution, stirring magnetically until completely dissolved. Weigh 1.0 g of Ti3AlC2 powder (400 mesh) and slowly add it to the etching solution under magnetic stirring.
[0020] The beaker was placed in a 35°C constant temperature water bath and reacted for 30 hours with magnetic stirring at 300 rpm. After the reaction was completed, the product was transferred to a centrifuge tube, washed with deionized water by centrifugation, and the supernatant was discarded. The washing was repeated (washed with hydrochloric acid followed by washing with deionized water until the pH reached 6), and the product was collected.
[0021] The obtained product was dispersed in deionized water and exfoliated by sonication in an ice bath for 1 h under an Ar atmosphere. After exfoliation, the suspension was centrifuged at 3500 r / min for 30 min. The supernatant was collected and freeze-dried to obtain the exfoliated MXene nanosheets.
[0022] 3. Preparation of corrosion-resistant and wear-resistant particles; 1 g of PDDA@SiC was ultrasonically dispersed in 20 mL of deionized water to obtain suspension A. 0.5 g of the exfoliated MXene nanosheets were taken and diluted with deionized water to 20 mL to obtain dispersion B. Suspension A and dispersion B were mixed and stirred at 400 rpm for 45 min at room temperature. This allowed the positively charged PDDA@SiC to adsorb the negatively charged MXene nanosheets through electrostatic attraction.
[0023] After stirring, the supernatant was discarded by centrifugation. The precipitate was washed twice with deionized water and twice with anhydrous ethanol. Then it was dried in a vacuum drying oven at 60℃ for 12 hours to obtain SiC@MXene particles.
[0024] 1 g of SiC@MXene particles were ultrasonically dispersed in 100 mL of anhydrous ethanol. Then, 0.05 g of hydrolyzed KH-560 solution was slowly added dropwise to the suspension. The mixture was heated to 70 °C and magnetically stirred for 6 h. The precipitate was collected by centrifugation and washed three times with anhydrous ethanol and twice with deionized water. Finally, it was dried in a vacuum oven at 60 °C for 12 h to obtain KH-560@SiC@MXene composite particles.
[0025] 4. Surface activation treatment of fiber bundles; 1200D UHMWPE multifilament was selected as the core material, and 16 bundles of UHMWPE multifilament were twisted together and surface activated by corona treatment. The corona treatment power was 800W, and the treatment speed was 6m / min.
[0026] 5. Transition coating formation; The treated fiber bundles were impregnated in a maleic anhydride-grafted polyolefin / waterborne polyurethane composite primer. The primer consisted of: Maleic anhydride-grafted polyethylene (EPOLENE® C-18): 4wt%; waterborne polyurethane (Covestro Bayhydrol® UH 650): 6wt%; silane coupling agent KH-560: 0.5wt%; deionized water: balance.
[0027] The impregnation time is 3 minutes, followed by drying at 70°C for 8 minutes to form an interface transition layer.
[0028] 6. Formation of protective coating; Fiber bundles with a transition coating on their surface are impregnated in a polyurea / polyurethane composite coating solution. The coating solution (by weight of components) includes: polyurea prepolymer (purchased from Allnex): 60 parts; polyurethane elastomer (purchased from Covestro): 40 parts; polytetrafluoroethylene micro powder: 5 parts; anti-corrosion and wear-resistant particles: 8 parts; silicone antifouling additive: 1 part; antioxidant: 0.5 parts.
[0029] The impregnation time is 5 minutes, followed by curing at 80°C for 25 minutes, and then heat setting at 90°C and tensile strength of 8% for 20 minutes.
[0030] Comparative Example 1: Basically the same as Example 1, except that the fiber bundles were not subjected to surface activation treatment.
[0031] Comparative Example 2: It is basically the same as Example 1, except that the fiber bundle after surface activation treatment did not undergo the transition coating formation step, but directly underwent the protective coating step.
[0032] To verify the effects of surface activation treatment and transition coating on the interfacial bonding performance between UHMWPE fiber bundles and protective coating, surface wettability test, coating adhesion durability test, and adhesion stability test after artificial seawater aging were conducted on the wires prepared in Example 1, Comparative Example 1, and Comparative Example 2, respectively.
[0033] 1. Surface wettability test; Because the surface of the UHMWPE fiber bundles is curved and the diameter of the individual filaments is small, it is not convenient to accurately measure the static contact angle. Therefore, UHMWPE films without surface activation treatment and UHMWPE films that have undergone surface activation under the same corona treatment conditions as in Example 1 were selected as test samples. The UHMWPE films and UHMWPE fiber bundles are made of the same material.
[0034] The static contact angles of deionized water and the composite primer used in Example 1 on the surfaces of two types of UHMWPE films were measured using a contact angle meter. Five locations were randomly selected for each sample for measurement, and the average value was taken as the test result.
[0035] The static contact angles of the untreated UHMWPE film to deionized water and composite primer were 121.6° and 96.8°, respectively; after corona treatment, the static contact angles of the UHMWPE film to deionized water and composite primer decreased to 58.7° and 37.5°, respectively.
[0036] Test results show that after corona treatment, the contact angle of deionized water on the UHMWPE surface decreased by about 51.7%, and the contact angle of the composite primer on the UHMWPE surface decreased by about 61.3%. This indicates that corona treatment can significantly improve the surface energy of UHMWPE material and the wetting, spreading and penetration ability of the composite primer on the fiber surface, which is beneficial to the formation of a uniform and continuous transition coating.
[0037] X-ray photoelectron spectroscopy was used to analyze the elemental composition of UHMWPE films before and after surface activation treatment. The oxygen-to-carbon atomic ratio of the UHMWPE film without surface activation treatment was 0.031, while that of the UHMWPE film after corona treatment increased to 0.168.
[0038] This demonstrates that corona treatment introduces oxygen-containing polar groups such as hydroxyl, carbonyl, and carboxyl groups onto the surface of UHMWPE materials, providing polar interaction sites for the transition coating. Simultaneously, corona discharge induces a slight etching effect on the fiber surface, forming fine grooves and a micro-rough structure, providing physical anchoring sites for the transition coating.
[0039] 2. Coating adhesion durability test; Wires of 300 mm length obtained from Examples 1, 1, and 2 were cut as samples. Each sample was placed in an environment with a temperature of 23±2℃ and a relative humidity of 50±5% for 24 hours before testing. Five parallel samples were set up in each group.
[0040] Weigh each group of wire samples before treatment and record the mass as m1; take another UHMWPE fiber bundle of the same length that has not undergone surface activation, transition coating and protective coating treatment, weigh its mass and record it as m0.
[0041] Each group of wire samples was bent 180° repeatedly around a cylindrical mandrel with a diameter of 5 mm at a bending frequency of 60 times / min and a total of 1000 bending cycles. After bending, the samples were completely immersed in deionized water and treated for 30 min under ultrasonic conditions at a frequency of 40 kHz and an ultrasonic power of 100 W.
[0042] After ultrasonic treatment, the sample is removed, the sample surface is rinsed with deionized water, and then dried at 60°C to constant weight. The mass of the treated wire is recorded as m2.
[0043] Calculate the coating retention rate using the following formula: Coating retention rate = (m2-m0) / (m1-m0)×100%.
[0044] The coating retention rate test results of the wires obtained in Example 1, Comparative Example 1 and Comparative Example 2 are shown in Table 1.
[0045] Table 1. Effects of surface activation treatment and transition coating on coating adhesion durability
[0046] As shown in Table 1, the coating retention rate of the wire obtained in Example 1 after repeated bending and ultrasonic treatment was 95.2%, which was 16.6 percentage points and 11.1 percentage points higher than that of Comparative Example 1 and Comparative Example 2, respectively.
[0047] Comparative Example 1 did not undergo surface activation treatment, and the composite primer could not fully wet and evenly spread on the UHMWPE fiber surface. The transition coating mainly relied on weak physical adhesion to the fiber. After repeated bending, fine, elongated cracks first appeared on the surface of the wire in Comparative Example 1, distributed along the fiber axis. After ultrasonic treatment, some cracks further expanded and formed sheet-like peeling, and the transition coating and protective coating peeled off simultaneously in some locations, as well as localized exposure of fiber bundles.
[0048] Although Comparative Example 2 underwent surface activation treatment, no transition coating was applied between the UHMWPE fiber bundles and the outer polyurea / polyurethane protective coating. Due to the differences in polarity, elastic modulus, and deformation capacity between the UHMWPE fibers and the outer protective coating, stress concentration easily occurs at the interface between the two during bending. After repeated bending, the surface of the wire in Comparative Example 2 showed dense network-like microcracks and local bulges; after ultrasonic treatment, some crack edges curled up, and strip-like or block-like peeling occurred, but the degree of fiber exposure was lower than that in Comparative Example 1.
[0049] Example 1 employs both surface activation treatment and transition coating. After 1000 cycles of bending and 30 minutes of ultrasonic treatment, the protective coating remains continuous overall, with only a few shallow creases and scattered micro-cracks appearing at locations with large bending curvatures. No obvious flaking, interface lifting, or large-area fiber exposure was observed.
[0050] The above results indicate that surface activation treatment can improve the bonding stability between the transition coating and UHMWPE fibers; the transition coating can alleviate the deformation differences and interfacial stress concentration between the UHMWPE fiber bundles and the polyurea / polyurethane protective coating.
[0051] 3. Adhesion stability test after artificial seawater aging.
[0052] The wires obtained in Example 1, Comparative Example 1, and Comparative Example 2 were completely immersed in artificial seawater. The salinity of the artificial seawater was 35±1 g / L, the immersion temperature was 25±2℃, and the continuous immersion time was 30 days. The artificial seawater was replaced every 3 days during the immersion period. Five parallel samples were set up for each group.
[0053] After soaking, the samples were removed, rinsed with deionized water, and dried to constant weight at 23±2℃. Subsequently, following the above-mentioned coating adhesion durability test method, each group of wires aged in artificial seawater was subjected to 1000 reciprocating bends and 30 minutes of ultrasonic treatment, and the coating retention rate was measured again.
[0054] The coating retention rates of each group of wires after aging in artificial seawater are shown in Table 2.
[0055] Table 2 Coating retention rate of wires after aging in artificial seawater
[0056] After immersion in artificial seawater, the surface color and appearance of the wire obtained in Example 1 remained basically stable, with no visible blistering or large-area peeling. After repeated bending and ultrasonic treatment, only a few localized areas showed minor cracks, and the coating retention rate still reached 91.4%.
[0057] In Comparative Example 1, due to the lack of surface activation treatment, moisture and salt ions easily penetrated along the weakly bonded interface between the fibers and the transition coating. After aging in artificial seawater, the surface of the wire exhibited scattered small bubbles, interface whitening, and localized edge lifting. After repeated bending and ultrasonic treatment, the bubbly areas ruptured, the coating peeled off in flakes, some fiber bundles were clearly exposed, and the coating retention rate decreased to 65.8%.
[0058] In Comparative Example 2, no transition coating was applied. After aging in artificial seawater, localized interface separation and strip-like bulging occurred between the outer protective coating and the UHMWPE fiber bundle. After repeated bending and ultrasonic treatment, the bulging area expanded along the fiber axis and showed obvious edge lifting, network cracks, and localized strip-like peeling. The coating retention rate was 72.6%.
[0059] Compared to the unaged seawater, the coating retention rate in Example 1 decreased by only 3.8 percentage points, while Comparative Examples 1 and 2 decreased by 12.8 and 11.5 percentage points, respectively. This indicates that moisture and salt ions in artificial seawater exacerbate coating peeling in samples with weak interfacial bonding, while surface activation treatment combined with transition coating can effectively inhibit the penetration of corrosive media along the interface and delay the propagation of interfacial defects.
[0060] The test results above indicate that surface activation treatment can improve the polarity, surface energy, and wetting and spreading ability of the composite primer on the surface of UHMWPE fibers, providing polar action sites and physical anchoring sites for the transition coating. The transition coating can improve the interfacial compatibility between UHMWPE fiber bundles and polyurea / polyurethane protective coatings, and alleviate the interfacial stress concentration between the two during bending, stretching, and seawater immersion.
[0061] Therefore, the combination of surface activation treatment and transition coating can significantly improve the adhesion, bending and peeling resistance, and interfacial stability of the protective coating in a seawater environment.
[0062] Comparative Example 3: Basically the same as Example 1, except that no anti-corrosion and wear-resistant particles were added to the polyurea / polyurethane composite coating liquid.
[0063] The UHMWPE wires obtained from Examples 1 and 3 were subjected to anti-corrosion and wear-resistant treatment. After immersion in artificial seawater for 30 days and salt spray treatment for 240 hours, the UHMWPE wires treated in Example 1 retained 93.2% of their breaking strength, which was higher than the UHMWPE wires treated in Comparative Example 3 (84.7%). After friction and wear tests, the surface roughening degree of the UHMWPE wires treated in Example 1 was lower than that of the UHMWPE wires treated in Comparative Example 3.
[0064] The UHMWPE wire obtained by Example 1 was placed in a seawater environment for 90 days, and no obvious blistering or peeling of the coating occurred.
[0065] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire, characterized in that, Includes the following steps: After surface activation treatment, UHMWPE fiber bundles are immersed in a transitional coating solution, and then removed and dried after immersion. UHMWPE fiber bundles with a transition coating on their surface are impregnated in a protective coating solution, followed by curing and heat setting. The protective coating solution contains corrosion-resistant and wear-resistant particles, including silicon carbide and Ti3C2T adhering to the silicon carbide. x MXene nanosheets and grafted onto silicon carbide and / or Ti3C2T x Silane coupling agent on MXene nanosheets.
2. The method for preparing corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire according to claim 1, characterized in that, The transition coating solution comprises the following components by mass content: 2-8 wt% maleic anhydride-grafted polyethylene, 3-10 wt% waterborne polyurethane, 0.2-1 wt% silane coupling agent, and the balance being water.
3. The method for preparing corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire according to claim 1, characterized in that, Surface activation treatment is either oxygen plasma treatment or corona treatment.
4. The method for preparing corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire according to claim 1, characterized in that, The immersion time in the transition coating solution is 1-5 minutes; after immersion, the drying conditions are: 60-80℃, 5-10 minutes.
5. The method for preparing corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire according to claim 1, characterized in that, The protective coating comprises the following components by weight: 50-70 parts polyurea prepolymer, 30-50 parts polyurethane elastomer, 1-5 parts polytetrafluoroethylene micro powder, 5-10 parts anti-corrosion and wear-resistant particles, 0.5-2 parts silicone antifouling additive, and 0.2-1 part antioxidant.
6. The method for preparing corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire according to claim 1, characterized in that, The immersion time in the protective coating liquid is 2-10 minutes.
7. The method for preparing corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire according to claim 1, characterized in that, After immersion in the protective coating, the curing conditions are: 70-90℃, 20-30min; the heat setting conditions are: 85-100℃, under tension of 5-10% of the breaking strength of UHMWPE fiber bundles, 15-30min.
8. The method for preparing corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire according to claim 1, characterized in that, The preparation method of corrosion-resistant and wear-resistant particles is as follows: Silicon carbide microparticles were calcined at 400-600℃ for 1-3 hours, then immersed in a mixed acid solution of concentrated sulfuric acid and hydrogen peroxide at a volume ratio of 3:1, treated at 70-90℃ for 0.5-2 hours, washed and dried, and dispersed in a polydiallyldimethylammonium chloride solution. The mixture was stirred at room temperature for 2-4 hours, and then washed and dried to obtain positively charged modified silicon carbide microparticles. Modified silicon carbide microparticles with Ti3C2T x MXene dispersion mixture, wherein modified silicon carbide microparticles and Ti3C2T x The mass ratio of MXene was (1-5):
1. After adjusting the pH to 6-8, the mixture was stirred at room temperature for 30-60 minutes. After centrifugation and washing, the composite particles were obtained. The obtained composite particles are dispersed in anhydrous ethanol, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane, accounting for 5-10% of the mass of the composite particles, is added. The mixture is then stirred at 60-80℃ for 4-8 hours, washed, and vacuum dried.
9. A corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire, characterized in that, It is prepared by the method described in any one of claims 1-8.
10. The application of the corrosion-resistant and wear-resistant ultra-high molecular weight polyethylene wire prepared by the method according to any one of claims 1-8 in marine aquaculture products.