Preparation method of durable photothermal heating fabric based on nano-silver layered loading

By treating polyester fabrics with alkali and polydopamine, silver nanoparticles and threads were prepared. Combined with silane coupling agent and polydimethylsiloxane encapsulation, the problem of limited photothermal conversion performance of polyester fabrics was solved, and a highly efficient and durable photothermal heating effect was achieved.

CN123108932APending Publication Date: 2026-11-17HUZHOU UNIVERSAL GRAVITY OUTDOOR TECHNOLOGY CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610932987.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-06-26
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, polyester fabrics have difficulty achieving efficient spectral absorption and rapid heat diffusion over a wide wavelength range. Single-morphology nano-silver materials are difficult to form a heat conduction network on the fabric surface, which limits photothermal conversion performance.

Method used

Silver nanoparticles and silver nanowires were prepared by surface treatment of fabrics with alkali solution and polydopamine. The nanoparticles were then encapsulated with silane coupling agent and polydimethylsiloxane to achieve layered loading of silver nanoparticles, construct a silver nano network, and enhance photothermal properties.

Benefits of technology

It achieves high-efficiency photothermal performance and durability of fabrics. The polydimethylsiloxane encapsulation layer fixes the nano-silver to prevent performance degradation, making it suitable for mass production and with wide applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108932A_ABST
    Figure CN123108932A_ABST
Patent Text Reader

Abstract

This invention relates to a method for preparing a durable photothermal heating fabric based on layered loading of silver nanoparticles, comprising: sequentially treating the fabric with an alkaline solution and polydopamine to obtain a pretreated fabric; preparing silver nanoparticles (AgNPs) and silver nanowires (AgNWs) using a polyol method; immersing the pretreated fabric in an AgNPs dispersion, ultrasonically impregnating it, and then vacuum drying it to obtain a modified fabric / AgNPs; surface treating the modified fabric / AgNPs with a silane coupling agent to obtain pretreated modified fabric / AgNPs; immersing the pretreated modified fabric / AgNPs in an AgNWs dispersion, ultrasonically impregnating it, and then vacuum drying it to obtain modified fabric / AgNPs-AgNWs; mixing a polydimethylsiloxane prepolymer with a curing agent and dissolving it in n-hexane solvent to obtain a coating solution; uniformly coating the coating solution onto the surface of the modified fabric / AgNPs-AgNWs; and heating and curing to obtain a durable photothermal heating fabric. The fabric of this invention exhibits excellent photothermal performance and durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of functional textile materials technology, specifically relating to a method for preparing a durable photothermal heating fabric based on nano-silver layered loading. Background Technology

[0002] Polyester (polyester fiber) is widely used due to its excellent mechanical properties, chemical resistance and cost advantage. However, its smooth surface, high inertness and lack of functional groups make it difficult to directly and firmly load functional nanomaterials, which restricts its application in smart textiles, personal thermal management, photothermal therapy and other fields.

[0003] In existing technologies, surface modification is often performed first to introduce a functional layer onto the surface of polyester. In studies using silver nanoparticles to impart photothermal properties to polyester fabrics, nanomaterials with a single morphology are typically chosen, such as silver nanoparticles (AgNPs). Due to the localized surface plasmon resonance effect of AgNPs, the loaded fabric exhibits strong absorption and photothermal conversion capabilities in the visible light region. However, because the nanoparticles are independent of each other, it is difficult to form a heat conduction network on the fabric surface, limiting the overall heating efficiency and rate. On the other hand, silver nanowires (AgNWs) are used. Due to the linear structure of AgNWs, the nanowires interlock to form a network structure when mixed with other materials, which is beneficial for heat conduction. Furthermore, compared to AgNPs, AgNWs have a wider absorption wavelength in the near-infrared region. However, the surface of AgNWs is relatively smooth, and the light absorption per unit mass is lower than that of nanoparticles, resulting in insufficient initial light capture efficiency.

[0004] Whether loading AgNPs or AgNWs alone, their photothermal conversion performance is often limited by the inherent wavelength spectral absorption and thermal conduction characteristics of a single morphology, making it difficult to achieve a balance between efficient spectral absorption and rapid heat diffusion over a wide wavelength range. Summary of the Invention

[0005] Based on the aforementioned shortcomings and deficiencies in the prior art, one of the objectives of this invention is to at least solve one or more of the aforementioned problems in the prior art. In other words, one of the objectives of this invention is to provide a method for preparing a durable photothermal heating fabric based on nano-silver layered loading that meets one or more of the aforementioned requirements.

[0006] To achieve the above-mentioned objectives, the present invention adopts the following technical solution: A method for preparing a durable photothermal heating fabric based on nano-silver layered loading includes the following steps: (1) The fabric is surface-treated with alkali solution and polydopamine in sequence to obtain pretreated fabric; Silver nanoparticles (AgNPs) and silver nanowires (AgNWs) were prepared using the polyol method. (2) The pretreated fabric was immersed in AgNPs dispersion, ultrasonically impregnated and then vacuum dried to obtain modified fabric / AgNPs; (3) The modified fabric / AgNPs were surface-treated with a silane coupling agent to obtain pretreated modified fabric / AgNPs; (4) The pretreated modified fabric / AgNPs was immersed in the AgNWs dispersion, ultrasonically impregnated and then vacuum dried to obtain the modified fabric / AgNPs-AgNWs; (5) Mix the polydimethylsiloxane prepolymer with the curing agent and dissolve it in n-hexane solvent to obtain a coating solution. Apply the coating solution evenly to the surface of the modified fabric / AgNPs-AgNWs and heat to cure to obtain a durable photothermal heating fabric.

[0007] As a preferred embodiment, in step (1), the alkaline solution is a 5-10 wt% NaOH aqueous solution, and the ultrasonic treatment time is 30-90 min.

[0008] As a preferred embodiment, in step (1), the fabric treated with alkali is immersed in a Tris buffer solution of polydopamine and stirred at 30-40°C for 12-24 hours, and then washed and dried to obtain the pretreated fabric. The pH of the Tris buffer solution is 8.0–8.8.

[0009] As a preferred embodiment, in step (1), the polyol method includes: Using ethylene glycol (EG) as a solvent and reducing agent, polyvinylpyrrolidone (PVP) as a stabilizer, and soluble chloride and bromide salts as morphology control agents, silver nitrate precursor solution was slowly added dropwise to the above reaction system at 150–180 °C. By changing the volume ratio of the two morphology control agents, silver nanoparticles (AgNPs) and silver nanowires (AgNWs) were prepared respectively.

[0010] As a preferred embodiment, the concentration of PVP in EG is 1-2 wt%, the concentration of silver nitrate in the silver nitrate precursor solution is 1-2 wt%, the slow dripping rate is 1.25-1.5 mL / h, and the reaction time is 1-2 h.

[0011] As a preferred embodiment, the soluble chloride salt is selected from at least one of sodium chloride, ferric chloride, copper chloride, and lithium chloride, and the soluble bromide salt is selected from at least one of sodium bromide and potassium bromide.

[0012] As a preferred embodiment, in step (2), the AgNPs dispersion is AgNPs dispersed in ethanol with a concentration of 2-4 mg / mL; the ultrasonic power is 50-100 W; the immersion time is 10-30 min; and the immersion is repeated 2-4 times.

[0013] As a preferred embodiment, in step (3), the modified solution is prepared by dissolving silane coupling agent KH550 in an aqueous ethanol solution at a concentration of 1-3 wt% and adjusting the pH to 4-5. The modified fabric / AgNPs were immersed in the modification solution at a reaction temperature of 40–60°C for 1–2 hours. After the reaction was completed, the fabric was washed and dried.

[0014] As a preferred embodiment, in step (4), the AgNWs dispersion is AgNWs dispersed in ethanol with a concentration of 2-4 mg / mL; the ultrasonic power is 50-100 W; the immersion time is 10-30 min; and the immersion is repeated 2-4 times.

[0015] As a preferred embodiment, in step (5), the concentration of polydimethylsiloxane prepolymer in the coating solution is 5-20 wt%, the coating solution is uniformly coated with a scraper, the wet film thickness is controlled at 50-200 μm, the curing temperature is 60-100℃, and the curing time is 1-2 h.

[0016] As a preferred embodiment, the fabric is a polyester fabric, nylon fabric, spandex fabric, blended fabric, or similar fabric.

[0017] Compared with the prior art, the beneficial effects of this invention are: (1) The sequential construction of silver nanowires and particles on the fiber surface of the present invention: By performing a multi-level surface pretreatment of the fabric by "physical etching-chemical anchoring-molecular bridging", the nano-silver is loaded on the fiber surface. In particular, the silver nanoparticles and silver nanowires are loaded on the fiber surface in sequence, so that the fiber surface has both silver nanoparticles with significant plasma resonance effect and silver nanowires to build a silver nano network. The silver nanoparticles and silver nanowires are loaded in layers in sequence, with clear structural layers, which optimizes the photothermal heating performance of the fabric. (2) The fabric of the present invention has excellent photothermal properties and is durable: the layered loading ensures the efficient and firm loading of nano-silver on the fiber surface, laying the foundation for excellent photothermal properties; the polydimethylsiloxane PDMS encapsulation layer, while maintaining the original feel and breathability of the fabric, further fixes the nano-silver on the fiber and isolates the nano-silver from the external environment, effectively preventing performance degradation caused by friction, washing and oxidation, and further improving its photothermal performance durability; the PDMS encapsulation layer additionally gives the fabric hydrophobicity, expanding the practical application range of the fabric; (3) The photothermal heating functional fabric preparation process of the present invention is highly controllable and widely applicable: from interface activation to PDMS encapsulation, the entire process is solution treatment, the conditions are simple and easy to operate, the parameters are easy to adjust, and it is suitable for large-scale production. This pretreatment system has universality and can also provide a reference for the preparation of functional fabrics by loading other functional nanomaterials (such as graphene, Mxene, zinc oxide, silicon dioxide, titanium dioxide, etc.). Attached Figure Description

[0018] Figure 1 SEM images of the polyester surface in Example 1 of this invention: (a) PET fabric; (b) PET fiber; Figure 2 The polyester fabric of Example 1 of this invention is at 1000W / m 2 Infrared thermal images at different times under light intensity irradiation; Figure 3 This is a SEM image of the polyester fibers after alkali pretreatment in Example 2 of the present invention; Figure 4 This is a SEM image of polyester fibers pretreated with alkali and dopamine in Example 2 of the present invention; Figure 5 SEM images of silver nanoparticles, silver nanowires, and silver nanowire particles from Example 2 of this invention; Figure 6 This is a SEM image of polyester fibers loaded with silver nanoparticles after alkali + dopamine pretreatment in Example 2 of the present invention. Figure 7 This is a SEM image of polyester fibers loaded with silver nanoparticles after alkali + dopamine pretreatment in Example 2 of the present invention, followed by KH550 treatment and then loading with silver nanowires. Figure 8 The polyester fabric loaded with silver nanoparticles in Example 2 of this invention, and the polyester fabric loaded with silver nanoparticles and silver nanowires in layers sequentially, are shown at 1000 W / m 2 Infrared thermal images at different times under light intensity irradiation; Figure 9 This is a SEM image of the polyester fabric loaded with silver nanowires after pretreatment with alkali + dopamine + KH550 in Example 3 of the present invention. Figure 10 The polyester fabric loaded with silver nanowires after pretreatment with alkali + dopamine + KH550 in Example 3 of this invention is at 1000W / m 2 Infrared thermal images at different times under light intensity irradiation; Figure 11 This is a SEM image of the distribution of silver nanowires and silver nanoparticles on a polyester fabric loaded with silver nanowires after pretreatment with alkali + dopamine + KH550 in Example 3 of the present invention. Figure 12 This is a TEM image of PVDF fibers containing silver nanoparticles and silver nanowires in Example 4 of the present invention. Figure 13 The PVDF fiber membrane containing silver nanoparticles and silver nanowires in Example 4 of this invention is at 1000 W / m 2Infrared thermal images at different times under light intensity irradiation (subscripts 1, 2, and 3 represent irradiation for 1 min, 3 min, and 5 min, respectively). Figure 14 This is the time-temperature change curve of the PVDF fiber membrane containing silver nanoparticles and silver nanowires in Example 4 of the present invention. Figure 15 This is a diagram illustrating the mechanism of action between dopamine and KH550 in Example 5 of the present invention for the formation of polydopamine. Figure 16 This is a SEM image of a polyester fabric with layered loading of silver nanoparticles and silver nanowires based on PDMS encapsulation in Embodiment 5 of the present invention. Figure 17 This is the durability test result of the polyester fabric based on PDMS encapsulation with layered loaded silver nanoparticles and silver nanowires in Example 5 of the present invention. Detailed Implementation

[0019] The following provides a detailed description of the preparation method of the durable photothermal heating fabric based on nano-silver layered loading according to the present invention.

[0020] The method for preparing a durable photothermal heating fabric based on nano-silver layered loading according to the present invention includes the following steps: (1) The fabric was surface treated with sodium hydroxide (NaOH) and polydopamine (PDA) respectively, washed with deionized water and dried in a vacuum oven to obtain the pretreated fabric. The fabrics are selected from polyester fabrics, nylon fabrics, spandex fabrics, blended fabrics and similar fabrics, and the specific selection can be made according to the actual application requirements. The sodium hydroxide (NaOH) used above is a 5-10 wt% NaOH aqueous solution, and the ultrasonic treatment time is 30-90 min. The specific concentration and treatment time can be determined according to the actual application requirements. The fabric treated with sodium hydroxide (NaOH) was immersed in a Tris buffer solution of polydopamine and stirred at 30–40°C for 12–24 hours. After washing and drying, the pretreated fabric was obtained. The pH of the Tris buffer solution was 8.0–8.8. The specific stirring temperature, time, and pH could be determined according to the actual application requirements. Specifically, after adjusting the pH of the Tris buffer solution to 8.0–8.8 with HCl, dopamine (DA) is dissolved in the Tris-HCl buffer solution, and dopamine undergoes self-polymerization to generate polydopamine (PDA) to prepare a PDA-Tris solution.

[0021] (2) Nanosilver nanoparticles with different morphologies were prepared by the polyol method; Ethylene glycol (EG) was used as a solvent and reducing agent, polyvinylpyrrolidone (PVP) as a stabilizer, and sodium chloride (NaCl) and sodium bromide (NaBr) as morphology control agents. A silver nitrate precursor solution was slowly added dropwise to the reaction system under heating conditions of 150–180 °C. The generation and morphology regulation of silver nanoparticles were achieved by changing the volume ratio of the two morphology control agents (NaCl:NaBr = 1–5 mL: 1 mL). After washing and purification, the reaction product was finally dispersed in ethanol to obtain silver nanoparticle (AgNPs) and silver nanowire (AgNWs) dispersions. The concentration of PVP in EG is 1-2 wt%, the concentration of silver nitrate in the silver nitrate precursor solution is 1-2 wt%, the slow dripping rate is 1.25-1.5 mL / h, and the reaction time is 1-2 h. The specific reference can be determined according to the actual application requirements. The sodium chloride mentioned above can also be replaced by at least one of sodium chloride, ferric chloride, copper chloride, and lithium chloride, and the sodium bromide mentioned above can also be replaced by at least one of sodium bromide and potassium bromide.

[0022] (3) The pretreated fabric was immersed in the AgNPs dispersion, ultrasonically impregnated and then vacuum dried to obtain the modified fabric / AgNPs-AgNWs; The AgNPs dispersion is AgNPs dispersed in ethanol at a concentration of 2–4 mg / mL; the ultrasonic power is 50–100 W; the immersion time is 10–30 min; and the immersion is repeated 2–4 times. The specific parameters can be determined according to the actual application requirements.

[0023] (4) The modified fabric / AgNPs were surface treated with silane coupling agent KH550, washed with deionized water and dried in a vacuum oven to obtain pretreated modified fabric / AgNPs. Specifically, the modification solution is prepared by dissolving silane coupling agent KH550 in an ethanol aqueous solution at a concentration of 1–3 wt% and adjusting the pH to 4–5; immersing the modified fabric / AgNPs in the modification solution at a reaction temperature of 40–60℃ for a reaction time of 1–2 hours; washing and drying after the reaction to obtain the pretreated modified fabric / AgNPs; specific parameters can be determined according to actual application requirements.

[0024] (5) The pretreated modified fabric / AgNPs was immersed in the AgNWs dispersion, ultrasonically impregnated and then vacuum dried to obtain the modified fabric / AgNPs-AgNWs; Specifically, the AgNWs dispersion is AgNWs dispersed in ethanol at a concentration of 2–4 mg / mL; the ultrasonic power is 50–100 W; the immersion time is 10–30 min; and the immersion is repeated 2–4 times. The specific parameters can be determined according to the actual application requirements.

[0025] (6) Mix polydimethylsiloxane PDMS prepolymer and curing agent in proportion and dissolve in n-hexane solvent to obtain coating solution. Apply coating solution evenly to fabric surface with a scraper and heat to cure PDMS crosslinking. Finally, a strong, uniform and durable coating is formed on fabric surface to obtain durable photothermal heating fabric. The concentration of polydimethylsiloxane prepolymer in the coating solution is 5-20 wt%. The coating solution is uniformly applied using a scraper, the wet film thickness is controlled at 50-200 μm, the curing temperature is 60-100℃, and the curing time is 1-2 h. Specific parameters can be determined according to actual application requirements.

[0026] The following specific embodiments further explain the preparation method of the durable photothermal heating polyester fabric based on nano-silver layered loading of the present invention.

[0027] Example 1: Unmodified polyester fabric; The purchased polyester plain weave fabric was ultrasonically cleaned with deionized water and dried. The resulting scanning electron microscope (SEM) image of the polyester fabric is shown below. Figure 1 As shown, the original polyester fiber surface is smooth, uniform, and has a clear outline. Therefore, the nanomaterial has a weak bonding force with the inert polyester surface and is easily detached due to friction or washing, resulting in rapid performance degradation and poor long-term stability.

[0028] A xenon lamp was used as the light source to simulate solar radiation, and it was shone vertically onto the fabric surface with a fixed light intensity of 1000 W / m. 2 (i.e., under sunlight), during the irradiation process, an infrared thermal imager is used to record the temperature changes of the fabric in real time, and the resulting temperature changes are as follows: Figure 2 As shown, the subscripts 1, 2, 3, and 4 of time t represent irradiation for 1 min, 10 min, 30 min, and 60 min, respectively. Due to the inherent properties of the fabric, it has a certain ability to heat up after xenon lamp irradiation, and finally stabilizes at around 41.5℃.

[0029] Example 2: Layered loading of silver nanoparticles (AgNPs) and silver nanowires (AgNWs); The preparation steps of the photothermal heated fabric in this embodiment are as follows: The polyester fabric from Example 1 was immersed in a 5 wt% NaOH solution and ultrasonically cleaned for 30 minutes at room temperature. It was then rinsed multiple times with deionized water until its surface pH reached neutral. Finally, it was dried at 60°C. The surface structure of the polyester fabric after alkali treatment is as follows: Figure 3 As shown, compared with the untreated fiber in Example 1, the fiber surface after alkali treatment has obvious pits, grooves and etching stripes, which provides a larger specific surface area and binding sites for subsequent modification.

[0030] (2) Prepare a 50 mM Tris buffer solution, adjust the pH to 8.5 with HCl, dissolve a certain mass of dopamine (DA) in the Tris-HCl buffer solution, and the dopamine undergoes self-polymerization to generate polydopamine (PDA) to prepare a 1 mg / mL PDA-Tris solution; place the polyester fabric pretreated by alkali etching in step (1) in the PDA-Tris solution (liquor ratio 1:50) and stir at 100 rpm for 12 h at 35 °C using a shaker; finally, wash the fabric three times with deionized water and then dry it in an oven at 40 °C. The surface structure of the polyester fabric pretreated with alkali and dopamine is as follows. Figure 4 As shown, after the polyester fabric that has undergone surface alkali etching pretreatment is further modified by dopamine polymerization, the surface morphology of the fiber changes significantly. The pits, grooves and etching stripes formed by alkali etching are covered by a dense layer of polydopamine nanoparticles, and the surface exhibits a typical granular rough structure, indicating that polydopamine has been successfully coated on the fiber surface.

[0031] (3) Nano-silver was prepared by the polyol method. The specific experimental steps are as follows: First, 1.68 g of polyvinylpyrrolidone (PVP) powder was added to 100 mL of ethylene glycol (EG) solvent. After being magnetically stirred at room temperature until completely dissolved, the solution was transferred to a three-necked flask. NaCl and NaBr were used as mixing control agents, and 3 mM of NaCl in EG solution and 3 mM of NaBr in EG solution were added dropwise to control the volume ratio of NaCl / EG and NaBr / EG solution. The reaction was heated in an oil bath at 160°C for 1 h. Under light-protected conditions, 0.5 g of silver nitrate (AgNO3) was dissolved in 25 mL of EG. After stirring and sonication, a clear AgNO3 solution was obtained. Then, the solution was pumped at 1.25 mL / h using a peristaltic pump. -1 The solution was slowly added dropwise to the reaction system at a certain rate, and the reaction was continued to be heated for 1 hour until the solution turned bright gray. After the reaction was completed, the solution was cooled to room temperature, and an appropriate amount of the reaction product was taken, washed by centrifugation with anhydrous ethanol several times, and then dried to obtain nano silver for later use. When the volume ratio of NaCl / EG and NaBr / EG solutions is controlled at 1 mL:1 mL during the preparation process, silver nanoparticles (AgNPs) can be obtained, with the structure shown below. Figure 5 As shown in (a); When the volume ratio of NaCl / EG and NaBr / EG solutions is controlled at 5 mL:1 mL, silver nanowires (AgNWs) can be obtained, with the structure shown below. Figure 5 As shown in (b); When the volume ratio of NaCl / EG and NaBr / EG solutions is controlled at 3 mL:1 mL, a mixture of silver nanowires and silver nanoparticles, namely silver nanowire particles (AgNWPs), can be obtained, with the structure shown below. Figure 5 As shown in (c); This embodiment yielded silver nanoparticles with regular morphology, silver nanowires with small diameter and high aspect ratio, and mixtures of silver nanoparticles and silver nanowires; for AgNWPs, the silver nanoparticles filled the gaps in the interlaced arrangement of silver nanowires, filling the blanks in the one-dimensional silver nanowire arrangement space.

[0032] (4) The polyester fabric (5cm×5cm) pretreated with alkali and dopamine was immersed in a 2mg / mL AgNPs ethanol dispersion, ultrasonically impregnated at 100W for 20min, and then vacuum dried at 60℃ for 30min. The process was repeated 3 times to obtain a polyester fabric with silver nanoparticles loaded on the surface. The obtained fabric was labeled as PET / AgNPs, and its structure is as follows. Figure 6 As shown, AgNPs are distributed relatively evenly on the fiber, with no obvious agglomeration and a high loading capacity.

[0033] (5) Dissolve 1% (v / v) KH550 in a mixed solvent of ethanol / water (95:5, v / v), adjust the pH to 4.5 with acetic acid, hydrolyze at room temperature for 30 min, then immerse the PET / AgNPs fabric in the solution and react at 50°C for 1 h; remove the fabric, ultrasonically clean it with ethanol for 10 min to remove unreacted KH550, and dry it at 60°C. (6) The PET / AgNPs fabric obtained after step (5) was immersed in a 2 mg / mL AgNWs ethanol dispersion, ultrasonically impregnated at 100 W for 20 min, and then vacuum dried at 60 °C for 30 min. The process was repeated 3 times to obtain a polyester fabric with silver nanoparticles AgNPs and silver nanowires AgNWs loaded on the surface. The obtained fabric was labeled as PET / AgNPs-AgNWs, and its structure is as follows. Figure 7 As shown, the high loading of silver nanowires covers the AgNPs that were initially loaded. At this point, the underlying AgNPs can no longer be observed, and a large number of silver nanowires on the surface interlock to form a distinct network structure.

[0034] The photothermal conversion performance of fabrics was evaluated using a xenon lamp to simulate solar radiation: the xenon lamp source was vertically irradiated onto the fabric surface, and the light intensity was adjusted to 1000 W·m. -2 (Under standard sunlight), during irradiation, the temperature change of the sample surface is monitored in real time, and surface thermal images are recorded at fixed intervals using an infrared thermal imager. The resulting temperature changes are as follows: Figure 8 As shown, the subscripts 1, 2, 3, and 4 of time t represent irradiation for 1 min, 10 min, 30 min, and 60 min, respectively. The PET / AgNPs fabric exhibits a significantly faster photothermal response than the PET fabric in Example 1, and reaches a stable saturation state within about 60 min, with a surface temperature of 62.9°C. The difference from the PET fabric is mainly attributed to the localized surface plasmon resonance effect of AgNPs. The polyester fabric PET / AgNPs-AgNWs obtained in this embodiment, with AgNPs and AgNWs sequentially loaded on its surface, exhibits a significantly faster photothermal response than the PET / AgNPs fabric loaded with only one layer of silver nanoparticles. It reaches a stable saturation state within about 60 minutes, with a surface temperature as high as 72.8°C. This significant difference is mainly attributed to the significant local surface plasmon resonance effect of AgNPs in the fabric, the continuous heat conduction channels constructed by AgNWs, and the synergistic effect of AgNPs and AgNWs, which makes the PET / AgNPs-AgNWs fabric exhibit a higher steady-state temperature and better photothermal conversion performance.

[0035] Example 3: Silver nanowires (AgNWPs) loaded only; The difference between the photothermal heating fabric in this embodiment and that in Embodiment 2 is: The polyester fabric was pretreated sequentially with NaOH + dopamine + KH550 as described in Example 2, then immersed in a 2 mg / mL silver nanowire AgNWPs ethanol dispersion, ultrasonically impregnated at 100 W for 20 min, and vacuum dried at 60 °C for 30 min. This process was repeated three times to obtain a photothermal heated PET / AgNWPs fabric, the structure of which is as follows. Figure 9 As shown, compared with Example 2, both zero-dimensional nanoparticles and one-dimensional silver nanowires can be observed on the surface of the polyester fiber loaded with silver nanowires. The silver nanowires intersect to form a three-dimensional conductive network, and the silver nanoparticles are distributed in the gaps between the nanowires.

[0036] The photothermal conversion performance of fabrics was evaluated using a xenon lamp to simulate solar radiation: the xenon lamp source was vertically irradiated onto the fabric surface, and the light intensity was adjusted to 1000 W·m. -2 (Under standard sunlight), during irradiation, the temperature change of the sample surface is monitored in real time, and surface thermal images are recorded at fixed intervals using an infrared thermal imager. The resulting temperature changes are as follows: Figure 10 As shown, the subscripts 1, 2, 3, and 4 of time t represent irradiation of 1 min, 10 min, 30 min, and 60 min, respectively. After simulating solar radiation, the photothermal heating fabric PET / AgNWPs exhibited a significantly faster photothermal response than the PET fabric in Example 1 but slower than in Example 2, reaching a stable saturation state within approximately 60 min, with a surface temperature of 64.2 °C. The faster photothermal response than the PET fabric in Example 1 is attributed to the localized surface plasmon resonance effect of AgNPs in AgNWPs, the continuous heat conduction channels constructed by AgNWs, and the synergistic effect of AgNPs and AgNWs. The slower photothermal response than the PET / AgNPs-AgNWs fabric in Example 2 is because the AgNPs are distributed in the gaps between the nanowires, such as... Figure 11 As shown, this not only blocks the overlap between AgNWs, but also makes them prone to detaching from between silver nanowires, thus affecting heat transfer.

[0037] Example 4: Photothermal heating type polyvinylidene fluoride (PVDF) fiber membrane with silver nanowires (AgNWPs) loaded in fibers; To compare the photothermal conversion performance of fabrics with silver nanoparticles encapsulated inside fibers and those loaded on the fiber surface, this embodiment uses wet spinning to load silver nanoparticles and silver nanowires inside PVDF fibers to obtain PVDF@AgNWPs fiber membranes. The temperature rise of the fiber membrane under xenon lamp irradiation when AgNWPs are inside the fibers is analyzed.

[0038] The specific experimental procedure is as follows: 2 wt% (relative to the wet spinning solution) of silver nanowires (AgNWPs) were ultrasonically dispersed in a mixed solvent of DMF and acetone (weight ratio 6:4); then, 16 wt% of PVDF powder was added to the AgNWPs mixed dispersion, and the mixture was magnetically stirred at 60°C for 4 hours to form a uniform spinning solution; PVDF@AgNWPs fiber membranes were obtained by wet spinning.

[0039] TEM structure of fiber membrane as follows Figure 12 As shown, to ensure proper spinning and fiber quality, the amount of silver nanoparticles encapsulated inside the fiber is far less than the amount of silver nanoparticles loaded on the fiber surface. Therefore, the probability of silver nanoparticles overlapping and forming a network structure inside the fiber is greatly reduced. Consequently, the photothermal conversion performance of the PVDF@AgNWPs fiber membrane obtained in this embodiment is inferior to that of the PET fabrics with silver nanoparticles loaded on their surfaces in Examples 2 and 3.

[0040] Photothermal conversion tests were conducted on PVDF@AgNWPs fiber membranes, and the temperature changes were as follows: Figure 13 As shown, the subscripts 1, 2, and 3 of time b represent irradiation for 1 min, 3 min, and 5 min, respectively. The resulting time-temperature change curves are shown below. Figure 14 As shown, after 5 minutes of illumination, the surface temperature of the PVDF@AgNWPs fiber membrane stabilized at approximately 48°C, which is similar to the photothermal conversion performance of the PET fabric in Example 1. This further demonstrates the advanced nature of the preparation method of the durable photothermal heating functional polyester fabric based on nano-silver provided by this invention.

[0041] Example 5: Durable photothermal heating polyester fabric with layered loading of AgNPs and AgNWs; This embodiment is based on embodiment 2, but with PDMS encapsulation. In Example 2, the mechanism of action of dopamine after self-polymerization to form polydopamine and KH550 is as follows: Figure 15 As shown; since silver nanoparticles cannot completely cover the fiber surface, in step (5) of Example 2, KH550 reacts with the remaining PDA on the fiber surface that is not covered by AgNPs (i.e., does not react with AgNPs); the present invention first grafts silver nanoparticles onto the polydopamine surface, and then grafts silver nanowires onto the KH550 surface, realizing the layered loading of AgNPs and AgNWs on the PET fiber surface from the perspective of "chemical anchoring-molecular bridging". Compared with Example 3, which first pre-treats PET fibers with alkali + dopamine + KH550, and then loads silver nanowires AgNWPs (i.e., simultaneously loads silver nanoparticles and silver nanowires), the layered loading of silver nanoparticles and silver nanowires in Example 2 has better durability, which also reflects the advanced nature of the preparation method of durable photothermal heating functional polyester fabric based on nano-silver provided by the present invention.

[0042] Specifically, in this embodiment, PDMS prepolymer and curing agent are mixed at a ratio of 10:1 and dissolved in n-hexane, and stirred evenly to prepare a coating solution with a concentration of 5wt%. The photothermal heated polyester fabric PET / AgNPs-AgNWs substrate of Example 2 is flattened and fixed, and the coating solution is uniformly coated onto the fabric surface using a scraper. The wet film thickness after scraping is controlled at 100μm. Subsequently, the coated fabric is placed in an oven and heated and cured at 80°C for 1 hour to allow PDMS to crosslink and form, resulting in a durable photothermal heated polyester fabric PDSM@PET / AgNPs-AgNWs. (3) The PET / AgNPs-AgNWs fabric encapsulated in PDMS was subjected to friction, ultrasonic washing, and wet oxidation, and then subjected to photothermal heating tests. The temperature changes obtained after 10 minutes of irradiation are as follows: Figure 17 As shown.

[0043] The PET / AgNPs-AgNWs fabric obtained in Example 2 has a fast photothermal response and a high steady-state temperature, but long-term exposure to air inevitably leads to silver oxidation and a reduced service life. To address this, a flexible polymer layer, PDMS, is used to physically encapsulate and isolate the loaded silver nanoparticles. Figure 16 As shown, while maintaining the fabric's porous structure, the durability and practicality of the functional layer are further enhanced.

[0044] In addition, the PDMS-encapsulated PET / AgNPs-AgNWs fabric was subjected to photothermal heating tests after 40 cycles of rubbing, 10 cycles of ultrasonic washing, and 48 hours of wet oxidation. The temperature changes obtained after 10 minutes of irradiation are shown below. Figure 17As shown, PDMS encapsulation can effectively prevent nanomaterials from falling off due to friction and washing, and isolate them from oxygen and water vapor to inhibit chemical aging, so that the photothermal properties remain basically stable after multiple washes. In addition, while maintaining the softness and breathability of the substrate, it can also give it excellent hydrophobic and anti-fouling properties.

[0045] In the above embodiments, whether silver nanoparticles (AgNPs) and silver nanowires (AgNWs) are loaded in layers, or silver nanowires (AgNWPs) are loaded alone, the amount of Ag loaded must be kept consistent for effect comparison.

[0046] Given that there are numerous embodiments of the present invention, and the raw materials and quantities involved can be selected within a limited range according to actual needs, and that the experimental data for each embodiment are extensive and numerous, it is not suitable to list and describe them one by one here. However, the content to be verified and the final conclusions obtained in each embodiment are similar. Therefore, the verification content of each embodiment will not be described one by one here.

[0047] The above description is merely a detailed explanation of preferred embodiments and principles of the present invention. For those skilled in the art, there may be changes in specific implementation methods based on the ideas provided by the present invention, and these changes should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing a durable photothermal heating fabric based on nano-silver layered loading, characterized in that, Includes the following steps: (1) The fabric is surface-treated with alkali solution and polydopamine in sequence to obtain pretreated fabric; Silver nanoparticles (AgNPs) and silver nanowires (AgNWs) were prepared using the polyol method. (2) The pretreated fabric was immersed in AgNPs dispersion, ultrasonically impregnated and then vacuum dried to obtain modified fabric / AgNPs; (3) The modified fabric / AgNPs were surface-treated with a silane coupling agent to obtain pretreated modified fabric / AgNPs; (4) The pretreated modified fabric / AgNPs was immersed in the AgNWs dispersion, ultrasonically impregnated and then vacuum dried to obtain the modified fabric / AgNPs-AgNWs; (5) Mix the polydimethylsiloxane prepolymer with the curing agent and dissolve it in n-hexane solvent to obtain a coating solution. Apply the coating solution evenly to the surface of the modified fabric / AgNPs-AgNWs and heat to cure to obtain a durable photothermal heating fabric.

2. The preparation method according to claim 1, characterized in that, In step (1), the alkaline solution is a 5-10 wt% NaOH aqueous solution, and the ultrasonic treatment time is 30-90 min.

3. The preparation method according to claim 1, characterized in that, In step (1), the fabric treated with alkali is immersed in a Tris buffer solution of polydopamine and stirred at 30-40°C for 12-24 hours. Then it is washed and dried to obtain the pretreated fabric. The pH of the Tris buffer solution is 8.0–8.

8.

4. The preparation method according to claim 1, characterized in that, In step (1), the polyol method includes: Using ethylene glycol (EG) as a solvent and reducing agent, polyvinylpyrrolidone (PVP) as a stabilizer, and soluble chloride and bromide salts as morphology control agents, silver nitrate precursor solution was slowly added dropwise to the above reaction system at 150–180 °C. By changing the volume ratio of the two morphology control agents, silver nanoparticles (AgNPs) and silver nanowires (AgNWs) were prepared respectively.

5. The preparation method according to claim 4, characterized in that, The concentration of PVP in EG is 1-2 wt%, the concentration of silver nitrate in the silver nitrate precursor solution is 1-2 wt%, the slow dripping rate is 1.25-1.5 mL / h, and the reaction time is 1-2 h.

6. The preparation method according to claim 4, characterized in that, The soluble chloride salt is selected from at least one of sodium chloride, ferric chloride, copper chloride, and lithium chloride, and the soluble bromide salt is selected from at least one of sodium bromide and potassium bromide.

7. The preparation method according to claim 1, characterized in that, In step (2), the AgNPs dispersion is AgNPs dispersed in ethanol at a concentration of 2-4 mg / mL; the ultrasonic power is 50-100W; the immersion time is 10-30 min; and the immersion is repeated 2-4 times.

8. The preparation method according to claim 1, characterized in that, In step (3), the modified solution is prepared by dissolving silane coupling agent KH550 in an aqueous ethanol solution at a concentration of 1-3 wt% and adjusting the pH to 4-5. The modified fabric / AgNPs were immersed in the modification solution at a reaction temperature of 40–60°C for 1–2 hours. After the reaction was completed, the fabric was washed and dried.

9. The preparation method according to claim 1, characterized in that, In step (4), the AgNWs dispersion is AgNWs dispersed in ethanol at a concentration of 2-4 mg / mL; the ultrasonic power is 50-100W; the immersion time is 10-30 min; and the immersion is repeated 2-4 times.

10. The preparation method according to claim 1, characterized in that, In step (5), the concentration of polydimethylsiloxane prepolymer in the coating solution is 5-20 wt%. The coating solution is uniformly coated with a scraper, the wet film thickness is controlled at 50-200 μm, the curing temperature is 60-100℃, and the curing time is 1-2 h.