A lightweight, high-elasticity microfiber synthetic leather base fabric and its preparation method

By utilizing the synergistic effect of bicomponent core-sheath composite fibers and microsphere fillers, the problems of lightweight and high elasticity of microfiber base fabrics have been solved, and the preparation of ultra-lightweight, high-elasticity microfiber synthetic leather base fabrics has been achieved. These fabrics possess excellent compression resilience and tear strength, making them suitable for high-end products.

CN123108951APending Publication Date: 2026-11-17禾欣可乐丽超纤皮(嘉兴)有限公司 +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611400859.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing microfiber base fabrics have significant limitations in terms of lightweighting and high elasticity. Traditional manufacturing processes result in base fabrics that are too heavy and lack elasticity, making it difficult to meet the lightweighting and flexible coating requirements of high-end products.

Method used

By using two-component core-sheath composite fibers and controlling the mass ratio of core-sheath components and the use of microsphere fillers, combined with needle punching and impregnation slurry treatment, ultra-lightweight, high-elasticity microfiber synthetic leather base fabric is prepared. This includes using hollow glass microspheres, foamed microspheres, or silica microspheres to form a hollow structure and a porous elastomer network.

Benefits of technology

It achieves ultra-lightweight and high elasticity of the base fabric, maintains sufficient tear strength, has the feel of high-grade natural leather and multi-dimensional elasticity, and meets the comfort and flexibility requirements of high-end products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108951A_ABST
    Figure CN123108951A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric. The method first prepares a bicomponent composite fiber with a specific core-sheath structure, wherein the sheath is PA or PET, and the core is PE, COPET, or PVA, with a core-sheath mass ratio of 30:70-50:50. Subsequently, the fiber is processed into a low-density fiber (0.18-0.26 g / cm³). 3 Nonwoven fabric. The key step is impregnation with a slurry containing special fillers, including polyurethane resin, hollow glass microspheres / foamed microspheres / silica microspheres. After impregnation, coagulation, weight reduction (removal of core components), oiling, and drying, the base fabric is finally obtained. By combining low-density nonwoven fabric, microspheres in the slurry, and the hollow structure formed after fiber weight reduction, significant lightweighting and high elasticity of the base fabric are synergistically achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of microfiber base fabric preparation technology, specifically relating to an ultralight, high-elasticity microfiber synthetic leather base fabric and its preparation method. Background Technology

[0002] Microfiber synthetic leather, due to its appearance, feel, and physical properties being similar to natural leather, and its advantages such as uniform specifications and ease of processing, has been widely used in footwear, bags, furniture, automotive interiors, and apparel. Its core performance lies in the microfiber synthetic leather base fabric used. An ideal microfiber base fabric should, in addition to mechanical strength and durability, also possess lighter weight and superior elasticity to meet the increasingly demanding requirements of high-end products for lightweight, flexible coverage, and comfort.

[0003] However, conventional microfiber base fabric products currently on the market still have significant limitations in terms of lightweighting and high elasticity, mainly due to their traditional manufacturing processes and structures:

[0004] 1) High weight: In order to ensure the strength and fullness of the base fabric, traditional processes usually use a high non-woven fabric needle punching density and use solid polyurethane resin for impregnation and filling. This results in a high apparent density of the final product, which affects the lightweight level of the finished product.

[0005] 2) Insufficient elasticity: The elasticity of conventional base fabric mainly depends on the elasticity of polyurethane resin itself and the bending recovery of fibers. The single continuous resin phase and solid fiber structure limit the overall compression resilience and multi-dimensional fluffy elasticity of the base fabric, making it difficult to achieve the high elasticity of high-grade natural leather or certain special sponge materials.

[0006] While the industry has a clear demand for lightweight, highly elastic microfiber base fabrics, simply reducing density or replacing a single material often leads to a significant decrease in the mechanical properties of the base fabric (such as tear strength) or an inability to consistently achieve sustained high elasticity. Therefore, a novel systematic preparation method is needed to synergistically achieve both "ultra-lightweight" and "highly elastic" base fabrics without sacrificing key physical properties. Summary of the Invention

[0007] To address the above problems, the present invention aims to provide an ultralight, high-elasticity microfiber synthetic leather base fabric and its preparation method.

[0008] The specific technical solution is as follows:

[0009] A method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric includes the following steps:

[0010] S1. Preparation of bicomponent sheath-core composite fiber: PA or PET is used as the sheath component, and PE, COPET or PVA is used as the core component. The mass ratio of the sheath component to the core component is controlled to be 30:70-50:50. The bicomponent sheath-core composite fiber is obtained by melt spinning.

[0011] S2. Preparation of nonwoven fabric: The bicomponent core-sheath composite fiber obtained in step S1 is processed by needle punching or needle punching and ironing to produce a fabric with a density of 0.18-0.26 g / cm³. 3 Non-woven fabric;

[0012] S3. Impregnation and post-treatment: The nonwoven fabric obtained in step S2 is impregnated in an impregnation slurry, and then coagulation, weight reduction, oiling and drying are carried out in sequence to obtain ultra-lightweight high-elastic microfiber synthetic leather base fabric.

[0013] In step S3, the impregnating slurry contains polyurethane resin and microspheres, and the microspheres are selected from at least one of hollow glass microspheres, foamed microspheres, and silica microspheres.

[0014] Furthermore, the polyurethane resin solid content in the impregnated slurry is 15%-25%, the microsphere solid content is 10%-30%, the total solid content of the impregnated slurry is 25%-40%, and the viscosity at 40℃ is 2000-20000 cps.

[0015] Furthermore, the particle size of the microspheres is 1-30 μm.

[0016] Furthermore, in step S3, the reduction process is toluene reduction, alkali reduction, or hot water reduction.

[0017] Furthermore, the polyurethane resin is a solvent-based polyurethane resin or a water-based polyurethane resin.

[0018] The beneficial effects of this invention are as follows:

[0019] (1) Ultra-lightweight: This invention controls the density of the nonwoven fabric to be between 0.18 and 0.26 g / cm³. 3 The material has a lower density, and low-density microsphere fillers such as hollow glass microspheres, foamed microspheres or silica microspheres are introduced into the impregnation slurry. The hollow structure formed after the fiber is reduced in weight also works together to significantly reduce the apparent density of the product while ensuring the physical properties of the base fabric, thus achieving ultra-lightweight base fabric.

[0020] (2) High elasticity: The microspheres in the impregnating slurry form a porous elastomer network after solidification, giving the base fabric excellent compression resilience; at the same time, the core fiber is removed after weight reduction treatment to form hollow ultrafine fiber. The hollow structure further enhances the bending flexibility and elastic recovery ability of the fiber, making the base fabric fluffy, soft and highly elastic, close to the feel of high-grade natural leather.

[0021] (3) Stable mechanical properties: The present invention uses a two-component composite fiber with a specific core-sheath mass ratio (30:70-50:50). After the sheath is reduced in weight, it still maintains sufficient fiber strength and entanglement, ensuring that the tear strength of the base fabric does not decrease significantly due to the lightweighting process, thus achieving a good balance between ultra-lightweight, high elasticity and strength. Attached Figure Description

[0022] Figure 1 This is a cross-sectional scanning electron microscope (SEM) image of the ultralight and highly elastic microfiber substrate prepared in Example 2 of the present invention;

[0023] Figure 2 This is a cross-sectional scanning electron microscope (SEM) image of the ultralight and highly elastic microfiber substrate prepared in Example 3 of the present invention. Detailed Implementation

[0024] The present invention will be further described below with reference to the accompanying drawings and embodiments, but the scope of protection of the present invention is not limited thereto.

[0025] Example 1

[0026] A method for preparing a common type of microfiber synthetic leather base fabric includes the following steps:

[0027] 1) PA6 is the sheath component and PE is the core component. After high-temperature melt spinning at 245℃ and subsequent spinning processes, a bicomponent sheath-core composite fiber that meets the subsequent requirements is obtained.

[0028] 2) The mass ratio of the core and sheath components is PA6:PE = 50:50;

[0029] 3) Nonwoven fabric with a density of 0.28 g / cm³ is obtained by needle punching and ironing bicomponent core-sheath composite fibers. 3 ;

[0030] 4) The nonwoven fabric is impregnated, and then coagulated, reduced with toluene, oiled, and dried to obtain a common type of microfiber base fabric. The impregnating slurry contains 32% solvent-based polyurethane resin, has a total solid content of 32%, and a viscosity of 8500 cps at 40℃.

[0031] Example 2

[0032] A method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric includes the following steps:

[0033] 1) PA6 is used as the sheath component and PE is used as the core component. After high-temperature melt spinning at 245℃ and subsequent spinning processes, a bicomponent sheath-core composite fiber that meets the subsequent requirements is obtained.

[0034] 2) The mass ratio of the core and sheath components is PA6:PE = 45:55;

[0035] 3) Nonwoven fabric with a density of 0.24 g / cm³ is obtained by needle punching and ironing bicomponent core-sheath composite fibers. 3 ;

[0036] 4) The nonwoven fabric is impregnated, then coagulated, reduced with toluene, oiled, and dried to obtain an ultra-lightweight, high-elasticity microfiber base fabric. The impregnation slurry contains 15% solvent-based polyurethane resin, 15% hollow glass microspheres (5μm), and 30% total solids. The viscosity at 40℃ is 8500 cps.

[0037] The cross-sectional scanning electron microscope (SEM) image of the ultralight, high-elasticity microfiber substrate prepared in this embodiment is shown below. Figure 1 As shown, the distribution of microspheres in the impregnated slurry within the fiber network and the hollow fiber structure formed after weight reduction treatment are illustrated.

[0038] Example 3

[0039] A method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric includes the following steps:

[0040] 1) PA66 is used as the sheath component and PE is used as the core component. After high-temperature melt spinning at 265℃ and subsequent spinning processes, a bicomponent sheath-core composite fiber that meets the subsequent requirements is obtained.

[0041] 2) Core-sheath component mass ratio: PA66:PE = 40:60;

[0042] 3) Nonwoven fabric with a density of 0.25 g / cm³ is obtained by needle punching and ironing bicomponent core-sheath composite fibers. 3 ;

[0043] 4) The nonwoven fabric is impregnated, and then solidified, reduced with toluene, oiled and dried to obtain an ultra-lightweight and high-elastic microfiber base fabric. The impregnation slurry has a solvent-based polyurethane resin solid content of 16%, silica microspheres (10μm) solid content of 16%, total solid content of 32%, and viscosity of 9400 cps at 40℃.

[0044] The cross-sectional scanning electron microscope (SEM) image of the ultralight, high-elasticity microfiber substrate prepared in this embodiment is shown below. Figure 2 As shown, the morphology of silica microspheres uniformly dispersed in a polyurethane matrix and the overall loose and porous microstructure of the substrate fabric are demonstrated.

[0045] Example 4

[0046] A method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric includes the following steps:

[0047] 1) PET is used as the sheath component and PE is used as the core component. After high-temperature melt spinning at 270℃ and subsequent spinning processes, a bicomponent sheath-core composite fiber that meets the subsequent requirements is obtained.

[0048] 2) Core-sheath component mass ratio: PET:PE = 38:62;

[0049] 3) Nonwoven fabric with a density of 0.255 g / cm³ is obtained by needle punching and ironing bicomponent core-sheath composite fibers. 3 ;

[0050] 4) The nonwoven fabric is impregnated, and then solidified, reduced with toluene, oiled and dried to obtain an ultra-lightweight and high-elastic microfiber base fabric. The impregnation slurry contains 20% solvent-based polyurethane resin, 18% hollow glass microspheres (7μm) and 38% total solids. The viscosity at 40℃ is 11000 cps.

[0051] Example 5

[0052] A method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric includes the following steps:

[0053] 1) PET is used as the sheath component and COPET is used as the core component. After high-temperature melt spinning at 280℃ and subsequent spinning processes, a bicomponent sheath-core composite fiber that meets the requirements of subsequent processes is obtained.

[0054] 2) Core-sheath component mass ratio: PET:COPET = 35:65;

[0055] 3) Nonwoven fabric with a density of 0.26 g / cm³ is obtained by needle punching and ironing bicomponent core-sheath composite fibers. 3 ;

[0056] 4) The nonwoven fabric is impregnated, and then coagulated, alkali reduced, oiled and dried to obtain an ultra-lightweight and high-elastic microfiber base fabric. The impregnation slurry has a waterborne polyurethane solid content of 17%, a foamed microsphere (20μm) solid content of 20%, a total solid content of 37%, and a viscosity of 2300 cps at 40℃.

[0057] Example 6

[0058] A method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric includes the following steps:

[0059] 1) PET is used as the sheath component and PVA is used as the core component. After high-temperature melt spinning at 262℃ and subsequent spinning processes, a bicomponent sheath-core composite fiber that meets the subsequent requirements is obtained.

[0060] 2) Core-sheath component mass ratio: PET:PVA = 48:52;

[0061] 3) Nonwoven fabric with a density of 0.238 g / cm³ is obtained by needle punching and ironing bicomponent core-sheath composite fibers. 3 ;

[0062] 4) The nonwoven fabric is impregnated, and then solidified, reduced by hot water, oiled and dried to obtain an ultra-lightweight and high-elastic microfiber base fabric. The impregnation slurry has a waterborne polyurethane solid content of 18%, silica microspheres (16μm) solid content of 18%, a total solid content of 36%, and a viscosity of 2000 cps at 40℃.

[0063] Example 7

[0064] A method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric includes the following steps:

[0065] 1) PA6 is used as the sheath component and PVA is used as the core component. After high-temperature melt spinning at 230℃ and subsequent spinning processes, a bicomponent sheath-core composite fiber that meets the subsequent requirements is obtained.

[0066] 2) Core-sheath component mass ratio PA:PVA = 50:50;

[0067] 3) Nonwoven fabric with a density of 0.22 g / cm³ is obtained by needle punching and ironing bicomponent core-sheath composite fibers. 3 ;

[0068] 4) The nonwoven fabric is impregnated, and then solidified, reduced by hot water, oiled and dried to obtain an ultra-lightweight and high-elastic microfiber base fabric. The impregnation slurry has a waterborne polyurethane solid content of 20%, foamed microspheres (22μm) solid content of 16%, a total solid content of 36%, and a viscosity of 2400 cps at 40℃.

[0069] The above seven groups of samples underwent tests for resilience, apparent density, and tear strength. The test methods were in accordance with GB / T 6670-2008: Determination of Resilience Performance of Flexible Foam Polymer Materials by Falling Ball Method, GB / T 39500-2020: Determination of Apparent Density and Mass per Unit Area (Bulk Density Conversion Combined with Thickness) of Leather (Physical and Mechanical Testing), and QB / T 2711-2005: Determination of Tear Strength of Leather (Double-Sided Tear Method). All tests were conducted under a base fabric thickness of 1.5 mm. The test results are shown in Table 1 below.

[0070] Table 1 Summary of rebound rate and density of samples prepared in Examples 1-7

[0071]

[0072] The data results above show that by improving the spinning process and the density of the original fabric, the sample with added microspheres exhibited significantly improved resilience and density. This indicates that improving the spinning process and the density of the original fabric, along with the addition of microspheres, has a significant effect on improving the elasticity and lightweight properties of the microfiber base fabric, while the tear strength changes little. This method can provide a new approach for the preparation of ultralight, high-elasticity microfiber synthetic leather base fabric.

[0073] The above description is merely a preferred embodiment of the present invention. It should be noted that the scope of protection of the present invention is not limited thereto. Any person skilled in the art who, within the technical scope disclosed in the present invention, conceives of the invention and makes equivalent substitutions or modifications based on the technical solution of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric, characterized in that, Includes the following steps: S1. Preparation of bicomponent sheath-core composite fiber: PA or PET is used as the sheath component, and PE, COPET or PVA is used as the core component. The mass ratio of the sheath component to the core component is controlled to be 30:70-50:

50. The bicomponent sheath-core composite fiber is obtained by melt spinning. S2. Preparation of nonwoven fabric: The bicomponent core-sheath composite fiber obtained in step S1 is processed by needle punching or needle punching and ironing to produce a fabric with a density of 0.18-0.26 g / cm³. 3 Non-woven fabric; S3. Impregnation and post-treatment: The nonwoven fabric obtained in step S2 is impregnated in an impregnation slurry, and then coagulation, weight reduction, oiling and drying are carried out in sequence to obtain ultra-lightweight high-elastic microfiber synthetic leather base fabric. In step S3, the impregnating slurry contains polyurethane resin and microspheres, and the microspheres are selected from at least one of hollow glass microspheres, foamed microspheres, and silica microspheres.

2. The method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric as described in claim 1, characterized in that, The impregnated slurry contains 15%-25% polyurethane resin solids, 10%-30% microsphere solids, and a total solids content of 25-40%, with a viscosity of 2000-20000 cps at 40℃.

3. The method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric as described in claim 1, characterized in that, The microspheres have a particle size of 1-30 μm.

4. The method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric as described in claim 1, characterized in that, In step S3, the reduction treatment is toluene reduction, alkali reduction, or hot water reduction.

5. The method for preparing an ultralight, high-elasticity, microfiber synthetic leather base fabric as described in claim 2, characterized in that, The polyurethane resin is either solvent-based or water-based.