A modification method to improve the bonding properties of pulp fibers

By using a one-step method to synergistically modify pulp fibers through demethylation and hydroxymethylation in an acidic catalytic system, the problems of high energy consumption and pollution associated with existing pulp fiber modification methods are solved. This method improves fiber bonding performance and enhances the bulk and tensile strength of paper.

CN123108974APending Publication Date: 2026-11-17CENTRAL SOUTH UNIVERSITY OF FORESTRY AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202610974047.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-01
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing pulp fiber modification methods suffer from high energy consumption and pollution, and it is difficult to address the low hydroxyl accessibility caused by lignin coverage in chemimechanical pulp, resulting in poor fiber binding performance and making it unsuitable for high-strength packaging paper products.

Method used

A one-step method was adopted in an acidic catalytic system to improve the reactivity of cellulose and lignin by combining demethylation and hydroxymethylation reactions through a hydroxymethylation-rich solution and cationization modification, thereby enhancing the hydrogen bonding and cross-linking ability between fibers and achieving synergistic modification of lignin by demethylation and hydroxymethylation.

Benefits of technology

It significantly improves the content of active groups and fiber bonding force of pulp fibers, enhances the bulk and tensile strength of paper, simplifies the process, saves time and costs, and solves the problems of high energy consumption and pollution in traditional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108974A_ABST
    Figure CN123108974A_ABST
Patent Text Reader

Abstract

This invention discloses a modification method for improving the bonding properties of pulp fibers, belonging to the field of fiber modification technology. The modification method of this invention includes the following steps: (1) preparing a hydroxymethylation-rich solution; (2) hydroxymethylation of pulp fibers; (3) cationic modification; and (4) preparation of pulp fibers combining hydroxymethylation and cationic modification. This invention develops an acidic molten salt hydrate system to achieve hydroxymethylation and demethylation modification of lignin molecules in pulp fibers in a one-step process. Based on this, the modified pulp is further cationic modified to enhance the bonding force between fibers. The modification method of this invention can significantly improve the printing surface strength and tensile strength of paper while maintaining high bulk, without significantly increasing chemical consumption and reaction steps, overcoming the problem of difficulty in achieving both strength improvement and bulk reduction in traditional modification technologies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of fiber modification technology, and more specifically to a modification method for improving the bonding performance of pulp fibers. Background Technology

[0002] my country possesses abundant lignocellulosic biomass resources, generating approximately 924 million tons of forest residue annually. Utilizing forest residue for pulping and papermaking is a key to ensuring the security of fiber raw material supply and is of great significance for promoting rural revitalization and the circular economy.

[0003] The existing chemimechanical pulp made from forest residues has poor fiber bonding strength, making it unsuitable for large-scale production of high-strength packaging paper. Therefore, there is an urgent need to develop surface functional modification technologies to enhance pulp fiber quality. Selecting appropriate chemical modification methods to structurally modify pulp fibers is an effective way to improve their reactivity and functionalization. For example, reactions such as oxidation, esterification, etherification, and graft polymerization can introduce new functional groups onto the fiber surface, thereby improving the fiber's mechanical properties and cross-linking ability. However, existing modification methods based on cellulose components typically suffer from high chemical and energy consumption, difficulty in reusing modifiers and solvents, and significant pollution emissions. Furthermore, because the fiber surface of chemimechanical pulp is largely covered by lignin, the accessibility of hydroxyl groups is much lower than that of cellulose-based chemical pulps. Therefore, activation modification of the lignin components in pulp fibers has become an effective means to improve fiber bonding performance. Summary of the Invention

[0004] In order to overcome the above-mentioned shortcomings of the existing technology, the purpose of this invention is to provide a modification method to improve the binding performance of pulp fibers, so as to solve the problem that existing pulp fiber modification methods mostly act on cellulose components alone, which not only have high energy consumption and pollution, but also have difficulty in taking into account the low accessibility of hydroxyl groups caused by lignin coverage in chemimechanical pulp.

[0005] The technical solution of this invention to solve the above-mentioned technical problems is as follows: A modification method for improving the bonding performance of pulp fibers is provided, comprising the following steps: (1) Preparation of hydroxymethylated solution: Formaldehyde solution and hydrobromic acid solution are added to lithium bromide solution to prepare hydroxymethylated solution; (2) Hydroxymethylation of pulp fibers: Add block pulp fibers to the hydroxymethylation solution in step (1), and then stir and react at 70-100℃ for 1-3 hours to obtain hydroxymethylated pulp fibers. (3) Cationic modification: After drying the hydroxymethylated pulp fiber from step (2), a solvent is added to it and stirred at 30-50℃ for 30-60 min; then a modifier is added to the obtained product, the pH value is adjusted to 11-13, and finally the reaction is carried out at 70-100℃ for 5-8 h to obtain cationic pulp. (4) Preparation of pulp fibers combining hydroxyl-rich treatment and cationic modification: The cationic pulp from step (3) is filtered and washed to obtain pulp fibers combining hydroxyl-rich treatment and cationic modification.

[0006] Furthermore, in step (1), the mass fraction of formaldehyde solution is 0.3-0.5 wt%; the mass fraction of hydrobromic acid solution is 0.3-0.5 wt%; and the mass fraction of lithium bromide solution is 40-60 wt%.

[0007] Furthermore, in step (3), the solvent is a mixture of isopropanol and water.

[0008] Furthermore, the mass ratio of isopropanol to water is 1:1-3.

[0009] Furthermore, in step (3), the modifier is 3-chloro-2-hydroxypropyltrimethoxyammonium chloride, 2,3-epoxypropyltrimethylammonium chloride, or acrylamide quaternary ammonium salt.

[0010] Furthermore, acrylamide quaternary ammonium salts use propylene groups as the polymerizable active groups.

[0011] Furthermore, in step (3), the mass ratio of hydroxymethylated pulp fiber, solvent and modifier is 0.5-1:2-3:2-3.

[0012] The present invention has the following beneficial effects: (1) Compared with traditional methods for chemical modification of pulp fibers, this invention is the first to introduce formaldehyde into an acidic catalytic system in a one-step process to achieve synergistic modification of residual lignin in pulp by demethylation and hydroxymethylation. Specifically, the demethylation reaction converts the methoxy group (-OCH3) in lignin into a phenolic hydroxyl group (-OH), significantly increasing the active sites in the system; the hydroxymethylation reaction introduces a hydroxymethyl (-CH2OH) group onto the aromatic ring of lignin. The synergistic effect of both not only improves the reactivity of lignin but also enhances the hydrogen bonding and cross-linking ability between fibers. Therefore, this invention uses a one-step method to demethylate and hydroxymethylate pulp fibers, obtaining pulp fibers with a higher content of active groups by controlling the chemical structure of lignin, thereby achieving improved printing surface strength while maintaining high bulk. Compared with existing technologies, this method significantly simplifies the process flow, saves time and labor costs, and improves the bonding performance of pulp fibers without significantly reducing fiber yield, thus overcoming the shortcomings of high energy consumption, high pollution, and insufficient fiber strength in existing technologies.

[0013] (2) This invention develops an acidic molten salt hydrate system to achieve hydroxymethylation and demethylation modification of lignin molecules in pulp fibers in a one-step process: on the one hand, new hydroxymethyl groups are introduced on the fiber surface, and on the other hand, methyl groups in lignin are selectively removed, exposing more phenolic and aliphatic hydroxyl groups, thereby increasing the overall hydroxyl content of pulp fibers. Based on this, this invention further cationically modifies the modified pulp to enhance the bonding force between fibers. This method can significantly improve the printing surface strength and tensile strength of paper while maintaining high bulk, without significantly increasing chemical consumption and reaction steps, overcoming the problem that it is difficult to achieve both strength improvement and bulk reduction in traditional modification technologies.

[0014] (3) The modification method of the present invention can also effectively improve the chemical uniformity and reaction consistency of the fiber surface, improve the quality of the fiber bonding interface inside the paper, further prevent mechanical failure caused by insufficient bonding force between fibers, and thus improve the tensile strength of the paper. The content of phenolic hydroxyl groups in pulp fibers treated with hydroxyl-rich treatment and cationic modification increased by 30-50%, while the normal bulk of paper made from pulp fibers not treated with hydroxyl-rich treatment and cationic modification ranged from 2.3 to 3.3 cm. 3 The tensile strength ranges from 13 to 17 N·m / g. The modified pulp fiber bulk is increased by 10-30%, and the tensile strength is increased by 10-30%. Attached Figure Description

[0015] Figure 1 This is a schematic diagram of the lignin modification method in pulp fibers according to the present invention; Figure 2 The graph shows the performance test results of pulp fibers with different modification methods. Detailed Implementation

[0016] The examples given below are for illustrative purposes only and are not intended to limit the scope of the invention. Unless otherwise specified, conditions in the examples are performed under standard conditions or as recommended by the manufacturer. Reagents or instruments whose manufacturers are not specified are all commercially available products.

[0017] This invention provides a method for enhancing the binding properties of pulp fibers by combining hydroxylation treatment with cationic modification. Unlike traditional methods that only employ demethylation or hydroxymethylation, or a two-step process to achieve both sequentially, this invention uses a one-step method, simultaneously demethylating and hydroxymethylating lignin molecules (see...). Figure 1 ).

[0018] Example 1: A modification method for improving the bonding properties of pulp fibers includes the following steps: (1) Preparation of lithium bromide solution: Add 6.3g of lithium bromide and 11.7g of deionized water to a round-bottom flask, stir in an oil bath to obtain a 35wt% lithium bromide solution; (2) Preparation of hydroxymethylated solution: Add 0.3 mL of formaldehyde solution (0.4 wt%) and 0.1 mL of hydrobromic acid solution (0.5 wt%) to the 35 wt% lithium bromide solution in step (1) to prepare hydroxymethylated solution; (3) Hydroxymethylation of pulp fibers: Add block pulp fibers to the hydroxymethylation solution in step (2), and then stir and react for 3 hours in an oil bath at 90°C and 500 rpm to obtain hydroxymethylated pulp fibers. (4) Cationic modification: After drying the hydroxymethylated pulp fiber from step (3), add isopropanol / water mixed solvent (the mass ratio of isopropanol to water is 1:1) to it and stir at 30°C for 30 min to fully disperse it; then add 3-chloro-2-hydroxypropyltrimethoxyammonium chloride to the obtained product, adjust the pH value to 11 with 20wt% NaOH, and react at 90°C for 5 h to obtain cationic pulp; wherein, the mass ratio of hydroxymethylated pulp fiber (dry weight), isopropanol / water mixed solvent and 3-chloro-2-hydroxypropyltrimethoxyammonium chloride is 1:3:3; (5) Preparation of pulp fiber combining hydroxylation treatment and cationic modification: The product obtained in step (4) is filtered and washed to remove residues and obtained.

[0019] Example 2: A modification method for improving the bonding properties of pulp fibers includes the following steps: (1) Preparation of lithium bromide solution: Add 6.1g of lithium bromide and 6.1g of deionized water to a round bottom flask, stir in an oil bath to obtain a 50wt% lithium bromide solution; (2) Preparation of hydroxymethylated solution: Add 0.3 mL of formaldehyde solution (0.5 wt%) and 0.05 mL of hydrobromic acid solution (0.3 wt%) to the 50 wt% lithium bromide solution in step (1) to prepare hydroxymethylated solution; (3) Hydroxymethylation of pulp fibers: Add block pulp fibers to the hydroxymethylation solution in step (2), and then stir and react for 3 hours in an oil bath at 70°C and 400 rpm to obtain hydroxymethylated pulp fibers. (4) Cationic modification: After drying the hydroxymethylated pulp fiber from step (3), add isopropanol / water mixed solvent (the mass ratio of isopropanol to water is 1:1) and stir at 40°C for 40 min to fully disperse it; then add 3-chloro-2-hydroxypropyltrimethoxyammonium chloride to the obtained product, adjust the pH value to 12 with 20wt% NaOH, and react at 70°C for 8 h to obtain cationic pulp; wherein, the mass ratio of hydroxymethylated pulp fiber (dry weight), isopropanol / water mixed solvent and 3-chloro-2-hydroxypropyltrimethoxyammonium chloride is 1:3:3; (5) Preparation of pulp fiber combining hydroxylation treatment and cationic modification: The product obtained in step (4) is filtered and washed to remove residues and obtained.

[0020] Example 3: A modification method for improving the bonding properties of pulp fibers includes the following steps: (1) Preparation of lithium bromide solution: 63g of lithium bromide and 117g of deionized water were placed in a round-bottom flask and stirred in an oil bath to obtain a 35wt% lithium bromide solution. (2) Preparation of hydroxymethylated solution: Add 0.3 mL of formaldehyde solution (0.5 wt%) and 0.05 mL of hydrobromic acid solution (0.3 wt%) to the 35 wt% lithium bromide solution in step (1) to prepare hydroxymethylated solution; (3) Hydroxymethylation of pulp fibers: block pulp fibers are added to the hydroxymethylation solution in step (2), and then stirred and reacted in an oil bath at 80°C and 600 rpm for 2 hours to obtain hydroxymethylated pulp fibers. (4) Cationic modification: After drying the hydroxymethylated pulp fiber from step (3), add isopropanol / water mixed solvent (the mass ratio of isopropanol to water is 1:1) to it and stir at 50°C for 60 min to fully disperse it; then add 3-chloro-2-hydroxypropyltrimethoxyammonium chloride to the obtained product, adjust the pH value to 13 with 20wt% NaOH, and react at 80°C for 7 h to obtain cationic pulp; wherein, the mass ratio of hydroxymethylated pulp fiber (dry weight), isopropanol / water mixed solvent and 3-chloro-2-hydroxypropyltrimethoxyammonium chloride is 1:3:3; (5) Preparation of pulp fiber combining hydroxylation treatment and cationic modification: The product obtained in step (4) is filtered and washed to remove residues and obtained.

[0021] Comparative Example 1: A modification method for improving the binding properties of pulp fibers (demethylation only) includes the following steps: (1) Preparation of lithium bromide solution: 6.3g of lithium bromide and 11.7g of deionized water are placed in a round-bottom flask and stirred in an oil bath until the lithium bromide is completely dissolved to obtain a 35wt% lithium bromide solution. (2) Preparation of demethylation solution: Add 0.1 mL of hydrobromic acid solution (0.5 wt%) to the 35 wt% lithium bromide solution in step (1) to prepare the demethylation solution; (3) Demethylation of pulp fibers: The block pulp fibers are added to the demethylation solution in step (2), and then stirred in an oil bath at 90°C and 500 rpm for 3 hours to obtain demethylated pulp fibers.

[0022] Comparative Example 2: A modification method for improving the binding properties of pulp fibers (hydroxymethylation only) includes the following steps: (1) Preparation of hydroxymethylation solution: Add 15 mL of 37 wt% formaldehyde solution and 5 mL of hydrobromic acid (0.5 wt%) to a round-bottom flask and stir in an oil bath; (2) Hydroxymethylation of pulp fibers: The block pulp fibers are added to the hydroxymethylation solution in step (1), and then stirred and reacted for 3 hours in an oil bath at 90°C and 500 rpm to obtain hydroxymethylated pulp fibers. (3) The product obtained in step (2) is filtered and washed to remove residues and obtain the product.

[0023] Comparative Example 3: A modification method for improving the binding properties of pulp fibers (cationization only) includes the following steps: adding block pulp fibers to an isopropanol / water mixed solvent (the mass ratio of isopropanol to water is 1:1), stirring at 30°C for 30 min to ensure thorough dispersion; then adding 3-chloro-2-hydroxypropyltrimethoxyammonium chloride, adjusting the pH to 11-12 with 20wt% NaOH, reacting at 90°C for 5 h, and filtering and washing the resulting product to remove residues to obtain cationized pulp; wherein the mass ratio of pulp fibers (octane-dry weight), isopropanol / water mixed solvent, and 3-chloro-2-hydroxypropyltrimethoxyammonium chloride is 1:3:3.

[0024] Test Example: Performance Testing The following performance tests were performed on the unmodified pulp fibers, the pulp fibers of Examples 1-3 that combined hydroxylation treatment and cationic modification, and the modified pulp fibers of Comparative Examples 1-3: (1) Measurement of phenolic hydroxyl groups: 10 mg of unmodified pulp fiber, hydroxylated and cationic modified pulp fiber from Examples 1-3, and modified pulp fiber from Comparative Examples 1-3 were weighed, dried, and ground. Then, 10 mL of distilled water was added to prepare pulp. In order to allow the Folin-Ciocalteu reagent to react better with the phenolic hydroxyl groups in the lignin of the pulp sample, the above pulp was placed in a refrigerator at 4°C for 1 hour to allow it to fully absorb water and swell. Then, 5 mL of Folin-Ciocalteu reagent was added, and after mixing evenly, 15 mL of 20 wt% Na2CO3 solution was added between 120 min to bring the total volume to 50 mL. The reaction was stirred for 2 hours, and then centrifuged to separate the supernatant. The absorbance at 760 nm was measured using a sample with a phenol concentration of 0 as a blank. The measured absorbance was compared with the concentration-absorbance value standard curve to obtain the content of phenolic hydroxyl groups in different pulp samples.

[0025] (2) Measurement of total hydroxyl content: Unmodified pulp fibers, pulp fibers of Examples 1-3 with hydroxyl-enriched treatment and cationic modification, and modified pulp fibers of Comparative Examples 1-3 were freeze-dried. 30 mg of oven-dried pulp fibers were added to 1 mL of 60 wt% LiBr / DMSO solution and stirred at 60 °C until a homogeneous system was formed. 400 μL of sample solution was fully dissolved in a 500 μL mixed solution of deuterated pyridine and deuterated chloroform (1.6:1 v / v). 100 μL of cyclohexanol (10.85 mg / mL) was used as an internal standard. Then, 100 μL of trivalent chromium acetylacetone was added as a relaxant (5 mg / mL) (both the internal standard and relaxant were prepared from the above mixed solvent). Finally, 100 μL of phosphorylation reagent TMDP100 was added and reacted for 15 min before measurement. The quantitative P-spectrum operation used inversion gating decoupling technology, with a pulse angle of 30°, a pulse time of 4 s, a relaxation time of 10 s, and 256 scans.

[0026] (3) Measurement of bulk: Unmodified pulp fibers, hydroxylated and cationic modified pulp fibers of Examples 1-3, and modified pulp fibers of Comparative Examples 1-3 were respectively written onto laboratory hand-made sheets with uniform basis weight. The thickness gauge was used to lift the measuring head and place a single sample in it, and then slowly lowered it to make contact with the paper sample. The reading was taken after the pointer stabilized. Three points were measured at different positions for each sample and the average value was taken. The result was calculated using the formula "bulk = thickness (μm) ÷ basis weight (g / m²)".

[0027] (4) Measurement of tensile strength: Using a special cutter, cut the unmodified pulp fibers, the hydroxylated and cationic modified pulp fibers of Examples 1-3, and the modified pulp fibers of Comparative Examples 1-3 into strips of standard size (e.g., 15 mm wide). Clamp both ends of the strips with clamps to prevent slippage. Start the instrument and stretch at a specified constant speed until it breaks, and record the maximum force it can withstand.

[0028] Depend on Figure 2 It can be seen that, compared with unmodified pulp fiber, the modified pulp fiber prepared in Example 1 has a 30% higher phenolic hydroxyl content, resulting in a 15% increase in bulk and a 21% increase in tensile strength after papermaking. The modified pulp fiber prepared in Example 2 has a 35% higher phenolic hydroxyl content, resulting in a 17% increase in bulk and a 16% increase in tensile strength after papermaking. The modified pulp fiber prepared in Example 3 has a 25% higher phenolic hydroxyl content, resulting in a 22% increase in bulk and a 17% increase in tensile strength after papermaking. Compared with the pulp fiber of Comparative Example 1, the modified pulp fiber prepared in Example 1 has a 17% higher phenolic hydroxyl content and a 31% higher total hydroxyl content, resulting in a 19% increase in bulk and a 14% increase in tensile strength after papermaking. Compared with the pulp fiber of Comparative Example 2, the modified pulp fiber prepared in Example 1 had a 27% higher phenolic hydroxyl content and a 22% higher total hydroxyl content. After being made into paper, the bulk was increased by 18% and the tensile strength was increased by 17%. Compared with the pulp fiber of Comparative Example 3, the modified pulp fiber prepared in Example 1 had a 34% higher phenolic hydroxyl content and a 42% higher total hydroxyl content. After being made into paper, the bulk was increased by 9% and the tensile strength was increased by 10%.

[0029] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A modification method for improving the bonding properties of pulp fibers, characterized in that, Includes the following steps: (1) Preparation of hydroxymethylated solution: Formaldehyde solution and hydrobromic acid solution are added to lithium bromide solution to prepare hydroxymethylated solution; (2) Hydroxymethylation of pulp fibers: Add block pulp fibers to the hydroxymethylation solution in step (1), and then stir and react at 70-100℃ for 1-3 hours to obtain hydroxymethylated pulp fibers. (3) Cationic modification: After drying the hydroxymethylated pulp fiber from step (2), a solvent is added to it and stirred at 30-50℃ for 30-60 min; then a modifier is added to the obtained product, the pH value is adjusted to 11-13, and finally the reaction is carried out at 70-100℃ for 5-8 h to obtain cationic pulp. (4) Preparation of pulp fibers combining hydroxyl-rich treatment and cationic modification: The cationic pulp from step (3) is filtered and washed to obtain pulp fibers combining hydroxyl-rich treatment and cationic modification.

2. The modification method according to claim 1, characterized in that, The formaldehyde solution in step (1) has a mass fraction of 0.3-0.5 wt%; the hydrobromic acid solution has a mass fraction of 0.3-0.5 wt%; and the lithium bromide solution has a mass fraction of 40-60 wt%.

3. The modification method according to claim 1, characterized in that, The solvent mentioned in step (3) is a mixture of isopropanol and water.

4. The modification method according to claim 3, characterized in that, The mass ratio of isopropanol to water is 1:1-3.

5. The modification method according to claim 1, characterized in that, The modifier mentioned in step (3) is 3-chloro-2-hydroxypropyltrimethoxyammonium chloride, 2,3-epoxypropyltrimethylammonium chloride or acrylamide quaternary ammonium salt.

6. The modification method according to claim 5, characterized in that, The acrylamide quaternary ammonium salt uses a propylene group as the polymerizable active group.

7. The modification method according to claim 1, characterized in that, The mass ratio of the hydroxymethylated pulp fiber, solvent and modifier in step (3) is 0.5-1:2-3:2-3.