A super absorbent fluffy pulp and its preparation method
By constructing a multi-scale fiber network in fluff pulp and refining the structure using micron-sized and submicron-sized cellulose fibers, the problem of balancing the liquid absorption and dry bulk properties of fluff pulp is solved, achieving a significant improvement in both water absorption and dry bulk, while avoiding fiber brittleness and dust issues.
Patent Information
- Application Number
- CN202611602482.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to improve the liquid absorption and liquid retention capacity of fluff pulp while maintaining its fluffy state. Chemical oxidation and cross-linking modification leads to increased fiber brittleness and dust, while physical additive modification offers limited improvement. Raw material pretreatment fails to simultaneously improve water absorption.
A multi-scale fiber network is constructed using micron-scale and submicron-scale refined cellulose fibers. Fiber connections are enhanced through localized peeling structures and physical overlap nodes. Combined with freeze-drying and dispersing processes, a porous structure is formed to improve liquid absorption and fluffiness.
It achieves a synergistic improvement in the liquid absorption and dry bulk properties of fluff pulp, increasing water absorption by 15%~40% and dry bulk by 3%~24%, while avoiding increased fiber brittleness and dust.
Smart Images

Figure CN123108979A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of cellulose liquid-absorbing materials technology, and relates to a superabsorbent fluff pulp and its preparation method. Background Technology
[0002] Fluff pulp is a liquid-absorbing material mainly composed of natural cellulose fibers. Due to its good softness, high liquid absorption performance, and porous structure formed after fiber decomposition, it is widely used in hygiene products, medical care products, and other fields. As absorbent products develop towards lightweight, high absorbency, and rapid liquid absorption, higher requirements are placed on the liquid absorption performance, dry bulk, and liquid retention capacity of fluff pulp.
[0003] Currently, commercially available fluff pulp primarily achieves its liquid absorption function by mechanically debonding to form a fluffy fiber network. Since mechanical debonding mainly alters the degree of fiber separation and arrangement, it has limited ability to adjust the fiber morphology and pore size. The resulting fluff pulp is still dominated by long fibers and larger inter-fiber pores, with fewer fine-scale fiber structures and corresponding capillary pores. Therefore, while maintaining the original fluffy state, simply using mechanical debonding makes it difficult to further improve the capillary liquid absorption and liquid retention capacity of the fluff pulp.
[0004] Existing methods for improving the liquid absorption performance of fluff pulp mainly include chemical oxidative crosslinking modification, the addition of physical auxiliaries such as bulking agents / unbonding agents, and raw material pretreatment and fiber screening. However, these technical routes generally suffer from the technical bottleneck of being unable to simultaneously achieve both "liquid absorption performance" and "fluffy structure," specifically manifested in the following three typical dilemmas:
[0005] (1) Chemical oxidation and crosslinking modification route: It can improve water absorption and dry bulk, but excessive oxidation can easily lead to increased dust, and excessive crosslinking is not conducive to bulk and liquid conductivity, and may increase fiber brittleness.
[0006] Chemical oxidation crosslinking is a common method to improve the liquid absorption properties of fluff pulp. For example, patent application CN117286739A uses a method of sodium periodate oxidation combined with glutaraldehyde crosslinking to treat softwood pulp boards. The dry bulk of the fluff pulp obtained in Examples 1-3 of this patent is 25.20-25.84 cm. 3The water absorption rate is 11.52~11.69 g / g. The patent also points out that excessively high sodium periodate concentrations reduce the hydroxyl content on the fiber surface and increase dust after dissociation; excessive glutaraldehyde addition increases the number of crosslinking points between fibers and reduces pore size, which is detrimental to improving dry bulk and liquid conductivity; excessively long crosslinking time may also increase fiber brittleness. Therefore, the effect of this type of oxidation combined with crosslinking modification is affected by both the degree of oxidation and the degree of crosslinking, requiring precise control of the dosage of oxidant and crosslinking agent, as well as the reaction conditions. Excessive crosslinking not only leads to a decrease in dry bulk but also causes problems such as increased dust and increased fiber brittleness.
[0007] (2) Physical additive modification route: can improve dry bulk and liquid absorption performance, but the overall improvement is limited.
[0008] Adding physical additives such as leavening agents and unbonding agents is another mainstream approach to improving the dry bulk of fluff pulp. Patent application CN113789680A discloses a method for mixing bamboo pulp fibers with wood pulp fibers and then treating the mixture with unbonding agents and leavening agents. The fluff pulp obtained in Examples 1-9 of this patent application has a dry bulk of 18.02-19.62 cm⁻¹. 3 / g, water absorption is 8.52~9.12g / g; in Example 12 without added debonding agents and leavening agents, the dry bulkiness is 17.21cm. 3 The absorbance was 7.58 g / g, indicating that the addition of debonding agents and bulking agents can improve the dry bulk and liquid absorption properties of fluff pulp. However, the addition of debonding agents may affect the liquid absorption and matting strength of fluff pulp by weakening the hydrogen bonds between fibers. Therefore, it is necessary to use debonding agents and bulking agents in combination to adjust the properties of fluff pulp. This type of method mainly relies on the adsorption or penetration of auxiliaries on the fiber surface to change the bonding state between fibers. Its treatment effect is related to the type, amount and ratio of auxiliaries, and the improvement of liquid absorption performance by relying solely on physical auxiliaries is limited.
[0009] (3) Raw material pretreatment and fiber screening route: can obtain higher dry bulk, but water absorption is not improved simultaneously.
[0010] Raw material pretreatment and fiber screening are existing technical approaches for regulating the properties of fluff pulp. The literature (Research on the process of preparing *Bambusa textilis* fluff pulp by mild alkali pretreatment [J]. China Pulping, 2022, 41(4):22-29.) uses *Bambusa textilis* as raw material. Based on sulfate pulping, mild alkali pretreatment and grading screening are used to remove some hemicellulose, ash, and impurities, and long fibers are selected to prepare fluff pulp. The dry bulk of the obtained *Bambusa textilis* fluff pulp is 24.62 cm. 3 / g, higher than the 21.98cm of the control product fluff pulp. 3 / g; however, its water absorption is 13.15g / g, lower than the 14.70g / g of the comparative commercial fluff pulp. It can be seen that raw material pretreatment and long fiber screening can obtain fluff pulp with higher dry bulk, but the water absorption has not been increased accordingly.
[0011] The aforementioned technologies can improve the liquid absorption and dry fluffiness of fluff pulp to some extent, but the treatment effect is affected by factors such as the degree of reaction, the ratio of additives, the characteristics of raw materials, and pulping conditions. There is still room for further improvement in the synergistic regulation of these two aspects. Therefore, developing a superabsorbent and fluffy fluff pulp with both good liquid absorption and dry fluffiness properties, and its preparation method, is of practical significance. Summary of the Invention
[0012] The purpose of this invention is to solve the problems existing in the prior art and to provide a super absorbent fluffy pulp and its preparation method.
[0013] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0014] A superabsorbent and fluffy fluff pulp includes a fluff pulp matrix and a cellulose-modified component dispersed in the fluff pulp matrix;
[0015] The fluff pulp matrix is a fluffy fiber network formed by long fluff pulp fibers;
[0016] Cellulose-modified components include micron-sized cellulose fibers and submicron-sized refined cellulose structures;
[0017] Micron-sized cellulose fibers have localized delamination structures on their surface or edges; localized delamination structures include regions where the fiber surface layer is partially raised, delaminated, or separated from the fiber body.
[0018] Submicron-scale cellulose refinement structures include fibrous refinement structures and fragmented refinement structures;
[0019] Micron-sized cellulose fibers are dispersed in a fluffy fiber network. The micron-sized cellulose fibers are in contact with at least one of the following: fluff pulp long fibers and other micron-sized cellulose fibers, forming physical overlap nodes. Submicron-sized cellulose refined structures fill local areas of the interfiber pores and are in contact with adjacent fibers that form the interfiber pores. The interfiber pores include at least one of the following: pores formed between fluff pulp long fibers, between micron-sized cellulose fibers, and between fluff pulp long fibers and micron-sized cellulose fibers.
[0020] The aforementioned fiber structures collectively form a multi-scale, fluffy fiber network with long fibers of fluff pulp as the main skeleton, micron-sized cellulose fibers as overlapping units, and submicron-sized refined cellulose structures as local connecting units.
[0021] The superabsorbent and fluffy pulp of this invention possesses both excellent liquid absorption and dry fluffiness properties because the pulp matrix is a fluffy fiber network formed by long fibers. The interlaced long fibers of the pulp constitute a dry support skeleton and form relatively large inter-fiber pores with a certain degree of connectivity. These pores facilitate rapid liquid entry and diffusion and provide space for liquid storage. The loose arrangement of the long fibers of the pulp keeps the pulp at a low bulk density, forming the structural basis for its liquid absorption and dry fluffiness properties.
[0022] The cellulose-modified components include micron-sized cellulose fibers and submicron-sized refined cellulose structures. The micron-sized cellulose fibers are dispersed within a loose fiber network. These fibers contact each other with long fibers from the fluff pulp and at least one other micron-sized cellulose fiber, forming physical overlap nodes. This increases the connection points and geometric constraints between fibers, reducing relative slippage. During drying, the contacting fiber surfaces approach each other, facilitating hydrogen bond formation and further securing the physical overlap nodes, thereby improving the dry structural stability of the loose fiber network.
[0023] Micron-sized cellulose fibers have localized peeling structures on their surface or edges. Because the peeling occurs locally, the micron-sized cellulose fibers still retain the fiber body that can play a supporting role. The localized peeling structure increases the roughness of the fiber surface and the contact area, providing more contact sites for the formation of physical overlap nodes between the micron-sized cellulose fibers and the long fibers of fluff pulp, as well as for the attachment of the submicron-sized cellulose refinement structure. At the same time, it increases the chance of liquid contact with the cellulose surface.
[0024] Submicron-scale cellulose refinement structures include fibrous refinement structures and fragmented refinement structures. Fiber-like refinement structures extend along the fiber surface or bridge adjacent fibers, while fragmented refinement structures adhere to the fiber surface or interfiber pores. When submicron-scale cellulose refinement structures fill localized areas of interfiber pores, they can contact or form bridges with adjacent fibers, thereby increasing the contact area between fibers, strengthening local connections, and reducing relative slippage between fibers, which helps maintain the dry-state structural stability of the loose fiber network. When submicron-scale cellulose refinement structures occupy localized spaces within pores, they can also form smaller capillary pores with surrounding fibers, thereby enhancing local capillary attraction and facilitating liquid absorption and retention.
[0025] When the submicron-scale cellulose refinement structure is located in the pores between long fibers of fluff pulp and contacts adjacent long fibers of fluff pulp, it can help stabilize the original fiber connection of the fluff pulp matrix; when the submicron-scale cellulose refinement structure is located in the pores between micron-scale cellulose fibers and contacts adjacent micron-scale cellulose fibers, it can strengthen the internal connection of the cellulose modified component; when the submicron-scale cellulose refinement structure is located in the pores between long fibers of fluff pulp and micron-scale cellulose fibers and contacts both, it can enhance the interfacial bonding between the cellulose modified component and the fluff pulp matrix.
[0026] Because the submicron-scale cellulose refinement structure only fills localized areas of the inter-fiber pores, the larger unfilled pores in the fluffy fiber network can still be used for rapid liquid entry and storage, while the locally formed smaller capillary pores facilitate capillary diffusion and retention of the liquid. Simultaneously, the physical overlap nodes and the bridging structure formed by the submicron-scale cellulose refinement structure reduce fiber slippage and pore shrinkage in the dry state. Therefore, this fluff pulp retains a large liquid absorption space and a fluffy skeleton while forming smaller capillary pores that facilitate liquid diffusion and retention, thus achieving a balance between liquid absorption performance and dry fluffiness.
[0027] As a preferred technical solution:
[0028] As described above, the superabsorbent fluff pulp has a mass ratio of fluff pulp matrix to cellulose-modified component of 10~20:1. Within this ratio range, the cellulose-modified component can be uniformly dispersed in the fluff pulp matrix, and the product's liquid absorption performance and dry fluffiness performance can be stably maintained. By adjusting this mass ratio, the product's liquid absorption rate and saturation capacity can be flexibly adjusted to meet different application requirements.
[0029] The superabsorbent and fluffy pulp described above has the following characteristics: the average diameter of the long fibers is 32.1~32.3μm, and the average length is 2.23~2.32mm; the average diameter of the micron-sized cellulose fibers is 25~35μm, and the average length is 235~285μm; the average diameter of the fibrous refined structure is 0.1~1μm, and the average length is 10~15μm; and the average projected length of the fragmented refined structure is 0.5~1μm, and the average projected width is 0.1~0.7μm.
[0030] As described above, the super absorbent and fluffy fluff pulp has an average dry loft of 16-20 cm. 3 The water absorption rate is 3%~24% higher than that of fluff pulp matrix, and the average water absorption is 14~17g / g, which is 15%~40% higher than that of fluff pulp matrix.
[0031] The average dry bulk and average water absorption were obtained by averaging the dry bulk and water absorption of three samples tested according to GB / T 21331-2021 standard. This results in good universality and repeatability: under different proportions of cellulose modification components and different fiber sizes and morphological parameters, the product performance consistently falls within the above range, without exhibiting polarization phenomena such as increased water absorption but a sharp drop in dry bulk, or high dry bulk but low water absorption. Using untreated fluff pulp matrix as a control, some samples showed an increase in water absorption of 15% to 40%, while maintaining or slightly improving dry bulk; for example, a dry bulk of 19.72 cm⁻¹. 3 The sample with a density of / g had a water absorption of 16.54g / g and a dry loft of 17.91cm. 3 The sample had a water absorption of 15.16 g / g and a dry loft of 18.04 cm. 3 The sample with a dry bulk density of / g had a water absorption capacity of 14.37g / g. From the above performance data on dry bulk density and water absorption capacity, it can be seen that this product has excellent liquid absorption capacity and the ability to maintain its bulky structure, with both aspects achieving a synergistic improvement.
[0032] This invention also provides a method for preparing a superabsorbent fluff pulp as described in any of the preceding claims. The method involves preparing a fluff pulp matrix and a cellulose-modified component, wet mixing the two, and then sequentially freeze-drying and dispersing the mixture to obtain the superabsorbent fluff pulp. The wet mixing is used to ensure the cellulose-modified component is fully dispersed in the fluff pulp matrix. Freeze-drying is used to reduce the shrinkage and collapse of the fiber network during the drying process. Before freeze-drying, the material needs to be pre-frozen to prevent the material from boiling over and causing structural collapse. Dispersing is used to dissociate the freeze-dried aggregates and form a fluffy fiber network.
[0033] As a preferred technical solution:
[0034] The preparation process of the cellulose modified component as described above is as follows: cellulose raw material is added to an organic acid solution, and a hydrolysis reaction is carried out at a preset hydrolysis temperature. After the preset hydrolysis time is reached, sufficient hot water is added to the reaction system to terminate the hydrolysis reaction. The mixture is then vacuum filtered while hot to obtain a water-containing filter cake. The cake is then centrifuged and washed to remove residual organic acid and water-soluble hydrolysis products. The washed precipitate is then redispersed in deionized water, mechanically decomposed, and freeze-dried to obtain the cellulose modified component. The concentration of the organic acid solution is 40~70wt%, the preset hydrolysis temperature is 80~110℃, and the preset hydrolysis time is 50~90min. By adjusting the above hydrolysis process parameters, the degree of hydrolysis can be controlled, thereby regulating the size and morphology of the fiber. The preset hydrolysis time is a suitable reaction termination window, which can form a multi-scale refined morphology on the cellulose surface while retaining the fiber body that can play a supporting role, ensuring the skeletal support performance of the modified component.
[0035] like Figure 11 As shown, organic acids exhibit both acid hydrolysis and esterification effects on cellulose. The reactive hydroxyl groups on the cellulose molecular chain undergo esterification with the carboxyl groups of organic acids such as oxalic acid and maleic acid, introducing carboxyl groups into the fiber structure, thereby altering the chemical properties of the fiber surface and enhancing its hydrophilicity. Simultaneously, under hydrolysis intensities of 40–70 wt%, 80–110 °C, and 50–90 min, the hydrogen ions generated by the dissociation of organic acids can catalyze the partial hydrolysis of β-1,4-glycosidic bonds in the cellulose molecular chain, exacerbating the breakage of the cellulose molecular chain and weakening the fiber wall structure.
[0036] Because cellulose fibers have a non-uniform structure, hydrolysis preferentially occurs on the fiber surface, in structural defects, and in relatively disordered and easily accessible areas, while hydrolysis is slower in the relatively ordered and tightly bound areas inside the fiber. Therefore, some of the fiber bulk is preserved, forming micron-sized cellulose fibers; the weak areas on the fiber surface and inside the fiber wall are weakened, creating conditions for subsequent mechanical decomposition.
[0037] After the preset hydrolysis time is reached, sufficient hot water is added to dilute the organic acid and inhibit further hydrolysis. Using hot water to terminate the reaction maintains the system temperature, preventing the organic acid from crystallizing due to temperature decrease and ensuring a uniform dispersion of the hydrolysis products, facilitating subsequent hot vacuum filtration and washing. Residual organic acid and water-soluble hydrolysis products are then removed by hot vacuum filtration and centrifugal washing. When the washed precipitate is redispersed and mechanically dispersed, the weakened fiber surface layer, fiber wall layer, and fine fiber bundles peel, dissociate, or partially break, forming fibrous and fragmented refined structures, respectively.
[0038] Freeze-drying reduces the shrinkage and re-aggregation of refined structures during the drying process, which is beneficial for preserving the multi-scale morphology formed after mechanical dissociation. Therefore, the combined effects of partial hydrolysis of organic acids, subsequent mechanical dissociation, and freeze-drying result in cellulose-modified components that simultaneously include micron-sized cellulose fibers and submicron-sized refined cellulose structures.
[0039] The organic acids used in this preparation process can be recycled and reused, which helps to reduce raw material costs and waste emissions.
[0040] As described above, the cellulose raw material is coniferous fiber pulp (IP pulp derived from southern slash pine of the United States); the organic acid solution is maleic acid solution or oxalic acid solution.
[0041] Cellulose-modified components can be prepared using coniferous fluff pulp, which is the same type as fluff pulp matrix. There is no need to introduce exogenous materials. The two have the same chemical composition, good interfacial bonding and uniform dispersion, which can avoid the compatibility problems common to the addition of exogenous modifiers. Using maleic acid or oxalic acid as hydrolysis reagents, stable cellulose-modified components and final products can be obtained.
[0042] In the method described above, the mass ratio of cellulose raw material to organic acid solution is 1:20~100;
[0043] The hydrolysis reaction is accompanied by stirring at a speed of 150~350 rpm. Stirring can ensure that the cellulose raw material and the organic acid solution are in full contact, thus ensuring that the hydrolysis reaction proceeds uniformly.
[0044] The hot water is deionized water at 70~90℃, and the mass of the hot water is 1~2 times the mass of the reaction system. This temperature range can ensure that the organic acid remains in a dissolved state. Combined with the hot vacuum filtration operation, it can prevent the organic acid from crystallizing and precipitating at low temperature. Adding hot water can dilute the concentration of organic acid and terminate the hydrolysis reaction.
[0045] Centrifugal washing involves dispersing the aqueous filter cake in deionized water, centrifuging at 2500~4000×g for 5~15min, discarding the supernatant and collecting the precipitate, repeating 5~8 times. Here, "×g" is the relative centrifugal force / RCF. This centrifugation parameter can effectively separate and remove residual organic acids and water-soluble hydrolysis products to obtain the target multi-scale cellulose modified component.
[0046] Mechanical dissolution involves mechanically stirring at a speed of 150-300 rpm for 20-30 minutes. This stirring parameter ensures that the precipitate is fully dispersed in deionized water to form a uniform suspension, thus guaranteeing the effectiveness of mechanical dissolution.
[0047] As described above, the preparation process of the fluff pulp matrix is as follows: the cellulose pulp board is dry-dispersed to obtain the fluff pulp matrix. The dry dispersing can be carried out using a nail-type disperser to disperse the pulp board into a fluffy fibrous state.
[0048] The wet mixing process described above is as follows: deionized water is added to the fluff pulp matrix for pre-wetting, and the mass of the deionized water is 8 to 15 times the mass of the fluff pulp matrix. Then, cellulose-modified components are added and mixed evenly.
[0049] The amount of water in the fluff pulp matrix is not enough to achieve uniform dispersion of the cellulose-modified components in the fluff pulp matrix. Therefore, a small amount of deionized water needs to be added to promote the uniform dispersion of the dry powdered cellulose-modified components in the fluff pulp matrix and to achieve structural fixation through the interaction between cellulose hydroxyl groups during the subsequent drying process.
[0050] Beneficial effects:
[0051] (1) The present invention disperses cellulose modified components containing micron-sized cellulose fibers and submicron-sized cellulose refined structures in the fluffy fiber network of the fluff pulp matrix to construct a multi-scale synergistic fiber network structure. While retaining a large liquid absorption space and fluffy support skeleton, it forms capillary pores that facilitate liquid diffusion and retention, thereby achieving a synergistic improvement in liquid absorption performance and dry fluffy performance.
[0052] (2) The present invention uses cellulose raw materials to prepare cellulose modified components, which have the same chemical composition as the fluff pulp matrix, good interfacial bonding and uniform dispersion. No external modifier is required, which avoids the problems of increased fiber brittleness and increased dust caused by chemical oxidation crosslinking modification, as well as the problem of poor compatibility caused by external physical additives.
[0053] (3) The present invention can flexibly adjust the liquid absorption rate and saturation capacity of the product by adjusting the addition ratio and structural parameters of the cellulose modified component, adapt to different application requirements, and the product performance has good universality and repeatability. Attached Figure Description
[0054] Figure 1 The image shows the scanning electron microscope (SEM) morphology (163×) of the cellulose-modified component in Example 1.
[0055] Figure 2 The image shows the scanning electron microscope (SEM) morphology (1360×) of the cellulose-modified component in Example 1.
[0056] Figure 3 The image shows the scanning electron microscope (SEM) morphology of the cellulose-modified component in Example 4 (218×).
[0057] Figure 4 The image shows the scanning electron microscope (SEM) morphology (3970×) of the cellulose-modified component in Example 4.
[0058] Figure 5 The scanning electron microscope (SEM) image (2000×) of the fluff pulp matrix in Example 3 is shown.
[0059] Figure 6 This is a scanning electron microscope (SEM) image (200×) of the fluff pulp matrix in Example 3.
[0060] Figure 7 The image shows the scanning electron microscope (5000×) morphology of the cellulose-modified component in Example 1.
[0061] Figure 8 The image shows the scanning electron microscope (SEM) morphology (250×) of the cellulose-modified component in Example 1.
[0062] Figure 9 The scanning electron microscope (SEM) image (200×) of the superabsorbent fluff pulp in Example 1.
[0063] Figure 10 The scanning electron microscope (SEM) image (2500×) of the superabsorbent fluff pulp in Example 1.
[0064] Figure 11 This is a schematic diagram of the esterification reaction mechanism between organic acids and cellulose.
[0065] Figure 12 A schematic diagram of the structure of superabsorbent fluff pulp;
[0066] Among them, 1-fluff pulp matrix, 2-cellulose modified component, 21-micron-sized cellulose fibers, 211-partially peeled structure, 22-submicron-sized refined cellulose structure, 221-fibrous refined structure, 222-fragmented refined structure, 3-physical overlapping node, 4-interfiber pores. Detailed Implementation
[0067] The present invention will be further described below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.
[0068] Unless otherwise specified, the solvent for the solutions mentioned below is water.
[0069] In the following text, the dimensional parameters of the superabsorbent fluff pulp are all average values. The microscopic morphology images of the samples from different fields of view were collected using a scanning electron microscope. For the long fibers and micron-sized cellulose fibers of the fluff pulp, 50 fibers were randomly selected for diameter and length measurement, for the fibrous refined structure, 50 fibers were randomly selected, and for the fragmented refined structure, 100 fibers were randomly selected for size measurement. The arithmetic mean was obtained by statistical calculation.
[0070] The embodiments of this invention disclose specific manufacturers and brand information of the relevant substances. This content is only intended to fully disclose the technical solution, enabling those skilled in the art to understand, reproduce, and verify the technical effects of this invention. It is an exemplary description of the implementation methods and not a limitation on the scope of protection of this invention. Those skilled in the art should understand that, without departing from the core technical concept and substantive technical solution of this invention, similar equivalent raw materials produced by other manufacturers can be used to implement this invention. Such equivalent substitutions and conventional modifications all fall within the scope of protection of this invention, and the protection boundary of this invention should not be limited based on the specific manufacturers and brand information recorded in the embodiments.
[0071] The parameter ranges and material selections described in this invention are effective implementation ranges derived from extensive preliminary variable screening experiments. The following embodiments do not exhaustively list all feasible material ratios and process parameter combinations; only representative formulation systems and process conditions are selected for effect verification. This design is not intended to limit the scope of protection of this invention. Those skilled in the art can adjust any parameter based on the parameter ranges defined in this invention to achieve stable preparation of superabsorbent and fluffy pulp, and these adjustments do not exceed the scope of protection defined by the claims of this invention.
[0072] Example 1
[0073] A method for preparing superabsorbent and fluffy pulp, the specific steps of which are as follows:
[0074] (1) Preparation of main materials;
[0075] Cellulose pulp board: Softwood pulp board, manufactured by International Paper, brand name SuperSoft®;
[0076] Cellulose raw material: pine fiber pulp board, manufactured by International Paper, brand name SuperSoft®;
[0077] Organic acid solution: maleic acid solution, concentration 60 wt%;
[0078] Hot water: 80℃ deionized water;
[0079] (2) Preparation of fluff pulp matrix and cellulose-modified components;
[0080] The preparation process of the fluff pulp matrix is as follows: the cellulose pulp board is dry-dispersed to obtain the fluff pulp matrix; the dispersing speed is 8000 rpm and the dispersing time is 40 s;
[0081] The preparation process of the cellulose-modified component is as follows: cellulose raw material is added to an organic acid solution and hydrolyzed at 100℃ with stirring at 200 rpm. After 60 min, hot water is added to the reaction system to terminate the hydrolysis reaction. The mixture is then vacuum filtered while hot to obtain a water-containing filter cake. The water-containing filter cake is dispersed in deionized water and centrifuged at 3500×g for 10 min. The supernatant is discarded and the precipitate is collected. This process is repeated 6 times to remove residual organic acid and water-soluble hydrolysis products. The washed precipitate is then redispersed in deionized water and mechanically stirred at 150 rpm for 20 min before freeze-drying to obtain the cellulose-modified component. The mass ratio of cellulose raw material to organic acid solution is 1:57.14, and the mass of hot water is 1.47 times the mass of the reaction system.
[0082] (3) Preparation of superabsorbent fluff pulp;
[0083] Deionized water was added to the fluff pulp matrix for pre-wetting, followed by the addition of cellulose-modified components and thorough mixing. The mixture was then freeze-dried and dispersed sequentially to obtain superabsorbent and fluffy fluff pulp. The mass of deionized water was 10 times the mass of the fluff pulp matrix, and the mass ratio of the fluff pulp matrix to the cellulose-modified components was 10:1. The freeze-drying temperature was -83℃, and the time was 40 hours. The dispersion speed was 8000 rpm, and the dispersion time was 30 seconds.
[0084] like Figures 1-2 , Figures 7-10 as well as Figure 12 As shown, the final superabsorbent fluff pulp consists of a fluff pulp matrix 1 and a cellulose-modified component 2 dispersed in the fluff pulp matrix 1. The fluff pulp matrix 1 is a fluffy fiber network formed by long fluff pulp fibers. The cellulose-modified component 2 consists of micron-sized cellulose fibers 21 and submicron-sized cellulose refinement structures 22. The surface or edge of the micron-sized cellulose fibers 21 has a local peeling structure 211, which is a region where the fiber surface is locally raised, layered, or partially separated from the fiber body. The submicron-sized cellulose refinement structure 22 consists of fibrous refinement structures. The structure consists of 221 and fragmented refined structure 222. Micron-sized cellulose fibers 21 are dispersed in a fluffy fiber network. Micron-sized cellulose fibers 21 are in contact with at least one of fluff pulp long fibers and other micron-sized cellulose fibers and form physical overlap nodes 3. Submicron-sized refined cellulose structures 22 fill local areas of interfiber pores 4 and are in contact with adjacent fibers forming interfiber pores 4. Interfiber pores 4 are at least one of the pores formed between fluff pulp long fibers, between micron-sized cellulose fibers 21, and between fluff pulp long fibers and micron-sized cellulose fibers 21.
[0085] The average diameter of the fluff pulp long fibers is 32.16 μm and the average length is 2.3 mm; the average diameter of the micron-sized cellulose fibers 21 is 27.46 μm and the average length is 243.66 μm; the average diameter of the fibrous refined structure 221 is 0.66 μm and the average length is 13.75 μm; the average projected length of the fragmented refined structure 222 is 0.88 μm and the average projected width is 0.54 μm.
[0086] The average dry loft of the superabsorbent and fluffy wool pulp is 19.72 cm. 3 / g, which is 23.8% higher than fluff pulp matrix 1, and the average water absorption is 16.54g / g, which is 34.91% higher than fluff pulp matrix 1.
[0087] Example 2
[0088] A method for preparing superabsorbent and fluffy pulp, the specific steps of which are as follows:
[0089] (1) Preparation of main materials;
[0090] Cellulose pulp board: Softwood pulp board, manufactured by International Paper, brand name SuperSoft®;
[0091] Cellulose raw material: pine fiber pulp board, manufactured by International Paper, brand name SuperSoft®;
[0092] Organic acid solution: maleic acid solution, concentration 60 wt%;
[0093] Hot water: 80℃ deionized water;
[0094] (2) Preparation of fluff pulp matrix and cellulose-modified components;
[0095] The preparation process of the fluff pulp matrix is as follows: the cellulose pulp board is dry-dispersed to obtain the fluff pulp matrix; the dispersing speed is 8000 rpm and the dispersing time is 40 s;
[0096] The preparation process of the cellulose-modified component is as follows: cellulose raw material is added to an organic acid solution and hydrolyzed at 100℃ with stirring at 200 rpm. After 60 min, hot water is added to the reaction system to terminate the hydrolysis reaction. The mixture is then vacuum filtered while hot to obtain a water-containing filter cake. The water-containing filter cake is dispersed in deionized water and centrifuged at 3500×g for 10 min. The supernatant is discarded and the precipitate is collected. This process is repeated 6 times to remove residual organic acid and water-soluble hydrolysis products. The washed precipitate is then redispersed in deionized water and mechanically stirred at 150 rpm for 20 min before freeze-drying to obtain the cellulose-modified component. The mass ratio of cellulose raw material to organic acid solution is 1:57.14, and the mass of hot water is 1.47 times the mass of the reaction system.
[0097] (3) Preparation of superabsorbent fluff pulp;
[0098] Deionized water was added to the fluff pulp matrix for pre-wetting, followed by the addition of cellulose-modified components and thorough mixing. The mixture was then freeze-dried and dispersed sequentially to obtain superabsorbent and fluffy fluff pulp. The mass of deionized water was 8 times the mass of the fluff pulp matrix, and the mass ratio of the fluff pulp matrix to the cellulose-modified components was 20:1. The freeze-drying temperature was -83.5℃, and the time was 36 hours. The dispersion speed was 8000 rpm, and the dispersion time was 20 seconds.
[0099] The final superabsorbent fluff pulp consists of a fluff pulp matrix and a cellulose-modified component dispersed in the fluff pulp matrix. The fluff pulp matrix is a fluffy fiber network formed by long fluff pulp fibers. The cellulose-modified component consists of micron-sized cellulose fibers and submicron-sized cellulose refined structures. The surface or edge of the micron-sized cellulose fibers has a local peeling structure, which is a region where the fiber surface is locally raised, layered, or partially separated from the fiber body. The submicron-sized cellulose refined structure consists of fibrous refined structures and fragmented refined structures. The micron-sized cellulose fibers are dispersed in the fluffy fiber network. The micron-sized cellulose fibers are in contact with at least one of the long fluff pulp fibers and other micron-sized cellulose fibers and form physical overlap nodes. The submicron-sized cellulose refined structures fill the local area of the interfiber pores and are in contact with adjacent fibers that form the interfiber pores. The interfiber pores are at least one of the pores formed between long fluff pulp fibers, between micron-sized cellulose fibers, and between long fluff pulp fibers and micron-sized cellulose fibers.
[0100] The average diameter of the fluff pulp long fibers was 32.17 μm and the average length was 2.29 mm; the average diameter of the micron-sized cellulose fibers was 27.46 μm and the average length was 243.66 μm; the average diameter of the fibrous refined structure was 0.66 μm and the average length was 13.75 μm; and the average projected length of the fragmented refined structure was 0.88 μm and the average projected width was 0.54 μm.
[0101] The average dry loft of the superabsorbent and fluffy wool pulp is 16.53 cm. 3 / g, which is 3.77% higher than that of fluff pulp matrix, and the average water absorption is 15.13g / g, which is 23.41% higher than that of fluff pulp matrix.
[0102] Example 3
[0103] A method for preparing superabsorbent and fluffy pulp, the specific steps of which are as follows:
[0104] (1) Preparation of main materials;
[0105] Cellulose pulp board: Softwood pulp board, manufactured by International Paper, brand name SuperSoft®;
[0106] Cellulose raw material: pine fiber pulp board, manufactured by International Paper, brand name SuperSoft®;
[0107] Organic acid solution: maleic acid solution, concentration 50 wt%;
[0108] Hot water: 80℃ deionized water;
[0109] (2) Preparation of fluff pulp matrix and cellulose-modified components;
[0110] The preparation process of the fluff pulp matrix is as follows: the cellulose pulp board is dry-dispersed to obtain the fluff pulp matrix; the dispersing speed is 8000 rpm and the dispersing time is 40 s;
[0111] The preparation process of the cellulose-modified component is as follows: cellulose raw material is added to an organic acid solution and hydrolyzed at 100℃ with stirring at 180 rpm. After 60 min, hot water is added to the reaction system to terminate the hydrolysis reaction. The mixture is then vacuum filtered while hot to obtain a water-containing filter cake. The water-containing filter cake is dispersed in deionized water and centrifuged at 3500×g for 10 min. The supernatant is discarded and the precipitate is collected. This process is repeated 5 times to remove residual organic acid and water-soluble hydrolysis products. The washed precipitate is then redispersed in deionized water and mechanically stirred at 200 rpm for 25 min before freeze-drying to obtain the cellulose-modified component. The mass ratio of cellulose raw material to organic acid solution is 1:60, and the mass of hot water is 1.63 times the mass of the reaction system.
[0112] (3) Preparation of superabsorbent fluff pulp;
[0113] Deionized water was added to the fluff pulp matrix for pre-wetting, followed by the addition of cellulose-modified components and thorough mixing. The mixture was then freeze-dried and dispersed sequentially to obtain superabsorbent and fluffy fluff pulp. The mass of deionized water was 15 times the mass of the fluff pulp matrix, and the mass ratio of the fluff pulp matrix to the cellulose-modified components was 10:1. The freeze-drying temperature was -85℃, and the time was 48 hours. The dispersion speed was 8000 rpm, and the dispersion time was 30 seconds.
[0114] The final superabsorbent fluff pulp consists of a fluff pulp matrix (scanning electron microscopy morphology as shown in the figure). Figure 5 and Figure 6The matrix consists of a fluff pulp matrix (as shown) and a cellulose-modified component dispersed in the fluff pulp matrix. The fluff pulp matrix is a fluff pulp long fiber network. The cellulose-modified component consists of micron-sized cellulose fibers and submicron-sized cellulose refined structures. The surface or edge of the micron-sized cellulose fibers has a local peeling structure, which is a region where the fiber surface is locally raised, layered, or partially separated from the fiber body. The submicron-sized cellulose refined structure consists of fibrous refined structures and fragmented refined structures. The micron-sized cellulose fibers are dispersed in the fluff pulp matrix. The micron-sized cellulose fibers are in contact with at least one of the fluff pulp long fibers and other micron-sized cellulose fibers and form physical overlap nodes. The submicron-sized cellulose refined structures fill the local area of the interfiber pores and are in contact with adjacent fibers that form the interfiber pores. The interfiber pores are at least one of the pores formed between fluff pulp long fibers, between micron-sized cellulose fibers, and between fluff pulp long fibers and micron-sized cellulose fibers.
[0115] The average diameter of the fluff pulp long fibers was 32.14 μm and the average length was 2.26 mm; the average diameter of the micron-sized cellulose fibers was 31.66 μm and the average length was 278.99 μm; the average diameter of the fibrous refined structure was 0.84 μm and the average length was 14.6 μm; and the average projected length of the fragmented refined structure was 0.94 μm and the average projected width was 0.67 μm.
[0116] The average dry loft of the superabsorbent and fluffy wool pulp is 19.1 cm. 3 / g, which is 19.9% higher than that of fluff pulp matrix, and the average water absorption is 14.91g / g, which is 21.62% higher than that of fluff pulp matrix.
[0117] Example 4
[0118] A method for preparing superabsorbent and fluffy pulp, the specific steps of which are as follows:
[0119] (1) Preparation of main materials;
[0120] Cellulose pulp board: Softwood pulp board, manufactured by International Paper, brand name SuperSoft®;
[0121] Cellulose raw material: pine fiber pulp board, manufactured by International Paper, brand name SuperSoft®;
[0122] Organic acid solution: oxalic acid solution, concentration 60 wt%;
[0123] Hot water: 80℃ deionized water;
[0124] (2) Preparation of fluff pulp matrix and cellulose-modified components;
[0125] The preparation process of the fluff pulp matrix is as follows: the cellulose pulp board is dry-dispersed to obtain the fluff pulp matrix; the dispersing speed is 8000 rpm and the dispersing time is 40 s;
[0126] The preparation process of the cellulose-modified component is as follows: cellulose raw material is added to an organic acid solution and hydrolyzed at 100℃ with stirring at 300 rpm. After 60 min, hot water is added to the reaction system to terminate the hydrolysis reaction. The mixture is then vacuum filtered while hot to obtain a water-containing filter cake. The water-containing filter cake is dispersed in deionized water and centrifuged at 3500×g for 10 min. The supernatant is discarded and the precipitate is collected. This process is repeated 8 times to remove residual organic acid and water-soluble hydrolysis products. The washed precipitate is then redispersed in deionized water and mechanically stirred at 150 rpm for 20 min before freeze-drying to obtain the cellulose-modified component. The mass ratio of cellulose raw material to organic acid solution is 1:50, and the mass of hot water is 1.18 times the mass of the reaction system.
[0127] (3) Preparation of superabsorbent fluff pulp;
[0128] Deionized water was added to the fluff pulp matrix for pre-wetting, followed by the addition of cellulose-modified components and thorough mixing. The mixture was then freeze-dried and dispersed sequentially to obtain superabsorbent and fluffy fluff pulp. The mass of deionized water was 10 times the mass of the fluff pulp matrix, and the mass ratio of the fluff pulp matrix to the cellulose-modified components was 10:1. The freeze-drying temperature was -83.1℃, and the time was 40 hours. The dispersion speed was 8000 rpm, and the dispersion time was 30 seconds.
[0129] The final superabsorbent and fluffy fluff pulp consists of a fluff pulp matrix and a cellulose-modified component dispersed in the fluff pulp matrix (scanning electron microscopy morphology as shown in figure). Figure 3 and Figure 4The structure (as shown) comprises a fluff pulp matrix consisting of a fluff pulp long fiber network, a cellulose-modified component consisting of micron-sized cellulose fibers and submicron-sized cellulose refined structures, wherein the surface or edge of the micron-sized cellulose fibers has a local peeling structure, which is a region where the fiber surface is partially raised, layered, or partially separated from the fiber body, and the submicron-sized cellulose refined structure consists of fibrous refined structures and fragmented refined structures. The micron-sized cellulose fibers are dispersed in the fluff pulp long fibers and at least one of other micron-sized cellulose fibers, and form physical overlap nodes. The submicron-sized cellulose refined structures fill the local area of the interfiber pores and contact the adjacent fibers that form the interfiber pores. The interfiber pores are at least one of the pores formed between fluff pulp long fibers, between micron-sized cellulose fibers, and between fluff pulp long fibers and micron-sized cellulose fibers.
[0130] The average diameter of the fluff pulp long fibers was 32.21 μm and the average length was 2.32 mm; the average diameter of the micron-sized cellulose fibers was 29.68 μm and the average length was 241.7 μm; the average diameter of the fibrous refined structure was 0.53 μm and the average length was 13.4 μm; and the average projected length of the fragmented refined structure was 0.85 μm and the average projected width was 0.41 μm.
[0131] The average dry loft of the superabsorbent and fluffy wool pulp is 17.91 cm. 3 / g, which is 12.43% higher than that of fluff pulp matrix, and the average water absorption is 15.16g / g, which is 23.65% higher than that of fluff pulp matrix.
[0132] Example 5
[0133] A method for preparing superabsorbent and fluffy pulp, the specific steps of which are as follows:
[0134] (1) Preparation of main materials;
[0135] Cellulose pulp board: Softwood pulp board, manufactured by International Paper, brand name SuperSoft®;
[0136] Cellulose raw material: pine fiber pulp board, manufactured by International Paper, brand name SuperSoft®;
[0137] Organic acid solution: oxalic acid solution, concentration 48.4 wt%;
[0138] Hot water: 80℃ deionized water;
[0139] (2) Preparation of fluff pulp matrix and cellulose-modified components;
[0140] The preparation process of the fluff pulp matrix is as follows: the cellulose pulp board is dry-dispersed to obtain the fluff pulp matrix; the dispersing speed is 8000 rpm and the dispersing time is 40 s;
[0141] The preparation process of the cellulose-modified component is as follows: cellulose raw material is added to an organic acid solution and hydrolyzed at 100℃ with stirring at 150 rpm. After 60 min, hot water is added to the reaction system to terminate the hydrolysis reaction. The mixture is then vacuum filtered while hot to obtain a water-containing filter cake. The water-containing filter cake is dispersed in deionized water and centrifuged at 3500×g for 10 min. The supernatant is discarded and the precipitate is collected. This process is repeated 7 times to remove residual organic acid and water-soluble hydrolysis products. The washed precipitate is then redispersed in deionized water and mechanically stirred at 300 rpm for 30 min before freeze-drying to obtain the cellulose-modified component. The mass ratio of cellulose raw material to organic acid solution is 1:62, and the mass of hot water is 1.06 times the mass of the reaction system.
[0142] (3) Preparation of superabsorbent fluff pulp;
[0143] Deionized water was added to the fluff pulp matrix for pre-wetting, followed by the addition of cellulose-modified components and thorough mixing. The mixture was then freeze-dried and dispersed sequentially to obtain superabsorbent and fluffy fluff pulp. The mass of deionized water was 12 times the mass of the fluff pulp matrix, and the mass ratio of the fluff pulp matrix to the cellulose-modified components was 10:1. The freeze-drying temperature was -84.7℃, and the time was 42 hours. The dispersion speed was 8000 rpm, and the dispersion time was 30 seconds.
[0144] The final superabsorbent fluff pulp consists of a fluff pulp matrix and a cellulose-modified component dispersed in the fluff pulp matrix. The fluff pulp matrix is a fluffy fiber network formed by long fluff pulp fibers. The cellulose-modified component consists of micron-sized cellulose fibers and submicron-sized cellulose refined structures. The surface or edge of the micron-sized cellulose fibers has a local peeling structure, which is a region where the fiber surface is locally raised, layered, or partially separated from the fiber body. The submicron-sized cellulose refined structure consists of fibrous refined structures and fragmented refined structures. The micron-sized cellulose fibers are dispersed in the fluffy fiber network. The micron-sized cellulose fibers are in contact with at least one of the long fluff pulp fibers and other micron-sized cellulose fibers and form physical overlap nodes. The submicron-sized cellulose refined structures fill the local area of the interfiber pores and are in contact with adjacent fibers that form the interfiber pores. The interfiber pores are at least one of the pores formed between long fluff pulp fibers, between micron-sized cellulose fibers, and between long fluff pulp fibers and micron-sized cellulose fibers.
[0145] The average diameter of the fluff pulp long fibers is 32.11 μm and the average length is 2.3 mm; the average diameter of the micron-sized cellulose fibers is 30.11 μm and the average length is 270.2 μm; the average diameter of the fibrous refined structure is 0.71 μm and the average length is 14.53 μm; the average projected length of the fragmented refined structure is 0.9 μm and the average projected width is 0.58 μm.
[0146] The average dry loft of the superabsorbent and fluffy wool pulp is 18.04 cm. 3 The average water absorption is 14.37 g / g, which is 13.25% higher than that of fluff pulp matrix, and the average water absorption is 17.21% higher than that of fluff pulp matrix.
Claims
1. A super absorbent and fluffy pulp, characterized in that, It includes a fluff pulp matrix and a cellulose-modified component dispersed in the fluff pulp matrix; The fluff pulp matrix is a fluffy fiber network formed by long fluff pulp fibers; Cellulose-modified components include micron-sized cellulose fibers and submicron-sized refined cellulose structures; Micron-sized cellulose fibers have localized delamination structures on their surface or edges; localized delamination structures include regions where the fiber surface layer is partially raised, delaminated, or separated from the fiber body. Submicron-scale cellulose refinement structures include fibrous refinement structures and fragmented refinement structures; Micron-sized cellulose fibers are dispersed in a fluffy fiber network. The micron-sized cellulose fibers are in contact with each other and form physical overlap nodes with fluff pulp long fibers and other micron-sized cellulose fibers. Submicron-sized cellulose refined structures fill local areas of inter-fiber pores and are in contact with adjacent fibers that form inter-fiber pores. The interfiber pores include at least one of the pores formed between fluff pulp long fibers, between micron-sized cellulose fibers, and between fluff pulp long fibers and micron-sized cellulose fibers.
2. The super absorbent and fluffy pulp according to claim 1, characterized in that, The mass ratio of fluff pulp matrix to cellulose-modified component is 10~20:
1.
3. The super absorbent and fluffy pulp according to claim 1, characterized in that, The average diameter of the long fibers in the fluff pulp is 32.1~32.3μm, and the average length is 2.23~2.32mm; the average diameter of the micron-sized cellulose fibers is 25~35μm, and the average length is 235~285μm; the average diameter of the fibrous refined structure is 0.1~1μm, and the average length is 10~15μm; the average projected length of the fragmented refined structure is 0.5~1μm, and the average projected width is 0.1~0.7μm.
4. The super absorbent and fluffy pulp according to any one of claims 1 to 3, characterized in that, The average dry loft of super absorbent and fluffy fluff pulp is 16~20cm. 3 The water absorption rate is 3%~24% higher than that of fluff pulp matrix, and the average water absorption is 14~17g / g, which is 15%~40% higher than that of fluff pulp matrix.
5. A method for preparing a superabsorbent, fluffy pulp as described in any one of claims 1 to 4, characterized in that, The fluff pulp matrix and cellulose-modified component were prepared separately, and then the two were wet-mixed and freeze-dried and dispersed in sequence to obtain superabsorbent fluff pulp.
6. The method according to claim 5, characterized in that, The preparation process of the cellulose modified component is as follows: cellulose raw material is added to an organic acid solution, and a hydrolysis reaction is carried out at a preset hydrolysis temperature. After the preset hydrolysis time is reached, hot water is added to the reaction system to terminate the hydrolysis reaction. The mixture is then vacuum filtered while hot to obtain a water-containing filter cake. The filter cake is then removed by centrifugation and washing to remove residual organic acid and water-soluble hydrolysis products. The washed precipitate is then redispersed in deionized water, mechanically decomposed, and freeze-dried to obtain the cellulose modified component. The concentration of the organic acid solution is 40~70wt%, the preset hydrolysis temperature is 80~110℃, and the preset hydrolysis time is 50~90min.
7. The method according to claim 6, characterized in that, The cellulose raw material is coniferous fiber pulp; the organic acid solution is maleic acid solution or oxalic acid solution.
8. The method according to claim 6, characterized in that, The mass ratio of cellulose raw material to organic acid solution is 1:20~100; The hydrolysis reaction is accompanied by stirring at a speed of 150~350 rpm; The hot water is deionized water at 70~90℃, and the mass of the hot water is 1~2 times the mass of the reaction system; Centrifugal washing involves dispersing the water-containing filter cake in deionized water, centrifuging at 2500~4000×g for 5~15min, discarding the supernatant and collecting the precipitate, and repeating 5~8 times. Mechanical dissolution involves mechanically stirring at a speed of 150-300 rpm for 20-30 minutes.
9. The method according to claim 5, characterized in that, The preparation process of fluff pulp matrix is as follows: dry breaking up cellulose pulp boards to obtain fluff pulp matrix.
10. The method according to claim 5, characterized in that, The specific process of wet mixing is as follows: deionized water is added to the fluff pulp matrix for pre-wetting, and the mass of the deionized water is 8 to 15 times the mass of the fluff pulp matrix. Then, cellulose modification components are added and mixed evenly.
Citation Information
Patent Citations
Bamboo fiber fluff pulp as well as preparation method and application thereof
CN113789680A
Method for improving absorption performance of fluff pulp
CN117286739A